High-purity vanadium oxide electrode and preparation method thereof
Through a multi-stage deep impurity removal process, high-purity vanadium pentoxide is prepared using activated alumina, modified lignin sulfonate, etc., which solves the problems of incomplete impurity removal and environmental pollution in the existing process, simplifies the process and improves the vanadium recovery rate and electrode performance, making it suitable for lithium battery positive electrode materials.
Patent Information
- Application Number
- CN202511206526.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-27
- Publication Date
- 2025-09-30
- Estimated Expiration
- 2045-08-27
AI Technical Summary
The existing high-purity vanadium pentoxide preparation process does not completely remove impurities, causes serious environmental pollution, and has a complex process flow. The treatment of alkaline vanadium leaching solution has problems with complex impurity forms and the introduction of magnesium impurities, resulting in poor performance of the prepared vanadium oxide electrode.
A multi-stage deep impurity removal process is adopted, using activated alumina adsorption columns, a composite impurity remover with modified lignin sulfonate as the main agent, calcium hydroxide suspension and flocculant, ion exchange columns, etc., combined with a calcination step, to prepare high-purity vanadium pentoxide and high-purity vanadium oxide electrodes.
It achieves efficient and synchronous removal of impurity elements, solves the environmental pollution problem in traditional processes, simplifies the process, improves the vanadium recovery rate and electrode performance, and meets the requirements of lithium battery positive electrode materials.
Smart Images

Figure CN120717510A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of hydrometallurgy, and particularly relates to a high-purity vanadium oxide electrode and a preparation method thereof. Background Art
[0002] Vanadium pentoxide (V2O5) is an electrode material with important applications in electrochemistry. The purity of V2O5 is a key factor affecting its electrode performance. The presence of impurities or insufficient purity can directly affect the electrochemical properties of the electrode (such as specific capacity, cycling stability, and rate capability) by altering the material's crystal structure, electronic conductivity, ion diffusion pathways, and chemical stability.
[0003] Currently, the industrial production of high-purity vanadium pentoxide mainly adopts the ammonium salt precipitation process, which has the following technical bottlenecks: 1. Incomplete impurity removal: Traditional sulfidation methods for removing heavy metals produce toxic H2S gas. The removal efficiency of iron and aluminum impurities by pH adjustment is low (usually only down to 100-200 ppm), and silicon and phosphorus impurities are difficult to remove simultaneously.
[0004] 2. Serious environmental pollution: The existing technology uses sulfuric acid to adjust the pH to 2-3 for impurity removal, which produces a large amount of ammonia-containing wastewater; the use of phosphate precipitants can easily lead to the cyclic accumulation of phosphorus.
[0005] 3. Complex process flow: The "solvent extraction-ion exchange" combined process requires large equipment investment and high organic phase loss; some technologies also require multi-stage calcination (500℃→700℃→900℃) to obtain high-purity products.
[0006] The existing technology for treating alkaline vanadium leachate (mainly NaVO3, pH 9-11) has obvious shortcomings: (1) direct acidification will release a large amount of ammonia; (2) impurities exist in complex forms (Na2SiO3, Na3PO4, etc.); (3) the magnesium salt dephosphorization agent used will introduce new magnesium impurities (residual amount >300ppm).
[0007] In view of this, there is still room for improvement in the process of preparing high-purity vanadium pentoxide using alkaline vanadium leaching solution as raw material and using it as raw material to prepare electrodes. Summary of the Invention
[0008] The main purpose of the present invention is to address the deficiencies in the above-mentioned prior art and provide a method for preparing high-purity vanadium pentoxide using alkaline vanadium leachate as a raw material and using the same as a raw material to prepare high-purity vanadium pentoxide. The present invention aims to solve the problems of incomplete impurity removal, serious environmental pollution, and complex process flow in the existing high-purity vanadium pentoxide preparation process, as well as the deficiencies in the existing alkaline vanadium leachate treatment, which lead to the poor performance of the prepared vanadium oxide electrode.
[0009] In order to achieve the above object, the present invention adopts the following technical solutions: According to a first aspect of the present invention, there is provided a method for preparing a high-purity vanadium oxide electrode, comprising the following steps: S1: pretreating the alkaline vanadium leaching solution using an activated alumina adsorption column to obtain a pretreated solution; S2: adding a composite impurity remover containing modified lignin sulfonate as a main agent to the pretreated liquid for primary impurity removal, and obtaining a primary impurity removal filtrate after solid-liquid separation; S3: adding a calcium hydroxide suspension and a flocculant to the primary impurity removal filtrate to perform secondary impurity removal, and obtaining a secondary impurity removal filtrate after solid-liquid separation; S4: Purifying the secondary impurity-removed filtrate using an ion exchange column to obtain a purified liquid; S5: adding ammonium salt to the purified liquid to precipitate vanadium to obtain ammonium metavanadate crystals; S6: calcining the ammonium metavanadate crystals to obtain high-purity vanadium pentoxide; S7: preparing a high-purity vanadium oxide electrode using the high-purity vanadium pentoxide.
[0010] According to some embodiments of the present invention, step S1 includes: passing the alkaline vanadium leaching solution through an activated alumina adsorption column at a flow rate of 1-5 BV / h and controlling the temperature to 40-60° C. to obtain the pretreatment solution.
[0011] According to some embodiments of the present invention, step S2 includes: adding the composite impurity remover with modified lignin sulfonate as the main agent to the pretreatment liquid, maintaining the pH at 9-10, reacting for 30-90 minutes under stirring conditions, and obtaining the primary impurity removal filtrate after solid-liquid separation.
[0012] According to some embodiments of the present invention, step S3 includes: heating the primary impurity removal filtrate to 60-100° C., adding the calcium hydroxide suspension and the flocculant, aging for 30-60 minutes, and obtaining the secondary impurity removal filtrate after solid-liquid separation.
[0013] According to some embodiments of the present invention, step S4 includes: passing the secondary impurity-removed filtrate through the ion exchange column at a flow rate of 1.5-2 BV / h to obtain the purified liquid.
[0014] According to some embodiments of the present invention, step S5 includes: adjusting the pH of the purified liquid to 8-9, adding the ammonium salt, and crystallizing at 30-90° C. for 1-2 hours to obtain the ammonium metavanadate crystals.
[0015] According to some embodiments of the present invention, step S6 includes: calcining the ammonium metavanadate crystals in stages under an oxygen atmosphere, first raising the temperature to 300°C at 5-10°C / min and keeping the temperature for 0.5-1.5 hours, and then raising the temperature to 550°C at 2-8°C / min and keeping the temperature for 1-3 hours to obtain the high-purity vanadium pentoxide.
[0016] According to some embodiments of the present invention, the main agent of the composite impurity remover is aminopolysaccharide-modified lignin sulfonate, and the composite impurity remover further includes citrate.
[0017] According to some embodiments of the present invention, the added amount of the composite impurity remover is 1.1-1.3 times the molar amount of vanadium in the alkaline vanadium leaching solution.
[0018] According to some embodiments of the present invention, in the composite impurity remover, the mass ratio of lignin sulfonate, citrate, and amino polysaccharide is 5-8:2-1:1.
[0019] According to some embodiments of the present invention, the composite impurity remover is prepared by the following method: lignin sulfonate and amino polysaccharide are mixed in proportion, potassium persulfate solution is added, and oxidation modification is carried out at 60-80°C for 1-3 hours to obtain amino polysaccharide-modified lignin sulfonate; the amino polysaccharide-modified lignin sulfonate is compounded with citrate to obtain the composite impurity remover.
[0020] According to some embodiments of the present invention, the amount of calcium hydroxide suspension added is 2-3 times the molar amount of phosphorus in the alkaline vanadium leachate in terms of calcium molar amount.
[0021] According to some embodiments of the present invention, the flocculant is a polyacrylamide flocculant with a mass fraction of 0.1-0.25%.
[0022] According to some embodiments of the present invention, the amount of ammonium salt added is NH4 + The molar amount is 2-3.5 times the molar amount of vanadium in the alkaline vanadium leaching solution.
[0023] According to a second aspect of the present invention, a high-purity vanadium oxide electrode prepared by the above method is provided.
[0024] By adopting the above technical solution, the present invention has the following beneficial effects: The present invention utilizes alkaline vanadium leachate as raw material, producing high-purity vanadium pentoxide (V2O5 ≥ 99.9%) through a multi-stage deep impurity removal process. High-performance electrodes are then prepared using this high-purity vanadium pentoxide as raw material. Specifically, the present invention pre-treats the alkaline vanadium leachate using an activated alumina adsorption column to remove some silicon impurities and co-adsorbed aluminum. A composite impurity remover based on modified lignin sulfonate is then used for primary impurity removal to remove phosphorus, aluminum, and residual silicon impurities. Secondary impurity removal is then performed using calcium hydroxide and a flocculant to remove some phosphorus, residual silicon, and co-precipitated aluminum impurities. Finally, an ion exchange column is used for deep purification to remove some aluminum and silicon impurities, as well as calcium impurities introduced in the previous step. This results in a highly purified solution. Vanadium is then precipitated from the purified solution, and the resulting ammonium metavanadate crystals are calcined to produce high-purity vanadium pentoxide. The high-purity vanadium oxide electrode prepared using this high-purity vanadium pentoxide has excellent specific capacity, cycle stability and rate performance.
[0025] The solution of the present invention adopts an environmentally friendly impurity removal agent system to achieve efficient and simultaneous removal of impurity elements such as silicon, phosphorus, and aluminum. The impurity content in the final product is Si ≤ 2 ppm, P ≤ 2 ppm, and Al ≤ 2 ppm, while also solving the ammonia nitrogen pollution problem caused by traditional acidic impurity removal processes. The solution of the present invention avoids equipment corrosion and ammonia emissions caused by the use of strong acids and alkalis. The solution of the present invention simplifies the existing high-purity V2O5 production process. Compared with traditional processes, the solution of the present invention increases the vanadium recovery rate by over 98.5% and reduces the cost of impurity removal agents. The V2O5 obtained by the solution of the present invention has a specific surface area of 15-18 m² / g (nitrogen adsorption method) and Na and K contents are both less than 2 ppm, meeting the requirements of positive electrode materials for batteries (e.g., lithium batteries). BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The present invention provides a flow chart of the method for preparing a high-purity vanadium oxide electrode. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0028] As required, specific embodiments of the present invention are disclosed in this specification; however, it should be understood that the disclosed embodiments are merely illustrative of the invention, which may be implemented in various alternative forms. In the following description, various operating parameters and components are described in connection with various contemplated embodiments. These specific parameters and components are provided herein as examples only and are not intended to be limiting.
[0029] The first aspect of the present invention provides a method for preparing a high-purity vanadium oxide electrode, such as Figure 1 As shown, the method includes the following steps: S1: pre-treating alkaline vanadium leaching solution using an activated alumina adsorption column to obtain a pre-treated solution; S2: adding a composite impurity remover with modified lignin sulfonate as a main agent to the pre-treated solution for primary impurity removal, and obtaining a primary impurity removal filtrate after solid-liquid separation; S3: adding a calcium hydroxide suspension and a flocculant to the primary impurity removal filtrate for secondary impurity removal, and obtaining a secondary impurity removal filtrate after solid-liquid separation; S4: purifying the secondary impurity removal filtrate using an ion exchange column to obtain a purified solution; S5: adding ammonium salt to the purified solution to precipitate vanadium to obtain ammonium metavanadate crystals; S6: calcining the ammonium metavanadate crystals to obtain high-purity vanadium pentoxide; S7: preparing a high-purity vanadium oxide electrode using the high-purity vanadium pentoxide.
[0030] The present invention utilizes alkaline vanadium leachate as raw material, producing high-purity vanadium pentoxide through a multi-stage deep impurity removal process. High-performance electrodes are then prepared using this high-purity vanadium pentoxide as raw material. Specifically, the alkaline vanadium leachate is first pretreated using an activated alumina adsorption column to remove some silicon impurities and co-adsorbed aluminum. A composite impurity remover based on modified lignin sulfonate is then used for primary impurity removal to remove phosphorus, aluminum, and residual silicon impurities. Secondary impurity removal is then performed using calcium hydroxide and a flocculant to remove some phosphorus, residual silicon, and co-precipitated aluminum impurities. Finally, an ion exchange column is used for deep purification to remove some aluminum and silicon impurities, as well as calcium impurities introduced in the previous step. This results in a deeply purified solution. Vanadium is then precipitated from the purified solution, and the resulting ammonium metavanadate crystals are calcined to obtain high-purity vanadium pentoxide. High-purity vanadium oxide electrodes prepared using this high-purity vanadium pentoxide exhibit excellent specific capacity, cycle stability, and rate performance.
[0031] The solution of the present invention adopts an environmentally friendly impurity removal agent system, achieving efficient and simultaneous removal of impurity elements such as silicon, phosphorus, and aluminum, while simultaneously solving the ammonia nitrogen pollution problem generated by traditional acidic impurity removal processes. The solution of the present invention avoids equipment corrosion and ammonia emissions caused by the use of strong acids and strong bases. The solution of the present invention simplifies the existing high-purity V2O5 production process. Compared with traditional processes, the method of the present invention has the advantages of high vanadium recovery rate, low impurity removal agent cost, and simple production process.
[0032] In the present invention, an alkaline vanadium leachate refers to an alkaline vanadium-containing solution. The present invention does not specify the composition of the alkaline vanadium leachate. The method of the present invention is suitable for treating alkaline vanadium leachates containing impurity elements such as silicon, phosphorus, and aluminum. In the example described below, the alkaline vanadium leachate contains 20-38 g / L of V, 800-1200 mg / L of Si, 300-500 mg / L of P, and 200-400 mg / L of Al, with a pH of 9-11.
[0033] The solution of the present invention is described in detail below in conjunction with each step.
[0034] In step S1, the alkaline vanadium leachate is pretreated using an activated alumina adsorption column to remove some silicon impurities and co-adsorbed aluminum from the alkaline vanadium leachate. Using an activated alumina adsorption column for silicon removal offers advantages such as high silicon removal efficiency, ease of operation, low cost, and strong adaptability.
[0035] Activated alumina has a high specific surface area and rich mesoporous structure (2-50 nm), which can retain colloidal silica or polysilicic acid in solution through physical adsorption, especially when the silica particle size matches the pore size. At the same time, non-dissociated silicic acid molecules (H4SiO4) can be adsorbed on the alumina surface through van der Waals forces.
[0036] In some embodiments, step S1 includes passing an alkaline vanadium leachate through an activated alumina adsorption column at a flow rate of 1-5 BV / h to obtain a pretreated solution. This flow rate range facilitates the adsorption of silicon by the activated alumina, thereby achieving excellent silicon removal. The flow rate of the alkaline vanadium leachate can typically, but not limited to, be 1 BV / h, 2 BV / h, 3 BV / h, 4 BV / h, or 5 BV / h.
[0037] In some embodiments, in step S1, the temperature is controlled at 40-60°C. This temperature range achieves a good balance between adsorption efficiency and energy consumption. A temperature that is too low will result in a slow adsorption rate, thereby affecting adsorption efficiency. A temperature that is too high will increase energy consumption and may damage the activated alumina structure. The temperature can typically, but not limited to, be set at 40°C, 45°C, 50°C, 55°C, or 60°C. Preferably, the temperature is controlled at 50°C.
[0038] In some embodiments, in step S1, the activated alumina particle size in the activated alumina adsorption column is 1-2 mm.
[0039] In some embodiments, step S1 may remove approximately 40% of the silicon.
[0040] When the activated alumina adsorption column reaches saturation, it can be regenerated to remove adsorbed pollutants, restore its adsorption activity, and enable reuse. The regeneration method for the activated alumina adsorption column is to backwash it with a 5% NaOH solution and then activate it with 3% H2SO4. The regeneration efficiency is >95%.
[0041] In step S2, a composite impurity remover containing a modified lignin sulfonate as a primary agent is added to the pretreatment liquid for primary impurity removal, thereby removing some silicon, phosphorus, and aluminum impurities from the pretreatment liquid. Using a composite impurity remover containing a modified lignin sulfonate as a primary agent to remove some silicon, phosphorus, and aluminum impurities has the advantages of significant impurity removal, wide application range, and environmental friendliness.
[0042] In some embodiments, the main agent of the composite impurity remover is aminopolysaccharide-modified lignin sulfonate, and the composite impurity remover further comprises citrate. In other words, the composite impurity remover is made of lignin sulfonate, citrate and aminopolysaccharide.
[0043] Lignin sulfonate, citrate, and amino polysaccharides can achieve efficient impurity removal through synergistic action. Lignin sulfonate is an anionic surfactant with excellent dispersibility and solubility in water of all hardness levels. Its aqueous solution is chemically stable and biodegradable. It has excellent chelating ability for silicon, phosphorus, and aluminum ions, making it suitable as a chelating agent for removing silicon, phosphorus, and aluminum impurities from solutions. Citrate is a weak acid salt with a chelating effect. It can form stable complexes with metal ions in solution, thereby reducing the metal ion concentration and achieving the purpose of impurity removal. Citrate also has a certain pH-regulating effect, helping to optimize the impurity removal environment. Amino polysaccharides are a class of polysaccharides containing amino groups (-NH2) or amino derivatives (such as acetylamino). They are composed of amino-containing monosaccharides connected by glycosidic bonds. They combine the biocompatibility of polysaccharides with the chemical activity of amino groups. They are natural polymers with excellent adsorption and flocculation properties. They can remove impurities such as silicon, phosphorus, and aluminum from solutions through adsorption and can aggregate impurity particles through flocculation, facilitating separation. The three ingredients work together, combining the chelation of lignin sulfonate, the complexation of citrate, and the adsorption and flocculation of aminopolysaccharides to more comprehensively and efficiently remove various impurities from the solution. Furthermore, since lignin sulfonate and aminopolysaccharides are both natural or naturally derived substances, and citrate is a relatively environmentally friendly reagent, this composite impurity remover is less polluting to the environment than traditional chemical impurity removers.
[0044] The lignin sulfonate may be sodium lignin sulfonate, potassium lignin sulfonate, calcium lignin sulfonate, magnesium lignin sulfonate, ammonium lignin sulfonate, etc., preferably the corresponding sodium salt or potassium salt. The citrate may be trisodium citrate, sodium dihydrogen citrate, potassium dihydrogen citrate, ammonium dihydrogen citrate, disodium hydrogen citrate, etc., preferably the corresponding sodium salt or potassium salt. The amino polysaccharide may be chitosan, chitosan oligosaccharide, etc.
[0045] In some embodiments, the lignin sulfonate is sodium lignin sulfonate, the citrate is trisodium citrate, and the amino polysaccharide is chitosan.
[0046] In some embodiments, the amount of the composite impurity remover added is 1.1-1.3 times the molar amount of vanadium in the alkaline vanadium leachate. Here, "additional amount" refers to the total molar amount of the substances in the composite impurity remover, i.e., the total molar amount of lignin sulfonate, citrate, and aminopolysaccharide. The amount of the composite impurity remover added can typically, but not limited to, be 1.1, 1.2, or 1.3 times the molar amount of vanadium in the alkaline vanadium leachate.
[0047] In some embodiments, the mass ratio of lignin sulfonate, citrate, and amino polysaccharide in the composite impurity remover is 5-8:2-1:1. This ratio helps achieve the best impurity removal effect.
[0048] In some embodiments, a composite impurity remover is prepared by mixing lignin sulfonate and amino polysaccharide in appropriate proportions, adding potassium persulfate solution, and subjecting the mixture to oxidative modification at 60-80°C for 1-3 hours to obtain an amino polysaccharide-modified lignin sulfonate. The amino polysaccharide-modified lignin sulfonate is then compounded with citrate to obtain the composite impurity remover. Potassium persulfate (K2S2O8) primarily acts as a free radical initiator and oxidant, promoting the chemical crosslinking and structural modification of the lignin sulfonate and amino polysaccharide. Thermal decomposition generates free radicals that oxidize the lignin sulfonate and amino polysaccharide, initiating a graft copolymerization reaction. Subsequently, the amino polysaccharide-modified lignin sulfonate and citrate are physically mixed. The reaction temperature can typically, but not limited to, be 60°C, 65°C, 70°C, 75°C, or 80°C, and the reaction time can typically, but not limited to, be 1 hour, 1.5 hours, 2 hours, 2.5 hours, or 3 hours.
[0049] In some embodiments, step S2 comprises: adding a composite impurity remover to the pretreated liquid, maintaining the pH at 9-10, reacting for 30-90 minutes under stirring, and obtaining a primary impurity-removed filtrate after solid-liquid separation. The pH can typically, but not limited to, be adjusted to 9.0, 9.2, 9.4, 9.6, 9.8, or 10, and the reaction time can typically, but not limited to, be set to 30 minutes, 40 minutes, 50 minutes, 60 minutes, 70 minutes, 80 minutes, or 90 minutes.
[0050] For example, in one specific example, sodium lignin sulfonate and chitosan are mixed in appropriate proportions, and then a 0.1 mol / L potassium persulfate solution (20% of the solid mass, calculated as potassium persulfate mass) is added. Oxidative modification is carried out at 60-80°C for 1-3 hours, followed by compounding with trisodium citrate to produce a composite impurity remover. The composite impurity remover is added to the pretreated solution with a stirring rate of 200-500 rpm, maintaining a pH of 9-10. The solution reacts for 30-90 minutes, and is then filtered. The resulting filtrate is the primary impurity removal filtrate.
[0051] In step S3, a calcium hydroxide suspension and a flocculant are added to the primary impurity removal filtrate to perform secondary impurity removal, aiming to remove some phosphorus impurities, residual silicon, and co-precipitated aluminum impurities in the primary impurity removal filtrate. This impurity removal method has the advantages of high impurity removal efficiency, simple operation, and low cost.
[0052] Calcium hydroxide suspension and flocculant achieve deep removal of phosphorus in the primary impurity removal filtrate through the synergistic effect of chemical precipitation and flocculation enhancement. Calcium hydroxide provides an alkaline environment and Ca 2+ , causing phosphorus, silicon, and aluminum to precipitate. Flocculants aggregate these precipitates into large particles, improving solid-liquid separation efficiency. Coprecipitation causes Al(OH)3, CaSiO3, and Ca5(PO4)3OH to interlock, increasing impurity removal efficiency.
[0053] In some embodiments, step S3 comprises: heating the primary impurity removal filtrate to 60-100° C., adding a calcium hydroxide suspension and a flocculant, aging for 30-60 min, and obtaining a secondary impurity removal filtrate after solid-liquid separation. The reaction temperature can typically but not limitedly be set to 60° C., 65° C., 70° C., 75° C., 80° C., 85° C., 90° C., 95° C., or 100° C., and the aging time can typically but not limitedly be set to 30 min, 40 min, 50 min, or 60 min.
[0054] In some embodiments, the amount of calcium hydroxide suspension added is 2-3 times the molar amount of phosphorus in the alkaline vanadium leachate, calculated as calcium molar amount. The amount of calcium hydroxide suspension added can typically, but not limited to, be set to 2 times, 2.5 times, or 3 times the molar amount of phosphorus in the alkaline vanadium leachate.
[0055] In some embodiments, the flocculant is a polyacrylamide flocculant with a mass fraction of 0.1-0.25%.
[0056] For example, in a specific example, the first-stage impurity removal filtrate is heated to 60-100°C, Ca(OH)2 suspension is added to a Ca / P molar ratio of 2-3:1, and 0.1-0.25% polyacrylamide flocculant is added at the same time. After aging for 30-60 minutes, the filtrate is filtered and the resulting filtrate is the second-stage impurity removal filtrate.
[0057] In step S4, the secondary impurity removal filtrate is purified using an ion exchange column to remove some aluminum and silicon impurities, as well as calcium impurities introduced in the previous step. Using an ion exchange column for impurity removal has the advantages of significant impurity removal, environmental friendliness, and low cost.
[0058] In some embodiments, step S4 includes passing the secondary impurity removal filtrate through the ion exchange column at a flow rate of 1.5-2 BV / h. This flow rate range is conducive to obtaining excellent impurity removal effect. The flow rate of the secondary impurity removal filtrate can typically but not limited to be set to 1.5 BV / h, 1.6 BV / h, 1.7 BV / h, 1.8 BV / h, 1.9 BV / h, 2 BV / h.
[0059] In some embodiments, the ion exchange column is an ion exchange column packed with D201 macroporous resin.
[0060] In some embodiments, the ion exchange column has a column height-to-diameter ratio of 5:1.
[0061] In some embodiments, the residual Al in the purified solution is less than 5 mg / L, and the residual Si is less than 5 mg / L.
[0062] In step S5, ammonium salt is added to the purified liquid to precipitate vanadium.
[0063] In some embodiments, step S5 comprises: adjusting the pH of the purified solution to 8-9, adding an ammonium salt, and crystallizing at 30-90° C. for 1-2 hours to obtain ammonium metavanadate crystals. The pH can typically, but not limited to, be adjusted to 8.0, 8.2, 8.4, 8.6, 8.8, or 9.0. The reaction temperature can typically, but not limited to, be set to 30° C., 40° C., 50° C., 60° C., 70° C., 80° C., or 90° C., and the reaction time can typically, but not limited to, be set to 1 hour, 1.5 hours, or 2 hours.
[0064] In some embodiments, the amount of ammonium salt added is NH4 + The molar amount is 2-3.5 times the molar amount of vanadium in the alkaline vanadium leachate. The amount of ammonium salt added can typically, but not limited to, be set to 2 times, 2.5 times, 3 times, or 3.5 times the molar amount of vanadium in the alkaline vanadium leachate.
[0065] In some embodiments, the ammonium salt is ammonium carbonate or ammonium sulfate.
[0066] In step S6, the ammonium metavanadate crystals are calcined to obtain vanadium pentoxide.
[0067] In some embodiments, step S6 comprises: calcining the ammonium metavanadate crystals in an oxygen atmosphere in stages, first heating the temperature to 300° C. at a rate of 5-10° C. / min and holding the temperature for 0.5-1.5 hours, then heating the temperature to 550° C. at a rate of 2-8° C. / min and holding the temperature for 1-3 hours, to obtain high-purity vanadium pentoxide. The first stage heating rate can be typically, but not limited to, 5° C. / min, 6° C. / min, 7° C. / min, 8° C. / min, 9° C. / min, or 10° C. / min, and the first stage holding time can be typically, but not limited to, 0.5 hours, 1 hour, or 1.5 hours. The second stage heating rate can be typically, but not limited to, 2° C. / min, 3° C. / min, 4° C. / min, 5° C. / min, 6° C. / min, 7° C. / min, or 8° C. / min, and the second stage holding time can be typically, but not limited to, 1 hour, 1.5 hours, 2 hours, 2.5 hours, or 3 hours.
[0068] In step S7, a high-purity vanadium oxide electrode is prepared using high-purity vanadium pentoxide. High-purity vanadium pentoxide is a common positive electrode material for batteries (particularly lithium-ion batteries and zinc-ion batteries). High-purity vanadium pentoxide can be mixed with a conductive agent and a binder in a specific mass ratio to form a slurry. This slurry is then composited onto a current collector to form an electrode.
[0069] Specifically, in some embodiments, a high-purity vanadium oxide electrode is prepared by the following steps: 1. Electrode slurry preparation Slowly add the adhesive PVDF (10% wt) to N-methylpyrrolidone (NMP) and magnetically stir until completely dissolved (accelerated in a 50°C water bath). Then, sequentially add the conductive agent (one or both of carbon black and CNTs) and V2O5. Planetary stirring (200-400 rpm, 1-3 hours) is performed, followed by ultrasonic treatment (30 minutes) to eliminate agglomerates. The solids content of the slurry is controlled at 30-40%.
[0070] 2. Current collector processing and coating Current collector preparation: Aluminum foil (lithium battery, thickness 15-20 μm) or carbon-coated aluminum foil (sodium battery), ultrasonically cleaned with acetone / ethanol and dried.
[0071] Coating process: Use an automatic coater or doctor blade to control the wet film thickness to 150-200μm (dry film approximately 50-70μm). Coating speed 10-20 mm / s, and gap height adjusted according to slurry viscosity (usually 100-150μm).
[0072] 3. Drying and compaction Staged drying: let it stand at room temperature for 10-30 minutes to pre-volatilize the solvent, dry it with air at 60-80℃ for 30-60 minutes, and then transfer it to vacuum drying at 120-140℃ for 10-16 hours.
[0073] Roller compaction: Use a double roller machine to compact at a pressure of 5-10 MPa to make the electrode density reach 2.5-3.0 g / cm 3 (Thickness is reduced by 20~30% after compaction).
[0074] A second aspect of the present invention provides a high-purity vanadium oxide electrode prepared by the above method.
[0075] The present invention will be further described below with reference to specific examples, but the present invention is not limited thereto in any way. To avoid redundancy, the methods used are conventional methods unless otherwise specified.
[0076] Example 1 Raw material conditions: alkaline vanadium leaching solution pH = 10.2, containing V 35.6g / L, Si 980mg / L, P 380mg / L, Al 320mg / L, Fe 45mg / L.
[0077] The preparation method of high-purity vanadium oxide electrode comprises the following steps: Step 1: Raw material pretreatment: pass the alkaline vanadium leachate through an activated alumina adsorption column (Φ100×500mm, filled with 1-2mm particle size γ-Al2O3) at a flow rate of 3BV / h, control the temperature at 50±2°C, and detect the Si content in the effluent to be reduced to 602mg / L (removal efficiency 38.6%). Step 2: Primary impurity removal: prepare a composite impurity remover. Mix 50g of sodium lignin sulfonate with 10g of chitosan, add 12mL of 0.1mol / L potassium persulfate solution, modify at 75℃ for 2 hours, add 20g of trisodium citrate to compound, prepare a 10% aqueous solution, add 1.2 times the V molar amount of the composite impurity remover (i.e., 182g / m³ solution), stir at 300rpm, maintain pH = 9.5±0.1, react for 60 minutes, and after plate and frame filtration, measure: Si 48mg / L, P 52mg / L, Al 28mg / L; Step 3: Secondary impurity removal: heat the filtrate to 85°C, add Ca(OH)2 suspension at a ratio of Ca / P=2.5:1, and simultaneously add 0.2% anionic polyacrylamide (molecular weight 8 million). Stir at this temperature for 30 minutes and filter press. The filtrate composition is: P2.9 mg / L, Ca 81 mg / L. Step 4: Deep purification, through a Φ150×750mm D201 resin column (filling height 600mm), controlled flow rate 1.8BV / h, effluent detection: Al 1.8mg / L, Si 2.3mg / L, Ca <0.5mg / L; Step 5: Vanadium precipitation crystallization: adjust the pH to 8.7 with dilute sulfuric acid, add (NH4)2SO4 to NH4⁺ / V = 3:1 (molar ratio), and crystallize at 90°C for 90 minutes to obtain ammonium metavanadate crystals (purity 99.2%). Step 6: Calcination: First, heat the temperature in a muffle furnace to 300°C at 8°C / min and keep it for 1 hour, then heat it to 550°C at 5°C / min and keep it for 2 hours to obtain orange-red V2O5 powder. The test results are: purity: 99.96% (titration method), impurity content (ppm): Si 1.2, P 1.8, Al 1.5, Fe 0.8, specific surface area: 16.7m 2 / g (BET method), vanadium recovery rate: 98.9%; Step 7: Prepare a high-purity vanadium oxide electrode by mixing V2O5 powder with a conductive agent and an adhesive in a certain mass ratio to obtain a slurry, and compound the slurry onto a current collector to obtain a high-purity vanadium oxide electrode.
[0078] Example 2 Raw material conditions: alkaline vanadium leaching solution pH = 9.8, containing V 32.4g / L, Si 1120mg / L, P 460mg / L, Al280mg / L, Fe 35mg / L.
[0079] The preparation method of high-purity vanadium oxide electrode comprises the following steps: Step 1: Raw material pretreatment: pass the alkaline vanadium leaching solution through an activated alumina adsorption column (Φ100×500mm, filled with 1-2mm particle size γ-Al2O3) at a flow rate of 2BV / h, control the temperature at 50±2℃, and the Si content of the effluent is reduced, with a removal rate of 42.1%; Step 2: Primary impurity removal, prepare a composite impurity remover, take 60g sodium lignin sulfonate and 10g chitosan, add 12mL 0.1mol / L potassium persulfate solution, modify at 60℃ for 2 hours, add 15g trisodium citrate to compound, prepare a 10% aqueous solution, add 1.1 times the V molar amount of the composite impurity remover, stir at 350rpm, maintain pH=9.7, react for 60 minutes, and after plate and frame filtration, measure: Si 50mg / L, P 51mg / L, Al 30mg / L; Step 3: Secondary impurity removal: heat the filtrate to 95°C, add Ca(OH)2 suspension at a ratio of Ca / P=2.8:1, and simultaneously add 0.15% anionic polyacrylamide (molecular weight 8 million). Stir at this temperature for 40 minutes and filter press. The filtrate composition is: P 3.2 mg / L, Ca 85 mg / L. Step 4: Deep purification, using a Φ150×750mm D201 resin column (filling height 600mm), controlling the flow rate to 1.6BV / h, and the effluent detection: Al 1.9mg / L, Si 2.1mg / L, Ca <0.5mg / L; Step 5: Precipitate vanadium crystals, adjust the pH to 9 with dilute sulfuric acid, add (NH4)2CO3 to NH4 + / V=2.5:1 (molar ratio), crystallization at 90°C for 60 minutes to obtain ammonium metavanadate crystals (purity 99.91%); Step 6: Calcination: First, heat the temperature to 300°C at 6°C / min and keep it for 1 hour in a muffle furnace, then heat it to 550°C at 6°C / min and keep it for 2 hours to obtain orange-red V2O5 powder. The test results are: purity: 99.94% (titration method), impurity content (ppm): Si 1.2, P 1.6, Al 1.4, Fe 0.9, specific surface area: 16.7m 2 / g (BET method), vanadium recovery rate: 98.5%; Step 7: Prepare a high-purity vanadium oxide electrode by mixing V2O5 powder with a conductive agent and an adhesive in a certain mass ratio to obtain a slurry, and compound the slurry onto a current collector to obtain a high-purity vanadium oxide electrode.
[0080] Example 3 Raw material conditions: alkaline vanadium leaching solution pH = 10.5, containing V 37.4g / L, Si 850mg / L, P 320mg / L, Al 320mg / L, Fe 42mg / L.
[0081] The preparation method of high-purity vanadium oxide electrode comprises the following steps: Step 1: Raw material pretreatment: pass the alkaline vanadium leaching solution through an activated alumina adsorption column (Φ100×500mm, filled with 1-2mm particle size γ-Al2O3) at a flow rate of 3BV / h, control the temperature at 50±2℃, and the Si content in the effluent is reduced, with a removal rate of 41.2%; Step 2: Primary impurity removal, prepare a composite impurity remover, take 70g sodium lignin sulfonate and 10g chitosan, add 12mL 0.1mol / L potassium persulfate solution, modify at 80℃ for 2 hours, add 20g trisodium citrate to compound, prepare a 10% aqueous solution, add 1.1 times the V molar amount of the composite impurity remover, stir at 350rpm, maintain pH=9.5, react for 60 minutes, and after plate and frame filtration, measure: Si 45mg / L, P 56mg / L, Al 33mg / L; Step 3: Secondary impurity removal: heat the filtrate to 80°C, add Ca(OH)2 suspension at a ratio of Ca / P=2.4:1, and simultaneously add 0.2% anionic polyacrylamide (molecular weight 8 million). Stir at this temperature for 40 minutes and filter press. The filtrate composition: P 3mg / L, Ca 88mg / L. Step 4: Deep purification, through a Φ150×750mm D201 resin column (filling height 600mm), controlled flow rate 1.6BV / h, effluent detection: Al 1.8mg / L, Si 2mg / L, Ca <0.5mg / L; Step 5: Precipitate vanadium crystals, adjust the pH to 9 with dilute sulfuric acid, add (NH4)2CO3 to NH4 + / V=2.8:1 (molar ratio), crystallization at 90°C for 60 minutes to obtain ammonium metavanadate crystals; Step 6: Calcination: First, heat the temperature in a muffle furnace to 300°C at 7°C / min and keep it for 1 hour, then heat it to 550°C at 5°C / min and keep it for 1 hour to obtain orange-red V2O5 powder. The test results are: purity: 99.95% (titration method), impurity content (ppm): Si 1.21, P 1.5, Al 1.6, Fe 0.9, specific surface area: 15.8m 2 / g (BET method), vanadium recovery rate: 98.9%; Step 7: Prepare a high-purity vanadium oxide electrode by mixing V2O5 powder with a conductive agent and an adhesive in a certain mass ratio to obtain a slurry, and compound the slurry onto a current collector to obtain a high-purity vanadium oxide electrode.
[0082] Batteries were assembled using the high-purity vanadium oxide electrodes prepared in the above examples and their performance was tested. For example, button-type cells were assembled in an argon glove box (H₂O / O₂ concentration <0.1 ppm): The positive electrode consisted of the V₂O₅ electrode sheet prepared in the above examples; the negative electrode consisted of a lithium sheet (counter electrode) or a sodium sheet; the separator consisted of Celgard 2400; and the electrolyte consisted of 1M LiPF₆ dissolved in EC / DMC (1:1 volume ratio) or 1M NaPF₆ dissolved in EC / DEC. Testing demonstrated that the discharge capacity of the cells reached 250-280 mAh / g in the first cycle at 0.2C (1C = 294 mA / g), with a capacity retention of ≥80% after 100 cycles (carbon composites will be required for performance optimization).
[0083] In summary, the solution of the present invention can (1) simultaneously and efficiently remove silicon, phosphorus, and aluminum in the alkaline system; (2) avoid equipment corrosion and ammonia emissions caused by the use of strong acids and strong bases; and (3) simplify the existing high-purity V2O5 production process. Specifically, compared with the existing technology, the following beneficial effects can be achieved: 1. Significantly improved impurity removal efficiency: the impurity content in the final product is Si≤2ppm, P≤2ppm, Al≤2ppm (ICP-MS detection); 2. Environmentally friendly: the pH of the whole process is maintained at 8-10, ammonia volatilization is reduced by more than 85%, and the total nitrogen in the wastewater is <50mg / L; 3. Improved economic benefits: compared with the traditional process, the vanadium recovery rate is increased by more than 98.5%, and the cost of the impurity remover is reduced; 4. Excellent product performance: the specific surface area of the obtained V2O5 is 15-18m 2 / g (nitrogen adsorption method), with Na and K contents both below 2ppm, meeting the requirements for positive electrode materials for batteries (especially lithium batteries). Electrodes prepared using this high-purity vanadium pentoxide exhibit excellent specific capacity, cycle stability, and rate performance.
[0084] Finally, it should be noted that the embodiments described above are only some of the embodiments of the present invention, not all of them. The detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but rather merely represents selected embodiments of the present invention. All other embodiments derived by persons of ordinary skill in the art based on the embodiments of the present invention without inventive effort are also within the scope of protection of the present invention.
Claims
1. A method for preparing a high-purity vanadium oxide electrode, characterized in that: The following steps are involved: S1: pretreating the alkaline vanadium leaching solution using an activated alumina adsorption column to obtain a pretreated solution; S2: adding a composite impurity remover containing modified lignin sulfonate as a main agent to the pretreated liquid for primary impurity removal, and obtaining a primary impurity removal filtrate after solid-liquid separation; S3: adding a calcium hydroxide suspension and a flocculant to the primary impurity removal filtrate to perform secondary impurity removal, and obtaining a secondary impurity removal filtrate after solid-liquid separation; S4: Purifying the secondary impurity-removed filtrate using an ion exchange column to obtain a purified liquid; S5: adding ammonium salt to the purified liquid to precipitate vanadium to obtain ammonium metavanadate crystals; S6: calcining the ammonium metavanadate crystals to obtain high-purity vanadium pentoxide; S7: preparing a high-purity vanadium oxide electrode using the high-purity vanadium pentoxide.
2. The method for preparing a high-purity vanadium oxide electrode according to claim 1, wherein: Include one or more of the following: Step S1 comprises: passing the alkaline vanadium leaching solution through an activated alumina adsorption column at a flow rate of 1-5 BV / h and controlling the temperature at 40-60° C. to obtain the pretreatment solution; Step S2 comprises: adding the composite impurity remover containing modified lignin sulfonate as a main agent to the pretreated liquid, maintaining the pH at 9-10, reacting for 30-90 minutes under stirring conditions, and obtaining the primary impurity removal filtrate after solid-liquid separation; Step S3 comprises: heating the primary impurity-removed filtrate to 60-100° C., adding the calcium hydroxide suspension and the flocculant, aging for 30-60 minutes, and performing solid-liquid separation to obtain the secondary impurity-removed filtrate; Step S4 comprises: passing the secondary impurity-removed filtrate through the ion exchange column at a flow rate of 1.5-2 BV / h to obtain the purified liquid; Step S5 comprises: adjusting the pH of the purified solution to 8-9, adding the ammonium salt, and crystallizing at 30-90° C. for 1-2 hours to obtain the ammonium metavanadate crystals; Step S6 includes: calcining the ammonium metavanadate crystals in an oxygen atmosphere in stages, first increasing the temperature to 300° C. at 5-10° C. / min and keeping the temperature for 0.5-1.5 hours, then increasing the temperature to 550° C. at 2-8° C. / min and keeping the temperature for 1-3 hours, to obtain the high-purity vanadium pentoxide.
3. The method for preparing a high-purity vanadium oxide electrode according to claim 1 or 2, characterized in that: The main component of the composite impurity remover is aminopolysaccharide modified lignin sulfonate, and the composite impurity remover also includes citrate.
4. The method for preparing a high-purity vanadium oxide electrode according to claim 3, wherein: The added amount of the composite impurity remover is 1.1-1.3 times the molar amount of vanadium in the alkaline vanadium leaching solution.
5. The method for preparing a high-purity vanadium oxide electrode according to claim 3, characterized in that: In the composite impurity remover, the mass ratio of lignin sulfonate, citrate and amino polysaccharide is 5-8:2-1:
1.
6. The method for preparing a high-purity vanadium oxide electrode according to claim 3, characterized in that: The composite impurity remover is prepared by the following method: After mixing lignin sulfonate and amino polysaccharide in proportion, adding potassium persulfate solution, oxidizing and modifying at 60-80°C for 1-3 hours to obtain amino polysaccharide-modified lignin sulfonate; The aminopolysaccharide modified lignin sulfonate is compounded with citrate to obtain the composite impurity remover.
7. The method for preparing a high-purity vanadium oxide electrode according to claim 1, wherein: The amount of the calcium hydroxide suspension added is 2-3 times the molar amount of phosphorus in the alkaline vanadium leaching solution in terms of calcium molar amount.
8. The method for preparing a high-purity vanadium oxide electrode according to claim 1, wherein: The flocculant is a polyacrylamide flocculant with a mass fraction of 0.1-0.25%.
9. The method for preparing a high-purity vanadium oxide electrode according to claim 1, wherein: The amount of ammonium salt added is NH4 + The molar amount is 2-3.5 times the molar amount of vanadium in the alkaline vanadium leaching solution.
10. A high-purity vanadium oxide electrode, characterized in that: The method is prepared by the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of ultra-pure vanadium pentoxide
CN105800689A
Preparing method of astronavigation tablet vanadium pentoxide
CN108085517A
Method for preparing vanadium pentoxide positive electrode material from sodium vanadium liquid
CN112266020A
Method for removing silicon and phosphorus in vanadium slag sodium salt roasting production system
CN115976341A
Method of manufacturing sodium-metal oxide
EP0000398A1
Cited By
Purification method for preparing high-purity vanadium pentoxide from vanadate crude product
CN121377115A
Regeneration method of waste graphite felt electrode of vanadium battery
CN121484108A
A method for regenerating a vanadium cell waste graphite felt electrode
CN121484108B