Method for preparing tin oxide layer in perovskite battery through magnetron sputtering and perovskite battery
By using at least two targets for magnetron sputtering in perovskite solar cells to form columnar plasma, the probability of collision and ionization between electrons and reactive gases is increased, thus solving the problem of instability of the tin oxide layer and improving the cycle stability and deposition rate of perovskite solar cells.
Patent Information
- Application Number
- CN202411138496.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2026-03-03
Smart Images

Figure CN121593004A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of perovskite battery technology, and relates to the electron transport layer in perovskite batteries, and more particularly to a method for preparing a tin oxide layer in a perovskite battery by magnetron sputtering and the perovskite battery itself. Background Technology
[0002] Perovskite solar cells have high requirements for the conductivity and stability of their electron transport layer. An electron transport layer with high conductivity and stability helps to improve the cycle stability of perovskite solar cells.
[0003] The electron transport layer materials for perovskite solar cells include metal oxides, organic compounds, and composite materials. Among them, metal oxides include SnO2, and commonly used preparation methods include magnetron sputtering and sol-gel methods.
[0004] For example, in existing technologies for magnetron sputtering electron transport layers on the surface of perovskite layers, the sputtering chamber needs to be evacuated and then argon gas is introduced as the working gas. An orthogonal magnetic field and a high-voltage electric field are applied between the target and the anode, causing the argon gas to ionize into argon ions and electrons under the influence of the electric field. Since a certain negative high voltage is applied to the target, the electrons emitted from the cathode target have an increased probability of ionization with the working gas under the influence of the magnetic field. In this way, electrons will form a high-density plasma near the sputtering surface of the target. Under the influence of the Lorentz force, the argon ions are accelerated towards the cathode and bombard the target surface at high speed. The atoms sputtered from the cathode follow the principle of momentum conversion, detach from the cathode target surface with high kinetic energy, and then fly to the perovskite layer to deposit into a film.
[0005] However, existing magnetron sputtering methods suffer from problems such as excessive energy, uneven deposition, and substrate damage, leading to defects or instability in the prepared tin oxide layer within perovskite solar cells. Therefore, there is a need for a method for preparing tin oxide layers in perovskite solar cells using magnetron sputtering, which reduces damage and improves cycle stability, as well as a perovskite solar cell itself. Summary of the Invention
[0006] The purpose of this invention is to provide a method for preparing a tin oxide layer in a perovskite solar cell using magnetron sputtering, and a perovskite solar cell itself. The method can increase the probability of collisional ionization between electrons and reactive gas during magnetron sputtering, effectively improving the degree of ionization of the reactive gas, increasing the deposition rate of the electron transport layer on the substrate, and avoiding the bombardment of the substrate by electrons with high kinetic energy, thereby effectively reducing damage to the substrate. At the same time, it also suppresses the temperature rise of the perovskite layer during magnetron sputtering, ensuring the cycle stability of the perovskite solar cell.
[0007] To achieve this objective, the present invention adopts the following technical solution:
[0008] In a first aspect, the present invention provides a method for preparing a tin oxide layer in a perovskite solar cell by magnetron sputtering, the method comprising:
[0009] A tin oxide layer is deposited on the deposition surface of the substrate by magnetron sputtering using at least two targets as cathodes.
[0010] Any of the aforementioned target materials has a magnetic field perpendicular to its sputtering surface;
[0011] The normal direction of any of the sputtering surfaces of the target is perpendicular to the normal direction of the substrate deposition surface;
[0012] The central axes of any two sputtering surfaces of the target material intersect;
[0013] The central axis of the space enclosed by the at least two targets intersects with the deposition surface of the substrate.
[0014] In the method provided by this invention, the substrate is a perovskite layer. Magnetron sputtering is performed using the method provided by this invention. Secondary electrons generated by the target material, which serves as the cathode, are interacted with by electric and magnetic fields, effectively confining them within a space enclosed by at least two targets to form a columnar plasma. This increases the probability of collisional ionization between electrons and the reactive gas, effectively enhancing the ionization degree of the reactive gas and increasing the deposition rate of the electron transport layer on the perovskite layer surface. Furthermore, since the plasma formed by secondary electrons is confined within a space enclosed by at least two targets, the bombardment of the substrate by electrons with high kinetic energy can be avoided, effectively reducing damage to the substrate. It also suppresses the temperature rise of the perovskite layer during magnetron sputtering, ensuring the cycle stability of the perovskite solar cell.
[0015] Preferably, the oxygen partial pressure of the reaction gas in the magnetron sputtering is 0-15%.
[0016] Preferably, the absolute pressure during magnetron sputtering is 0.3-0.8 Pa.
[0017] Preferably, the magnetron sputtering power is 100-150W.
[0018] Preferably, the magnetron sputtering time is 5-20 minutes.
[0019] Preferably, the method includes pre-sputtering prior to magnetron sputtering.
[0020] Preferably, the target material comprises at least one of SnO2.
[0021] Preferably, the distance between any two targets is such that an effective glow reaction can occur.
[0022] Preferably, magnets are provided on the opposite sides of the sputtering surface of the target material;
[0023] The magnet generates a magnetic field perpendicular to the sputtering surface of the target material, and the magnetic strength of the magnet is 0.14-0.18T.
[0024] In a second aspect, the present invention provides a perovskite solar cell, wherein the electron transport layer in the perovskite solar cell is prepared by the method described in the first aspect.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The magnetron sputtering method provided by this invention allows secondary electrons generated by the target material serving as the cathode to be effectively controlled within a space enclosed by at least two targets through the interaction of electric and magnetic fields, forming a columnar plasma. This increases the probability of collisional ionization between electrons and the reactive gas, effectively enhancing the ionization degree of the reactive gas and increasing the deposition rate of the electron transport layer on the perovskite layer surface. Furthermore, since the plasma formed by secondary electrons is confined within a space enclosed by at least two targets, the bombardment of the substrate by electrons with high kinetic energy can be avoided, thereby effectively reducing damage to the substrate. It also suppresses the temperature rise of the perovskite layer during magnetron sputtering, ensuring the cycle stability of the perovskite solar cell. Attached Figure Description
[0027] Figure 1 The diagram illustrates the method of Example 1, where hollow spheres represent secondary electrons and solid spheres represent sputtered ions.
[0028] Figure 2 This is a schematic diagram of the target distribution in the method of Example 1, where the dashed area represents the space enclosed by two targets;
[0029] Figure 3 This is a schematic diagram of the target distribution in the method of Example 13, where the dashed area represents the space enclosed by the three targets;
[0030] Figure 4 This is a schematic diagram of the target distribution in the method provided in Example 14. The dashed area represents the space enclosed by the four targets.
[0031] Wherein: 1, substrate; 2, target material; 3, magnet. Detailed Implementation
[0032] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0033] An embodiment of the present invention provides a method for preparing an electron transport layer in a perovskite solar cell by magnetron sputtering, the method comprising:
[0034] An electron transport layer is deposited on the deposition surface of a substrate by magnetron sputtering using at least two targets as cathodes.
[0035] Any of the aforementioned target materials has a magnetic field perpendicular to its sputtering surface;
[0036] The normal direction of any of the sputtering surfaces of the target is perpendicular to the normal direction of the substrate deposition surface;
[0037] The central axes of any two sputtering surfaces of the target material intersect;
[0038] The central axis of the space enclosed by the at least two targets intersects with the deposition surface of the substrate.
[0039] The method provided by this invention further includes a step of gas replacement in the magnetron sputtering cavity to ensure a stable gas atmosphere during magnetron sputtering.
[0040] The method provided by this invention involves a specific arrangement of the target material as the cathode, and the generation of a magnetic field perpendicular to the sputtering surface of each target material, making the magnetic field parallel to the electric field. During magnetron sputtering, the magnetron sputtering cavity is grounded as the anode. When argon ions bombard the sputtering surface of the target material, the secondary electrons ejected from the sputtering surface are accelerated by an external electric field perpendicular to the sputtering surface and bound by the magnetic field in that direction, causing the secondary electrons to undergo Lorentz motion. Therefore, the secondary electrons generated by the target material as the cathode are effectively controlled within the space enclosed by at least two targets by the interaction of electric and magnetic fields, forming a columnar plasma. This increases the probability of collisional ionization between electrons and the reactant gas, effectively enhancing the degree of ionization of the reactant gas and increasing the deposition rate of the electron transport layer on the substrate surface. Furthermore, since the plasma formed by secondary electrons is confined within the space enclosed by at least two targets, the bombardment of the substrate by electrons with high kinetic energy can be avoided, thereby effectively reducing damage to the substrate. At the same time, it also suppresses the temperature rise of the perovskite layer during magnetron sputtering, ensuring the cycle stability of the perovskite solar cell.
[0041] In the method provided by the present invention, the number of targets used is at least two, for example, two, three, four, five or six, but not limited to the listed values. Other unlisted values within the range are also applicable.
[0042] In some embodiments, the central axis of the space enclosed by the at least two targets is perpendicular to the plane containing the deposition surface of the substrate; as a further preferred embodiment, the central axis of the space enclosed by the at least two targets coincides with the central axis of the deposition surface of the substrate.
[0043] In some embodiments, the projections of the at least two targets onto the plane containing the deposition surface of the substrate are uniformly distributed. For example, when magnetron sputtering uses two targets, the angle between the central axes of adjacent targets is 180°; when magnetron sputtering uses three targets, the angle between the central axes of adjacent targets is 120°; when magnetron sputtering uses four targets, the angle between the central axes of adjacent targets is 90°; that is, when magnetron sputtering uses n targets, the angle between the central axes of adjacent targets is 360° / n, where n is a positive integer ≥ 2.
[0044] The electron transport layer material in perovskite solar cells includes metal oxides. The reaction gas used in the magnetron sputtering of this invention is an argon-oxygen mixture. By controlling the oxygen partial pressure during magnetron sputtering, it is beneficial to improve the quality of the obtained electron absorption layer. Moreover, it is beneficial to control the chemical composition of the electron transport layer, and it is also beneficial to further improve the deposition rate.
[0045] During magnetron sputtering, the oxygen partial pressure of the reactant gas affects the matching between the tin oxide layer and C60 in the perovskite solar cell. In order to achieve the protective effect of the tin oxide layer on the perovskite layer, in some embodiments, the oxygen partial pressure of the reactant gas in the magnetron sputtering is 0-15%, for example, it can be 0%, 2%, 5%, 10% or 15%, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0046] The pressure during magnetron sputtering is related to the stress state inside the resulting electron transport layer. Controlling the appropriate magnetron sputtering pressure is beneficial to improving the quality of the resulting electron transport layer and the bonding strength between the electron transport layer and the substrate.
[0047] In some embodiments, the absolute pressure during magnetron sputtering is 0.3-0.8 Pa, for example, it can be 0.3 Pa, 0.4 Pa, 0.5 Pa, 0.6 Pa or 0.8 Pa, but is not limited to the listed values. Other values within the range listed are also applicable.
[0048] The higher the power of magnetron sputtering, the greater the plasma density, which can improve the efficiency of magnetron sputtering. Moreover, appropriate power can promote the densification of the electron transport layer, reduce the formation of columnar structures, and improve the uniformity of the electron transport layer. However, excessive power can also lead to more defects in the electron transport layer, affecting the cycle stability of perovskite solar cells.
[0049] In some embodiments, the magnetron sputtering power is 100-150W, for example, it can be 100W, 110W, 120W, 130W, 140W or 150W, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0050] In some embodiments, the magnetron sputtering time is 5-20 min, for example, 5 min, 10 min, 12 min, 15 min, 18 min or 20 min, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0051] The magnetron sputtering time is related to the thickness of the resulting electron transport layer. Within the magnetron sputtering time range of this invention, an electron transport layer with an average thickness of 10-30 nm can be obtained.
[0052] In some embodiments, the method includes pre-sputtering prior to magnetron sputtering.
[0053] This invention removes the aged layer on the target surface by performing pre-sputtering before the actual magnetron sputtering, thereby stabilizing the sputtered film. This invention does not specifically limit the power, pressure, or oxygen partial pressure of the pre-sputtering, as long as the aged layer on the target surface is removed.
[0054] In some embodiments, the target material includes SnO2.
[0055] In some embodiments, the distance between any two targets enables an effective glow reaction to occur.
[0056] For example, when the method provided by the present invention uses two targets for magnetron sputtering, the distance between the sputtering surfaces of the two targets is 30-60 mm, for example, it can be 30 mm, 40 mm, 50 mm or 60 mm, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0057] In some embodiments, magnets are provided on the opposite side of the sputtering surface of the target;
[0058] The magnet generates a magnetic field perpendicular to the sputtering surface of the target material. The magnetic strength of the magnet is 0.14-0.18T, for example, it can be 0.14T, 0.15T, 0.16T, 0.17T or 0.18T, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0059] The magnet includes a ring magnet or a waist magnet. The present invention does not specifically limit the shape of the magnet, as long as it can generate a magnetic field perpendicular to the sputtering surface of the target material.
[0060] One embodiment of the present invention provides a perovskite solar cell, wherein the tin oxide layer in the perovskite solar cell is prepared by the method for preparing the tin oxide layer in the perovskite solar cell by magnetron sputtering as described in any embodiment.
[0061] Example 1
[0062] This embodiment provides a method such as Figure 1 The method shown is for preparing a tin oxide layer in a perovskite solar cell by magnetron sputtering, the method comprising:
[0063] A tin oxide layer is deposited on the surface of a substrate 1 (C60 layer) by magnetron sputtering using two targets 2 as cathodes; the distance between the sputtering surfaces of the two targets 2 is 50 nm.
[0064] Both targets 2 are made of tin oxide;
[0065] A magnet 3 is provided on the opposite side of the sputtering surface of the target material 2. The magnet 3 generates a magnetic field perpendicular to the sputtering surface of the target material 2. The magnetic strength of the magnet 3 is 0.15T.
[0066] The normal direction of the sputtering surface of any of the target materials 2 is perpendicular to the normal direction of the deposition surface of the substrate 1;
[0067] The central axes of the two sputtering surfaces of the two targets 2 intersect, and the central axis of the space enclosed by the two targets 2 (see...) Figure 2 It coincides with the central axis of the deposition surface of the substrate 1.
[0068] The reaction gas for magnetron sputtering is argon, i.e., the oxygen partial pressure is 0%; the absolute pressure of magnetron sputtering is 0.3 Pa, the power is 120 W, and the time is 18 min, resulting in a tin oxide layer with an average thickness of 15 nm.
[0069] Example 2
[0070] This embodiment provides a method for preparing a tin oxide layer in a perovskite solar cell by magnetron sputtering. Except that the reaction gas used in magnetron sputtering is an argon-oxygen mixture and the oxygen partial pressure is 2%, everything else is the same as in Example 1.
[0071] Example 3
[0072] This embodiment provides a method for preparing a tin oxide layer in a perovskite solar cell by magnetron sputtering. Except that the reaction gas used in magnetron sputtering is an argon-oxygen mixture and the oxygen partial pressure is 5%, everything else is the same as in Example 1.
[0073] Example 4
[0074] This embodiment provides a method for preparing a tin oxide layer in a perovskite solar cell by magnetron sputtering. Except that the reaction gas used in magnetron sputtering is an argon-oxygen mixture and the oxygen partial pressure is 10%, everything else is the same as in Example 1.
[0075] Example 5
[0076] This embodiment provides a method for preparing a tin oxide layer in a perovskite solar cell by magnetron sputtering. Except that the reaction gas used in magnetron sputtering is an argon-oxygen mixture and the oxygen partial pressure is 15%, everything else is the same as in Example 1.
[0077] Example 6
[0078] This embodiment provides a method for preparing a tin oxide layer in a perovskite solar cell by magnetron sputtering. Except that the reaction gas used in magnetron sputtering is an argon-oxygen mixture and the oxygen partial pressure is 18%, everything else is the same as in Example 1.
[0079] Example 7
[0080] This embodiment provides a method for preparing a tin oxide layer in a perovskite solar cell by magnetron sputtering. Except for the magnetron sputtering power of 100W and the time of 20min, the rest is the same as in Example 2.
[0081] The average thickness of the tin oxide layer obtained in this embodiment is 14 nm.
[0082] Example 8
[0083] This embodiment provides a method for preparing an electron transport layer in a perovskite solar cell by magnetron sputtering. Except for the magnetron sputtering power of 150W and the time of 16min, the rest is the same as in Example 2.
[0084] The average thickness of the tin oxide layer obtained in this embodiment is 17 nm.
[0085] Example 9
[0086] This embodiment provides a method for preparing a tin oxide layer in a perovskite solar cell by magnetron sputtering. Except for the absolute pressure of magnetron sputtering being 0.5 Pa and the time being 14 min, the rest is the same as in Example 2.
[0087] The average thickness of the tin oxide layer obtained in this embodiment is 12 nm.
[0088] Example 10
[0089] This embodiment provides a method for preparing a tin oxide layer in a perovskite solar cell by magnetron sputtering. Except for the absolute pressure of magnetron sputtering being 0.7 Pa and the time being 20 min, the rest is the same as in Example 2.
[0090] The average thickness of the tin oxide layer obtained in this embodiment is 16 nm.
[0091] Example 11
[0092] This embodiment provides a method for preparing a tin oxide layer in a perovskite solar cell by magnetron sputtering. Except for the absolute pressure of magnetron sputtering being 0.8 Pa and the time being 20 min, the rest is the same as in Example 2.
[0093] The average thickness of the tin oxide layer obtained in this embodiment is 16 nm.
[0094] Example 12
[0095] This embodiment provides a method for preparing a tin oxide layer in a perovskite solar cell by magnetron sputtering. Except for the magnetron sputtering time of 5 minutes, the method is the same as in Example 2.
[0096] The average thickness of the tin oxide layer obtained in this embodiment is 5 nm.
[0097] Example 13
[0098] This embodiment provides a method for preparing a tin oxide layer in a perovskite solar cell by magnetron sputtering, the method comprising:
[0099] Magnetron sputtering was performed using three targets 2 as cathodes (see [reference]). Figure 3 A tin oxide layer is deposited on the surface of substrate 1 (C60 layer);
[0100] The material of all three targets 2 is tin oxide;
[0101] A magnet 3 is provided on the opposite side of the sputtering surface of the target material 2. The magnet 3 generates a magnetic field perpendicular to the sputtering surface of the target material 2. The magnetic strength of the magnet 3 is 0.15T.
[0102] The normal direction of the sputtering surface of any of the target materials 2 is perpendicular to the normal direction of the deposition surface of the substrate 1;
[0103] The central axes of the three sputtering surfaces of the three targets 2 intersect, and the three targets 2 enclose the central axis of the space (see...). Figure 3 It coincides with the central axis of the deposition surface of the substrate 1.
[0104] The reaction gas for magnetron sputtering is an argon-oxygen mixture with an oxygen partial pressure of 2%. The absolute pressure of magnetron sputtering is 0.3 Pa, the power is 120 W, and the time is 18 min, resulting in a tin oxide layer with an average thickness of 16 nm.
[0105] Example 14
[0106] This embodiment provides a method for preparing a tin oxide layer in a perovskite solar cell by magnetron sputtering, the method comprising:
[0107] Magnetron sputtering was performed using four targets 2 as cathodes (see [reference]). Figure 4 A tin oxide layer is deposited on the surface of substrate 1 (C60 layer);
[0108] The material of all four targets 2 is tin oxide;
[0109] A magnet 3 is provided on the opposite side of the sputtering surface of the target material 2. The magnet 3 generates a magnetic field perpendicular to the sputtering surface of the target material 2. The magnetic strength of the magnet 3 is 0.15T.
[0110] The normal direction of the sputtering surface of any of the target materials 2 is perpendicular to the normal direction of the deposition surface of the substrate 1;
[0111] The central axes of the four sputtering surfaces of the four targets 2 intersect, and the four targets 2 enclose the central axis of the space (see...). Figure 4 It coincides with the central axis of the deposition surface of the substrate 1.
[0112] The reaction gas for magnetron sputtering is an argon-oxygen mixture with an oxygen partial pressure of 2%. The absolute pressure of magnetron sputtering is 0.3 Pa, the power is 120 W, and the time is 18 min, resulting in a tin oxide layer with an average thickness of 16 nm.
[0113] Performance Characterization
[0114] I) An electron transport layer in a crystalline silicon / perovskite tandem solar cell is fabricated using the method provided in the above embodiments, and a crystalline silicon / perovskite tandem solar cell is provided. The fabrication method includes:
[0115] (1) A 150μm thick N-type single crystal silicon is sequentially pre-cleaned with ozone and deionized water, post-cleaned with a mixture of ozone and hydrofluoric acid, and then cleaned and etched with a mixture of hydrofluoric acid and nitric acid to form an N-type crystal silicon wafer with double-sided textured surface.
[0116] (2) A 2nm thick intrinsic hydrogenated amorphous silicon passivation layer is deposited on both sides of the N-type crystalline silicon wafer by PECVD to form the first passivation layer on the front side of the N-type crystalline silicon wafer. Then, a 9nm thick P-type hydrogenated amorphous silicon doped layer and a 6nm thick N-type hydrogenated amorphous silicon doped layer are deposited on both sides to form the second passivation layer on the back side of the N-type crystalline silicon wafer, thereby having a symmetrical bifacial cell structure.
[0117] (3) A 30 nm thick ITO (indium tin oxide) layer is deposited on the surface of the second passivation layer by sputtering;
[0118] (4) A 20 nm thick nickel oxide layer was deposited on the ITO surface by sputtering;
[0119] (5) Then, a perovskite layer with a thickness of 400 nm (CH(NH2)2PbI3) was deposited. 0.83 Cs 0.17 Pb(I 0.82 Br 0.18 )3, 1.66eV), a 1nm thick LiF layer and a 15nm thick C60 layer;
[0120] (6) The sputtering target of the electron transport layer is pre-sputtered to remove the aged layer on the surface, and then a tin oxide layer is deposited using the method in the embodiment;
[0121] (7) A 110 nm thick ITO layer is deposited sequentially on the front and back sides; then a 180 nm thick Ag gate line is screen printed on the back side and sintered and cured; a 1 μm thick Ag and a 90 nm thick MgF2 are vapor-deposited on the front side using a mask.
[0122] The photoelectric conversion efficiency, current density, open-circuit voltage, and fill factor of the obtained crystalline silicon / perovskite tandem solar cell were tested over a test area of 1 cm². 2 The test conditions were: AM1.5, 1000W / m2, 25±2℃; the results are shown in Table 1.
[0123] Table 1
[0124]
[0125]
[0126] II) The tin oxide layer in a single-cell perovskite solar cell is prepared using the method provided in the above embodiments, and a single-cell perovskite solar cell is provided. The preparation method includes:
[0127] A 20 nm thick nickel oxide layer and a 500 nm thick perovskite absorber layer (CH(NH2)2PbI3) were prepared on FTO (fluorine-doped tin oxide) glass, respectively. 0.83 Cs 0.17 Pb(I 0.9 Br 0.1 )3, 1.58eV), 15nm thick C60 layer;
[0128] The sputtering target is pre-sputtered to remove the aged layer on the surface, and then a tin oxide layer is deposited using the method described in the examples.
[0129] A 50 nm thick ITO layer and a 70 nm thick Cu layer were then deposited.
[0130] The photoelectric conversion efficiency, current density, open-circuit voltage, and fill factor of the obtained single-cell perovskite solar cell were tested, with a test area of 1 cm². 2 The test conditions were: AM1.5, 1000W / m2, 25±2℃; the results are shown in Table 2.
[0131] Table 2
[0132]
[0133]
[0134] In summary, the magnetron sputtering method provided by this invention allows secondary electrons generated by the target material as the cathode to be effectively controlled within a space enclosed by at least two targets through the interaction of electric and magnetic fields, forming a columnar plasma. This increases the probability of collisional ionization between electrons and the reactive gas, effectively enhancing the ionization degree of the reactive gas and increasing the deposition rate of the electron transport layer on the perovskite layer surface. Furthermore, since the plasma formed by secondary electrons is confined within a space enclosed by at least two targets, the bombardment of the substrate by electrons with high kinetic energy can be avoided, thereby effectively reducing damage to the substrate. It also suppresses the temperature rise of the perovskite layer during magnetron sputtering, ensuring the cycle stability of the perovskite solar cell.
[0135] The above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A method for preparing a tin oxide layer in a perovskite solar cell by magnetron sputtering, characterized in that, The method includes: A tin oxide layer is deposited on the deposition surface of the substrate by magnetron sputtering using at least two targets as cathodes. Each of the aforementioned targets has a magnetic field perpendicular to its sputtering surface; The normal direction of any of the sputtering surfaces of the target is perpendicular to the normal direction of the substrate deposition surface; The central axes of any two sputtering surfaces of the target material intersect; The central axis of the space enclosed by the at least two targets intersects with the deposition surface of the substrate.
2. The method according to claim 1, characterized in that, The oxygen partial pressure of the reaction gas in the magnetron sputtering is 0-15%.
3. The method according to claim 1, characterized in that, The absolute pressure during magnetron sputtering is 0.3-0.8 Pa.
4. The method according to claim 1, characterized in that, The magnetron sputtering power is 100-150W.
5. The method according to claim 1, characterized in that, The magnetron sputtering time is 5-20 minutes.
6. The method according to claim 1, characterized in that, The method includes pre-sputtering prior to magnetron sputtering.
7. The method according to claim 1, characterized in that, The target material includes SnO2.
8. The method according to claim 1, characterized in that, The distance between any two targets enables an effective glow reaction to occur.
9. The method according to claim 1, characterized in that, Magnets are provided on the opposite side of the sputtering surface of the target material; The magnet generates a magnetic field perpendicular to the sputtering surface of the target material, and the magnetic strength of the magnet is 0.14-0.18T.
10. A perovskite solar cell, characterized in that, The tin oxide layer in the perovskite solar cell is prepared by the method described in any one of claims 1-9.