Special phosphorus-free zinc-free seawater scale and corrosion inhibitor and preparation method thereof

By using natural polymer derivatives such as sulfonic acid-modified polyaspartic acid and quaternized chitosan, the problems of zinc ion contamination and poor stability in existing scale and corrosion inhibitors have been solved, resulting in a phosphorus-free and zinc-free scale and corrosion inhibitor with good scale inhibition and slow-release performance and broad metal material coverage.

CN120887559APending Publication Date: 2025-11-04QINGDAO TIANLAN ENVIRONMENT CO LTD

Patent Information

Application Number
CN202510987188.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-17
Publication Date
2025-11-04

AI Technical Summary

Technical Problem

Existing scale and corrosion inhibitors contain zinc ions, which may cause secondary pollution and have poor stability. Traditional formulations are prone to causing eutrophication and fluctuations in corrosion inhibition performance.

Method used

Natural polymer derivatives such as sulfonic acid-modified polyaspartic acid, quaternized chitosan, sulfonate copolymers, and polyepoxysuccinic acid are used to inhibit scaling through chelation, dispersion, and lattice distortion mechanisms, and form a protective film on the metal surface, achieving a phosphorus-free and zinc-free scale inhibition and corrosion inhibition effect.

Benefits of technology

This invention achieves a phosphorus-free and zinc-free scale and corrosion inhibitor, avoiding the accumulation of heavy metals and eutrophication in water. It has excellent scale inhibition and slow-release properties and broad metal coverage, making it suitable for seawater systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005504783030000091
    Figure BDA0005504783030000091
  • Figure BDA0005504783030000092
    Figure BDA0005504783030000092
  • Figure BDA0005504783030000101
    Figure BDA0005504783030000101
Patent Text Reader

Abstract

The invention relates to a phosphorus-free zinc-free seawater special-purpose scale and corrosion inhibitor, which comprises, by weight, 20-25% of sulfonic acid modified polyaspartic acid, 8-12% of quaternized chitosan, 5-10% of a sulfonate copolymer, 5-10% of polyepoxysuccinic acid, 1-3% of benzotriazole or methyl benzotriazole, 0.5-1% of sodium tungstate, and the balance of deionized water. According to the formula, traditional corrosion inhibitors such as phosphorus and zinc are completely abandoned, functions are achieved through natural polymer derivatives such as sulfonic acid modified polyaspartic acid and quaternized chitosan, and the scale and corrosion inhibitor has the following environmental protection advantages that the scale and corrosion inhibitor does not contain phosphorus and zinc elements at all, and water eutrophication and heavy metal accumulation caused by a traditional phosphorus and zinc formula are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a phosphorus-free and zinc-free scale and corrosion inhibitor specifically for seawater and its preparation method, belonging to the field of water treatment agents. Background Technology

[0002] Seawater desalination, as a strategic choice to address freshwater scarcity, is an essential requirement for ensuring national security and sustainable development, and also a necessity for the future survival and development of coastal areas. However, desalinated seawater is highly corrosive; using it as circulating cooling water can cause widespread corrosion of carbon steel pipes and equipment, directly threatening the safe operation of power plants and other industrial enterprises. Adding scale and corrosion inhibitors can effectively mitigate the corrosion of pipes by seawater. Currently, most publicly available patented formulations of seawater desalination corrosion inhibitors in China consist of rare earth salts, silicates, phosphates, and zinc salts, effectively inhibiting the corrosion of carbon steel and copper alloys by desalinated seawater. While traditional phosphorus-based formulations can effectively inhibit corrosion and scale, phosphorus emissions can lead to eutrophication, promoting algal blooms and red tides, threatening marine ecosystems. CN104140162B discloses a phosphorus-free scale and corrosion inhibitor using seawater as circulating cooling water and its preparation method. It is made from the following raw materials in weight percentage: 2-6% Mannich base quaternary ammonium salt, 5-20% aconitic acid-allyl sulfonic acid copolymer, 4-10% polyepoxysuccinic acid, 1-5% natural corrosion inhibitor, 5-15% sodium gluconate, 3-5% zinc sulfate heptahydrate, 0.6-1.1% BTA, and the balance being deionized water. This solution has high corrosion and scale inhibition performance and can solve the corrosion and scaling problem of seawater as circulating water. It is particularly suitable for various circulating water systems made of copper, carbon steel, and stainless steel. Moreover, it is phosphorus-free and has good environmental protection properties. However, the following problems exist: (1) The formula contains 3-5% zinc sulfate heptahydrate, which may lead to the accumulation of zinc ions in the water body and cause secondary pollution problems if used for a long time; (2) Extracts such as mango peel and citrus peel are easily affected by environmental pH and oxidation, resulting in poor stability and fluctuations in corrosion inhibition performance. Summary of the Invention

[0003] This invention provides a phosphorus-free and zinc-free scale and corrosion inhibitor for seawater and its preparation method, which solves the problems of secondary pollution caused by zinc ions in existing scale and corrosion inhibitors and the poor stability of existing scale and corrosion inhibitors.

[0004] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows:

[0005] A phosphorus-free and zinc-free scale and corrosion inhibitor for seawater, comprising, by weight percentage: 20-25% sulfonic acid-modified polyaspartic acid, 8-12% quaternized chitosan, 5-10% sulfonate copolymer, 5-10% polyepoxysuccinic acid, 1-3% benzotriazole or methylbenzotriazole, 0.5-1% sodium tungstate, and the balance being deionized water.

[0006] Further, preferably: the preparation method of the sulfonic acid modified polyaspartic acid is as follows: polysuccinimide is dissolved in 10% NaOH solution and stirred at 20°C for 30 min; then serine and aminosulfonic acid are dissolved in 10% NaOH solution respectively, added dropwise to the above mixture, and stirred at 40°C for 4 h. After the reaction is completed, the reaction solution is adjusted to neutral, anhydrous ethanol is added, and after the precipitate is generated, it is filtered and vacuum dried to obtain a light yellow substance, which is sulfonic acid modified polyaspartic acid.

[0007] Furthermore, preferably, the mass ratio of the polysuccinimide, serine, and aminosulfonic acid is 50:27:25.

[0008] Furthermore, preferably, the preparation method of the quaternized chitosan is as follows:

[0009] (1) Sodium alginate pre-dissolution: Sodium alginate is dissolved in 0.1mol / L CaCl2 solution to form sodium alginate with a concentration (w / v) of 2%. The solution is stirred at 60℃ and 100-150r / min for 1 hour until it is completely swollen and forms a transparent colloid.

[0010] (2) Chitosan dissolution: Chitosan was dissolved in 2% acetic acid aqueous solution to form a 50% (w / v) chitosan solution. The pH of the chitosan solution was adjusted to 11-12 with 0.5M NaOH solution.

[0011] (3) Hexadecyltrimethylammonium bromide was dissolved in ethanol to prepare a 50% (w / v) CTAB solution;

[0012] (4) Add CTAB solution dropwise to chitosan solution. Reaction temperature: 65-75℃, rotation speed 200-300rpm, stir for 2-4 hours.

[0013] (5) Add the pretreated SA colloid dropwise to the reaction solution of step (4), stir at 50-60℃ and 200-300 rpm for 1-2 hours;

[0014] (6) Cool the mixture to room temperature, add anhydrous ethanol, stir and let stand for 30 minutes, filter and collect the precipitate, wash the precipitate 2-3 times with deionized water, vacuum the precipitate, grind it through an 80-mesh sieve to obtain powdered quaternary ammonium salt modified chitosan.

[0015] Furthermore, preferably, the weight ratio of CTAB to chitosan is 0.4-0.6:1; and the weight ratio of sodium alginate to chitosan is 0.1-0.2:1.

[0016] Furthermore, preferably, the sulfonate copolymer is an acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer.

[0017] The preparation method of the phosphorus-free and zinc-free seawater-specific scale and corrosion inhibitor of the present invention includes the following steps:

[0018] (1) Dissolve sulfonic acid modified polyaspartic acid in deionized water, stir at 60°C for 1 hour until completely dissolved, and set aside.

[0019] (2) Mix the quaternized chitosan, sulfonate copolymer and polyepoxysuccinic acid evenly and dissolve them in deionized water;

[0020] (3) Mix the products from step 1 and step 2, add benzotriazole or methylbenzotriazole and sodium tungstate, stir for 2 hours, add deionized water, and adjust the pH to 7.8-8.2.

[0021] (4) The particle size is refined to D50 < 5μm by a sand mill, and then filled. Before filling, inert gas is introduced to replace oxygen.

[0022] The beneficial effects of this invention are:

[0023] The formulation of this invention completely abandons traditional corrosion inhibitors such as phosphorus and zinc, and achieves its function through natural polymer derivatives such as sulfonic acid-modified polyaspartic acid and quaternized chitosan. It has the following environmental advantages: the scale and corrosion inhibitor does not contain phosphorus or zinc, thus avoiding eutrophication and heavy metal accumulation in water bodies caused by traditional phosphorus and zinc formulations.

[0024] The product of this invention can be widely used in the field of scale inhibition and corrosion inhibition in seawater. The dosage is 10-30 mg / L, which is small and has a good scale inhibition and slow release effect.

[0025] The formulation of this invention is targeted at the high calcium (Ca) content of seawater. 2+ High magnesium (Mg) 2+ ), high sulfate (SO4) 2- The formula inhibits scaling through a triple mechanism of chelation, dispersion, and lattice distortion: the sulfonic acid groups of sulfonic acid-modified polyaspartic acid react with Ca... 2+ Mg 2+ It forms a stable complex; the long-chain polymer of the auxiliary scale inhibitor sulfonate copolymer disperses scale crystal nuclei through electrostatic repulsion, inhibiting the growth of scale such as CaCO3 and CaSO4; the epoxy groups of the synergistic scale inhibitor polyepoxysuccinic acid interfere with the lattice arrangement and destroy the scale layer structure, and have a good inhibition rate on complex scale such as calcium phosphate and silicate. Through their mutual cooperation, it has good scale inhibition and slow release performance.

[0026] The marine environment contains a variety of metal materials (carbon steel, stainless steel, copper alloys, titanium alloys, etc.). The formulation achieves full material coverage through anodic protection, cathodic protection, and film shielding: the quaternary ammonium groups of quaternized chitosan adsorb onto the metal surface, forming a dense anodic protective film, which has excellent corrosion and scale inhibition effects on carbon steel / stainless steel; benzotriazole or methylbenzotriazole reacts with Cu... + Formation of stable complexes inhibits pitting and crevice corrosion; sodium tungstate generates WO4 on the surface. 2- Passivation film, resisting Cl - The scale and corrosion inhibitor of this invention penetrates titanium / aluminum alloys and, through their interaction, has a wide range of applications. Detailed Implementation

[0027] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present invention without creative effort are also described.

[0028] The degree of deacetylation of chitosan is ≥90%, 80 mesh; the sodium alginate content is ≥95%, 80 mesh; and the viscosity is 700-800 mPa·s. The solid content of polyepoxysuccinic acid is 43%, and the pH (1% aqueous solution) is 11.2. The remaining raw materials are commercially available analytical grade reagents.

[0029] Preparation method of sulfonic acid modified polyaspartic acid: Polysuccinimide was dissolved in 10% NaOH solution and stirred at 20℃ for 30 min; then serine and aminosulfonic acid were dissolved separately in 10% NaOH solution and added dropwise to the above mixture, and stirred at 40℃ for 4 h. After the reaction was completed, the reaction solution was adjusted to neutral, anhydrous ethanol was added, and after the precipitate was formed, it was filtered and vacuum dried to obtain a light yellow substance, which is sulfonic acid modified polyaspartic acid; the mass ratio of polysuccinimide, serine and aminosulfonic acid was 50:27:25.

[0030] The preparation method of quaternized chitosan is as follows:

[0031] (1) Sodium alginate pre-dissolution: Sodium alginate was dissolved in 0.1 mol / L CaCl2 solution to form sodium alginate with a concentration (w / v) of 2%. The solution was stirred at 60°C and 150 rpm for 1 hour until it was completely swollen and formed a transparent colloid.

[0032] (2) Dissolution of chitosan: Chitosan was dissolved in a 2% (w / v) aqueous acetic acid solution to form a 50% (w / v) chitosan solution. The pH of the chitosan solution was adjusted to 11.5 with 0.5M NaOH solution.

[0033] (3) Hexadecyltrimethylammonium bromide was dissolved in ethanol to prepare a 50% (w / v) CTAB solution;

[0034] (4) Add CTAB solution dropwise to chitosan solution, reaction temperature: 60℃, speed: 300rpm, stir for 2 hours;

[0035] (5) Add the pretreated SA colloid dropwise to the reaction solution of step (4), stir at 55°C and 200 rpm for 2 hours.

[0036] (6) Cool the mixture to room temperature, add 3 times the volume of anhydrous ethanol, stir and let stand for 30 minutes, filter and collect the precipitate, wash the precipitate 3 times with deionized water, vacuum the precipitate, grind it through an 80-mesh sieve to obtain powdered quaternary ammonium salt modified chitosan.

[0037] The weight ratio of CTAB to chitosan is 0.4:1; the weight ratio of sodium alginate to chitosan is 0.1:1.

[0038] Example 1

[0039] A phosphorus-free and zinc-free scale and corrosion inhibitor for seawater, comprising, by weight percentage: 23% sulfonic acid modified polyaspartic acid, 12% quaternized chitosan, 6.5% sulfonate copolymer, 6% polyepoxysuccinic acid, 2% methylbenzotriazole, 0.5% sodium tungstate, and 50% deionized water.

[0040] Sulfonic acid-modified polyaspartic acid and quaternized chitosan are the products prepared above.

[0041] The sulfonate copolymer is an acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer.

[0042] Its preparation method includes the following steps:

[0043] (1) Dissolve sulfonic acid modified polyaspartic acid in deionized water, stir at 60°C and 300 r / min for 1 h until completely dissolved, and set aside.

[0044] (2) Mix the quaternized chitosan, sulfonate copolymer and polyepoxysuccinic acid evenly and dissolve them in deionized water;

[0045] (3) Mix the products from step 1 and step 2, add 1-3% benzotriazole or methylbenzotriazole, sodium tungstate, stir at 300 r / min for 2 h, add deionized water, and adjust the pH to 7.8.

[0046] (4) The particle size is refined to D50 < 5μm by a sand mill, and then filled. Before filling, inert gas is introduced to replace oxygen.

[0047] Example 2

[0048] A phosphorus-free and zinc-free scale and corrosion inhibitor for seawater, comprising, by weight percentage: 20% sulfonic acid-modified polyaspartic acid, 10% quaternized chitosan, 10% sulfonate copolymer, 8% polyepoxysuccinic acid, 1% methylbenzotriazole, 1% sodium tungstate, and 50% deionized water.

[0049] Sulfonic acid-modified polyaspartic acid and quaternized chitosan are the products prepared above.

[0050] The sulfonate copolymer is an acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer.

[0051] Its preparation method includes the following steps:

[0052] (1) Dissolve sulfonic acid modified polyaspartic acid in deionized water, stir at 60°C and 300 r / min for 1 h until completely dissolved, and set aside.

[0053] (2) Mix the quaternized chitosan, sulfonate copolymer and polyepoxysuccinic acid evenly and dissolve them in deionized water;

[0054] (3) Mix the products from step 1 and step 2, add methylbenzotriazole and sodium tungstate, stir at 300 r / min for 2 h, add deionized water, and adjust the pH to 8.2.

[0055] (4) The particle size is refined to D50 < 5μm by a sand mill, and then filled. Before filling, inert gas is introduced to replace oxygen.

[0056] Example 3

[0057] A phosphorus-free and zinc-free scale and corrosion inhibitor for seawater, comprising, by weight percentage: 25% sulfonic acid modified polyaspartic acid, 8% quaternized chitosan, 8% sulfonate copolymer, 5% polyepoxysuccinic acid, 3% methylbenzotriazole, 1% sodium tungstate, and 50% deionized water.

[0058] Sulfonic acid-modified polyaspartic acid and quaternized chitosan are the products prepared above.

[0059] The sulfonate copolymer is an acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer.

[0060] Its preparation method includes the following steps:

[0061] (1) Dissolve sulfonic acid modified polyaspartic acid in deionized water, stir at 60°C and 300 r / min for 1 h until completely dissolved, and set aside.

[0062] (2) Mix the quaternized chitosan, sulfonate copolymer and polyepoxysuccinic acid evenly and dissolve them in deionized water;

[0063] (3) Mix the products from step 1 and step 2, add methylbenzotriazole and sodium tungstate, stir at 300 r / min for 2 h, add deionized water, and adjust the pH to 7.8.

[0064] (4) The particle size is refined to D50 < 5μm by a sand mill, and then filled. Before filling, inert gas is introduced to replace oxygen.

[0065] Example 4

[0066] A phosphorus-free and zinc-free scale and corrosion inhibitor for seawater, comprising, by weight percentage: 22.5% sulfonic acid-modified polyaspartic acid, 11% quaternized chitosan, 5% sulfonate copolymer, 10% polyepoxysuccinic acid, 1% methylbenzotriazole, 0.5% sodium tungstate, and 50% deionized water.

[0067] Sulfonic acid-modified polyaspartic acid and quaternized chitosan are the products prepared above.

[0068] The sulfonate copolymer is an acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer.

[0069] Its preparation method includes the following steps:

[0070] (1) Dissolve sulfonic acid modified polyaspartic acid in deionized water at 60℃ and 300r / min for 1 hour until completely dissolved, and set aside for later use.

[0071] (2) Mix the quaternized chitosan, sulfonate copolymer and polyepoxysuccinic acid evenly and dissolve them in deionized water;

[0072] (3) Mix the products from steps 1 and 2, add methylbenzotriazole and sodium tungstate, stir at 300 r / min for 2 h, add deionized water, and adjust the pH to 8.0.

[0073] (4) The particle size is refined to D50 < 5μm by a sand mill, and then filled. Before filling, inert gas is introduced to replace oxygen.

[0074] Comparative Example 1 investigated the effect of different preparation methods of quaternized chitosan on product performance.

[0075] This is basically the same as Example 1, except that sodium alginate is removed and replaced with chitosan. The preparation method of quaternized chitosan is as follows:

[0076] (1) Dissolution of chitosan: Chitosan was dissolved in a 2% (w / v) aqueous acetic acid solution to form a 50% (w / v) chitosan solution. The pH of the chitosan solution was adjusted to 11.5 with 0.5M NaOH solution.

[0077] (2) Hexadecyltrimethylammonium bromide was dissolved in ethanol to prepare a 50% (w / v) CTAB solution;

[0078] (3) Add CTAB solution dropwise to chitosan solution, reaction temperature: 60℃, speed: 300rpm, stir for 2 hours;

[0079] (4) Cool the mixture to room temperature, add 3 times the volume of anhydrous ethanol, stir and let stand for 30 minutes, filter and collect the precipitate, wash the precipitate 3 times with deionized water, vacuum the precipitate, grind it through an 80-mesh sieve to obtain powdered quaternary ammonium salt modified chitosan; the weight ratio of CTAB to chitosan is 0.5:1.

[0080] Comparative Example 2

[0081] It is basically the same as Example 1, except that the quaternized chitosan is replaced with chitosan.

[0082] Comparative Example 3

[0083] It is basically the same as Example 1, except that the sulfonate copolymer is replaced with sulfonic acid modified polyaspartic acid.

[0084] Comparative Example 4

[0085] It is basically the same as Example 1, except that: polyepoxysuccinic acid is replaced by sulfonic acid modified polyaspartic acid.

[0086] The seawater was sourced from the nearshore waters of Jiaozhou Bay in Qingdao, and the relevant properties of the products were measured.

[0087] Table 1 Seawater Quality

[0088]

[0089]

[0090] Rotary plate test: Using 20# carbon steel and H68 brass plates as test materials, the corrosion inhibition performance of the agent was examined according to GB / T34550.1-2017 "Evaluation Methods for Performance of Seawater Cooling Water Treatment Agents Part 1: Determination of Corrosion Inhibition Performance," and a suitable composite corrosion inhibitor formulation was screened accordingly. The addition amount was 30 mg / L, seawater was concentrated 3 times, the temperature was controlled at 50℃, the rotation speed was 75 r / min, and the reaction time was 72 h.

[0091] Static scale inhibition test: Referring to GB / T34550.2-2017 "Evaluation Methods for Performance of Seawater Cooling Water Treatment Agents Part 2: Determination of Scale Inhibition Performance", a static scale inhibition test was used for rapid screening and evaluation of scale and corrosion inhibitors. The addition amount was 30 mg / L, the temperature was controlled at 80℃, and the reaction time was 24 h.

[0092] The specific measurement results are shown in Tables 2 and 3.

[0093] Table 2. Test results of rotating hanging plates for different products

[0094]

[0095]

[0096] Table 3. Static scale inhibition test results for different products

[0097] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Scale inhibition rate / % 98.6 98.1 98.3 97.9 95.3 92.1 90.2 89.6

[0098] As shown in Tables 2 and 3, the scale and corrosion inhibitor prepared by this invention has good slow-release and scale inhibition effects.

[0099] As can be seen from Comparative Examples 1 and 2, this invention uses sodium alginate and quaternary ammonium salt to modify chitosan. The carboxyl groups of sodium alginate react with the Ca in seawater. 2+ Mg 2+ The formation of a chelate network enhances the structural stability of the material in seawater. At the same time, the negatively charged groups of sodium alginate inhibit the attachment of marine microorganisms through electrostatic repulsion, reducing biofilm formation. Sodium alginate and the quaternary ammonium groups of hexadecyltrimethylammonium bromide are bonded by ionic bonds to form a dense protective film, reducing the metal corrosion rate.

[0100] Compared with Comparative Example 1, Example 1 showed a 7.4% increase in corrosion inhibition rate for 20# carbon steel, and compared with Comparative Example 2, a 14.6% increase in corrosion inhibition rate for 20# carbon steel.

[0101] Compared with Comparative Example 1, the scale inhibition rate of Example 1 was increased by 3.5%, and compared with Comparative Example 2, the scale inhibition rate was increased by 7.1%.

[0102] As shown in Comparative Examples 3 and 4, the sulfonate copolymer has excellent scale inhibition capabilities for CaSO4 and CaCO3, and good Fe2O3 dispersibility, which can effectively improve the scale inhibition and corrosion inhibition performance of the product.

[0103] Polyepoxysuccinic acid is a recognized high-efficiency, biodegradable, phosphorus-free scale inhibitor. In synergy with sulfonic acid-modified polyaspartic acid and sulfonic acid copolymers, it further enhances the scale inhibition effect of calcium carbonate and calcium sulfate, especially under high hardness and high alkalinity conditions.

[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A phosphorus-free and zinc-free scale and corrosion inhibitor specifically for seawater, characterized in that: By weight percentage, it includes 20-25% sulfonic acid modified polyaspartic acid, 8-12% quaternized chitosan, 5-10% sulfonate copolymer, 5-10% polyepoxysuccinic acid, 1-3% benzotriazole or methylbenzotriazole, 0.5-1% sodium tungstate, and the balance being deionized water.

2. The phosphorus-free and zinc-free seawater-specific scale and corrosion inhibitor according to claim 1, characterized in that: The preparation method of sulfonic acid modified polyaspartic acid is as follows: polysuccinimide is dissolved in 10% NaOH solution and stirred at 20°C for 30 min; then serine and aminosulfonic acid are dissolved in 10% NaOH solution respectively, and added dropwise to the above mixture, and stirred at 40°C for 4 h. After the reaction is completed, the reaction solution is adjusted to neutral, anhydrous ethanol is added, and after the precipitate is generated, it is filtered and vacuum dried to obtain a light yellow substance, which is sulfonic acid modified polyaspartic acid.

3. The phosphorus-free and zinc-free seawater-specific scale and corrosion inhibitor according to claim 2, characterized in that: The mass ratio of the polysuccinimide, serine, and aminosulfonic acid is 50:27:

25.

4. The phosphorus-free and zinc-free seawater-specific scale and corrosion inhibitor according to claim 1, characterized in that: The preparation method of the quaternized chitosan is as follows: (1) Sodium alginate pre-dissolution: Sodium alginate is dissolved in 0.1mol / L CaCl2 solution to form sodium alginate with a concentration (w / v) of 2%. The solution is stirred at 60℃ and 100-150r / min for 1 hour until it is completely swollen and forms a transparent colloid. (2) Chitosan dissolution: Chitosan was dissolved in 2% acetic acid aqueous solution to form a 50% (w / v) chitosan solution. The pH of the chitosan solution was adjusted to 11-12 with 0.5M NaOH solution. (3) Hexadecyltrimethylammonium bromide was dissolved in ethanol to prepare a 50% (w / v) CTAB solution; (4) Add CTAB solution dropwise to chitosan solution. Reaction temperature: 65-75℃, rotation speed 200-300rpm, stir for 2-4 hours. (5) Add the pretreated SA colloid dropwise to the reaction solution of step (4), stir at 50-60℃ and 200-300 rpm for 1-2 hours; (6) Cool the mixture to room temperature, add anhydrous ethanol, stir and let stand for 30 minutes, filter and collect the precipitate, wash the precipitate 2-3 times with deionized water, vacuum the precipitate, grind it through an 80-mesh sieve to obtain powdered quaternary ammonium salt modified chitosan.

5. The phosphorus-free and zinc-free seawater-specific scale and corrosion inhibitor according to claim 3, characterized in that: The weight ratio of CTAB to chitosan is 0.4-0.6:1; the weight ratio of sodium alginate to chitosan is 0.1-0.2:

1.

6. The phosphorus-free and zinc-free seawater-specific scale and corrosion inhibitor according to claim 1, characterized in that: The sulfonate copolymer is an acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer.

7. The method for preparing the phosphorus-free and zinc-free seawater-specific scale and corrosion inhibitor according to any one of claims 1-6, characterized in that, Includes the following steps: (1) Dissolve sulfonic acid modified polyaspartic acid in deionized water at 60-70℃ and 200-300 rpm for 1-2 hours until completely dissolved, and set aside. (2) Mix the quaternized chitosan, sulfonate copolymer and polyepoxysuccinic acid evenly and dissolve them in deionized water; (3) Mix the products from step 1 and step 2, add benzotriazole or methylbenzotriazole, sodium tungstate, stir continuously at 200-300 rpm for 2-3 hours, add deionized water, and adjust the pH to 7.8-8.

2. (4) The particle size is refined to D50 < 5μm by a sand mill, and then filled. Before filling, inert gas is introduced to replace oxygen.

Citation Information

Patent Citations

  • Phosphorus-free scale and corrosion inhibitors for use in circulating cooling water and their preparation method

    CN104140162B

  • Non-phosphate anti-incrustation corrosion inhibitor and preparation process thereof

    CN102010077A

  • Phosphorus-free scale and corrosion inhibitor and preparation method thereof

    CN110937698A

  • Preparation method of novel phosphorus-free grey water dispersing agent

    CN117466449A

  • Preparation and application of green marine antifouling coating based on quaternary ammonium salt chitosan

    CN118909489A

Cited By

  • Low-phosphorus efficient scale-inhibiting water treatment agent for high-pressure boiler and preparation method of low-phosphorus efficient scale-inhibiting water treatment agent

    CN121085440A

  • Low-phosphorus high-efficiency scale-inhibiting water treatment agent for high-pressure boiler and preparation method thereof

    CN121085440B

  • Scale inhibition and dispersion agent for reverse osmosis membrane as well as preparation method and application of scale inhibition and dispersion agent