Method for improving obdurability matching of titanium alloy by inducing FCC phase through high-temperature impact deformation

By inducing FCC phase transformation in titanium alloy through high-temperature impact deformation technology, combined with annealing and laser shock strengthening, the problem of insufficient strength and toughness matching of titanium alloy is solved, and efficient strength and toughness improvement and wide applicability are achieved, which is suitable for complex titanium alloy parts.

CN120719236APending Publication Date: 2025-09-30SHANGHAI JIAOTONG UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202510959346.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-11
Publication Date
2025-09-30

AI Technical Summary

Technical Problem

Existing technologies make it difficult to efficiently induce FCC phase transformation in titanium alloys, resulting in insufficient strength-toughness matching. Traditional methods also have high energy consumption and narrow applicability, making it difficult to meet the stringent requirements of modern engineering for strength-toughness coordination.

Method used

Through high-temperature impact deformation technology, combined with annealing, surface treatment and laser shock strengthening, high-temperature and high-speed impact deformation is used to directly induce the transformation of HCP phase to FCC phase under the synergistic effect of dynamic stress-temperature, forming a synergistic strengthening effect of FCC phase, nanotwins and residual compressive stress, and achieving grain refinement and strong-plastic matching.

Benefits of technology

The strength-toughness matching of titanium alloys has been significantly improved, the FCC phase content has reached 2.3 times that of traditional methods, and the fatigue life of the material has been increased by two orders of magnitude. It is suitable for titanium alloy parts with complex geometries, broadens the scope of application, and has the advantages of high efficiency, low consumption, and mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120719236A_ABST
    Figure CN120719236A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving obdurability matching of titanium alloy by inducing an FCC phase through high-temperature impact deformation, and belongs to the technical field of metal material phase change regulation and control. The method comprises the steps that after annealing treatment and surface treatment are conducted on a substrate material, the substrate material is sequentially covered with a sacrificial layer and a restraint layer and evenly pressed, the substrate material is placed on a heating table of a high-temperature impact deformation device to be preheated, and the substrate material is subjected to high-temperature impact deformation; according to the method, the energy required for transformation of the HCP phase to the FCC phase is reduced, the heating temperature and laser shock parameters are set, the HCP phase is induced to be transformed into the FCC phase under the dynamic stress-temperature synergistic effect through multi-pass laser shock peening and high-temperature and high-speed shock deformation, the FCC phase, nano twin crystals and residual compressive stress form the synergistic peening effect, and therefore the HCP phase is converted into the FCC phase. Further, the grain refinement process is accelerated, the strength and plasticity matching is improved, and the high-temperature impact deformation induces the FCC phase to improve the strength and toughness matching of the titanium alloy; the substrate is made of industrial pure titanium or titanium alloy. The method is suitable for high-strength parts with complex geometrical shapes, is more widely applicable than traditional rolling annealing, and provides reference for strengthening and toughening of titanium alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of metal material phase change control, and specifically relates to a method for improving the strength and toughness matching of titanium alloys by inducing FCC phases through high-temperature impact deformation. Background Art

[0002] Titanium and its alloys are widely used as structural materials in various engineering applications due to their high specific strength, excellent corrosion resistance, superior biocompatibility, and exceptional fracture toughness. These exceptional material properties have led to their widespread use in aircraft engines, turbine blades, bioimplants, and petrochemical facilities. At room temperature, titanium and its alloys primarily exist as the α phase with a hexagonal close-packed (HCP) structure, which transforms to the β phase with a body-centered cubic (BCC) structure at elevated temperatures. However, the HCP structure faces an inherent contradiction in service: on the one hand, the limited slip system in the α phase makes dislocation motion difficult at ultra-high strain rates, which can easily lead to stress concentration and fatigue failure. On the other hand, conventional thermomechanical treatments often result in a sudden drop in plasticity when increasing strength, making it difficult to meet the demanding "strength-toughness synergy" requirements of modern engineering. This contradiction is particularly prominent in dual-phase titanium alloys such as TC4, necessitating new microstructural control strategies.

[0003] The discovery of face-centered cubic (FCC) titanium offers a new approach to addressing this challenge. Theoretical studies have shown that the FCC phase not only coordinates the deformation of the HCP phase through 12 slip systems, but its low stacking fault energy also facilitates the formation of nanotwins, potentially achieving simultaneous improvements in strength and ductility. However, existing patented technologies for inducing the FCC phase face three obstacles: 1. Conventional rolling annealing requires a reduction of more than 85% combined with high-temperature annealing, which can lead to grain coarsening, and the FCC phase content is less than 22%; 2. Existing methods focus solely on the FCC phase transformation in pure titanium (hcp structure) and lack control over dual-phase titanium alloys such as TC4, severely limiting their industrial applicability; 3. A quantitative relationship between the FCC phase transformation and mechanical properties has not yet been established, leaving the degree of performance optimization unclear. Existing technologies employ laser shock or rolling annealing to induce the FCC phase transformation in pure titanium and achieve a certain proportion of FCC structure. However, these existing technologies target only pure titanium (hcp structure) and do not address the control of the FCC phase transformation in titanium alloys such as TC4, resulting in a limited applicability. The specific mechanism by which FCC phase formation affects the material's strength and toughness remains unclear. Furthermore, while the rolling-annealing method can produce FCC phases, its FCC content is low (≤22%) and requires extensive rolling (≥85% reduction) and prolonged high-temperature annealing (0.5-8 hours). This consumes a lot of energy and places significant restrictions on material size and shape.

[0004] In view of the problems of existing technologies such as narrow applicability, limited to pure titanium, low FCC phase content (≤22%), complex process and high energy consumption (requiring ≥85% reduction rolling and high temperature annealing), and unclear quantitative relationship between strengthening and toughening mechanism and performance, it is urgent to find a new method to improve the strength and toughness of titanium alloys to achieve efficient generation of FCC phase, synergistic improvement of strength and toughness, and adaptation to the processing of complex components. Summary of the Invention

[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a method for using high-temperature impact deformation to induce FCC phase to improve the strength-toughness matching of titanium alloys, so as to solve the technical problems of low efficiency, difficulty in control, strong plasticity inversion and process dependence on large deformation rolling and high-temperature annealing in titanium and titanium alloys.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions: The present invention discloses a method for improving the strength and toughness matching of titanium alloy by inducing FCC phase through high temperature impact deformation, comprising: After the base material is annealed and surface treated, it is covered with a sacrificial layer and a constraint layer in sequence. After uniform pressure is applied, it is placed on a heating table of a high-temperature impact deformation device for preheating. The energy required for the transformation of the HCP phase to the FCC phase is reduced by preheating. The heating temperature and laser shock parameters are set. After multiple laser shock strengthening, high-temperature and high-speed impact deformation is used to directly induce the HCP phase to transform into the FCC phase under the synergistic effect of dynamic stress-temperature. The FCC phase forms a synergistic strengthening effect with nano twins and residual compressive stress, thereby accelerating the grain refinement process and improving the strength-plasticity matching, so as to achieve high-temperature impact deformation-induced FCC phase to improve the strength-toughness matching of the titanium alloy. The base material is industrial pure titanium or titanium alloy.

[0007] Preferably, the annealing treatment of industrial pure titanium includes: keeping at 600-800°C for 1-4 hours under argon protection, followed by air cooling; Annealing treatment of titanium alloy includes: keeping at 900-980℃ for 1-4h under argon protection, followed by air cooling; The surface treatment includes: mechanically polishing the sample surface using 120-2500 mesh sandpaper in sequence to a surface roughness Ra ≤ 0.2 μm; and then ultrasonically cleaning in anhydrous ethanol for 10-30 minutes.

[0008] Preferably, the sacrificial layer is high-purity aluminum foil; the thickness of the sacrificial layer is 100-300 μm.

[0009] Preferably, the constraining layer is K9 glass; the thickness of the constraining layer is 1-5 mm.

[0010] Preferably, the heating stage is a programmable heating stage, adopts a PID temperature control system, and has a temperature accuracy of ±5°C; the heating rate is 10°C / min, the preheating temperature is 300~600°C, and the holding time is 10~15min; the heating stage also uses an infrared thermal imager to monitor the surface temperature of the substrate material in real time.

[0011] Preferably, the laser shock parameters include: spot diameter 2-4 mm, laser energy 1-10 J, and pulse frequency 8-15 Hz.

[0012] Preferably, the scanning path of the laser shock peening is zigzag, and the overlap rate of adjacent light spots is 30% to 50%.

[0013] Preferably, laser shock peening is repeated 1 to 5 times in the same area, and a new sacrificial layer is replaced after each laser shock peening; and water quenching is immediately performed after each laser shock peening is completed.

[0014] Preferably, after laser shock peening, the FCC phase is needle-shaped and curved directly below the shock wave, with a width of 20-30 nm and a content of 10%-40%.

[0015] Preferably, the method further comprises: confirming the FCC phase morphology and content by using transmission Kikuchi diffraction and transmission electron microscopy; testing the mechanical properties of the substrate material by using microhardness or tensile testing; The high temperature impact deformation device includes: Heating table, used to provide high temperature environment; A fixture, disposed on the heating table, for fixing the base material; The laser beam emitting device is located above the base material and is used to emit a laser beam vertically incident on the constrained layer on the surface of the base material to perform laser shock strengthening on the surface of the base material.

[0016] Compared with the prior art, the present invention has the following beneficial effects: The present invention discloses a method for improving the strength and toughness matching of titanium alloys by inducing FCC phases through high-temperature impact deformation. By integrating annealing, surface treatment, laser shock strengthening and high-temperature environment control, a complete and systematic titanium alloy strengthening and toughening treatment process is formed. This process is not only applicable to industrial pure titanium, but can also be extended to titanium alloys such as TC4, greatly broadening the application scope of the technology. The heating table can provide a stable high-temperature environment, and effectively reduce the energy barrier of the HCP to FCC phase transformation through preheating, making the phase change easier to occur, which is a key prerequisite for achieving efficient phase transformation. The synergistic effect of multi-pass laser shock strengthening and high temperature lays the foundation for achieving a high proportion of FCC phase in titanium alloys, which can significantly improve the strength and toughness matching of materials. The use of high-temperature and high-speed impact deformation technology can not only achieve a higher proportion of FCC phase in pure titanium (up to 40%), but also be extended to TC4 titanium alloys. At the same time, it can process titanium and titanium alloys with complex geometries, improve industrial applicability, and significantly improve the strength and toughness matching of materials. Compared with the existing technology, this method has three major breakthroughs: 1) High temperature reduces the phase change energy barrier, combined with >10 6 s -1 The transient high pressure (>2GPa) generated by the strain rate can obtain a 40% FCC phase content in pure titanium (2.3 times that of the traditional method), and for the first time achieve 20% FCC phase control in TC4 alloy; 2) The FCC phase forms a synergistic strengthening effect with nanotwins and residual compressive stress, thereby accelerating the grain refinement process and improving the strength-plasticity matching, which increases the fatigue life of the material by two orders of magnitude, fundamentally solving the "strength-plasticity inversion" dilemma; 3) The process parameters of this technology are highly controllable and suitable for complex geometries and high-strength components. It has a wider applicability than traditional rolling annealing, and provides an efficient, low-consumption, and mass-producible solution for the strengthening and toughening of titanium alloys.

[0017] Furthermore, pure titanium is heated at 600-800°C for 1-4 hours under argon protection, followed by air cooling, to eliminate work hardening and homogenize the grain structure. This not only provides a more stable structural foundation for subsequent impact deformation but also reduces deformation defects caused by structural inhomogeneity. TC4 titanium alloy is heated at 900-980°C for 1-4 hours under argon protection, followed by air cooling, to fully dissolve the β phase and stabilize the α phase, optimizing the original microstructure and facilitating more effective phase transformation and strengthening during the subsequent impact process. Gradual polishing with sandpaper from 120 to 2500 grit significantly reduces the surface roughness of the specimen to Ra ≤ 0.2μm, removes surface machining damage and impurities, and allows the laser impact energy to be more uniformly applied to the material surface, improving the consistency of the impact effect. Ultrasonic cleaning in anhydrous ethanol for 10-30 minutes thoroughly removes surface oil and wear debris, preventing contaminants from affecting the bonding strength between the sacrificial layer and the substrate material, as well as the transmission efficiency of the shock wave.

[0018] Furthermore, a 100-300μm thick high-purity aluminum foil is applied to the surface of the base material as a sacrificial layer to absorb laser energy and generate plasma shock waves. High-purity aluminum foil, as a sacrificial layer, can efficiently absorb laser energy. Under the action of the laser, the aluminum foil rapidly vaporizes to generate a plasma shock wave. This shock wave has the characteristics of high intensity and high strain rate, and is the key driving force for inducing phase transformation and deformation of titanium alloys. The thickness range of 100-300μm has been optimized to ensure that the aluminum foil has sufficient material to absorb laser energy and generate shock waves of sufficient intensity, while also avoiding excessive energy attenuation due to excessive thickness, which affects the impact effect.

[0019] Furthermore, a K9 glass layer with a thickness of 1 to 5 mm was placed on top of the aluminum foil as a constraining layer, and uniform pressure was applied using a rigid pressure block to ensure the efficient transmission of shock wave pressure. The K9 glass, acting as a constraining layer, effectively limits the expansion direction of the plasma, significantly enhancing the vertical pressure of the shock wave (up to >2 GPa). Higher shock wave pressure helps improve phase transition efficiency and increase the content of the FCC phase. The 1 to 5 mm thickness ensures that the constraining layer has sufficient rigidity to evenly transmit the shock wave pressure, avoiding uneven pressure distribution due to deformation of the constraining layer, thereby ensuring the uniformity of the titanium alloy surface treatment.

[0020] Furthermore, a PID temperature control system, combined with real-time infrared thermal imaging monitoring, achieves a temperature accuracy of ±5°C, ensuring that the specimen is uniformly maintained at the target temperature (300-600°C). Precise temperature control is crucial for ensuring consistent and repeatable phase transitions, avoiding variations in the degree of phase transition caused by local overheating or temperature variations. A moderate heating rate of 10°C / min prevents excessive temperature gradients within the specimen caused by rapid heating while also improving process efficiency. A holding time of 10-15 minutes ensures uniform temperature throughout the specimen, providing a stable thermodynamic environment for subsequent impact deformation and facilitating a uniform phase transition.

[0021] Furthermore, the spot diameter range of 2 to 4 mm can be selected according to the size of the treatment area and the required precision, making it suitable for local strengthening of parts with complex geometries. The adjustable range of laser energy from 1 to 10 J can meet the needs of different material thicknesses and performance requirements. Lower energy is suitable for shallow treatment or situations with high requirements for plasticity retention, while higher energy can achieve deeper phase transformation depths and stronger strengthening effects. The pulse frequency of 8-15 Hz ensures the efficiency of laser shock, allowing multiple shock treatments to be completed in a reasonable time while avoiding overheating of the sample due to excessive frequency.

[0022] Furthermore, the zigzag scanning path ensures uniform laser impact coverage across the specimen surface, avoiding blind spots and ensuring consistent phase transformation and strengthening across the entire treated area. A 30% to 50% spot overlap ensures surface treatment uniformity while avoiding excessive energy concentration and material damage caused by excessive overlap. A suitable overlap helps form a continuous strengthening layer and improves the uniformity of the FCC phase distribution.

[0023] Furthermore, repeating the impact 1 to 5 times gradually increases the phase transformation depth and FCC phase content, achieving a more significant strengthening and toughening effect through a cumulative effect. Furthermore, replacing a new sacrificial layer after each impact ensures stable energy transfer efficiency with each impact, avoiding attenuation of shock wave intensity due to sacrificial layer consumption. Immediate water quenching suppresses the reverse transformation of the FCC phase through rapid cooling, fixing the metastable FCC phase structure, and ensuring the preservation of the phase transformation effect, thereby ensuring improved material performance.

[0024] Furthermore, the needle-shaped and curved FCC phase structure has a high interfacial area, which can significantly improve the material's strength through phase transformation strengthening and grain refinement. The nanoscale size of 20-30nm enables the FCC phase to form a synergistic strengthening effect with nanotwins and residual compressive stress, effectively hindering dislocation movement, improving strength while retaining a certain degree of plasticity, and breaking the "strong-plastic inversion" dilemma. The FCC phase content of 10%-40% (pure titanium can reach 40%) is significantly higher than traditional methods and is the key factor in achieving a significant increase in material strength and toughness. For example, the yield strength of pure titanium is increased from 288MPa to 382MPa, and the fatigue life is increased by two orders of magnitude.

[0025] Furthermore, combined analysis using transmission Kikuchi diffraction and transmission electron microscopy accurately confirms the morphology (e.g., needle-like and curved features), size (nanoscale), and content of the FCC phase, providing intuitive microscopic evidence for process optimization and mechanism studies. Microhardness testing can quickly reflect the surface strengthening effect of the material. For example, the Vickers hardness of pure titanium increased from 104 HV to 160 HV, directly demonstrating the hardness-enhancing effect of impact treatment. Tensile testing quantitatively evaluates key mechanical properties such as yield strength and elongation through stress-strain curves, confirming the optimized strength-toughness balance. For example, the yield strength of TC4 increased from 856 MPa to 993 MPa while maintaining a stable elongation. These tests provide reliable performance data for practical applications. The fixture's securement of the substrate ensures no material displacement during the laser shock treatment, ensuring process stability and reliability. The vertical incidence of the laser beam, combined with the sacrificial and constraining layers, generates ultra-high strain rates and transient high pressures, providing the necessary mechanical conditions for inducing the FCC phase. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a schematic diagram of the high-temperature impact deformation device disclosed in the present invention; Figure 2 The microstructure of the pure titanium sample directly below the high-temperature impact disclosed in Example 1 of the present invention; wherein (a) is a phase diagram; (b) is a TEM morphology diagram; Figure 3 The microstructure of a pure titanium sample 200 μm from the surface under high temperature impact as disclosed in Example 1 of the present invention; wherein (a) is a phase diagram; (b) is a TEM morphology diagram; Figure 4 This is a stress-strain curve diagram of pure titanium disclosed in Example 1 of the present invention before and after high-temperature impact; Figure 5 The microstructure of the TC4 sample directly below the high-temperature impact disclosed in Example 2 of the present invention; wherein (a) is a phase diagram; (b) is a TEM morphology image; Figure 6 The stress-strain curve of TC4 disclosed in Example 2 of the present invention before and after high-temperature impact; Figure 7 This is the phase diagram of the TA1 sample after impact disclosed in Comparative Example 1 of the present invention.

[0027] Among them, 1. fixture; 2. base material; 3. sacrificial layer; 4. constraint layer; 5. laser beam; 6. heating platform. DETAILED DESCRIPTION

[0028] The technical solution of the present invention will be described clearly and completely below. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. All other embodiments derived by persons of ordinary skill in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0029] In the present invention, unless otherwise specified, all the embodiments and preferred implementation methods mentioned herein can be combined with each other to form a new technical solution.

[0030] In the present invention, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.

[0031] In the present invention, unless otherwise specified, percentages (%) or parts refer to percentages by weight or parts by weight relative to the composition.

[0032] In the present invention, unless otherwise specified, the components or preferred components involved can be combined with each other to form a new technical solution.

[0033] In this disclosure, unless otherwise specified, the numerical range "a-b" is an abbreviation for any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "6-22" indicates that all real numbers between "6-22" are listed herein, and "6-22" is merely an abbreviation for these numerical combinations.

[0034] The "range" disclosed in the present invention is in the form of lower limit and upper limit, which can be one or more lower limits, and one or more upper limits respectively.

[0035] In the present invention, the term "and / or" used herein refers to any combination and all possible combinations of one or more of the associated listed items, and includes these combinations.

[0036] In the present invention, unless otherwise specified, each reaction or operation step can be carried out sequentially or in accordance with the order. Preferably, the reaction method herein is carried out sequentially.

[0037] Unless otherwise indicated, the professional and scientific terms used herein are the same as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the described content can also be applied to the present invention.

[0038] The present invention provides a method for improving the strength-toughness matching of titanium alloy by inducing FCC phase through high-temperature impact deformation, comprising the following steps: Step 1: Substrate material pretreatment 1. Material selection: Industrial pure titanium (TA1) or TC4 (Ti6Al4V) titanium alloy is selected as the base material2.

[0039] 2. Annealing treatment: 1) Pure titanium: Under argon protection, heat at 600-800℃ for 1-4 hours, then air cool to eliminate work hardening and uniform grain structure.

[0040] 2) TC4 titanium alloy: Under argon protection, keep at 900-980℃ for 1-4h, then air cool to fully dissolve the β phase and stabilize the α phase.

[0041] 3.Surface treatment: 1) Use 120-2500 mesh sandpaper to mechanically polish the surface of the sample to ensure that the surface roughness Ra ≤ 0.2 μm.

[0042] 2) Perform ultrasonic cleaning in anhydrous ethanol for 10-30 minutes to remove surface oil and debris, and then blow dry.

[0043] Step 2: Laser shock peening system construction 1. Preparation of sacrificial layer and constrained layer: 1) Cover the surface of TA1 or TC4 prepared in step 1 with a 100-300 μm thick high-purity aluminum foil as a sacrificial layer 3 to absorb laser energy and generate plasma shock waves.

[0044] 2) Place K9 glass (thickness 1-5 mm) on top of the aluminum foil as the constraint layer 4 and apply uniform pressure with a rigid pressure block to ensure the efficiency of shock wave pressure transmission.

[0045] 2. Sample fixation: Install the assembled sample on a high-temperature resistant fixture 1 to ensure that there is no displacement during the laser impact process, as shown in the figure.

[0046] Step 3: High temperature environment control 1. Heating system settings: 1) Place the fixture 1 and the sample on a programmable heating table 6 and use a PID temperature control system with a temperature accuracy of ±5°C.

[0047] 2. Temperature stabilization: 1) Raise the temperature to the target temperature (300-600°C) at a rate of 10°C / min and keep it at that temperature for 10-15 minutes to make the temperature of the entire sample uniform.

[0048] 2) Use an infrared thermal imager to monitor the surface temperature of the sample in real time to ensure thermal equilibrium.

[0049] Step 4: Laser shock parameter optimization 1. Laser configuration: 1) Use a high-power Q-switched Nd:YAG laser (wavelength 1064nm, pulse width 15ns), spot diameter 2~4mm, laser energy 1~10J, and pulse frequency 8-15Hz.

[0050] 2. Impact path planning: 1) Laser beam 5 is incident vertically 2) A zigzag scanning path is used with an overlap rate of 50% between adjacent light spots to ensure uniform surface treatment.

[0051] Step 5: Multi-pass laser shock peening 1. Repeat the impact 1 to 5 times on the same area, replacing the aluminum foil after each impact.

[0052] 2. Water quench immediately after each impact to lock the metastable FCC phase.

[0053] The present invention has improvements and beneficial effects in four aspects: technical principle breakthrough, process parameter optimization, material performance enhancement, and industrial applicability expansion, as follows: In terms of technical principle breakthroughs, dynamic stress-temperature synergy induces efficient phase change High temperature reduces the phase change energy barrier By preheating the titanium alloy to 300~600℃, the energy required for the HCP to FCC phase transformation is reduced, making the phase transformation easier to occur.

[0054] High strain rate shock generates transient high pressure Combined with laser shock, the 6 s -1 By using ultra-high strain rates and transient high pressures greater than 2 GPa, a 40% FCC phase content was achieved in pure titanium (2.3 times that of traditional methods), and a 20% FCC phase was induced in TC4 alloy for the first time, breaking through the limitations of traditional processes in regulating FCC phases.

[0055] In terms of process parameter innovation, phase change efficiency is improved through multi-factor collaborative optimization Precise temperature control A PID temperature control system (accuracy ±5°C) and an infrared thermal imager are used for real-time monitoring to ensure that the sample is evenly kept at the target temperature (300-600°C) to avoid local overheating or uneven temperature that affects the consistency of phase change.

[0056] Laser shock path and overlap optimization A "zigzag" scanning path and a 30% to 50% spot overlap rate are used to ensure uniform surface treatment and avoid impact blind spots.

[0057] Multiple impacts (1 to 5 times) are combined with replacing the sacrificial layer 3 aluminum foil after each impact to ensure stable transmission of shock wave energy and improve the depth and uniformity of phase change.

[0058] Rapid water quenching to lock the metastable phase Water quenching is performed immediately after impact to suppress the FCC phase reversal transformation through rapid cooling, fix the metastable structure, and ensure that the phase change effect is retained.

[0059] In terms of improving material performance, the dilemma of "strength-plasticity inversion" has been solved The nano-sized needle-like FCC phase improves strength through phase transformation strengthening and grain refinement.

[0060] The impact-induced residual compressive stress and nanotwins form a synergistic effect with the FCC phase, further hindering dislocation movement, thereby improving strength while retaining plasticity.

[0061] The Vickers hardness of pure titanium is increased from 104HV to 160HV, the yield strength is increased from 288MPa to 382MPa, the elongation after fracture is maintained at 50%, and the strength-toughness match is optimized.

[0062] Through the synergistic strengthening effect, the fatigue life of the material is increased by two orders of magnitude, solving the problem of achieving both strength and plasticity in traditional processes.

[0063] In terms of industrial applicability expansion, it has the advantages of high efficiency, low consumption and strong universality Laser shock technology can be used to locally strengthen titanium alloy components with complex geometries, breaking through the limitations of traditional rolling and annealing processes on material shape.

[0064] Key parameters (temperature, laser energy, number of impacts, etc.) can be precisely controlled through programming, making it suitable for industrial mass production.

[0065] No complex chemical treatment is required, and phase change is achieved only through physical impact and temperature control, which has the advantages of high efficiency, low energy consumption and environmental friendliness.

[0066] It is not only applicable to industrial pure titanium, but can also be expanded to high-strength titanium alloys such as TC4, providing universal strengthening and toughening solutions for aerospace, medical equipment and other fields.

[0067] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings herein can be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0068] Figure 1 This is a schematic diagram of the high-temperature impact deformation device disclosed in the present invention; as can be seen from the figure, the high-temperature impact deformation device includes: a heating table 6 for providing a high-temperature environment, a clamp 1 arranged on the heating table 6 and used to fix the base material 2, the base material 2 mounted on the clamp 1, a sacrificial layer 3 covering the surface of the base material 2 and used to absorb laser energy and generate plasma shock waves, a constraint layer 4 placed above the sacrificial layer 3 and used to ensure the efficiency of shock wave pressure transmission, and a laser beam emitting device located above the sacrificial layer 3 and used to emit a laser beam 5 perpendicular to the surface of the constraint layer 4.

[0069] Example 1 A method for improving the strength-toughness matching of titanium alloy by inducing FCC phase through high-temperature impact deformation comprises the following steps: Step 1: Substrate material pretreatment 1. Material selection: Industrial pure titanium (TA1) was selected as the substrate material 2, and the TA1 titanium plate was cut into small specimens of 50 mm × 50 mm × 5 mm (±0.1 mm).

[0070] 2. Annealing treatment: 1) Pure titanium: Under argon protection, heat at 800℃ for 3h, then air cool to eliminate work hardening and uniform grain structure.

[0071] 3.Surface treatment: 1) Use 120-2500 mesh sandpaper to mechanically polish the surface of the sample to ensure that the surface roughness Ra ≤ 0.2 μm.

[0072] 2) Perform ultrasonic cleaning in anhydrous ethanol for 20 minutes to remove surface oil and debris, and then blow dry.

[0073] Step 2: Laser shock peening system construction 1. Preparation of sacrificial layer and constrained layer: 1) Cover the surface of TA1 prepared in step 1 with a 120 μm thick aluminum foil as a sacrificial layer 3 to absorb laser energy and generate plasma shock waves.

[0074] 2) Place K9 glass (3 mm thick) on top of the aluminum foil as the constraint layer 4 and apply uniform pressure with a rigid pressure block to ensure the efficiency of shock wave pressure transmission.

[0075] 2. Sample fixation: Install the assembled sample on the high temperature resistant fixture 1 to ensure that there is no displacement during the laser impact process.

[0076] Step 3: High temperature environment control 1. Heating system settings: 1) Place the fixture 1 and the sample on a programmable heating table 6 and use a PID temperature control system with a temperature accuracy of ±5°C.

[0077] 2. Temperature stabilization: 1) Raise the temperature to the target temperature of 400°C at a rate of 10°C / min and keep it at that temperature for 15 minutes to make the temperature of the entire sample uniform.

[0078] 2) Use an infrared thermal imager to monitor the surface temperature of the sample in real time to ensure thermal equilibrium.

[0079] Step 4: Laser shock parameter optimization 1. Laser configuration: 1) A high-power Q-switched Nd:YAG laser (wavelength 1064 nm, pulse width 15 ns) with a spot diameter of 2 mm, laser energy 1 J, and pulse frequency 10 Hz was used.

[0080] 2. Impact path planning: 1) Laser beam 5 is incident vertically; 2) A zigzag scanning path is used with an overlap rate of 50% between adjacent light spots to ensure uniform surface treatment.

[0081] Step 5: Multi-pass laser shock peening 1. Repeat the shock five times on the same area, replacing the aluminum foil after each shock.

[0082] 2. Water quench immediately after each impact to lock the metastable FCC phase.

[0083] Step 6: Microstructure and phase composition analysis 1. Cross-section preparation: Cut the strengthened zone in half along the X direction and along the direction of shock wave propagation (Z); mechanically grind and polish the resulting cross-section (ZX plane) to a mirror surface.

[0084] 2. FIB-TKD Ultrathin samples for TEM observation were prepared on the ZX plane using a focused ion beam (FIB) directly below the shock wave and 200 μm from the surface. After removal, transmission Kikuchi diffraction (TKD) and TEM analysis were used to confirm the FCC phase morphology and content. The results are as follows: Figure 2 and Figure 3 shown.

[0085] Figure 2 The microstructure of the pure titanium sample directly below the high-temperature impact disclosed in Example 1 of the present invention; wherein (a) is a phase diagram; (b) is a TEM morphology diagram; Figure 3 The microstructure of a pure titanium sample 200 μm from the surface under high-temperature shock, as disclosed in Example 1 of the present invention, is shown in Figure 1. (a) is a phase diagram, and (b) is a TEM image. Directly below the shock wave, the FCC phase is needle-shaped and curved, approximately 20–30 nm wide, and contains up to 40% of the phase. As the shock wave weakens, the FCC phase content decreases to approximately 12% at 200 μm from the surface, with a slender, needle-like morphology approximately 10 nm wide.

[0086] Step 7: Mechanical properties test Microhardness: Load 200 g, hold for 15 s, measure 5 points on the impact surface and take the average: Vickers hardness increases from 104 HV to 160 HV.

[0087] Tensile test: After 1J, 5 times of laser shock, pure titanium was cut into tensile specimens, and then -3 The sample was stretched at a strain rate of / s.

[0088] Figure 4 The stress-strain curve of pure titanium before and after high-temperature impact disclosed in Example 1 of the present invention is as follows; Figure 4 As shown in the figure, the yield strength increased from the original 288MPa to 382MPa, and the elongation after fracture decreased from 65% to 50%. The strength and toughness of pure titanium have been significantly improved.

[0089] Example 2 A method for improving the strength-toughness matching of titanium alloy by inducing FCC phase through high-temperature impact deformation comprises the following steps: Step 1: Substrate material pretreatment 1. Material selection: Industrial TC4 was selected as the substrate material 2, and the TC4 titanium plate was cut into small specimens of 50 mm × 50 mm × 5 mm (± 0.1 mm).

[0090] 2. Annealing treatment: 1) TC4: Under argon protection, keep at 950℃ for 3h, then air cool to fully dissolve the β phase and stabilize the α phase.

[0091] 3.Surface treatment: 1) Use 120-2500 grit sandpaper to mechanically polish the sample surface to ensure that the surface roughness Ra ≤ 0.2 μm.

[0092] 2) Perform ultrasonic cleaning in anhydrous ethanol for 20 min to remove surface oil and debris, and then blow dry.

[0093] Step 2: Laser shock peening system construction 1. Preparation of sacrificial layer and constrained layer: 1) Cover the TC4 surface prepared in step 1 with a 120 μm thick aluminum foil as a sacrificial layer 3 to absorb laser energy and generate plasma shock waves.

[0094] 2) Place K9 glass (3 mm thick) on top of the aluminum foil as the constraint layer 4 and apply uniform pressure with a rigid pressure block to ensure the efficiency of shock wave pressure transmission.

[0095] 2. Sample fixation: Install the assembled sample on the high temperature resistant fixture 1 to ensure that there is no displacement during the laser impact process.

[0096] Step 3: High temperature environment control 1. Heating system settings: 1) Place the fixture 1 and the sample on a programmable heating table 6 and use a PID temperature control system with a temperature accuracy of ±5°C.

[0097] 2. Temperature stabilization: 1) Raise the temperature to the target temperature of 500°C at a rate of 10°C / min and keep it at that temperature for 15 min to make the temperature of the entire sample uniform.

[0098] 2) Use an infrared thermal imager to monitor the surface temperature of the sample in real time to ensure thermal equilibrium.

[0099] Step 4: Laser shock parameter optimization 1. Laser configuration: 1) A high-power Q-switched Nd:YAG laser (wavelength 1064 nm, pulse width 15 ns) with a spot diameter of 3 mm, laser energy 5 J, and pulse frequency of 10 Hz was used.

[0100] 2. Impact path planning: 1) Laser beam 5 is incident vertically; 2) A zigzag scanning path is used with an overlap rate of 50% between adjacent light spots to ensure uniform surface treatment.

[0101] Step 5: Multi-pass laser shock peening 1. Repeat the shock five times on the same area, replacing the aluminum foil after each shock.

[0102] 2. Water quench immediately after each impact to lock the metastable FCC phase.

[0103] Step 6: Microstructure and phase composition analysis 1. Cross-section preparation: Cut the strengthened zone in half along the X direction and along the direction of shock wave propagation (Z); mechanically grind and polish the resulting cross-section (ZX plane) to a mirror surface.

[0104] 2. FIB-TKD A thin slice was prepared on the ZX plane at 200 μm below the shock wave using a focused ion beam (FIB). After removal, transmission Kikuchi diffraction (TKD) and TEM analysis were used to confirm the FCC phase morphology and content. The results are as follows: Figure 5 shown.

[0105] Figure 5 The microstructure of the TC4 sample directly below the high-temperature impact test disclosed in Example 2 of the present invention is shown in Figure 2. (a) is a phase diagram; (b) is a TEM image. As can be seen from the figures, TC4 has a dual-phase structure consisting of HCP and BCC phases. After five 5J high-temperature impacts, an FCC phase forms at 200 μm from the surface, with an FCC phase content of approximately 10%.

[0106] Step 7: Mechanical properties test Tensile test: After 5J and 5 times of laser shock, TC4 was cut into tensile specimens and then -3 The sample was stretched at a strain rate of / s.

[0107] Figure 6 The stress-strain curve of TC4 before and after high temperature impact disclosed in Example 2 of the present invention is shown in FIG. Figure 6 As shown in the figure, the yield strength increased from the original 856MPa to 922MPa, and the elongation after fracture decreased from 12% to 9%. The strength and toughness of TC4 titanium alloy were significantly improved.

[0108] Example 3 A method for improving the strength-toughness matching of titanium alloy by inducing FCC phase through high-temperature impact deformation comprises the following steps: Step 1: Substrate material pretreatment 1. Material selection: Industrial TC4 was selected as the substrate material 2, and the TC4 titanium plate was cut into small specimens of 50 mm × 50 mm × 5 mm (± 0.1 mm).

[0109] 2. Annealing treatment: 1) TC4: Under argon protection, keep at 950℃ for 3h, then air cool to fully dissolve the β phase and stabilize the α phase.

[0110] 3.Surface treatment: 1) Use 120-2500 grit sandpaper to mechanically polish the sample surface to ensure that the surface roughness Ra ≤ 0.2 μm.

[0111] 2) Perform ultrasonic cleaning in anhydrous ethanol for 20 min to remove surface oil and debris, and then blow dry.

[0112] Step 2: Laser shock peening system construction 1. Preparation of sacrificial layer and constrained layer: 1) Cover the TC4 surface prepared in step 1 with a 120 μm thick aluminum foil as a sacrificial layer 3 to absorb laser energy and generate plasma shock waves.

[0113] 2) Place K9 glass (3 mm thick) on top of the aluminum foil as the constraint layer 4 and apply uniform pressure with a rigid pressure block to ensure the efficiency of shock wave pressure transmission.

[0114] 2. Sample fixation: Install the assembled sample on the high temperature resistant fixture 1 to ensure that there is no displacement during the laser impact process.

[0115] Step 3: High temperature environment control 1. Heating system settings: 1) Place the fixture 1 and the sample on a programmable heating table 6 and use a PID temperature control system with a temperature accuracy of ±5°C.

[0116] 2. Temperature stabilization: 1) Raise the temperature to the target temperature of 500°C at a rate of 10°C / min and keep it at that temperature for 15 min to make the temperature of the entire sample uniform.

[0117] 2) Use an infrared thermal imager to monitor the surface temperature of the sample in real time to ensure thermal equilibrium.

[0118] Step 4: Laser shock parameter optimization 1. Laser configuration: 1) A high-power Q-switched Nd:YAG laser (wavelength 1064 nm, pulse width 15 ns) with a spot diameter of 3 mm, laser energy of 10 J, and pulse frequency of 10 Hz was used.

[0119] 2. Impact path planning: 1) Laser beam 5 is incident vertically; 2) A zigzag scanning path is used with an overlap rate of 50% between adjacent light spots to ensure uniform surface treatment.

[0120] Step 5: Multi-pass laser shock peening 1. Repeat the shock five times on the same area, replacing the aluminum foil after each shock.

[0121] 2. Water quench immediately after each impact to lock the metastable FCC phase.

[0122] Step 6: Microstructure and phase composition analysis 1. Cross-section preparation: Cut the strengthened zone in half along the X direction and along the direction of shock wave propagation (Z); mechanically grind and polish the resulting cross-section (ZX plane) to a mirror surface.

[0123] 2. FIB-TKD: Thin sections were prepared using a focused ion beam (FIB) on the ZX plane, below the shock wave at a depth of 200 μm. Transmission Kikuchi Diffraction (TKD) and TEM analysis were performed to confirm the FCC phase morphology and content, which was approximately 18%.

[0124] Step 7: Mechanical properties test Tensile test: After 10J, 5 times of laser shock, TC4 was cut into tensile specimens, and then -3 The sample was stretched at a strain rate of 1000 psi / s. The yield strength increased from the original 856 MPa to 993 MPa, and the elongation after fracture decreased from 12% to 8%. The strength and toughness of TC4 titanium alloy were significantly improved.

[0125] Example 4 A method for improving the strength-toughness matching of titanium alloy by inducing FCC phase through high-temperature impact deformation comprises the following steps, which differ from Example 1 in that: In step 1, the substrate material 2 is TA1, and the annealing treatment condition is 600° C. for 4 hours; during the surface treatment, ultrasonic cleaning is performed in anhydrous ethanol for 10 minutes.

[0126] In step 2, the thickness of the sacrificial layer 3 is 100 μm; the thickness of the constrained layer 4 is 1 mm.

[0127] In step 3, the target temperature is 300°C and the temperature is kept at this temperature for 14 minutes.

[0128] In step 4, the spot diameter is 3 mm, the laser energy is 2 J, the pulse frequency is 8 Hz, and the overlap rate of adjacent spots is 30%.

[0129] In step 5, perform 1 repetitive impact on the same area.

[0130] Example 5 A method for improving the strength-toughness matching of titanium alloy by inducing FCC phase through high-temperature impact deformation comprises the following steps, which differ from Example 1 in that: In step 1, the substrate material 2 is TA1, and the annealing temperature is 700° C.; during the surface treatment, ultrasonic cleaning is performed in anhydrous ethanol for 15 minutes.

[0131] In step 2, the thickness of the sacrificial layer 3 is 150 μm; the thickness of the constrained layer 4 is 2 mm.

[0132] In step 3, the target temperature is 350°C and the temperature is kept at this temperature for 13 minutes.

[0133] In step 4, the spot diameter is 4 mm, the laser energy is 4 J, the pulse frequency is 12 Hz, and the overlap rate of adjacent spots is 35%.

[0134] In step 5, perform 2 repeated impacts on the same area.

[0135] Example 6 A method for improving the strength-toughness matching of titanium alloy by inducing FCC phase through high-temperature impact deformation comprises the following steps, which differ from Example 1 in that: In step 1, the substrate material 2 is TC4, and the annealing treatment condition is 900° C. for 2 hours; during the surface treatment, ultrasonic cleaning is performed in anhydrous ethanol for 25 minutes.

[0136] In step 2, the thickness of the sacrificial layer 3 is 200 μm; the thickness of the constrained layer 4 is 4 mm.

[0137] In step 3, the target temperature is 450°C and the temperature is kept at this temperature for 12 minutes.

[0138] In step 4, the laser energy is 6 J, the pulse frequency is 15 Hz, and the overlap rate of adjacent spots is 40%.

[0139] In step 5, perform 3 repetitive shocks on the same area.

[0140] Example 7 A method for improving the strength-toughness matching of titanium alloy by inducing FCC phase through high-temperature impact deformation comprises the following steps, which differ from Example 1 in that: In step 1, the substrate material 2 is TC4, and the annealing condition is 980° C. for 1 hour; during the surface treatment, ultrasonic cleaning is performed in anhydrous ethanol for 30 minutes.

[0141] In step 2, the thickness of the sacrificial layer 3 is 300 μm; the thickness of the constrained layer 4 is 5 mm.

[0142] In step 3, the target temperature is 600°C and the temperature is kept at this temperature for 10 minutes.

[0143] In step 4, the spot diameter is 3 mm, the laser energy is 8 J, and the overlap rate of adjacent spots is 45%.

[0144] In step 5, perform 4 repetitive impacts on the same area.

[0145] Comparative Example 1 A method for improving the strength and toughness matching of titanium alloys without adding high temperature, comprising the following steps: 1. Material selection: Industrial pure titanium (TA1) was selected, and the TA1 titanium plate was cut into small specimens of 50 mm × 50 mm × 5 mm (±0.1 mm).

[0146] 2. Annealing treatment: 1) Pure titanium: Under argon protection, heat at 800℃ for 3h, then air cool to eliminate work hardening and uniform grain structure.

[0147] 3.Surface treatment: 1) Use 120-2500 grit sandpaper to mechanically polish the sample surface to ensure that the surface roughness Ra ≤ 0.2 μm.

[0148] 2) Perform ultrasonic cleaning in anhydrous ethanol for 20 min to remove surface oil and debris, and then blow dry.

[0149] Step 2: Laser shock peening system construction 1. Preparation of sacrificial layer and constrained layer: 1) Cover the surface of TA1 prepared in step 1 with a 120 μm thick aluminum foil as a sacrificial layer 3 to absorb laser energy and generate plasma shock waves.

[0150] 2) Place K9 glass (3 mm thick) on top of the aluminum foil as the constraint layer 4 and apply uniform pressure with a rigid pressure block to ensure the efficiency of shock wave pressure transmission.

[0151] 2. Sample fixation: Install the assembled sample on fixture 1 to ensure that there is no displacement during the laser impact process.

[0152] Step 3: Laser shock parameter optimization 1. Laser configuration: A high-power Q-switched Nd:YAG laser (wavelength 1064 nm, pulse width 15 ns) was used with a spot diameter of 2 mm, laser energy 1 J, and pulse frequency of 10 Hz.

[0153] 2. Impact path planning: 1) Laser beam 5 is incident vertically; 2) A zigzag scanning path is used with an overlap rate of 50% between adjacent light spots to ensure uniform surface treatment.

[0154] Step 4: Multi-pass laser shock peening Perform 5 repeated impacts on the same area, replacing the aluminum foil after each impact.

[0155] Step 5: Microstructure and phase composition analysis 1. Cross-section preparation: Cut the strengthened zone in half along the X direction and along the direction of shock wave propagation (Z); mechanically grind and polish the resulting cross-section (ZX plane) to a mirror surface.

[0156] 2. FIB-TKD: Using a focused ion beam (FIB), thin slices were prepared on the ZX plane, directly below the shock wave and 200 μm from the surface. After removal, transmission Kikuchi diffraction (TKD) was used to confirm the FCC phase morphology and content. The results are as follows: Figure 7 shown.

[0157] Figure 7 This is the phase diagram of the TA1 sample after impact disclosed in Comparative Example 1 of the present invention; it can be seen from the figure that directly below the shock wave, the FCC phase is needle-shaped, with a width of about 20nm and a content of only 3%.

[0158] Step 6: Mechanical properties test Microhardness: Load 200 g, hold for 15 s, measure 5 points on the impact surface and take the average: Vickers hardness increased from 104 HV to 126 HV.

[0159] Comparative Example 2 A method for improving the strength and toughness matching of titanium alloy, wherein the temperature is too high, comprises the following steps: 1. Material selection: Industrial pure titanium (TA1) was selected, and the TA1 titanium plate was cut into small specimens of 50 mm × 50 mm × 5 mm (±0.1 mm).

[0160] 2. Annealing treatment: 1) Pure titanium: Under argon protection, heat at 800℃ for 3h, then air cool to eliminate work hardening and uniform grain structure.

[0161] 3.Surface treatment: 1) Use 120-2500 grit sandpaper to mechanically polish the sample surface to ensure that the surface roughness Ra ≤ 0.2 μm.

[0162] 2) Perform ultrasonic cleaning in anhydrous ethanol for 20 min to remove surface oil and debris, and then blow dry.

[0163] Step 2: Laser shock peening system construction 1. Preparation of sacrificial layer and constrained layer: 1) Cover the surface of TA1 prepared in step 1 with a 120 μm thick aluminum foil as a sacrificial layer 3 to absorb laser energy and generate plasma shock waves.

[0164] 2) Place K9 glass (3 mm thick) on top of the aluminum foil as the constraint layer 4 and apply uniform pressure with a rigid pressure block to ensure the efficiency of shock wave pressure transmission.

[0165] 2. Sample fixation: Install the assembled sample on the high temperature resistant fixture 1 to ensure that there is no displacement during the laser impact process.

[0166] Step 3: High temperature environment control 1. Heating system settings: 1) Place the fixture 1 and the sample on a programmable heating table 6 and use a PID temperature control system with a temperature accuracy of ±5°C.

[0167] 2. Temperature stabilization: 1) Raise the temperature to the target temperature of 800°C at a rate of 10°C / min and keep it at that temperature for 15 min to make the temperature of the entire sample uniform.

[0168] 2) Use an infrared thermal imager to monitor the surface temperature of the sample in real time to ensure thermal equilibrium.

[0169] Step 4: Laser shock parameter optimization 1. Laser configuration: 1) A high-power Q-switched Nd:YAG laser (wavelength 1064 nm, pulse width 15 ns) with a spot diameter of 2 mm, laser energy 1 J, and pulse frequency 10 Hz was used.

[0170] 2. Impact path planning: 1) Laser beam 5 is incident vertically; 2) A zigzag scanning path is used with an overlap rate of 50% between adjacent light spots to ensure uniform surface treatment.

[0171] Step 5: Multi-pass laser shock peening 1. Repeat the shock five times on the same area, replacing the aluminum foil after each shock.

[0172] 2. Water quench immediately after each impact to lock the metastable FCC phase.

[0173] Step 6: Microstructure and phase composition analysis 1. Cross-section preparation: Cut the strengthened zone in half along the X direction and along the direction of shock wave propagation (Z); mechanically grind and polish the resulting cross-section (ZX plane) to a mirror surface.

[0174] 2. After removal, transmission Kikuchi diffraction (TKD) was used to confirm the FCC phase morphology and content. The results showed that the FCC phase was needle-shaped directly below the shock wave, with a content of approximately 3%.

[0175] Step 6: Mechanical properties test Microhardness: Load 200 g, hold for 15 s, measure 5 points on the impact surface and take the average: Vickers hardness increases from 104 HV to 118 HV.

[0176] Comparative Example 3 A method for improving the strength and toughness matching of titanium alloys, with an increased overlap ratio, comprising the following steps: 1. Material selection: Industrial TC4 was selected and the TC4 titanium plate was cut into small specimens of 50 mm × 50 mm × 5 mm (±0.1 mm).

[0177] 2. Annealing treatment: 1) TC4: Under argon protection, keep at 950℃ for 3h, then air cool to fully dissolve the β phase and stabilize the α phase.

[0178] 3.Surface treatment: 1) Use 120-2500 grit sandpaper to mechanically polish the sample surface to ensure that the surface roughness Ra ≤ 0.2 μm.

[0179] 2) Perform ultrasonic cleaning in anhydrous ethanol for 20 min to remove surface oil and debris, and then blow dry.

[0180] Step 2: Laser shock peening system construction 1. Preparation of sacrificial layer and constrained layer: 1) Cover the TC4 surface prepared in step 1 with a 120 μm thick aluminum foil as a sacrificial layer 3 to absorb laser energy and generate plasma shock waves.

[0181] 2) Place K9 glass (3 mm thick) on top of the aluminum foil as the constraint layer 4 and apply uniform pressure with a rigid pressure block to ensure the efficiency of shock wave pressure transmission.

[0182] 2. Sample fixation: Install the assembled sample on the high temperature resistant fixture 1 to ensure that there is no displacement during the laser impact process.

[0183] Step 3: High temperature environment control 1. Heating system settings: 1) Place the fixture 1 and the sample on a programmable heating table 6 and use a PID temperature control system with a temperature accuracy of ±5°C.

[0184] 2. Temperature stabilization: 1) Raise the temperature to the target temperature of 500°C at a rate of 10°C / min and keep it at that temperature for 15 min to make the temperature of the entire sample uniform.

[0185] 2) Use an infrared thermal imager to monitor the surface temperature of the sample in real time to ensure thermal equilibrium.

[0186] Step 4: Laser shock parameter optimization 1. Laser configuration: 1) A high-power Q-switched Nd:YAG laser (wavelength 1064 nm, pulse width 15 ns) with a spot diameter of 3 mm, laser energy 5 J, and pulse frequency of 10 Hz was used.

[0187] 2. Impact path planning: 1) Laser beam 5 is incident vertically; 2) A zigzag scanning path is used, with an overlap rate of 75% between adjacent light spots.

[0188] Step 5: Multi-pass laser shock peening 1. Repeat the shock five times on the same area, replacing the aluminum foil after each shock.

[0189] 2. Water quench immediately after each impact to lock the metastable FCC phase.

[0190] Step 6: Microstructure and phase composition analysis 1. Cross-section preparation: Cut the strengthened zone in half along the X direction and along the direction of shock wave propagation (Z); mechanically grind and polish the resulting cross-section (ZX plane) to a mirror surface.

[0191] 2. FIB-TKD: Thin sections were prepared using a focused ion beam (FIB) on the ZX plane, below the shock wave, at a depth of 200 μm. After removal, analysis using transmission Kikuchi diffraction (TKD) revealed no FCC phase at a depth of 200 μm.

[0192] In summary, the present invention provides a method for improving the strength and toughness matching of titanium alloy by inducing FCC phase through high temperature impact deformation. The temperature of high temperature treatment will directly affect the degree of phase transformation, and the overlap rate will affect the effect of laser shock, thereby affecting the degree of phase transformation. The present invention proposes to preheat titanium and titanium alloys to 300-600°C to reduce the energy required for HCP to FCC phase transformation, making the phase transformation easier to occur, and combining high strain rate (≥10 6 s -1) impact deformation, directly inducing the HCP to FCC phase transformation under the synergistic effect of dynamic stress and temperature. Utilizing high-temperature and high-speed impact deformation technology, an FCC phase content of up to 40% was achieved in pure titanium (2.3 times that of traditional methods), and for the first time, 20% FCC phase control was achieved in TC4 alloy. The FCC phase synergistically strengthens with nanotwins and residual compressive stress, accelerating grain refinement and improving strength-plasticity matching, increasing the material's fatigue life by two orders of magnitude and solving the "strength-plasticity inversion" problem. The process parameters are highly controllable, suitable for complex geometries and high-strength components, and have a wider applicability than traditional rolling annealing, providing an efficient, low-cost, and mass-producible solution for strengthening and toughening titanium alloys.

[0193] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for improving the strength-toughness matching of titanium alloy by inducing FCC phase through high temperature impact deformation, characterized in that: include: After the base material (2) is annealed and surface treated, it is covered with a sacrificial layer (3) and a constraint layer (4) in sequence, and after uniform pressure is applied, it is placed on a heating platform (6) of a high-temperature impact deformation device for preheating. The energy required for the transformation of the HCP phase into the FCC phase is reduced by preheating. The heating temperature and laser shock parameters are set. After multiple laser shock strengthening, high-temperature and high-speed impact deformation is used to directly induce the HCP phase to transform into the FCC phase under the synergistic effect of dynamic stress-temperature. The FCC phase forms a synergistic strengthening effect with nano twins and residual compressive stress, thereby accelerating the grain refinement process and improving the strength-plasticity matching, thereby achieving the high-temperature impact deformation-induced FCC phase to improve the strength-toughness matching of the titanium alloy; the base material (2) is industrial pure titanium or titanium alloy.

2. The method of improving the strength-toughness matching of titanium alloy by inducing FCC phase through high temperature impact deformation according to claim 1, characterized in that: The annealing treatment of industrial pure titanium includes: keeping the temperature at 600-800° C. for 1-4 hours under argon protection, and then air cooling; The annealing treatment of the titanium alloy includes: keeping the temperature at 900-980° C. for 1-4 hours under argon protection, and then air cooling; The surface treatment comprises: mechanically polishing the sample surface using sandpaper of 120 to 2500 meshes in sequence to a surface roughness of Ra≤0.2 μm; and then performing ultrasonic cleaning in anhydrous ethanol for 10-30 minutes.

3. The method of improving the strength-toughness matching of titanium alloy by inducing FCC phase through high temperature impact deformation according to claim 1, characterized in that: The sacrificial layer (3) is a high-purity aluminum foil; the thickness of the sacrificial layer (3) is 100-300 μm.

4. The method of improving the strength-toughness matching of titanium alloy by inducing FCC phase through high temperature impact deformation according to claim 1, characterized in that: The constraining layer (4) is K9 glass; the thickness of the constraining layer (4) is 1-5 mm.

5. The method of improving the strength-toughness matching of titanium alloy by inducing FCC phase through high temperature impact deformation according to claim 1, characterized in that: The heating platform (6) is a programmable heating platform that uses a PID temperature control system with a temperature accuracy of ±5°C; the heating rate is 10°C / min, the preheating temperature is 300~600°C, and the holding time is 10~15min; the heating platform (6) also uses an infrared thermal imager to monitor the surface temperature of the base material (2) in real time.

6. The method of improving the strength-toughness matching of titanium alloy by inducing FCC phase through high temperature impact deformation according to claim 1, characterized in that: The laser shock parameters include: spot diameter 2-4 mm, laser energy 1-10 J, and pulse frequency 8-15 Hz.

7. The method of improving the strength-toughness matching of titanium alloy by inducing FCC phase through high temperature impact deformation according to claim 1, characterized in that: The scanning path of the laser shock peening is zigzag, and the overlap rate of adjacent light spots is 30% to 50%.

8. The method of improving the strength-toughness matching of titanium alloy by inducing FCC phase through high temperature impact deformation according to claim 1, characterized in that: The laser shock peening is repeated 1 to 5 times in the same area, and a new sacrificial layer (3) is replaced after each laser shock peening; and water quenching is immediately performed after each laser shock peening is completed.

9. The method of improving the strength-toughness matching of titanium alloy by inducing FCC phase through high temperature impact deformation according to claim 1, characterized in that: After the laser shock strengthening, the FCC phase is needle-shaped and curved directly below the shock wave, with a width of 20-30 nm and a content of 10%-40%.

10. The method of improving the strength-toughness matching of titanium alloy by inducing FCC phase through high temperature impact deformation according to claim 1, characterized in that: It also includes: using transmission Kikuchi diffraction and transmission electron microscopy to analyze and confirm the FCC phase morphology and content; using microhardness or tensile testing to test the mechanical properties of the substrate material (2); The high temperature impact deformation device comprises: A heating platform (6) for providing a high temperature environment; A clamp (1) is disposed on a heating platform (6) and is used to fix the base material (2); A laser beam emitting device is located above the base material (2) and is used for emitting a laser beam (5) vertically incident on the constrained layer (4) on the surface of the base material (2), thereby performing laser shock strengthening on the surface of the base material (2).

Citation Information

Cited By

  • Laser welding process method for copper-aluminum composite flexible busbar

    CN121571811A

  • Equiaxial biphase nanocrystalline pure titanium as well as preparation method and application thereof

    CN122279745A