Brake pad adaptive to carbon-ceramic brake disc and preparation process of brake pad
By introducing a three-dimensional network structure of nano-silicon nitride modified ceramic fiber, carbon fiber and aramid fiber into the brake pad, combined with graphene composite lubricating particles and multiphase gradient binder, the wear, noise and friction coefficient fluctuation problems of carbon-ceramic brake discs are solved, and high-performance brake pad preparation is achieved.
Patent Information
- Application Number
- CN202511292890.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-11
- Publication Date
- 2025-10-14
- Estimated Expiration
- 2045-09-11
AI Technical Summary
Existing brake pads cannot effectively match carbon-ceramic brake discs, and have problems such as severe wear, loud noise, large fluctuations in friction coefficient, and high cost. In addition, traditional brake pads cannot meet the high performance requirements of carbon-ceramic discs.
Nano-silicon nitride modified ceramic fiber, carbon fiber and aramid fiber are used to form a three-dimensional network structure, combined with graphene composite lubricating particles, multiphase gradient binder and friction modifier. Through segmented curing and surface treatment, a brake pad with good thermal conductivity, shear resistance, wear resistance, good toughness and stable friction coefficient is prepared.
The brake pads and carbon ceramic discs are well matched, with the wear rate reduced by 40%, the noise reduced by 60%, the friction coefficient stable in a wide temperature range, the wear rate reduced by 70%, and the noise controlled below 65dB.
Smart Images

Figure SMS_1
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of brake pads, in particular to a brake pad matched with a carbon-ceramic brake disc and a preparation process thereof. BACKGROUND
[0002] The carbon-ceramic brake disc has become a core component of the braking system of high-end vehicles due to its advantages of light weight, high temperature resistance, stable friction performance, etc. It can effectively improve the braking response speed and sustained braking capacity of vehicles, and meet the stringent requirements of high-performance driving on the braking system. However, the high efficiency of the carbon-ceramic brake disc is highly dependent on the matched brake pad, and the performance of the brake pad directly affects the braking safety, stability and service life of the carbon-ceramic disc.
[0003] At present, there are two typical problems with brake pads matched with carbon-ceramic brake discs: special carbon-ceramic brake pads can match the performance of carbon-ceramic discs, but they need to be produced by a deposition process, which takes 15-20 days and is very costly, significantly increasing the cost of the vehicle braking system; traditional brake pads have a short production cycle (only about 2 days) and low cost, but due to the extremely high hardness of the carbon-ceramic disc, the traditional brake pads are prone to severe wear, and the hard abrasive ingredients (such as steel fibers and some oxides) contained therein can scratch the surface of the carbon-ceramic disc and damage the structure of the carbon-ceramic disc. In addition, the friction coefficient of the traditional brake pad fluctuates greatly in a wide temperature range, and it is prone to thermal recession at high temperatures, and the high-frequency noise problem unique to the carbon-ceramic system is also difficult to solve. SUMMARY
[0004] In view of the problems in the prior art, the present application provides a brake pad matched with a carbon-ceramic brake disc and a preparation process thereof, so that the prepared brake pad has the advantages of good heat conduction, shear resistance and wear resistance, good toughness, noise reduction, stable friction coefficient, low temperature reliability, high temperature braking force, stable braking and the like.
[0005] To achieve the above object, the technical scheme is as follows: The present application discloses a brake pad matched with a carbon-ceramic brake disc, which comprises the following components in percentage by weight: reinforcing fibers 25-57%, lubricant 22-49%, binder 7-17%, friction modifier 7.2-28.1%, and filler 3-23%. The reinforcing fibers are at least one of nano-silicon nitride modified ceramic fiber, carbon fiber and aramid fiber.
[0006] By setting the above technical scheme, the formula improves the structural strength and heat resistance by a high proportion of reinforcing fibers; the lubricant ensures stable friction and reduces wear and noise; the binder ensures the structural integrity at high temperatures; the friction modifier optimizes the friction coefficient; and the filler adjusts the density and cost. The synergistic effect of each component enables the obtained brake pad to be matched with the carbon-ceramic disc, achieving the effects of low wear, high temperature resistance, stable performance and noise reduction.
[0007] Preferably, the composition of the reinforcing fiber is as follows: nano-silicon nitride modified ceramic fiber 14-26%, carbon fiber 5-15%, and aramid fiber 6-16%, the carbon fiber being short fibers with a length of 3-6 mm.
[0008] By setting the above technical solution, the carbon fiber has good thermal conductivity, can quickly conduct the friction heat generated during braking, avoids local overheating, and at the same time enhances the shear resistance of the brake pad and reduces wear; the aramid fiber has excellent toughness, can absorb the vibration energy generated during braking, effectively suppresses the generation of noise, and at the same time improves the overall toughness of the brake pad; the nano-silicon nitride modified ceramic fiber, carbon fiber and aramid fiber are interwoven to form a three-dimensional network structure, which not only ensures the overall strength of the brake pad, but also avoids hard contact with the carbon ceramic brake disc. The carbon fiber is short cut to 3-6 mm, which is beneficial to uniform dispersion, can enhance the shear resistance of the brake pad and efficiently conduct heat.
[0009] Preferably, the preparation method of the nano-silicon nitride modified ceramic fiber is as follows: a1, adding KH-560 into an ethanol-water solution with a volume ratio of 3:1 to prepare a 5% concentration KH-560 ethanol-water solution; a2, placing the aluminum silicate fiber into the KH-560 ethanol-water solution, stirring in a constant temperature water bath at 65-70℃ for 2-2.5h, then taking out the fiber and drying in an oven at 120-130℃ for 2h to obtain activated fiber; a3, weighing the activated fiber and nano-silicon nitride at a mass ratio of 8:2, placing them into a high-speed blender, and stirring at a speed of 3500-4000r / min for 30-40min to make the nano-silicon nitride uniformly coated on the surface of the fiber; a4, placing the mixed fiber in a nitrogen-protected furnace, calcining at 850℃ for 2.5h, and then crushing to 3-7mm to obtain the nano-silicon nitride modified ceramic fiber.
[0010] By setting the above technical solution, the coating layer formed by coating the nano-silicon nitride on the surface of the activated fiber can provide good lubricity, avoiding scratching the carbon ceramic brake disc during braking; at the same time, the nano-silicon nitride dispersed on the surface of the fiber enhances the interfacial bonding force between the fiber and other components, and improves the structural stability of the brake pad in high temperature environment.
[0011] Preferably, the length of the aluminum silicate fiber is 5-10mm, and the particle size of the nano-silicon nitride is 20-50nm.
[0012] By setting the above technical scheme, the length of the aluminum silicate fiber is 5-10 mm, which can not only ensure the formation of effective skeleton support in the brake pad matrix and enhance the overall structural strength of the material, but also facilitate uniform mixing with other components; the particle size of the nano-silicon nitride is 20-50 nm, and the small particle size enables it to be more uniformly coated on the surface of the aluminum silicate fiber, increasing the contact area, which not only enhances the interfacial bonding force between the fiber and other components, but also improves the density and uniformity of the lubricating protective film by virtue of the nano-scale characteristics, reducing the hard contact between the fiber and the brake disc.
[0013] Preferably, the composition of the lubricant is as follows, in terms of weight percentage of the total components: graphene composite lubricating particles 8-18%, composite graphite 13-23%, and antimony sulfide 1-8%; The preparation method of the graphene composite lubricating particles is as follows: b1. Weigh natural graphite, graphene, and molybdenum disulfide according to a mass ratio of 6:1:3, and put them into a ball mill, and ball mill at a speed of 250 r / min for 1.5 h, then add 12% of the total solid mass of modified phenolic resin solution, and stir until a uniform paste is formed; b2. Spray the obtained paste, set the inlet temperature to 200℃, and the outlet temperature to 90℃, to obtain particles with a particle size of 60-120 μm, then place the particles in a nitrogen atmosphere and solidify them at 210-220℃ for 2-2.5 h, to obtain graphene composite lubricating particles.
[0014] By setting the above technical scheme, the antimony sulfide can improve the stability of the friction coefficient in a high-temperature environment, ensuring that the brake pad still has strong braking force at high temperatures; the graphene has excellent lubricating properties, which can enhance the continuity of the lubricating film; the natural graphite provides basic lubrication; the molybdenum disulfide can enhance the lubricating effect under high load, and the three components work together to achieve stable lubrication in a wide temperature range.
[0015] Preferably, the particle size of the natural graphite is 5-10 μm; the graphene is single-layered with a particle size of 0.5-2 μm; the particle size of the molybdenum disulfide is 1-3 μm; the modified phenolic resin is a modified phenolic resin with active groups such as rubber, cashew nut shell oil, and epoxy resin introduced, and the modified phenolic resin is dissolved in a 50% ethanol solution to form a modified phenolic resin solution.
[0016] By setting the above technical scheme, controlling the particle size of the natural graphite, graphene, and molybdenum disulfide can make them uniformly dispersed to enhance the lubricating and wear-reducing effect; introducing active groups into the modified phenolic resin can improve the compatibility with other components and the toughness of the material, and dissolving it in an ethanol solution can facilitate mixing and dispersion, ensuring stable material performance.
[0017] Preferably, the composite graphite is uniformly mixed with flake graphite and expanded graphite at a mass ratio of 2:1, wherein the particle size of the flake graphite is 5-20 μm, and the particle size of the expanded graphite is 10-50 μm.
[0018] By setting the above technical solution, the flake graphite has good lubrication continuity and stability, and can provide basic lubrication at room temperature; the expanded graphite will expand due to heat at high temperature (usually above 200℃) to form a dense protective layer, reducing the direct friction between the brake pad and the carbon ceramic brake disc, and filling the micro-pores of the friction surface. By mixing at a ratio of 2:1, the balance of lubrication performance can be achieved in a wide temperature range. If the particle size difference between the flake graphite and the expanded graphite is too large (such as the flake graphite being above 100 μm and the expanded graphite being below 10 μm), layering may occur during mixing, resulting in unbalanced local lubrication performance and affecting the friction stability of the brake pad. A similar particle size range of the two can avoid mixing layering, ensure the adaptation to the friction surface of the carbon ceramic brake disc, prevent scratching or friction vibration, and thus form a continuous and stable lubrication film, improving the friction stability of the brake pad.
[0019] Preferably, the binder is a multi-phase gradient binder, and the preparation method is as follows: c1. Take cashew nut shell oil modified phenolic resin, polyether ether ketone, and nitrile rubber powder at a mass ratio of 6:3:1, and add them into a twin-screw extruder, set the temperature of zone 1 to 130℃, the temperature of zone 2 to 160℃, and the temperature of zone 3 to 190℃, and set the screw speed to 250 r / min, and then melt blend; c2. Cut the extrudate obtained in c1 into particles of 3-5 mm with a granulator, dry the particles in a vacuum drying box at 78-80℃ for 4.5-5 h, freeze the particles in an environment at -30℃ for 3 h, take out the particles, and place them at room temperature, complete the temperature impact modification, and obtain the multi-phase gradient binder.
[0020] By setting the above technical solution, the limitation of the melt blending step enables the uniform compounding of the three raw materials, laying a foundation for the gradient performance of the binder; cutting the extrudate into 3-5 mm particles and drying them at 78-80℃ for 4.5-5 h can effectively remove moisture and volatile matter, ensuring the stability of the particle state; and the temperature impact modification of freezing the particles at -30℃ for 3 h and then restoring them to room temperature can optimize the internal stress distribution and interfacial bonding force of the material, ultimately forming a multi-phase gradient binder that can play a dominant role at different temperature ranges, and the particle-like form facilitates the direct addition of the binder as a raw material to the mixing process of brake pad preparation, ensuring its uniform dispersion with other components and fully exerting the binding effect.
[0021] Preferably, the composition of the friction modifier is as follows, based on the weight percentage of the total components: potassium titanate whiskers 3-13%, cashew nut shell oil friction powder 4-14%, and ultra-fine tin powder 0.2-1.1%, and the particle size of the ultra-fine tin powder is 3-5 μm. The composition of the filler is as follows: barite powder 2-12%, barium sulfate 1-11%.
[0022] By setting the above technical scheme, the potassium titanate whisker has a needle-like structure, which can enhance the structural strength of the brake pad, adjust the friction coefficient, and have a certain noise reduction effect; the cashew shell oil friction powder can improve the friction performance of the brake pad at low temperature, make the low-temperature braking more reliable, and reduce the noise during braking; the superfine tin powder has small particles, which can fill the micro voids of the friction surface, improve the contact state of the friction surface, reduce the friction fluctuation, and make the braking more stable. The particle size of the superfine tin powder is 3-5 μm, which can fill the voids of the friction surface, improve the contact state, and reduce the friction fluctuation. The barite powder and the barium sulfate act as inert fillers, which can adjust the density of the brake pad and assist in stabilizing the friction coefficient; the cooperation of these components makes the prepared brake pad have the advantages of good heat conduction, shear resistance and wear resistance, good toughness, noise reduction, stable friction coefficient, low-temperature reliability, high-temperature braking force, stable braking, etc.
[0023] The application also discloses a preparation process of the brake pad based on the adaptive carbon ceramic brake disc. S1, the nano silicon nitride modified ceramic fiber, carbon fiber and aramid fiber are taken in proportion, dried in an oven at 80 DEG C for 3h, and then added into a high-speed mixer after cooling to room temperature, stirred at a speed of 1100-1200r / min for 12-15min to make the fibers uniformly dispersed; S2, the multi-phase gradient binder softened in advance is added into the mixed fibers, the speed is adjusted to 1450-1500r / min, and then the graphene composite lubricating particles, composite graphite, potassium titanate whisker, cashew shell oil friction powder, antimony sulfide, barite powder, barium sulfate and superfine tin powder are sequentially added, and stirred at a speed of 1700-1800r / min for 25-30min, and the stirring cylinder wall is cleaned every 5min to ensure uniform mixing; S3, the brake pad preparation mold is preheated to 80 DEG C, the material mixed in S2 is loaded into the mold, a pressure of 7.5-8MPa is applied for pre-pressing for 3-4min, then the pressure is increased to 20-22MPa, and the pressure is maintained for 10-12min; S4, the material in the mold in S3 is subjected to a staged curing treatment: Stage one: heat preservation at 125-130 DEG C for 1.5-2h; Stage two: heating to 175-180 DEG C, and heat preservation for 2-2.5h; Stage three: heating to 215-220 DEG C, and heat preservation for 2-2.5h; Then, cooling to room temperature at a rate of 5 DEG C / min; S5, surface grinding the cured brake pad to make the surface roughness Ra reach 1.6-3.2 mu m, and finally placed in an oven at 200 DEG C for secondary curing for 3.5-4 h to remove residual volatile matter, so that the brake pad adapted to the carbon ceramic brake disc is obtained.
[0024] By setting the above technical scheme, the process ensures uniform combination of raw materials through fiber drying and dispersion, step-by-step high-speed mixing, improves density through segmented pre-pressing, reduces internal stress through step-by-step curing and controlled cooling, optimizes performance through surface treatment and secondary curing, and finally obtains a brake pad with stable structure and good friction surface adaptability, which can adapt to carbon ceramic brake discs and guarantee braking effect.
[0025] The beneficial effects of the present application are: The nano-silicon nitride modified ceramic fiber, carbon fiber and aramid fiber interweave to form a three-dimensional network structure, which not only ensures the overall strength of the brake pad, but also avoids hard contact with the carbon ceramic brake disc. The graphene composite lubricating particles are uniformly filled in the pores of the three-dimensional network, and during braking, these lubricating particles will synchronously release lubricating components to form a structure of "high-strength skeleton + self-adaptive lubricating film". This structure enables the brake pad to have a relatively high friction coefficient of 0.42-0.46 while maintaining a relatively low wear rate.
[0026] The cashew nut shell oil modified phenolic resin ensures the bonding strength of the brake pad at room temperature; the polyether ether ketone (PEEK) improves the structural strength of the material at high temperature; and the nitrile rubber powder enhances the toughness of the adhesive, so that the brake pad can better resist impact during braking. In addition, the multi-phase gradient adhesive plays a dominant role at different temperature stages. At low temperature (<200 DEG C), the cashew nut shell oil modified phenolic resin ensures good bonding performance; at medium temperature (200-400 DEG C), the polyether ether ketone (PEEK) maintains the structural strength of the material; and at high temperature (>400 DEG C), the elasticity of the nitrile rubber plays a role in buffering stress. This temperature response characteristic cooperates with the "temperature response release" characteristic of the graphene composite lubricating particles to make the friction coefficient fluctuate by ≤0.02 in the temperature range of 100-600 DEG C, which is much better than the traditional formula where the friction coefficient fluctuates by >0.05.
[0027] The aramid fiber and cashew nut shell oil friction powder together form an elastic buffer layer that can absorb more than 60% of the friction vibration energy, effectively reducing noise. The needle-like structure of the potassium titanate whisker can disperse the stress generated during braking and prevent local wear from intensifying. Through synergistic effect, the noise peak of the brake pad is controlled below 65 dB, and at the same time, the wear rate of the brake pad is reduced by 40%, and the wear rate of the carbon ceramic brake disc is reduced by more than 70%.
[0028] The flaky graphite has good lubricating continuity and stability, and can provide basic lubrication at room temperature; the expanded graphite can form a dense protective layer due to thermal expansion at high temperature (usually above 200 DEG C), reducing the direct friction between the brake pad and the carbon ceramic brake disc, and filling the micro-pores of the friction surface. By mixing at a ratio of 2:1, the balance of lubricating performance can be achieved in a wide temperature range. DETAILED DESCRIPTION
[0029] To make the objectives, technical solutions, and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the embodiments of the present application. Obviously, the described embodiments are only some of the embodiments of the present application, rather than all the embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by those of ordinary skill in the art without creative work fall within the scope of protection of the present application.
[0030] Embodiment 1: The present embodiment discloses a brake pad adapted to a carbon ceramic brake disc, and the composition of the brake pad in terms of weight percentage is as follows: nano-silicon nitride modified ceramic fiber 26%, graphene composite lubricating particle 8%, multi-phase gradient binder 7%, carbon fiber 10.8%, aramid fiber 6%, composite graphite 13%, potassium titanate whisker 9%, cashew shell oil friction powder 6%, antimony sulfide 8%, barite powder 3%, barium sulfate 3%, and ultra-fine tin powder 0.2%. The composite graphite is uniformly mixed with flaky graphite and expanded graphite at a mass ratio of 2:1, the particle size of the flaky graphite is 5 μm, and the particle size of the expanded graphite is 10 μm. The carbon fiber is a chopped fiber, and the length thereof is 3 mm. The particle size of the ultra-fine tin powder is 3 μm.
[0031] The preparation method of the nano-silicon nitride modified ceramic fiber is as follows: a1, KH-560 is added to an ethanol-water solution with a volume ratio of 3:1 to configure a 5% concentration of KH-560 ethanol-water solution; a2, aluminum silicate fibers with a length of 5 mm are put into the KH-560 ethanol-water solution, stirred in a constant temperature water bath at 65 DEG C for 2 h, and then the fibers are taken out and dried in an oven at 120 DEG C for 2 h to obtain activated fibers; a3, the activated fibers and nano-silicon nitride with a particle size of 20 nm are weighed at a mass ratio of 8:2 and put into a high-speed blender, and stirred at a speed of 3500 r / min for 30 min to make the nano-silicon nitride uniformly coated on the surface of the fibers; a4, the mixed fibers are placed in a nitrogen-protected furnace and calcined at 850 DEG C for 2.5 h, and then crushed to 3 mm after cooling to obtain the nano-silicon nitride modified ceramic fiber.
[0032] The preparation method of the graphene composite lubricating particle is as follows: b1. Take natural graphite with a particle size of 5 μm, graphene with a single-layer particle size of 0.5 μm, and molybdenum disulfide with a particle size of 1 μm in a mass ratio of 6:1:3, put them into a ball mill, and mill at a speed of 250 r / min for 1.5 h, then add 12% of the total solid mass of modified phenolic resin solution, and stir until a uniform paste is formed; wherein the modified phenolic resin is a modified phenolic resin with active groups such as rubber, cashew nut shell oil, and epoxy resin introduced, and the modified phenolic resin is dissolved in a 50% ethanol solution to form a modified phenolic resin solution; b2. Spray granulate the obtained paste, set the inlet temperature to 200℃ and the outlet temperature to 90℃, obtain particles with a particle size of 60 μm, then place the particles in a nitrogen atmosphere and cure them at 210℃ for 2 h to obtain graphene composite lubricating particles.
[0033] The preparation method of the multi-phase gradient binder is as follows: c1. Take cashew nut shell oil modified phenolic resin, polyether ether ketone, and nitrile rubber powder in a mass ratio of 6:3:1, add them into a twin-screw extruder, set the temperature of zone 1 to 130℃, the temperature of zone 2 to 160℃, and the temperature of zone 3 to 190℃, and set the screw speed to 250 r / min, and perform melt blending; c2. Cut the extrudate obtained in c1 into 3 mm particles, dry them in a vacuum drying oven at 78℃ for 4.5 h, and then freeze the particles in an environment at -30℃ for 3 h, take them out and place them at room temperature, complete the temperature impact modification, and obtain a multi-phase gradient binder.
[0034] The embodiment also discloses a preparation process of a brake pad adapted to a carbon ceramic brake disc, which comprises the following steps: S1. Take nano-silicon nitride modified ceramic fiber, carbon fiber, and aramid fiber in proportion, dry them in an oven at 80℃ for 3 h, cool them to room temperature, and then add them into a high-speed mixer and stir them at a speed of 1100 r / min for 12 min to uniformly disperse the fibers; S2. Add the multi-phase gradient binder softened in advance to the mixed fibers, adjust the stirring speed to 1450 r / min, and stir them for 18 min, then add graphene composite lubricating particles, composite graphite, potassium titanate whiskers, cashew nut shell oil friction powder, antimony sulfide, barite powder, barium sulfate, and ultra-fine tin powder in sequence, stir them at a speed of 1700 r / min for 25 min, and clean the stirring cylinder wall every 5 min to ensure uniform mixing; S3. Preheat a brake pad preparation mold to 80℃, put the mixed material in S2 into the mold, apply a pressure of 7.5 MPa for pre-pressing for 3 min, then increase the pressure to 20 MPa, and keep the pressure for 10 min; S4. Perform staged curing treatment on the material in the mold in S3: Stage one: keep temperature at 125℃ for 1.5h; Stage two: increase temperature to 175℃, keep for 2h; Stage three: increase temperature to 215℃, keep for 2h; Then cool down to room temperature with a rate of 5℃ / min; S5, polish the surface of the cured brake pad to make the surface roughness Ra reach 1.6μm, and finally place it in an oven at 200℃ for secondary curing for 3.5h to remove residual volatile components, thus obtaining the brake pad adapted to the carbon-toughened brake disc.
[0035] Example 2: This example discloses a brake pad adapted to the carbon-toughened brake disc, the composition of which is as follows in terms of weight percentage: nano-silicon nitride modified ceramic fiber 14%, graphene composite lubricating particle 18%, multi-phase gradient binder 17%, carbon fiber 5%, aramid fiber 12%, composite graphite 21.9%, potassium titanate whisker 3%, cashew nut shell oil friction powder 4%, antimony sulfide 1%, barite powder 2%, barium sulfate 1%, and ultra-fine tin powder 1.1%. The composite graphite is obtained by uniformly mixing flake graphite and expanded graphite at a mass ratio of 2:1, the particle size of the flake graphite is 20μm, and the particle size of the expanded graphite is 50μm. The carbon fiber is short fiber with a length of 6mm. The particle size of the ultra-fine tin powder is 5μm.
[0036] The preparation method of the nano-silicon nitride modified ceramic fiber is as follows: a1, add KH-560 to an ethanol-water solution with a volume ratio of 3:1 to prepare a 5% concentration KH-560 ethanol-water solution; a2, put aluminum silicate fibers with a length of 10mm into the KH-560 ethanol-water solution, stir in a constant temperature water bath at 70℃ for 2.5h, then take out the fibers and dry them in an oven at 130℃ for 2h to obtain activated fibers; a3, weigh the activated fibers and nano-silicon nitride with a particle size of 50nm at a mass ratio of 8:2, put them into a high-speed blender, and stir at a speed of 4000r / min for 40min to make the nano-silicon nitride uniformly coated on the surface of the fibers; a4, put the mixed fibers into a furnace under nitrogen protection, calcine at 850℃ for 2.5h, and then crush to 7mm after cooling, thus obtaining the nano-silicon nitride modified ceramic fiber.
[0037] The preparation method of the graphene composite lubricating particle is as follows: b1, weigh natural graphite with a particle size of 10μm, graphene with a single layer particle size of 2μm, and molybdenum disulfide with a particle size of 3μm at a mass ratio of 6:1:3, put them into a ball mill, and ball mill at a speed of 250r / min for 1.5h, then add a modified phenolic resin solution accounting for 12% of the total solid mass, and stir until a uniform paste is formed; wherein the modified phenolic resin is a modified phenolic resin into which active groups such as rubber, cashew nut shell oil, and epoxy resin are introduced, and the modified phenolic resin is dissolved in a 50% ethanol solution to form a modified phenolic resin solution; b2, the obtained paste is spray granulated, the inlet temperature is set to 200℃, the outlet temperature is set to 90℃, particles with a particle size of 120μm are obtained, and then the particles are cured in a nitrogen atmosphere at 220℃ for 2.5h to obtain graphene composite lubricating particles.
[0038] The preparation method of the multi-phase gradient binder is as follows: c1, cashew nut shell oil modified phenolic resin, polyether ether ketone, and nitrile rubber powder are weighed according to a mass ratio of 6:3:1, added into a twin-screw extruder, and melt blended by setting the temperature of zone 1 to 130℃, the temperature of zone 2 to 160℃, the temperature of zone 3 to 190℃, and the screw rotation speed to 250r / min; c2, the extrudate obtained in c1 is cut into 5mm particles by a particle cutter, dried in a vacuum drying box at 80℃ for 5h, and then frozen in an environment at -30℃ for 3h, taken out, and placed at room temperature to complete temperature impact modification, thereby obtaining a multi-phase gradient binder.
[0039] The embodiment also discloses a preparation process of a brake pad matched with a carbon ceramic brake disc, which comprises the following steps: S1, nano-silicon nitride modified ceramic fibers, carbon fibers, and aramid fibers are taken according to a proportion, dried in an oven at 80℃ for 3h, and then added into a high-speed mixer after cooling to room temperature, stirred at a rotation speed of 1200r / min for 15min to uniformly disperse the fibers; S2, the multi-phase gradient binder is added into the mixed fibers, the rotation speed is adjusted to 1500r / min, and the mixture is stirred for 20min, then graphene composite lubricating particles, composite graphite, potassium titanate whiskers, cashew nut shell oil friction powder, antimony sulfide, barite powder, barium sulfate, and ultra-fine tin powder are added in sequence, and the mixture is stirred at a rotation speed of 1800r / min for 30min, and the stirring cylinder wall is cleaned every 5min to ensure uniform mixing; S3, a brake pad preparation mold is preheated to 80℃, the material mixed in S2 is loaded into the mold, a pressure of 8MPa is applied for pre-pressing for 4min, then the pressure is increased to 22MPa, and the pressure is maintained for 12min; S4, the material in the mold in S3 is subjected to staged curing treatment: Stage one: heat preservation at 130℃ for 2h; Stage two: heating to 180℃, heat preservation for 2.5h; Stage three: heating to 220℃, heat preservation for 2.5h; then cooling to room temperature at a cooling rate of 5℃ / min; S5, surface grinding the cured brake pad to make the surface roughness Ra reach 3.2pm, and finally placing it in an oven at 200℃ for secondary curing for 4h to remove residual volatile components, thereby obtaining the brake pad adapted to the carbon-toughened brake disc.
[0040] In this embodiment, the composition of the brake pad adapted to the carbon-toughened brake disc is as follows in terms of weight percentage: nano-silicon nitride modified ceramic fiber 18%, graphene composite lubricating particle 11%, multi-phase gradient binder 12%, carbon fiber 9%, aramid fiber 10%, composite graphite 15%, potassium titanate whisker 7%, cashew nut shell oil friction powder 7%, antimony sulfide 4%, barite powder 4%, barium sulfate 2.5%, and superfine tin powder 0.5%. The composite graphite is uniformly mixed with flake graphite and expanded graphite at a mass ratio of 2:1, the particle size of the flake graphite is 10pm, and the particle size of the expanded graphite is 30pm. The carbon fiber is a chopped fiber with a length of 4mm. The particle size of the superfine tin powder is 4pm.
[0041] The preparation method of the nano-silicon nitride modified ceramic fiber is as follows: a1, adding KH-560 into an ethanol-water solution with a volume ratio of 3:1 to configure a 5% concentration KH-560 ethanol-water solution; a2, placing aluminum silicate fibers with a length of 7mm into the KH-560 ethanol-water solution, stirring in a constant-temperature water bath at 67℃ for 2.2h, then taking out the fibers and drying them in an oven at 125℃ for 2h to obtain activated fibers; a3, weighing the activated fibers and nano-silicon nitride with a particle size of 35nm at a mass ratio of 8:2, placing them into a high-speed blender, and stirring at a speed of 3700r / min for 35min to uniformly coat the nano-silicon nitride on the surface of the fibers; a4, placing the mixed fibers in a nitrogen-protected furnace, calcining at 850℃ for 2.5h, and then crushing to 5mm after cooling to obtain the nano-silicon nitride modified ceramic fiber.
[0042] The preparation method of the graphene composite lubricating particle is as follows: b1, weighing natural graphite with a particle size of 7pm, graphene with a single-layer particle size of 1pm, and molybdenum disulfide with a particle size of 2pm at a mass ratio of 6:1:3, placing them into a ball mill, and ball milling at a speed of 250r / min for 1.5h, then adding a modified phenolic resin solution accounting for 12% of the total mass of solids, and stirring until a uniform paste is formed; The modified phenolic resin is a modified phenolic resin with active groups such as rubber, cashew nut shell oil, and epoxy resin, and the modified phenolic resin is dissolved in a 50% ethanol solution to form a modified phenolic resin solution; b2, the obtained paste is spray granulated, the inlet temperature is set to 200 DEG C, the outlet temperature is set to 90 DEG C, the granules with a particle size of 90 mu m are obtained, then the granules are placed in a nitrogen atmosphere, and cured at 215 DEG C for 2h, thereby the graphene composite lubricating granules are obtained.
[0043] The preparation method of the multi-phase gradient binder is as follows: c1, the cashew shell oil modified phenolic resin, the polyether ether ketone, and the butyronitrile rubber powder are weighed according to the mass ratio of 6:3:1, and are added into a double screw extruder, the temperature of zone 1 is set to 130 DEG C, the temperature of zone 2 is set to 160 DEG C, the temperature of zone 3 is set to 190 DEG C, and the screw rotation speed is 250 r / min, and then the melt blending is carried out; c2, the extrudate obtained in c1 is cut into 4mm granules by a granulator, and is dried in a vacuum drying box at 79 DEG C for 4.7h, and then the granules are frozen at-30 DEG C for 3h, and are taken out and placed at room temperature, the temperature impact modification is completed, and the multi-phase gradient binder is obtained.
[0044] The embodiment also discloses a preparation process of the brake pad matched with the carbon ceramic brake disc. S1, the nano silicon nitride modified ceramic fiber, the carbon fiber, and the aramid fiber are taken according to the proportion, are placed in an oven at 80 DEG C and dried for 3h, and after cooling to room temperature, are added into a high-speed mixer and stirred at a rotation speed of 1150 r / min for 13 min, so that the fibers are uniformly dispersed; S2, the multi-phase gradient binder which is softened in advance is added into the mixed fibers, the rotation speed is adjusted to 1470 r / min, and stirring is carried out for 19 min, then the graphene composite lubricating granules, the composite graphite, the potassium titanate whisker, the cashew shell oil friction powder, the antimony sulfide, the barite powder, the barium sulfate, and the ultra-fine tin powder are sequentially added, stirring is carried out at a rotation speed of 1750 r / min for 27 min, and the stirring cylinder wall is cleaned every 5 min to ensure uniform mixing; S3, the brake pad preparation mold is preheated to 80 DEG C, the material mixed in S2 is loaded into the mold, a pressure of 7.7 MPa is applied for pre-pressing for 3.5 min, and then the pressure is increased to 21 MPa, and pressure maintaining is carried out for 11 min; S4, the material in the mold in S3 is subjected to staged curing treatment: Stage one: 127 DEG C is kept for 1.7h; Stage two: the temperature is increased to 177 DEG C, and keeping is carried out for 2h; Stage three: the temperature is increased to 217 DEG C, and keeping is carried out for 2h; Then, the temperature is cooled to room temperature at a rate of 5 DEG C / min; S5, the surface of the cured brake pad is ground, so that the surface roughness Ra reaches 2.5 mu m, and finally the brake pad is placed in an oven at 200 DEG C for secondary curing for 3.5h, and residual volatile components are removed, thereby the brake pad matched with the carbon ceramic brake disc is obtained.
[0045] Comparative Example 1: A brake pad adapted to a carbon-ceramic brake disc, the difference between the brake pad and Example 3 is that the nano-silicon nitride modified ceramic fiber is replaced by ordinary ceramic fiber.
[0046] Comparative Example 2: A brake pad adapted to a carbon-ceramic brake disc, the difference between the brake pad and Example 3 is that the graphene composite lubricating particles are replaced by equal amount of flake graphite.
[0047] Comparative Example 3: A brake pad adapted to a carbon-ceramic brake disc, the difference between the brake pad and Example 3 is that the multi-phase gradient binder is replaced by ordinary phenolic resin.
[0048] Comparative Example 4: A brake pad adapted to a carbon-ceramic brake disc, the difference between the brake pad and Example 3 is that the carbon fiber is not added and is replaced by equal amount of ceramic fiber.
[0049] Comparative Example 5: A brake pad adapted to a carbon-ceramic brake disc, the difference between the brake pad and Example 3 is that the aramid fiber is not added and is replaced by equal amount of carbon fiber.
[0050] Comparative Example 6: A brake pad adapted to a carbon-ceramic brake disc, the difference between the brake pad and Example 3 is that the composite graphite is only flake graphite (without expanded graphite).
[0051] Comparative Example 7: A brake pad adapted to a carbon-ceramic brake disc, the difference between the brake pad and Example 3 is that the potassium titanate whisker is not added.
[0052] Comparative Example 8: A brake pad adapted to a carbon-ceramic brake disc, the difference between the brake pad and Example 3 is that the amount of antimony sulfide is adjusted to 0.2%.
[0053] Comparative Example 9: A brake pad adapted to a carbon-ceramic brake disc, the difference between the brake pad and Example 3 is that in S3 of the preparation process, the pre-pressing does not use segmented pressing (directly 22 MPa).
[0054] Comparative Example 10: A brake pad adapted to a carbon-ceramic brake disc, the difference between the brake pad and Example 3 is that the highest temperature of the step curing is 180°C.
[0055] Comparative Example 11: A brake pad adapted to a carbon ceramic brake disc, the difference between the brake pad and example 3 is that the nano-silicon nitride modified ceramic fiber is not coated with silicon nitride (it has been activated, but not coated with nano-silicon nitride and subsequent calcination treatment, i.e. the fiber surface lacks a nano-silicon nitride coating layer).
[0056] Comparative example 12: A brake pad adapted to a carbon ceramic brake disc, the difference between the brake pad and example 3 is that all components in the preparation process are mixed at one time.
[0057] The brake pads obtained in examples 1-3 and comparative examples 1-12 were tested for friction coefficient, wear rate, thermal decay and noise performance, wherein: 1. Friction coefficient test Reference basis: refer to GB / T5763-2018 "Automobile brake pad" Test steps: 1) Cut a 30mm x 30mm x 8mm sample from the finished brake pad, polish the friction surface to flatness with sandpaper, clean with alcohol and dry.
[0058] 2) Fix the carbon ceramic brake disc (diameter 280mm) on the rotating disc of the constant speed friction tester, install the sample under the pressurizing arm, and ensure that the friction surface is completely attached.
[0059] 3) Set the test parameters: contact pressure 0.5MPa, sliding speed 4m / s, temperature range 100-500℃ (every 50℃ is a test point).
[0060] 4) At each temperature point, first heat for 10min, then start the tester for continuous friction for 20s, record the real-time friction force, and repeat the test for 3 times at each temperature point.
[0061] 5) Calculate the friction coefficient: μ = friction force ÷ (contact pressure x sample area), take the average value of 3 tests as the friction coefficient at this temperature point, and calculate the full temperature range friction coefficient fluctuation value (maximum value - minimum value).
[0062] 2. Wear rate test Reference basis: refer to ISO6310:2012 "Road vehicle brake pad wear test method" Test steps: 1) Weigh the initial mass of the brake pad sample (accurate to 0.001g), and measure the initial thickness of the carbon ceramic brake disc with a laser thickness gauge (take the average value of 3 points).
[0063] 2) Install the sample and carbon ceramic disc on the brake bench, set the simulated working conditions: vehicle speed 40-60km / h, braking deceleration 2.5m / s², braking interval 40s, total cycle 800 times.
[0064] 3) After the test, clean the surface of the test sample and carbon-ceramic disc with alcohol, and then re-weigh and measure the thickness after drying.
[0065] 4) Calculate the wear rate: Brake pad wear rate = (initial mass - mass after test) ÷ total braking work (unit: g / J) Carbon-ceramic disc wear rate = (initial average thickness - average thickness after test) ÷ total braking work (unit: mm / J).
[0066] 3. Hot degradation performance test Reference basis: Refer to GB / T34346-2017 "Automotive Brake Friction Material High Temperature Performance Test Method" Test steps: 1) Measure the friction coefficient μ1 at room temperature (25°C) according to the friction coefficient test method.
[0067] 2) Place the brake pad sample into the high-temperature furnace, and heat it to 550°C for 25 min, then immediately remove it and install it on the carbon-ceramic disc which has been preheated to 550°C.
[0068] 3) Test the friction coefficient μ2 at 550°C under the same parameters.
[0069] 4) Calculate the hot degradation rate: (μ2 ÷ μ1) × 100%.
[0070] 4. Noise test Reference basis: Refer to SAE J2521:2019 "Noise Measurement Method for Brake Pad and Brake Disc Assembly" Test steps: 1) Fix the brake system with brake pad and carbon-ceramic disc on the test bench in a semi-anechoic chamber (background noise ≤ 25 dB).
[0071] 2) Place a sound level meter (frequency range 100-8000 Hz) at a distance of 1.2 m from the brake disc, and align it with the center of the friction area.
[0072] 3) Set the brake pressure gradient: 0.3 MPa, 0.5 MPa, 0.7 MPa, brake 15 times under each pressure, each brake lasts for 3 s, interval 10 s.
[0073] 4) Record the noise peak value of each brake, and calculate the proportion of the number of times that the noise is ≥ 80 dB (noise occurrence rate).
[0074] The results are shown in Table 1.
[0075] Table 1 Performance parameters of brake pads obtained from Examples 1-3 and Comparative Examples 1-12
[0076] From Table 1 combined with Example 3, it can be seen that: In Comparative Example 1, the average friction coefficient decreased by 28.3%, and the carbon ceramic disc wear rate increased by 286.4%. The possible reason is that the ordinary ceramic fiber surface is smooth, and the adhesion to the matrix is weak, which is easy to fall off and become abrasive during braking, and aggravate the wear of the carbon ceramic disc. While the nano silicon nitride modified layer enhances the interface bonding through chemical bonding, and at the same time forms a lubricating protective film by using the low hardness characteristics of silicon nitride to reduce hard contact wear.
[0077] In Comparative Example 2, the friction coefficient fluctuation value increased by 305.6%, and the noise occurrence rate increased by 725%. The possible reason is that the interlayer slip characteristics of graphene in the graphene composite lubricating particles can fill the micro concave of the friction surface, making the contact more uniform. Using an equal amount of flake graphite to replace the graphene composite lubricating particles, the lubrication continuity of flake graphite is insufficient, leading to increased friction vibration and noise.
[0078] In Comparative Example 3, the thermal decay rate decreased by 27.2%, and the brake pad wear rate increased by 180%. The possible reason is that ordinary phenolic resin begins to decompose and become brittle above 300°C, resulting in structural collapse at high temperatures; the PEEK component in the multi-phase gradient binder maintains strength at high temperatures, and the nitrile rubber buffers stress, allowing the brake pad to maintain a stable structure at 550°C.
[0079] In Comparative Example 4, the friction coefficient decreased by 30.4%, and the thermal decay rate decreased by 25%. The possible reason is that the high thermal conductivity of carbon fiber can quickly disperse friction heat, avoiding the attenuation of the friction coefficient caused by local high temperature; without adding carbon fiber, the heat is concentrated on the friction surface, causing the lubricating components to fail quickly and the thermal decay to be obvious.
[0080] In Comparative Example 5, the noise peak increased by 27.7%, and the brake pad wear rate increased by 136%. The possible reason is that the high toughness of aramid fiber can absorb braking vibration energy, and at the same time enhance the material's tear resistance; the absence of aramid fiber increases the material's brittleness, making it prone to high-frequency vibration during friction, and the surface material is prone to peeling, aggravating the wear.
[0081] In Comparative Example 6, the friction coefficient fluctuation value increased by 227.8%, and the carbon ceramic disc wear rate increased by 208.5%. The possible reason is that expanded graphite expands to form a sealed lubricating layer at high temperatures, filling the pores on the surface of the carbon ceramic disc; when only flake graphite is used, the high-temperature lubrication is insufficient, leading to increased friction coefficient fluctuation and increased carbon ceramic disc wear.
[0082] In Comparative Example 7, the average friction coefficient decreased by 19.6%, and the brake pad wear rate increased by 104%. The possible reason is that the needle-like structure of potassium titanate whiskers can enhance the shear resistance of the friction surface, and at the same time, the friction coefficient is increased by the micro-convex effect; the absence of potassium titanate whiskers reduces the material's resistance to deformation, reducing the friction coefficient and accelerating the wear.
[0083] In the comparative example 8, the thermal recession rate is reduced by 15.2%, and the average friction coefficient is reduced by 17.4%. The possible reason is that antimony sulfide can stabilize the friction coefficient at high temperature, and when the amount of antimony sulfide is seriously insufficient, the friction coefficient above 500℃ decreases significantly, resulting in a decrease in thermal recession rate.
[0084] In the comparative example 9, the brake pad wear rate increases by 80%, and the friction coefficient fluctuation value increases by 172.2%. The possible reason is that the segmented pressurization reduces the internal porosity of the material through gradual densification, and the direct pressurization leads to uneven density, resulting in local stress concentration during friction, accelerated wear and decreased friction stability.
[0085] In the comparative example 10, the carbon ceramic disc wear rate increases by 274.6%, and the thermal recession rate decreases by 19.6%. The possible reason is that insufficient curing temperature leads to incomplete crosslinking of the multiphase gradient binder, which easily releases unreacted components at high temperature, pollutes the surface of the carbon ceramic disc and accelerates wear, and the insufficient structural strength leads to increased thermal recession.
[0086] In the comparative example 11, the friction coefficient is reduced by 15.2%, and the carbon ceramic disc wear rate increases by 150.8%. The possible reason is that the absence of the lubricating effect of the silicon nitride coating layer increases the direct friction between the ceramic fiber and the carbon ceramic disc, which not only reduces the friction efficiency, but also scratches the surface of the carbon ceramic disc.
[0087] In the comparative example 12, the friction coefficient fluctuation value increases by 138.9%, and the noise occurrence rate increases by 400%. The possible reason is that step-by-step mixing ensures uniform dispersion of the fibers to form a three-dimensional network, and one-time mixing easily leads to fiber agglomeration, resulting in uneven contact of the friction surface, increased vibration and noise.
[0088] In summary, the present application achieves a significant effect of increasing the friction coefficient by 53.3% (relative to comparative example 3) and reducing the carbon ceramic disc wear rate by 78.4% through the synergistic effect of the three core innovative components and the optimized preparation process, while solving the problems of thermal recession and noise in traditional formulations. Under the premise of a cost of only 1 / 5 of the special carbon ceramic brake pad, it reaches a level close to the special carbon ceramic brake pad.
[0089] The above examples are only used to illustrate the technical solutions of the present application, but not to limit it; although the present application has been described in detail with reference to the foregoing examples, those skilled in the art should understand that they can modify the technical solutions described in the foregoing examples, or make equivalent substitutions for part of the technical features; and these modifications or substitutions do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present application.
Claims
1. A brake pad adapted for a carbon-ceramic brake disc, characterized in that: The brake pad comprises the following components by weight: 25-57% reinforcing fiber, 22-49% lubricant, 7-17% binder, 7.2-28.1% friction modifier and 3-23% filler. The reinforcing fiber is at least one of nano-silicon nitride modified ceramic fiber, carbon fiber and aramid fiber.
2. The brake pad adapted for carbon-ceramic brake disc according to claim 1, characterized in that: Calculated by weight percentage of the total components, the components of the reinforcing fiber are as follows: 14-26% of nano silicon nitride modified ceramic fiber, 5-15% of carbon fiber and 6-16% of aramid fiber.
3. The brake pad adapted for carbon-ceramic brake disc according to claim 1 or 2, characterized in that: The preparation method of nano silicon nitride modified ceramic fiber is as follows: a1. Add KH-560 to an ethanol-water solution with a volume ratio of 3:1 to prepare a 5% concentration of KH-560 ethanol-water solution; a2. Place aluminum silicate fiber in a KH-560 ethanol-water solution and stir in a constant temperature water bath at 65-70°C for 2-2.5 hours. Then, take out the fiber and dry it in an oven at 120-130°C for 2 hours to obtain activated fiber. a3. Weigh activated fiber and nano-silicon nitride in a mass ratio of 8:2, place in a high-speed blender, and stir at a speed of 3500-4000 rpm for 30-40 min to evenly coat the nano-silicon nitride on the fiber surface; a4. Place the mixed fibers in a nitrogen-protected furnace, calcine at 850°C for 2.5 hours, and crush to 3-7 mm after cooling to obtain nano-silicon nitride modified ceramic fibers.
4. The brake pad adapted for a carbon-ceramic brake disc according to claim 3, characterized in that: The length of the aluminum silicate fiber is 5-10 mm, and the particle size of the nano silicon nitride is 20-50 nm.
5. The brake pad adapted for a carbon-ceramic brake disc according to claim 2, characterized in that: The lubricant comprises the following components, calculated in weight percentage of the total components: 8-18% of graphene composite lubricating particles, 13-23% of composite graphite, and 1-8% of antimony sulfide; The preparation method of graphene composite lubricating particles is as follows: b1. Natural graphite, graphene, and molybdenum disulfide were weighed in a mass ratio of 6:1:3, placed in a ball mill, and ball-milled at a speed of 250 r / min for 1.5 h. Subsequently, a modified phenolic resin solution accounting for 12% of the total solid mass was added and stirred until a uniform paste was formed; b2. The obtained paste is spray granulated with the inlet temperature set to 200°C and the outlet temperature set to 90°C to obtain particles with a particle size of 60-120 μm. The particles are then placed in a nitrogen atmosphere and cured at 210-220°C for 2-2.5 hours to obtain graphene composite lubricating particles.
6. The brake pad adapted for a carbon-ceramic brake disc according to claim 5, characterized in that: The particle size of natural graphite is 5-10 μm; the graphene is a single layer with a particle size of 0.5-2 μm; the particle size of molybdenum disulfide is 1-3 μm; the modified phenolic resin is a modified phenolic resin introduced with active groups such as rubber, cashew nut shell oil, and epoxy resin, and the modified phenolic resin is dissolved in a 50% ethanol solution to form a modified phenolic resin solution.
7. The brake pad adapted for a carbon-ceramic brake disc according to claim 6, characterized in that: The composite graphite is prepared by uniformly mixing flake graphite and expanded graphite in a mass ratio of 2:1, wherein the particle size of the flake graphite is 5-20 μm, and the particle size of the expanded graphite is 10-50 μm.
8. The brake pad adapted for a carbon-ceramic brake disc according to claim 7, characterized in that: The binder is a multiphase gradient binder, and its preparation method is as follows: c1. Cashew nut shell liquid-modified phenolic resin, polyetheretherketone, and nitrile rubber powder were weighed in a mass ratio of 6:3:1, added to a twin-screw extruder, and the temperature of zone 1, zone 2, and zone 3 were set to 130°C, 160°C, and 190°C, and the screw speed was set to 250 r / min for melt blending; c2. The extrudate obtained in c1 is cut into 3-5 mm particles by a pelletizer, dried in a vacuum drying oven at 78-80°C for 4.5-5 hours, and frozen at -30°C for 3 hours. The particles are then taken out and placed at room temperature to complete the temperature shock modification and obtain a multiphase gradient binder.
9. The brake pad adapted for a carbon-ceramic brake disc according to claim 8, characterized in that: The friction modifier comprises the following components, calculated by weight percentage of the total components: 3-13% potassium titanate whiskers, 4-14% cashew nut shell oil friction powder, and 0.2-1.1% ultrafine tin powder, wherein the particle size of the ultrafine tin powder is 3-5 μm; The composition of the filler is as follows: barite powder 2-12%, barium sulfate 1-11%.
10. A process for preparing a brake pad adapted to a carbon-ceramic brake disc according to claim 9, characterized in that: The preparation process includes the following steps: S1. Take nano-silicon nitride modified ceramic fiber, carbon fiber, and aramid fiber in proportion, place them in an oven at 80°C and dry for 3 hours. After cooling to room temperature, add them to a high-speed mixer and stir at a speed of 1100-1200 r / min for 12-15 minutes to evenly disperse the fibers. S2, add the multiphase gradient binder softened in advance to the mixed fiber, adjust the speed to 1450-1500r / min, stir for 18-20min, then add graphene composite lubricating particles, composite graphite, potassium titanate whiskers, cashew nut shell oil friction powder, antimony sulfide, barite powder, barium sulfate, ultrafine tin powder in sequence, stir at a speed of 1700-1800r / min for 25-30min, and stop every 5min to clean the mixing tank wall to ensure uniform mixing; S3. Preheat the brake pad preparation mold to 80°C, place the mixed material from S2 into the mold, apply a pre-pressing pressure of 7.5-8 MPa for 3-4 minutes, then increase the pressure to 20-22 MPa and maintain the pressure for 10-12 minutes; S4. Perform step-by-step curing on the material in the mold in S3: Stage 1: Keep warm at 125-130℃ for 1.5-2h; Stage 2: Heat to 175-180°C and keep warm for 2-2.5 hours; Stage 3: Heat to 215-220℃ and keep warm for 2-2.5h; Then it was cooled to room temperature at a cooling rate of 5°C / min; S5. The surface of the cured brake pad is ground to a surface roughness Ra of 1.6-3.2 μm. Finally, the brake pad is placed in an oven at 200° C. for secondary curing for 3.5-4 hours to remove residual volatiles, thereby obtaining a brake pad suitable for the carbon ceramic brake disc.
Citation Information
Patent Citations
Winch brake pad and manufacture method thereof
CN102900795A
Wear-resistant noise-reducing bionic double-layer ceramic brake pad and preparation method thereof
CN114110061A
Compounding process of carbon-ceramic brake disc compounded with carbon fibers
CN117466625A
Commercial disc brake without phenolic resin base and preparation method of commercial disc brake
CN117754934A
Disc brake pad and its manufacture
JP1999153165A
Cited By
Carbon ceramic disc brake pad and preparation method thereof
CN122628486A