Surface etching method for exposing dislocation defect of tellurium indium lead single crystal

By pretreating PIT single crystals and using a specific etching solution system, combined with ultrasonic assistance, dislocation defects were accurately revealed, solving the performance degradation problem caused by dislocations during PIT single crystal growth and achieving efficient defect characterization and process improvement.

CN121027143AActive Publication Date: 2025-11-28HARBIN INST OF TECH
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202511224061.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-29
Publication Date
2025-11-28
Estimated Expiration
2045-08-29

AI Technical Summary

Technical Problem

Existing PIT single crystals generally suffer from problems such as dislocations, strong optical absorption, and uneven element distribution during the growth process, which leads to performance degradation. The lack of effective defect characterization methods hinders their application in infrared lasers.

Method used

Pretreatment methods such as X-ray crystal orientation, multi-stage mechanical polishing, chemical mechanical polishing and ultrasonic cleaning are used, combined with a specific ratio of HIO3-CH3COOH-HF mixed etching solution and ultrasonic assistance, to accurately reveal dislocation defects inside the crystal and form a regular etch pit morphology.

Benefits of technology

This technology enables highly sensitive and reliable detection of dislocation defects in PIT single crystals, providing key technical support for evaluating crystal quality and guiding growth process optimization, while avoiding excessive surface etching.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121027143A_ABST
    Figure CN121027143A_ABST
Patent Text Reader

Abstract

The invention discloses a surface etching method for revealing dislocation defects of tellurium indium lead single crystals, and relates to a method for revealing crystal defects. The invention aims to provide a surface etching method capable of accurately exposing crystal defects. The method comprises the following steps: firstly, carrying out directional cutting, multi-stage mechanical polishing and chemical mechanical polishing on a PIT single crystal to obtain a smooth and damage-free surface; and reacting iodine with concentrated nitric acid to generate iodic acid as a main oxidant, adding hydrofluoric acid for activation, diluting with an acetic acid-water mixed solution, and etching the crystal at a low temperature of 10 + / -1 DEG C under ultrasonic assistance. According to the method, the regular triangular conical etching pit can be formed on the PIT single crystal (001) surface, the depth is 100-300 nm, the pit bottom points to the [001] direction, and the dislocation defect is clearly revealed. The method has the advantages of clear etching morphology, high sensitivity, high reliability and simplicity and convenience in operation, and can be applied to the fields of PIT single crystal quality evaluation, defect analysis and growth process optimization.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to a method for etching a tellurium-indium-lead single crystal. BACKGROUND

[0002] Infrared nonlinear optical crystals show important application value in key fields such as industry, medicine and energy. However, the currently commercialized chalcopyrite infrared crystals (such as AgGaS2, AgGaSe2 and ZnGeP2) generally have intrinsic defects such as low laser damage threshold and two-photon absorption, which seriously restricts their practical application in far-infrared high-power solid-state lasers. In order to meet the development needs of modern infrared laser technology, it is urgent to develop new crystal materials with the following characteristics: first, they can efficiently utilize 1064 nm pump laser output by Nd:YAG laser; second, their output wavelength range needs to cover more than 10 μm. Compared with phosphorus compounds, telluride crystals in chalcogenides have a significant advantage in realizing a wide infrared transmission range (especially covering the 10-14 μm atmospheric window) due to their lower phonon energy. Among them, ternary telluride PbIn6Te 10 (PIT) is attracting attention as a new nonlinear optical crystal material. PIT crystal belongs to the trigonal system with space group R32, and has excellent comprehensive performance: wide transmission band (1.3-31 μm), moderate birefringence (~0.05), large nonlinear optical coefficient (d 11 = 51 pm / V). Both theoretical simulation and experimental research (such as 5-25 μm tunable laser output has been realized by using 2 μm laser pumped optical parametric oscillation technology) have shown that PIT crystal has great potential to realize 10-30 μm laser output.

[0003] However, the PIT single crystals grown by the existing method generally face serious cracking, strong optical absorption and uneven element distribution in the crystal. The root cause is that PIT, as a non-uniform melting compound, it is difficult to accurately control the composition of the melt during the single crystal growth process, resulting in structural defects such as dislocations and inclusions in the crystal. These defects are the direct cause of cracking, deterioration of optical performance and uneven element distribution in the crystal, which seriously hinders the full play of the performance of PIT crystal and its practical application. At present, there is no direct method to find the defects in the crystal, therefore, while optimizing the crystal growth, it is urgent to develop a method that can effectively and intuitively characterize the internal structural defects (especially dislocations) of PIT single crystal, so as to deeply understand the defect causes, guide the improvement of growth process and select high-quality crystals. SUMMARY

[0004] In order to overcome the performance degradation problem caused by dislocation defects in the prior art PIT single crystal, a surface etching method for accurately revealing crystal defects is provided. In order to achieve the above-mentioned target, first, the surface of the PIT single crystal needs to be pretreated to construct a non-damaged crystal surface as a defect characterization basis. Ensure that the subsequent etching process only responds selectively to intrinsic defects in the crystal. Through the etching technology, the internal structural defects (especially dislocations) of the PIT single crystal are effectively and intuitively characterized, so as to deeply understand the defect causes, guide the growth process improvement and select high-quality crystals.

[0005] The surface etching method for revealing dislocation defects of a tellurium-indium-lead single crystal according to the present application is carried out in the following steps:

[0006] I. Pretreatment of PbIn6Te 10 (PIT) single crystal:

[0007] (1) Determine the crystal direction using an X-ray crystal orientation instrument, cut along the target crystal plane, and obtain a wafer;

[0008] (2) Use micron to sub-micron abrasives in sequence, and use multi-stage gradient mechanical polishing to gradually reduce the surface roughness, and use ultrasonic cleaning to remove the abrasive residues;

[0009] (3) Use alkaline colloidal polishing solution, use chemical mechanical polishing to eliminate the subsurface damage layer, and obtain a crystal with smooth and flat surface;

[0010] (4) The crystal surface is then sequentially subjected to organic solvent degreasing, dilute acid solution deoxidation, high-purity water multi-frequency ultrasonic rinsing, and finally inert gas blowing and low-temperature vacuum drying, to obtain a crystal with clean and hydrophobic surface; before carrying out the etching process, the PbIn6Te 10 (PIT) single crystal is subjected to systematic pretreatment to ensure surface integrity, which effectively eliminates micro-cracks caused by mechanical stress and surface adsorbed impurities, and provides a non-damaged substrate for subsequent accurate revelation of crystal defects;

[0011] II. Preparation of etching solution precursor:

[0012] Analyze pure iodine (I2) and mass percentage concentration ≥65% concentrated nitric acid (HNO3) in a molar ratio of 1:(8~12) are added to a corrosion-resistant container, and ultrasonic treatment is carried out in a closed and ventilated environment under the condition of ultrasonic power of 50~100W for 5~30 minutes to obtain an orange-red solution;

[0013] In this step, the oxidation reaction occurs: 10HNO3(conc.) + I2 → 2HIO3 + 10NO2↑ + 4H2O;

[0014] The reaction system changes from colorless to orange red, indicating the formation of iodic acid (HIO3) and nitrogen dioxide, and this step aims to build an acidic environment with HIO3 as the main oxidant, laying the foundation for subsequent crystal surface oxidation etching.

[0015] III. Etching liquid activation and temperature control: Add a 40%~49% mass percentage hydrofluoric acid solution (HF) drop by drop to the orange-red solution, and the addition amount is 10%~20% of the volume of concentrated nitric acid (HNO3), to obtain a colorless solution; The solution quickly fades to colorless, indicating that HF and residual iodide form volatile hydrogen iodide (HI↑), eliminating color interference and enhancing etching activity; Then add a mixture of acetic acid (CH3COOH) and deionized water in a volume ratio of 1: (1~2) to the colorless solution to obtain a dilution solution; Then cool the dilution solution to 10±1℃ in an ice water bath to obtain the etching liquid; The low-temperature etching liquid can inhibit side reactions and precisely control the etching rate;

[0016] IV. Single crystal etching and defect revelation: Immerse the crystal with a clean and hydrophobic surface obtained in step one into the etching liquid, and at the same time, start the ultrasonic, under the condition of ultrasonic frequency 40 kHz and ultrasonic power 50~150 W, assist etching for 3~10 minutes, then take out the crystal and ultrasonic clean with anhydrous ethanol for 60 seconds, and dry with nitrogen; In this step, the ultrasonic cavitation effect promotes the diffusion of the etchant in the micro area of the crystal surface, preferentially attacking the defect area such as dislocation exposure point, forming characteristic morphology of etch pits (such as triangular pyramid, hexagonal pyramid);

[0017] V. Defect characterization: Observe the crystal surface for etch pits by metallographic optical microscope or scanning electron microscope (SEM), and if there are etch pits, there are dislocation defects, thus completing the revelation of dislocation defects in tellurium indium lead single crystal.

[0018] Further, the abrasive used in the mechanical polishing process of step one is alumina powder.

[0019] Further, the organic solvent used in the organic solvent degreasing of step one is acetone,

[0020] Further, the dilute acid solution used in the removal of oxides in step one is a mixture of 5%~7% mass percentage dilute hydrochloric acid and 5%~7% mass percentage dilute nitric acid in a volume ratio of (2.5~3.5):1.

[0021] Further, the inert gas used in the inert gas blowing of step one is nitrogen.

[0022] Further, the ultrasonic treatment in step two is carried out under an ultrasonic power of 50~100 W.

[0023] Further, the ultrasonic assistance in step four is performed under the condition of ultrasonic frequency of 40 kHz and ultrasonic power of 50-150 W.

[0024] PIT crystal (chemical formula PbIn6Te 10 ) belongs to trigonal system, and the space group is R32. This crystal structure feature directly determines the shape of etching pits. The trigonal PIT crystal has a three-fold rotation symmetry axis along the c-axis, i.e., the

[001] direction, and multiple 2-fold rotation axes perpendicular to the c-axis. On the crystal surface (such as the (001) surface) perpendicular to the c-axis, the crystal symmetry exhibits three-fold rotation symmetry (120° rotation invariance). This means that the atomic arrangement and crystal surface orientation on the (001) projection surface have a 120° angle feature.

[0025] The etching process preferentially occurs at crystal defects (such as dislocation emergence points) because the energy of the defect region is higher and more susceptible to attack by chemical etchants. The etch pits are bounded by low-index crystal surfaces (such as the {101} or {110} surface family), which are controlled by the space group R32 in the trigonal system.

[0026] Due to the 3-fold symmetry of the trigonal system, the angle between the {101} or {110} surface family is fixed at 120° (determined by the lattice parameters a = b ≠ c, α = β = 90°, γ = 120°). During the etching process, the etchant selectively dissolves along these equivalent crystal surfaces, resulting in the formation of triangular pyramidal etch pits with the pyramidal apex pointing in the

[001] direction and the etch pit base exhibiting an equilateral triangle shape. However, for edge dislocations, the strain field is non-axially symmetric, and the etch pits produced on the (001) surface are usually asymmetric, possibly exhibiting an elongated shape (e.g., an isosceles triangle rather than an equilateral triangle) or having one side steeper than the others. Sometimes, it may exhibit a semi-hexagonal or irregular quadrilateral shape. For screw dislocations, the strain field is axially symmetric, and the emergence point of a pure screw dislocation on the (001) surface will produce a highly symmetric etch pit. For the (001) surface with R32 symmetry, this almost always exhibits a central symmetric, regular equilateral triangular or regular hexagonal etch pit, with the pit bottom usually being sharp.

[0027] The PIT (Lead Indium Telluride) surface etching method of this invention can form regular and clear triangular pyramidal etch pits on its (001) crystal plane based on the symmetry of the R32 space group of the trigonal crystal system, accurately revealing edge dislocation defects. This method achieves selective etching of defect areas by optimizing the formulation of the HIO3-CH3COOH-HF mixed etching solution system, combined with ultrasonic-assisted processing and precise temperature control, effectively avoiding excessive surface etching. The etch pits obtained by this invention have consistent morphology, sharp edges, and depths between 100 and 300 nm, exhibiting high sensitivity and high reliability. This provides key technical support for evaluating the quality of PIT single crystals, analyzing defect causes, and guiding the optimization of crystal growth processes. Attached Figure Description

[0028] Figure 1 The PbIn6Te treated in step one of Example 1 10 Optical photographs of (PIT) single-crystal surfaces;

[0029] Figure 2 This is a scanning electron microscope image of the PIT single crystal surface after etching in step four of Example 1;

[0030] Figure 3 This is a scanning electron microscope image of the PIT single crystal surface after etching in step four of Example 1. Detailed Implementation

[0031] The beneficial effects of the present invention will be verified using the following examples.

[0032] Example 1: The surface etching method for revealing dislocation defects in lead indium telluride single crystals in this example is performed according to the following steps:

[0033] I. On PbIn6Te 10 (PIT) single crystals undergo pretreatment:

[0034] (1) Using an X-ray crystallography system to determine the PbIn6Te 10 (PIT) The (001) crystal orientation of a single crystal is cut along this crystal plane to obtain a flat wafer with a thickness of 5.0 mm;

[0035] (2) The wafer was mechanically polished in stages using alumina (Al2O3) abrasive water suspension with particle sizes of 15 μm, 5 μm and 1 μm, for 10 minutes at each stage; after each stage of polishing, the wafer was placed in an ultrasonic cleaner with a frequency of 40 kHz and rinsed with deionized water for 1 minute to remove abrasive residue.

[0036] (3) using a basic colloidal silicon dioxide (SiO2) polishing solution with pH = 10.5, polishing for 60 minutes under the conditions of a rotation speed of 100 rpm and a pressure of 5 psi, to eliminate the subsurface damage layer and obtain a crystal with a smooth and flat surface;

[0037] (4) soaking the crystal in acetone for 10 minutes for degreasing, then in a mixed solution of dilute hydrochloric acid and dilute nitric acid for 10 minutes for removing oxides, then cleaning the crystal in deionized water using ultrasonic waves with a frequency of 40 kHz and 80 kHz alternately for 15 minutes, and finally blowing the surface of the wafer dry with high-purity nitrogen and drying the wafer in a vacuum drying oven at 60°C for 2 hours, to obtain a crystal with a clean and hydrophobic surface; the mixed solution of dilute hydrochloric acid and dilute nitric acid is a mixed solution of 5% by mass of dilute hydrochloric acid and 5% by mass of dilute nitric acid with a volume ratio of 3:1; before performing the etching process, the PbIn6Te 10 (PIT) single crystal is subjected to systematic pretreatment to ensure surface integrity, which effectively eliminates microcracks caused by mechanical stress and surface adsorbed impurities, providing a non-damage substrate for subsequent accurate exposure of crystal defects; the photograph of the crystal after step one is shown in Figure 1 From Figure 1 it can be seen that the surface of the crystal is smooth, bright and free of scratches.

[0038] II. Preparation of etching solution precursor:

[0039] 2.54 g of analytical pure iodine (I2) and 6.0 mL of 65% by mass concentrated nitric acid (HNO3) are added to a polytetrafluoroethylene container, and ultrasonic treatment is performed in a closed and ventilated environment under the condition of an ultrasonic power of 80 W for 30 minutes, to obtain an orange-red solution;

[0040] In this step, an oxidation reaction occurs: 10HNO3(conc.) + I2 → 2HIO3 + 10NO2↑ + 4H2O;

[0041] The reaction system changes from colorless to orange-red, indicating the formation of iodate (HIO3) and nitrogen dioxide, and this step aims to establish an acidic environment with HIO3 as the main oxidizing agent, laying a foundation for subsequent crystal surface oxidation etching.

[0042] III. Activation and temperature control of etching solution: 1.0 mL of 40% hydrofluoric acid solution (HF) was added dropwise to the orange-red solution to obtain a colorless solution; the solution faded to colorless rapidly, indicating that HF reacted with residual iodide to form volatile hydrogen iodide (HI↑), eliminating color interference and enhancing etching activity; then 5 mL of acetic acid (CH3COOH) and 10 mL of deionized water were added to the colorless solution to obtain a dilute solution; the dilute solution was then cooled to 10±1°C in an ice water bath to obtain an etching solution; the low-temperature etching solution can inhibit side reactions and precisely control the etching rate;

[0043] IV. Single crystal etching and defect exposure: the crystal with a clean and hydrophobic surface obtained in step I was immersed in the etching solution, and ultrasonic was turned on at the same time; the etching was assisted for 5 minutes under the conditions of ultrasonic frequency of 40 kHz and ultrasonic power of 100 W; after the crystal was taken out, it was ultrasonically cleaned with anhydrous ethanol for 60 seconds and dried with nitrogen; in this step, the ultrasonic cavitation effect promotes the diffusion of the etchant in the micro area of the crystal surface, preferentially attacking the defect area such as dislocation exposure point, and forming characteristic morphology etch pits (such as triangular pyramid and hexagonal pyramid);

[0044] V. Defect characterization: the crystal surface was observed by scanning electron microscopy (SEM), and the scanning electron microscope photos are shown in Figure 2 and Figure 3 As can be seen from Figure 2 and Figure 3 , the etch pit depth is 100-300 nm, the pit wall is clear and sharp, the vertex points to the

[001] crystal direction, the dislocation type is a blade dislocation, the dislocation defect is precisely exposed and there is no over-etching, and the exposure of the tellurium indium lead single crystal dislocation defect is completed.

[0045] The method of the embodiment can precisely expose the dislocation defects of the tellurium indium lead single crystal, and has the advantages of high sensitivity and high fidelity.

Claims

1. A surface etching method for revealing dislocation defects using indium lead telluride single crystal, characterized in that, This method is performed in the following steps: I. On PbIn6Te 10 Single crystal pretreatment: (1) Use an X-ray crystallography instrument to determine the crystal orientation, cut along the target crystal plane to obtain a wafer; (2) Use micron-sized to submicron-sized abrasives in sequence, and use multi-level gradient mechanical polishing to gradually reduce the surface roughness, while using ultrasonic cleaning to remove abrasive residues; (3) Using alkaline colloidal polishing solution, chemical mechanical polishing is used to eliminate the subsurface damage layer and obtain crystals with smooth and flat surfaces; (4) The crystal surface is then subjected to organic solvent degreasing, dilute acid solution deoxidation, high-purity water multi-frequency ultrasonic rinsing, and finally inert gas purging and low-temperature vacuum drying to obtain a crystal with a clean hydrophobic surface. II. Preparation of Etching Solution Precursor: Analytical pure iodine and concentrated nitric acid with a mass percentage concentration ≥65% were added to a corrosion-resistant container at a molar ratio of 1:(8~12). The container was then ultrasonically treated for 5~30 minutes in a closed and ventilated environment under an ultrasonic power of 50~100W to obtain an orange-red solution. III. Activation and Temperature Control of Etching Solution: Add hydrofluoric acid solution with a mass percentage concentration of 40%~49% dropwise to the orange-red solution, with the amount added being 10%~20% of the volume of concentrated nitric acid, to obtain a colorless solution; then add a mixture of acetic acid and deionized water at a volume ratio of 1:(1~2) to dilute the colorless solution to obtain a diluted solution; then place the diluted solution in an ice-water bath to cool to 10±1℃ to obtain the etching solution; IV. Single Crystal Etching and Defect Exposure: The crystal with a clean hydrophobic surface obtained in step one is immersed in the etching solution, and ultrasound is turned on at a frequency of 40 kHz and an ultrasonic power of 50~150 W for 3~10 minutes to assist etching. After removing the crystal, it is ultrasonically cleaned with anhydrous ethanol for 60 seconds and dried with nitrogen. V. Defect Characterization: The presence of pits on the crystal surface is observed using a metallographic optical microscope or a scanning electron microscope. The presence of pits indicates dislocation defects, thus revealing the dislocation defects in the lead indium telluride single crystal.

2. The surface etching method for revealing dislocation defects in a lead indium telluride single crystal according to claim 1, characterized in that, The abrasive used in the mechanical polishing process described in step one is alumina powder.

3. A surface etching method for revealing dislocation defects in a lead indium telluride single crystal according to claim 1 or 2, characterized in that, The organic solvent used in the degreasing process described in step one is acetone.

4. A surface etching method for revealing dislocation defects in a lead indium telluride single crystal according to claim 1 or 2, characterized in that, The dilute acid solution used in step one for removing oxides is a mixture of dilute hydrochloric acid with a mass percentage concentration of 5% to 7% and dilute nitric acid with a mass percentage concentration of 5% to 7% in a volume ratio of (2.5 to 3.5):

1.

5. A surface etching method for revealing dislocation defects in a lead indium telluride single crystal according to claim 1 or 2, characterized in that, The inert gas used for inert gas purging in step one is nitrogen.

6. A surface etching method for revealing dislocation defects in a lead indium telluride single crystal according to claim 1 or 2, characterized in that, The ultrasonic treatment described in step two is performed under conditions where the ultrasonic power is 50~100W.

7. A surface etching method for revealing dislocation defects in a lead indium telluride single crystal according to claim 1 or 2, characterized in that, The ultrasound assistance described in step four is performed under the conditions of an ultrasound frequency of 40 kHz and an ultrasound power of 50~150 W.

Citation Information

Patent Citations

  • Compositions for chemical mechanical planarization of copper

    CN101240147A

  • Novel etching solution used in oxide material system, and etching method and application thereof

    CN103980905A

  • Chemical etching method for bismuth selenide material

    CN105543980A

  • Dislocation detection method of rare earth metal oxide crystal

    CN113740331A

  • Method for detecting dislocation density of CVD (chemical vapor deposition) monocrystal diamond