Thixotropy quantitative characterization method of lithium slag-tailing cemented filling slurry

Through multi-stage thixotropy testing and thixotropic quantitative characterization methods, the problem of inaccurate thixotropy experimental results of lithium slag-tailings cemented filling slurry was solved, more accurate thixotropy analysis was achieved, production costs and waste emissions were reduced, and a scientific mine filling theory was provided.

CN120801106APending Publication Date: 2025-10-17NORTH CHINA UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202510922817.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-04
Publication Date
2025-10-17

AI Technical Summary

Technical Problem

The thixotropy test results of existing lithium slag-tailings cemented filling slurries have low accuracy. The traditional three-interval thixotropy test method is greatly affected by the test procedure. Different shear times and rates lead to large errors in the results and cannot accurately reflect the actual thixotropy level of the flow in the pipeline.

Method used

A multi-stage thixotropic test method is adopted, including the static stage, the variable shear stage and the structural recovery stage, combined with the thixotropic quantitative characterization method. By constructing a curve of the apparent viscosity changing with time, the thixotropy of the slurry is calculated using the structural recovery rate and flocculation rate formula to reduce experimental errors.

Benefits of technology

The accuracy of quantitative characterization of thixotropy of lithium slag-tailings cemented filling slurry is improved, which reduces mine production costs, reduces solid waste emissions, provides a scientific theoretical basis for filling work, and meets environmental protection needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120801106A_ABST
    Figure CN120801106A_ABST
Patent Text Reader

Abstract

The invention provides a thixotropy quantitative characterization method of lithium slag-tailings cemented filling slurry, and relates to the technical field of metal ore remaining tailings and lithium slag treatment. Comprising the following steps: preparing to-be-tested slurry and setting test parameters; starting a rheometer to test the to-be-tested slurry to obtain multi-stage thixotropic data of the to-be-tested slurry; according to the multi-stage thixotropic data, constructing a curve of the apparent viscosity changing along with the test time; carrying out data fitting on the curve by adopting a thixotropic quantitative characterization method so as to obtain specific fitting parameters and a flocculation rate; calculating the thixotropy of the slurry by using a structural recovery rate formula; and analyzing and characterizing the thixotropy of the slurry by using the obtained structure recovery rate and flocculation rate to obtain a characterization result. The problem that in the prior art, the thixotropy experiment result is low in accuracy is solved.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of processing of metal mine tailings and lithium residue, and particularly relates to a method for quantitatively characterizing the thixotropy of lithium residue-tailing sand cemented filling slurry. BACKGROUND

[0002] With the vigorous development of the global lithium battery industry, the production is increasing year by year, and the annual output is as high as 1.2 million tons, and the cumulative emission is 10 million tons. The utilization rate of lithium residue is low, and the existing treatment means is mainly open-air storage, which causes serious land waste and environmental pollution. Lithium residue contains rich amorphous silicon aluminum components and has pozzolanic activity, which can be used as a cementing supplementary material for preparing slurry. A lot of research has been conducted to explore the effectiveness of lithium residue as a cementing supplementary material, and it has been confirmed that lithium residue can significantly enhance the mechanical properties of the filling body and also change the rheological properties of the slurry. Lithium residue-containing filling slurry is a new type of mine filling material, which is mainly prepared from tailings, lithium residue and cement as raw materials, and is transported to the underground goaf by a conveying pipeline to form a filling body with certain strength in the underground goaf, thereby stabilizing the underground space.

[0003] A rotational rheometer is an important tool for testing the rheological properties of a sample, which can provide real-time sample parameters and provide a certain theoretical basis for the research on material conveying in the industrial and scientific fields. The rotational rheometer applies continuous shear to the sample by rotating motion with controlled torque and shear rate. The change of the sample with time is detected by applying continuous shear. Through the measurement of torque and rotational speed, the corresponding rheological parameters can be calculated.

[0004] Thixotropy is described as the phenomenon that the viscosity continuously decreases with shear when shear is applied to a sample in a static state, and the viscosity recovers after the shear is stopped. With further research, thixotropy is summarized as the transition between solid-like and liquid-like caused by flow, and the thixotropy of the reaction slurry also becomes based on the change of viscosity. Since the change of shear stress lags behind the change of shear rate due to thixotropy, the early thixotropy experiment uses a thixotropic ring to characterize, which increases the shear rate from 0 s -1 to a certain value within a certain time, and then decreases to 0 s -1The area surrounded by the rising line and the falling line of the gamma-t diagram is taken as the thixotropy capacity of the fluid. However, the test is greatly affected by the test procedure, and different shear time and shear rate can increase or decrease the thixotropic loop area, and the shear history at each point of the test is different, and the test cannot be constrained as a variable. Subsequently, a three-interval thixotropy test (3ITT) was proposed, in which the slurry was sheared at a constant shear rate, the shear history of each point was fixed, and the shear process was divided into three steps: static stage, shear stage and structure recovery stage. A constant and small shear rate is used in the static stage to obtain the viscosity of the slurry in the static stage, a constant high shear rate is used in the shear stage to destroy the microstructure of the fluid, and the slurry enters a state of dynamic balance between recovery and destruction. In the structure recovery stage, the same shear method as in the static stage is used to obtain the viscosity recovery degree of the fluid, which characterizes the thixotropy of the slurry. However, the use of too large or too small shear rate in the recovery stage can increase or decrease the viscosity recovery time and the viscosity reorganization rate, resulting in certain errors in the results and failing to reflect the true thixotropy level of the fluid in the pipeline.

[0005] In the traditional three-interval thixotropy test, the ratio of the apparent viscosity in the structure recovery stage to that in the static stage is often used to quantify the thixotropy of the fluid. The ratio of the apparent viscosities at different times is not a constant value and is accidental, and the change of the data taken at will will greatly affect the judgment of the thixotropy of the fluid by the researchers. SUMMARY

[0006] In order to overcome the shortcomings of the prior art, the purpose of the present application is to provide a method for quantifying and characterizing the thixotropy of lithium residue-tailing sand cemented filling slurry, which solves the problem of low accuracy of thixotropy test results in the prior art.

[0007] To achieve the above-mentioned purpose, the present application provides the following solutions:

[0008] A method for quantifying and characterizing the thixotropy of lithium residue-tailing sand cemented filling slurry, comprising:

[0009] Preparing the slurry to be tested and setting the test parameters;

[0010] Starting the rheometer to test the slurry to be tested and obtaining multi-stage thixotropy data of the slurry to be tested;

[0011] According to the multi-stage thixotropy data, a curve of apparent viscosity changing with test time is constructed.

[0012] The curve is data-fitted using the thixotropy quantification characterization method to obtain specific fitting parameters and flocculation rate;

[0013] The thixotropy of the slurry is calculated using the formula of structure recovery rate;

[0014] The obtained structure recovery rate and flocculation rate are used to analyze and characterize the thixotropy of the slurry, and a characterization result is obtained.

[0015] Preferably, the preparation of the slurry to be tested and the setting of the test parameters include:

[0016] The sample to be tested is placed in the coaxial cylinder flow, and the rheometer test rotor is installed in the corresponding card slot of the rheometer;

[0017] The test parameters in the rheometer software are set to prepare the slurry to be tested, and the slurry with different ratios of lithium-containing slag filling is obtained.

[0018] Preferably, the test parameters include:

[0019] The static stage shear method, the static stage shear rate, the static stage test time, the sampling point number, the variable shear stage shear method, the variable shear stage shear rate, the variable shear stage test time, the structure recovery stage shear method, the structure recovery stage shear rate, and the structure recovery stage test time.

[0020] Preferably, the multi-stage thixotropy data include:

[0021] The static stage thixotropy data, the variable shear stage thixotropy data, and the structure recovery stage thixotropy data.

[0022] Preferably, the static stage adopts a controlled shear rate method for shearing, and the shear rate is set to a constant 0.01 s -1 , the holding time is 60 s, and the sampling point number is 100;

[0023] The variable shear stage adopts a controlled shear rate method for shearing, and the shear rate is increased from 0.01 s -1 to 80 s -1 at a constant speed, the rising time is 60 s, and the sampling point number is 100;

[0024] The structure recovery stage adopts a controlled shear rate method for shearing, and the shear rate is set to a constant 0.01 s -1 , the holding time is 60 s, and the sampling point number is 100.

[0025] Preferably, the thixotropy quantification characterization method is used to perform data fitting on the curve to obtain specific fitting parameters and a flocculation rate, including:

[0026] The static stage thixotropy data and the structure recovery stage thixotropy data are fitted using a thixotropy quantification characterization formula to obtain an apparent viscosity asymptote value of the corresponding stage;

[0027] The flocculation rate is determined according to the apparent viscosity asymptote value.

[0028] Preferably, the expression of the apparent viscosity evolution model is:

[0029] η = η ∞ + (η(0) - η ∞ ) e -ξt ;

[0030] wherein η ∞ is the apparent viscosity asymptotic value, η(0) is the initial viscosity, ξ is the flocculation rate, and t is the relative test time.

[0031] Preferably, the formula of the structure recovery rate is:

[0032]

[0033] wherein η ∞3 is the apparent viscosity of the sample in the structure recovery phase, and η ∞1 is the apparent viscosity of the sample in the static phase.

[0034] The present application discloses the following technical effects:

[0035] The present application provides a thixotropy quantitative characterization method of lithium slag-tailings cemented filling material slurry, comprising:

[0036] The method comprises the following steps: preparing a to-be-tested slurry and setting test parameters; starting a rheometer to test the to-be-tested slurry, and obtaining multi-stage thixotropy data of the to-be-tested slurry; constructing a curve of apparent viscosity changing with test time according to the multi-stage thixotropy data; adopting a thixotropy quantification characterization method to perform data fitting on the curve to obtain specific fitting parameters and flocculation rate; using a formula of structure recovery rate to calculate the thixotropy of the slurry; and using the obtained structure recovery rate and flocculation rate to analyze and characterize the thixotropy of the slurry, and obtaining a characterization result. BRIEF DESCRIPTION OF DRAWINGS

[0037] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the prior art, the following will briefly introduce the drawings needed to be used in the embodiments. Obviously, the drawings in the following description are only some embodiments of the present application, and for those skilled in the art, other drawings can also be obtained from these drawings without any creative labor.

[0038] Figure 1 A thixotropy quantification characterization method flow chart of lithium slag-tailing cemented filling slurry is provided for the embodiments of the present application.

[0039] Figure 2 A shear rate changing with test time diagram of the thixotropy test method with a variable shear stage and three intervals is provided for the embodiments of the present application, in which the horizontal coordinate is experimental test time, and the vertical coordinate is shear rate value changing with test time. The test is divided into three stages, the first stage is a static stage, the second stage is a shear stage, and the third stage is a structure recovery stage.

[0040] Figure 3The static phase and structure recovery phase apparent viscosity curve schematic diagram obtained by the thixotropy test method with the variable shear stage three intervals provided by the embodiment of the present application is shown in the figure, the horizontal coordinate is the experimental test time, and the vertical coordinate is the apparent viscosity value obtained by the experiment, and no data is recorded in the second test stage;

[0041] Figure 4 The static phase and structure recovery phase apparent viscosity curve model fitting curve schematic diagram obtained by the thixotropy test method with the variable shear stage three intervals provided by the embodiment of the present application is shown in the figure, wherein, Figure 4 (a) is a static phase apparent viscosity curve model fitting curve schematic diagram, in which the solid line is a fitting curve, and the dotted line is an experimental test value, Figure 4 (b) is a recovery phase apparent viscosity curve model fitting curve schematic diagram, in which the solid line is a fitting curve, and the dotted line is an experimental test value;

[0042] Figure 5 The structure recovery rate schematic diagram of the slurry under different lithium residue contents provided by the embodiment of the present application is shown in the figure, the structure recovery rate value of the slurry under different lithium residue contents;

[0043] Figure 6 The structure recovery phase apparent viscosity curve model fitting curve schematic diagram obtained by the thixotropy test method with the variable shear stage three intervals provided by the embodiment of the present application is shown in the figure, in which the horizontal coordinate is the experimental test time, and the vertical coordinate is the apparent viscosity value obtained by the experiment, and the solid line is the apparent viscosity evolution model fitting curve;

[0044] Figure 7 The structure recovery rate schematic diagram of the slurry under different lithium residue contents provided by the embodiment of the present application is shown in the figure, the structure recovery rate value of the slurry under different lithium residue contents. DETAILED DESCRIPTION

[0045] The technical solutions in the embodiments of the present application will be described clearly and completely below with reference to the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative labor fall within the scope of protection of the present application.

[0046] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the present application will be further described in detail below with reference to the drawings and specific embodiments.

[0047] As Figure 1 shown, the present application provides a thixotropy quantitative characterization method of lithium residue-tailing sand cemented filling slurry, comprising:

[0048] Step 100: preparing the slurry to be tested and setting the test parameters;

[0049] Step 200: Start the rheometer to test the slurry to be tested, and obtain multi-stage thixotropy data of the slurry to be tested;

[0050] Step 300: According to the multi-stage thixotropy data, a curve of apparent viscosity changing with test time is constructed; wherein the 3-stage data is constructed.

[0051] Step 400: The curve is fitted by using a thixotropy quantitative characterization method to obtain specific fitting parameters and flocculation rate;

[0052] Step 500: The thixotropy of the slurry is calculated by using the formula of structure recovery rate;

[0053] Step 600: The thixotropy of the slurry is analyzed and characterized by using the obtained structure recovery rate and flocculation rate, and a characterization result is obtained.

[0054] Specifically, the structure recovery rates of different proportioning slurries are compared, and the experimental group with a larger structure recovery rate shows more obvious thixotropy. The flocculation rates of different proportioning slurries are compared, and the experimental group with a larger value shows faster aggregation of solid particles inside. That is, the structure recovery rate represents the thixotropy of the slurry, and the larger the structure recovery rate, the greater the thixotropy of the slurry.

[0055] Further, the preparation of the slurry to be tested and the setting of the test parameters include:

[0056] The sample to be tested is placed in the coaxial cylinder flow and placed in the corresponding slot of the rheometer, and the rheometer test rotor is installed;

[0057] The test parameters in the rheometer software are set for the preparation of the slurry to be tested, and different proportioning lithium-containing residue filling slurries are obtained.

[0058] Further, the test parameters include:

[0059] Static stage shear mode, static stage shear rate, static stage test time, sampling point number, variable shear stage shear mode, variable shear stage shear rate, variable shear stage test time, structure recovery stage shear mode, structure recovery stage shear rate, and structure recovery stage test time.

[0060] Specifically, the test temperature remains constant, and the time consumed by each stage of the prepared fluid remains constant.

[0061] Further, the multi-stage thixotropy data includes:

[0062] Static stage thixotropy data, variable shear stage thixotropy data, and structure recovery stage thixotropy data.

[0063] Further, the static stage adopts a control shear rate method for shearing, the shear rate is set to be constant 0.01 s -1 , the holding time is 60 s, and the sampling point number is 100.

[0064] The variable shear stage adopts a control shear rate method for shearing, the shear rate is increased from 0.01 s -1 to 80 s at a constant speed -1 , the rising time is 60 s, and the sampling point number is 100.

[0065] The structure recovery stage adopts a control shear rate method for shearing, the shear rate is set to be constant 0.01 s -1 , the holding time is 60 s, and the sampling point number is 100.

[0066] Further, the thixotropic quantitative characterization method is used to fit the curve to obtain specific fitting parameters and flocculation rates, including:

[0067] The thixotropic data of the static stage and the structure recovery stage are fitted by using a thixotropic quantitative characterization formula to obtain the apparent viscosity asymptotic value of the corresponding stage.

[0068] The flocculation rate is determined according to the apparent viscosity asymptotic value.

[0069] Specifically, the apparent viscosity-time curve based on the static stage and the structure recovery stage includes:

[0070] The apparent viscosity curve is constructed in the static stage, and the static stage apparent viscosity is taken as the y-axis and the static stage time is taken as the x-axis.

[0071] The apparent viscosity curve is constructed in the structure recovery stage, and the structure recovery stage apparent viscosity is taken as the y-axis and the structure recovery stage time is taken as the x-axis.

[0072] Further, the apparent viscosity curve with the test time of each stage is constructed, and the state equation and the structure evolution equation of the thixotropic material are obtained according to the classical structure dynamic evolution equation, and the equation is:

[0073]

[0074] Wherein, η(t) is the time-dependent apparent viscosity (Pa·s), λ(t) is the internal structure parameter of the slurry, is the shear rate (s -1 ).

[0075] The change of the slurry structure is mainly composed of three parts: the thermal motion of solid particles and shear rupture The transient structure parameter evolution equation can be expressed as:

[0076]

[0077] The solid particle thermal motion term of the slurry can be expressed as:

[0078]

[0079] where k1 is an empirical parameter related to the thermal motion of the solid particles in the slurry, and λ0 is an initial structure parameter of the slurry. The shear rupture term can be expressed as:

[0080]

[0081] where k2 is a parameter related to the shear rupture term.

[0082] Substituting the solid particle thermal motion term and the shear rupture term into the transient structure parameter evolution equation gives:

[0083] Simplifying the above equation gives:

[0084]

[0085] Let Equilibrium state λ s The following equation can be obtained:

[0086]

[0087] Integrating the transient structure parameter evolution equation gives:

[0088]

[0089] where C is a constant term coefficient.

[0090] The constant term C can be derived relative to the test time t = 0 as:

[0091]

[0092] where is the structure parameter when the relative test time is 0.

[0093] The structure parameter evolution equation can be rewritten as:

[0094]

[0095] Linking the structure evolution and the macroscopic apparent viscosity evolution using the Coussot state equation, the apparent viscosity can be expressed as:

[0096] η = η0(1 + λ);

[0097] Wherein, η is the apparent viscosity, η0, λ are material parameters.

[0098] The structure parameter evolution equation is substituted into the macroscopic apparent viscosity evolution equation, and the apparent viscosity evolution model is:

[0099]

[0100] In the apparent viscosity evolution model, let η ∞ = η e (1+λ s ) be the steady-state viscosity-related parameter, and η(0) = η0(1-λ0) be the initial viscosity, so as to facilitate writing, the apparent viscosity evolution model can be simplified as:

[0101] η = η ∞ +(η(0)-η ∞ )e -ξt ;

[0102] Wherein, η ∞ is the apparent viscosity asymptotic value, η(0) is the initial viscosity, ξ is the flocculation rate, and t is the relative test time.

[0103] The structure recovery rate (R) is the ratio of the slurry viscosity (η ∞3 ) in the recovery stage to the static stage viscosity (η ∞1 ), and the formula is:

[0104]

[0105] Wherein, η ∞3 is the apparent viscosity of the sample in the structure recovery stage, and η ∞1 is the apparent viscosity of the sample in the static stage.

[0106] Further, the structure recovery rates of the filling slurries with different lithium slag contents are shown in Table 1 as follows:

[0107] Table 1

[0108]

[0109] The fitting parameters of the filling slurries with different lithium slag contents are shown in Table 2 as follows:

[0110] Table 2

[0111]

[0112] Through the thixotropic test containing the three intervals of variable shear stage, the fitting error is small by using the thixotropic quantitative characterization method, which can reflect the apparent viscosity evolution in the static stage and the structure recovery stage, and provides a reference for the pipeline transportation of mines.

[0113] Specifically,Figure 2 The horizontal coordinate is the experimental test time, and the vertical coordinate is the shear rate value changing with the test time. The test is divided into three stages, the first stage is the static stage, the second stage is the shear stage, and the third stage is the structure recovery stage;

[0114] Figure 3 The horizontal coordinate is the experimental test time, and the vertical coordinate is the apparent viscosity value obtained by experiment. No data is recorded in the second stage of the test;

[0115] Figure 4 (a) is a schematic diagram of the apparent viscosity curve model fitting curve in the static stage. In the diagram, the solid line is the fitting curve, and the dotted line is the experimental test value, Figure 4 (b) is a schematic diagram of the apparent viscosity curve model fitting curve in the recovery stage. In the diagram, the solid line is the fitting curve, and the dotted line is the experimental test value;

[0116] Figure 5 is the structure recovery rate value of the slurry under different lithium slag contents;

[0117] Figure 6 is the horizontal coordinate of the experimental test time, and the vertical coordinate is the apparent viscosity value obtained by experiment. The solid line is the apparent viscosity evolution model fitting curve;

[0118] Figure 7 is the structuring rate value of the slurry under different lithium slag contents.

[0119] The various embodiments in the specification are described in a progressive manner, and each embodiment focuses on the difference from other embodiments. The same and similar parts between various embodiments can be referred to each other.

[0120] The principles and implementation modes of the present application are described by applying specific examples in this paper. The above description of the embodiments is only used to help understand the method of the present application and its core idea; at the same time, for those skilled in the art, according to the idea of the present application, the specific implementation mode and application range will be changed. In summary, the content of the specification should not be understood as a limitation of the present application.

Claims

1. A method for quantitatively characterizing the thixotropy of lithium slag-tailings cemented filling slurry, characterized in that: include: Prepare the slurry to be tested and set the test parameters; Starting the rheometer to test the slurry to be tested, and obtaining multi-stage thixotropic data of the slurry to be tested; Based on the multi-stage thixotropic data, a curve showing the change of apparent viscosity with test time was constructed; The curve is fitted with data using a thixotropic quantitative characterization method to obtain specific fitting parameters and flocculation rate; The thixotropy of the slurry was calculated using the formula for structural recovery rate; The obtained structural recovery rate and flocculation rate were used to analyze and characterize the thixotropy of the slurry, and the characterization results were obtained.

2. The method for quantitatively characterizing the thixotropy of a lithium slag-tailings cemented filling slurry according to claim 1, characterized in that: The step of preparing the slurry to be tested and setting the test parameters includes: Place the sample to be tested in the coaxial cylindrical flow, place it in the corresponding slot of the rheometer, and install the rheometer test rotor; The test parameters in the rheometer software were set to prepare the slurry to be tested, and lithium slag-filled slurries with different proportions were obtained.

3. The method for quantitatively characterizing the thixotropy of a lithium slag-tailings cemented filling slurry according to claim 2, characterized in that: The test parameters include: Shear mode in static stage, shear rate in static stage, test time in static stage, number of sampling points, shear mode in variable shear stage, shear rate in variable shear stage, test time in variable shear stage, shear mode in structural recovery stage, shear rate in structural recovery stage and test time in structural recovery stage.

4. The method for quantitatively characterizing the thixotropy of a lithium slag-tailings cemented filling slurry according to claim 2, wherein: The multi-stage thixotropic data includes: Thixotropic data in static stage, thixotropic data in variable shear stage and thixotropic data in structural recovery stage.

5. The method for quantitatively characterizing the thixotropy of a lithium slag-tailings cemented filling slurry according to claim 2, characterized in that: The shear rate was controlled in the static stage and the shear rate was set to a constant 0.01s -1 , the holding time is 60s, and the number of sampling points is 100; The variable shear stage adopts the controlled shear rate method to perform shearing, and the shear rate is 0.01s -1 Rise at a constant speed to 80s -1 , the rise time is 60s, and the number of sampling points is 100; During the structural recovery phase, shearing was performed using the controlled shear rate method, with the shear rate set to a constant 0.01s -1 , the holding time is 60s, and the number of sampling points is 100.

6. The method for quantitatively characterizing the thixotropy of a lithium slag-tailings cemented filling slurry according to claim 4, characterized in that: The method of using a thixotropic quantitative characterization method to perform data fitting on the curve to obtain specific fitting parameters and flocculation rate includes: The thixotropic data in the static stage and the thixotropic data in the structural recovery stage are fitted using an apparent viscosity evolution model to obtain asymptotic values ​​of the apparent viscosity in the corresponding stages; The flocculation rate was determined from the apparent viscosity asymptotic value.

7. The method for quantitatively characterizing the thixotropy of a lithium slag-tailings cemented filling slurry according to claim 6, characterized in that: The expression of the apparent viscosity evolution model is: the=the ∞ +(n(0)-n ∞ )e -ξt ; Among them, η ∞ is the asymptotic value of apparent viscosity, η(0) is the initial viscosity, ξ is the flocculation rate, and t is the relative test time.

8. The method for quantitatively characterizing the thixotropy of a lithium slag-tailings cemented filling slurry according to claim 1, characterized in that: The formula for the structural recovery rate is: Among them, η ∞3 is the apparent viscosity of the sample in the structural recovery stage, η ∞1 It is the apparent viscosity of the sample in the static stage.

Citation Information

Cited By

  • Lithium slag-based low-carbon cementitious material, preparation method and application thereof

    CN122355676A

  • Preparation method of lithium slag-based cementitious materials by particle size range regulation and chemical synergistic activation

    CN122562357A