Preparation method of water-permeable material for water-permeable tree surrounding brick

By introducing zwitterionic grafted porous silica-alumina dispersion, magnesium silicate gel composite magnesium carbonate dispersion, and ettringite composite hydroxyapatite whiskers into permeable tree paving materials, the shortcomings of permeable materials in terms of structural stability and durability are solved, achieving higher structural stability and pore connectivity, and improving the overall performance of permeable tree paving.

CN121929963APending Publication Date: 2026-04-28GUANGDONG ASIA SPORTS IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610149592.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-02-03
Publication Date
2026-04-28

AI Technical Summary

Technical Problem

Existing permeable tree embankment bricks have problems in the structural construction process, such as discontinuous distribution of cementitious phase, unclear aggregate connection relationship, insufficient stability of pore structure, and lack of targeted control over the distribution of cementitious material, resulting in insufficient overall structural stability and durability.

Method used

A zwitterionic grafted porous silica-alumina dispersion, magnesium silicate gel composite magnesium carbonate dispersion, and ettringite composite hydroxyapatite whiskers are combined with aggregates to construct a composite inorganic interface structure through interfacial interactions, ensuring aggregate connection stability and pore connectivity, forming a continuous pore space and a stable cementing system.

Benefits of technology

It improves the structural stability and durability of permeable tree embankment bricks, ensuring the integrity of the overall structure and the continuity of pore channels under load and environmental changes, thus extending the service life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121929963A_ABST
    Figure CN121929963A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a water-permeable material for a water-permeable tree surrounding brick, belongs to the technical field of preparation of water-permeable brick materials, and aims to solve the technical problem that the mechanical property and durability of the water-permeable tree surrounding brick prepared from the water-permeable material in the prior art need to be further improved. The zwitterionic grafted porous silicon-aluminum dispersion, the magnesium-silicon gel composite magnesium carbonate dispersion and the ettringite composite hydroxyapatite whisker are introduced in the preparation process, and a continuous cementation structure, an interface transition structure and a space constraint support structure are cooperatively constructed on different structural scales; a stable and matched composite system is formed among the cementing phase, the aggregate and the pore structure, and the coordination and stability of the whole structure of the water-permeable tree surrounding brick are effectively maintained through the synergistic configuration of the multiple components in the system, so that the structure integrity and the use reliability are considered while the material meets the water-permeable requirement; the method is suitable for the field of garden and municipal permeable pavement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of permeable brick material preparation technology, specifically to a method for preparing a permeable material for permeable tree surround bricks. Background Technology

[0002] In the field of urban infrastructure and landscaping engineering, permeable tree pavers, as a component that combines rainwater infiltration, soil aeration, and landscape paving functions, largely depend on the permeable material system used. Existing permeable tree pavers are mostly based on cement-based or other inorganic cementitious materials, using aggregates of different gradations to form interconnected pore structures to meet permeability requirements. In this type of material system, the cementing phase is responsible for achieving particle consolidation, the aggregates form the main load-bearing skeleton, and the pore structure provides channels for water infiltration. Different components are interconnected in terms of structural scale and mode of action. With the diversification of application scenarios, related technologies are gradually shifting from single material selection to comprehensive research on material composition, interface structure, and molding processes. The systematic design of permeable materials has become one of the important development directions in this field.

[0003] Existing permeable tree embankment bricks often use cementitious systems composed of single or few components. During the structural construction process, the distribution of the cementitious phase on the aggregate surface is often discontinuous, and the connection between coarse and fine aggregates is not clear enough. After molding, local weak connection areas are easily formed. Under load or external force, the deformation response of different areas inside the material is difficult to be consistent, and the force transmission path is prone to interruption or deviation, thus affecting the overall structural stability. In addition, some material systems lack effective structural adjustment mechanisms at the aggregate interface, making it difficult to buffer local stress concentration.

[0004] Meanwhile, existing processes typically rely on aggregate gradation to naturally form pores, which have insufficient stability at the pore boundaries and are prone to deformation or collapse during molding, loading, or environmental changes, affecting the connectivity of the pores. Furthermore, the distribution of cementing materials in the pore areas lacks targeted control and may enter the main pores and interfere with the water permeability pathways. During long-term use, the interfacial bonding state and local structure of the material are prone to change under conditions of temperature changes, moisture migration, and repeated friction, making it difficult to maintain the overall structural consistency and service stability over a long period.

[0005] To address this technical deficiency, a solution is proposed. Summary of the Invention

[0006] The purpose of this invention is to provide a method for preparing permeable materials for permeable tree paving bricks, which solves the technical problem that the mechanical properties and durability of permeable tree paving bricks prepared from permeable materials in the prior art need to be further improved.

[0007] The objective of this invention can be achieved through the following technical solutions: A method for preparing a permeable material for permeable tree embankment bricks includes the following steps: S1. Add zwitterionic grafted porous silica-alumina dispersion, magnesium silicate gel composite magnesium carbonate dispersion and deionized water to a mixing tank and stir. After mixing evenly, add ettringite composite hydroxyapatite whiskers and continue stirring for 3-5 minutes to obtain modified slurry. S2. Add coarse and fine aggregates to the mixing tank, dry mix for 30-60 seconds, then add gel material, continue mixing for 30-60 seconds, then add modified slurry and mix for 120-180 seconds to obtain permeable material.

[0008] The reaction principle for preparing permeable materials is as follows: In aqueous multiphase systems, the Ca released during the hydration of P.O42.5 ordinary Portland cement... 2+ Silicate and aluminate species interact with the zwitterionic grafted porous silica-alumina dispersion, magnesium silicate gel composite magnesium carbonate dispersion, and ettringite composite hydroxyapatite whiskers dispersed in the system. The polar groups on the surface of the zwitterionic grafted porous silica-alumina dispersion participate in the formation of a stable adsorption and coordination environment. The magnesium silicate gel phase and magnesium carbonate phase in the magnesium silicate gel composite magnesium carbonate dispersion are synergistically distributed with cement hydration products through ion exchange and weak chemical bonding. The ettringite composite hydroxyapatite whiskers are oriented on the surface of coarse and fine aggregates, thereby constructing a composite inorganic interface structure between the aggregates and cementitious materials, and thus preparing a permeable material.

[0009] Furthermore, in step S1, the ratio of zwitterionic grafted porous silica-alumina dispersion, magnesium silicate gel composite magnesium carbonate dispersion, deionized water and ettringite composite hydroxyapatite whiskers is 1g:1g:10mL:2g. Furthermore, in step S2, the ratio of coarse aggregate, fine aggregate, gel material, and modified slurry is 100g:5g:21-24g:12g, wherein the coarse aggregate is basalt crushed stone with a particle size of 5-8mm, the fine aggregate is quartz sand with a particle size of 0.8-1.0mm, and the gel material is P.O42.5 ordinary Portland cement.

[0010] Furthermore, the zwitterionic grafted porous silica-alumina dispersion is prepared by the following method: A1. Add porous silica-alumina gel microparticles, 3-glycidyl etheroxypropyltrimethoxysilane and anhydrous ethanol to a reaction vessel and stir. After mixing evenly, add deionized water and adjust the pH of the reaction system to 4.5-5.0 with glacial acetic acid. Then heat the reaction vessel to 55-65℃ and keep it at that temperature for 2-4 hours. Post-treatment yields epoxy-grafted porous silica-alumina microparticles. A2. Add epoxidized grafted porous silica-alumina microparticles and mixed solvent to a reaction vessel and stir. After uniform dispersion, heat the reaction vessel to 45-55℃ and add N,N-dimethyl-1,3-propanediamine. Keep the temperature and stir for 2-3 hours. Then, cool the reaction vessel to 35-45℃ and add 1,3-propanesulfonyl lactone. Continue to keep the temperature and stir for 6-8 hours. Post-treatment yields zwitterionic grafted porous silica-alumina dispersion.

[0011] The reaction principle for preparing zwitterionic grafted porous silica-alumina dispersions is as follows: Under weakly acidic conditions, a condensation reaction occurs between the silanol groups on the surface of the porous silica-alumina gel and the silanol groups formed by the hydrolysis of organosilane molecules, causing the organic side links containing epoxy groups to be grafted onto the surface of the inorganic framework. Subsequently, the epoxy groups undergo a ring-opening reaction under the nucleophilic action of amine compounds to generate a quaternary ammonium intermediate structure. This structure further undergoes an addition reaction with lactone compounds, simultaneously introducing positive and negatively charged groups onto the molecular chain, thereby constructing a stable organic zwitterionic structure on the surface of the inorganic silica-alumina framework, and thus preparing a zwitterionic grafted porous silica-alumina dispersion.

[0012] Further, in step A1, the ratio of the porous silica-alumina gel microparticles, 3-glycidoxypropyltrimethoxysilane, anhydrous ethanol and deionized water is 16-18g:6-8mL:100mL:2mL. The post-treatment includes: after the reaction is completed, filtering to collect the solid, washing it three times with anhydrous ethanol, and vacuum drying it in a drying oven at 60°C for 6 hours to obtain epoxy-grafted porous silica-alumina microparticles. Further, in step A2, the ratio of the epoxidized grafted porous silica-alumina microparticles, the mixed solvent, N,N-dimethyl-1,3-propanediamine, and 1,3-propanesulfonyl lactone is 12-16g:80-100mL:3-5mL:4-6g. The mixed solvent is obtained by mixing deionized water and anhydrous ethanol at a ratio of 1mL:4mL. The post-treatment includes: filtering and collecting the solid after the reaction, washing it three times with anhydrous ethanol, and vacuum drying it in a drying oven at 60°C for 6-8 hours to obtain a zwitterionic grafted porous silica-alumina dispersion.

[0013] Furthermore, the preparation method of porous silica-alumina gel microparticles is as follows: methyl orthosilicate, aluminum isopropoxide and anhydrous ethanol are added to a reaction vessel and stirred. After the mixture is uniform, deionized water is added and saturated ammonia is used to adjust the pH of the reaction system to 9-10. The reaction vessel is heated to 35°C and stirred for 2-3 hours. Then, ammonium bicarbonate is added and stirred for 10-20 minutes. After post-treatment, porous silica-alumina gel microparticles are obtained.

[0014] The reaction principle for preparing porous silica-alumina gel microparticles is as follows: Under alkaline conditions, methyl orthosilicate hydrolyzes to generate silanol-containing species, while aluminum isopropoxide hydrolyzes simultaneously to form aluminum hydroxyl coordination structures. The two gradually construct an amorphous network with Si-O-Al bonds as the connecting units through hydroxyl condensation reactions. The synergistic effect of solvent and water molecules in the system regulates the hydrolysis and condensation rates, making the gel structure tend to be homogenized. The introduction of ammonium bicarbonate changes the local ionic environment and participates in the gas release process, thereby inducing the formation of pores in the gel skeleton, and finally preparing porous silica-alumina gel microparticles.

[0015] Furthermore, in the preparation of porous silica-alumina gel microparticles, the ratio of methyl orthosilicate, aluminum isopropoxide, anhydrous ethanol, deionized water and ammonium bicarbonate is 20-24 mL: 8-10 mL: 100 mL: 50 mL: 2-3 g. The post-treatment includes: after stirring, pouring the obtained sol into a mold, letting it stand at 20-25℃ for 16-20 h, then cutting the obtained gel material into 3 mm particles, and then vacuum drying at 60-80℃ for 8 h to obtain porous silica-alumina gel microparticles.

[0016] Furthermore, the ettringite-hydroxyapatite whiskers are prepared by the following method: B1. Add calcium hydroxide and deionized water to the reaction vessel and stir until a slurry is formed. Then, heat the reaction vessel to 30-40℃ and add aluminum sulfate octahydrate. Keep it warm and stir for 10-15 minutes. Then, add calcium sulfate dihydrate and stir for 1-2 hours. After post-treatment, needle-shaped ettringite crystal nuclei are obtained. B2. Add needle-shaped ettringite crystal nuclei and deionized water to a reaction vessel and stir. After the mixture is evenly dispersed, add saturated ammonia water to adjust the pH of the reaction vessel system to 9.5-10.5. Heat the reaction vessel to 35-45℃ and add equal amounts of calcium nitrate and diammonium hydrogen phosphate in 10 batches with an interval of 10 minutes between additions. After the addition is complete and the mixture is kept warm and stirred for 1 hour, transfer the reaction solution to a hydrothermal reaction vessel. Heat the hydrothermal reaction vessel to 120-160℃ and keep it warm for 6-8 hours. The post-treatment yields ettringite composite hydroxyapatite whiskers.

[0017] The reaction principle for preparing ettringite-hydroxyapatite whiskers is as follows: In a strongly alkaline aqueous system, Ca 2+ Al(OH)4 - With SO4 2- Coordination and precipitation reactions occur between them, preferentially growing to form [Ca6Al2(OH)2]. 12 ] 2+ The ettringite phase, consisting of a framework, sulfate, and water of crystallization, exhibits a stable structure. Its crystal structure displays anisotropic growth characteristics along specific crystal orientations. Furthermore, in an alkaline environment containing calcium and phosphorus precursors, the Ca released from the solution... 2+ With PO43- The calcium phosphate phase is gradually formed through nucleation and structural rearrangement. The hydroxyapatite lattice undergoes heterogeneous precipitation on the surface of ettringite and undergoes lattice ordering under hydrothermal conditions to form a composite crystal structure in which the two phases coexist. Finally, ettringite composite hydroxyapatite whiskers are prepared.

[0018] Further, in step B1, the ratio of calcium hydroxide, deionized water, aluminum sulfate octahydrate and calcium sulfate dihydrate is 12-18g:200-220mL:24-30g:10-15g. The post-treatment includes: after stirring, cooling the reaction vessel to room temperature and aging for 8-12h, filtering to collect the solid, washing with anhydrous ethanol until neutral, and vacuum drying in a drying oven at 60℃ for 6-8h to obtain needle-shaped ettringite crystal nuclei. Furthermore, in step B2, the ratio of the needle-like ettringite crystal nuclei, deionized water, calcium nitrate, and diammonium hydrogen phosphate is 8-12g:200mL:10-16g:5-8g. The post-treatment includes: filtering and collecting the solid after natural cooling, washing with anhydrous ethanol until neutral, and vacuum drying in a drying oven at 60°C for 6-8 hours to obtain ettringite composite hydroxyapatite whiskers.

[0019] Furthermore, the preparation method of the magnesium silicate gel composite magnesium carbonate is as follows: magnesium oxide and deionized water are added to a reaction vessel and stirred until a slurry is formed. The reaction vessel is then heated to 60-80°C and hydrated silica is added. After stirring for 2-4 hours, mineralization is carried out, and the magnesium silicate gel composite magnesium carbonate dispersion is obtained through post-treatment.

[0020] The reaction principle for preparing magnesium silicate gel composite magnesium carbonate dispersion is as follows: Under aqueous conditions, magnesium oxide undergoes hydration and forms magnesium-containing hydroxyl species, gradually releasing Mg from the system. 2+ A magnesium silicate gel network characterized by Mg-O-Si bonds is constructed by coordination and condensation reactions with silanol groups on the surface of hydrated silica. Subsequently, in a carbon dioxide-containing environment, some free or weakly bound magnesium species undergo carbonation reactions with CO2 to generate a magnesium carbonate phase, which coexists with the magnesium silicate gel phase to form a composite structure, thereby preparing a magnesium silicate gel composite magnesium carbonate dispersion.

[0021] Furthermore, in the preparation of magnesium silicate gel composite magnesium carbonate dispersion, the ratio of magnesium oxide, deionized water and hydrated silica is 15-18g:200mL:25-35g. The post-treatment includes: after mineralization, filtering to collect the solid, washing with anhydrous ethanol until neutral, and vacuum drying in a drying oven at 60℃ for 6-8h to obtain magnesium silicate gel composite magnesium carbonate dispersion. Furthermore, the mineralization step is as follows: after the reaction system is placed in a curing chamber with a humidity of 70-90% for 1-2 hours, carbon dioxide is introduced into the curing chamber and the temperature of the curing chamber is controlled at 20-40℃ and the pressure at 0.2-0.4MPa, and the constant temperature and pressure treatment is carried out for 2-6 hours.

[0022] The present invention has the following beneficial effects: In the structural construction of permeable tree embankments, the zwitterionic grafted porous silica-alumina dispersion prepared in this invention forms a continuous distribution on the aggregate surface as the main cementing phase, ensuring a clear connection between coarse and fine aggregates after molding and providing basic support for subsequent structural stability. Furthermore, the magnesium silicate gel composite magnesium carbonate dispersion is distributed between aggregates and at interfaces, working synergistically with the silica-alumina skeleton during hardening to maintain relatively consistent deformation characteristics at aggregate connection points under stress, avoiding localized stress concentration. Additionally, ettringite composite hydroxyapatite whiskers are embedded in the cementing system in a dispersed state, providing support and constraint to the connection nodes between aggregates, allowing for continuous transmission of stress within the material. The synergistic effect of the spatial distribution and structural configuration of these three materials ensures that the permeable tree embankments maintain the integrity and stability of the overall structure under load.

[0023] During the formation and maintenance of the pore structure, zwitterionic grafted porous silica-alumina dispersion forms a stable coating on the aggregate surface, ensuring clear gap boundaries when the aggregates are in contact with each other, thereby constructing a continuous pore space. The magnesium silicate gel composite magnesium carbonate dispersion exists in a dispersed form in the system, mainly distributed at the aggregate connection points, which plays a role in fixing the aggregate spacing and preventing it from entering the main pore area and interfering with the pore connectivity. Furthermore, the ettringite composite hydroxyapatite whiskers are distributed along the pore boundaries and aggregate contact areas, which constrain the pore morphology during molding and use, reducing the deformation of the pore structure due to load or environmental changes. Through the synergistic configuration of the above materials in the pore structure, the pore structure maintains its predetermined shape and continuous channels under load conditions.

[0024] During long-term service, the zwitterionic grafted porous silica-alumina dispersion forms a stable interface with the aggregate, enabling the material to maintain a relatively consistent structural response under temperature changes and moisture migration conditions. Meanwhile, the magnesium silicate gel composite magnesium carbonate dispersion is distributed in the interface and microporous region, which regulates the local structure during repeated environmental changes, keeping the bonding state between the cementing system and the aggregate stable. The ettringite composite hydroxyapatite whiskers form a dispersed support on the material surface and in areas susceptible to external influences, limiting structural changes under friction and cyclic conditions. The synergistic distribution and action of the three materials during service enable the permeable tree embankment to maintain a stable structural state under the combined influence of various external factors. Attached Figure Description

[0025] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0026] Figure 1 This is a SEM image of the zwitterionic grafted porous silica-alumina dispersion prepared in Example 3 of the present invention. Figure 2 This is a SEM image of the ettringite-hydroxyapatite whiskers prepared in Example 6 of the present invention. Figure 3 This is a SEM image of the magnesium silicate gel composite magnesium carbonate dispersion prepared in Example 9 of the present invention. Detailed Implementation

[0027] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0028] In this application, the hydrated silica used was purchased from Shanghai Yuanye Biotechnology Co., Ltd., with the product number T25908; the P.O42.5 ordinary silicate cement used was purchased from Shenzhen Tairun Cement Co., Ltd., with the product number P.O42.5.

[0029] Example 1: This example provides a method for preparing zwitterionic grafted porous silica-alumina dispersion, including the following steps: Step 1: Preparation of porous silica-alumina gel microparticles Weigh out 20.0 mL of methyl orthosilicate, 8.0 mL of aluminum isopropoxide, and 100.0 mL of anhydrous ethanol and add them to a reaction vessel. Stir until the mixture is homogeneous, then add 50.0 mL of deionized water and adjust the pH of the reaction system to 9 using saturated ammonia. Heat the reaction vessel to 35°C and stir for 2 hours. Then add 2.0 g of ammonium bicarbonate and stir for 10 minutes. After stirring, pour the resulting sol into a mold and let it stand at 20°C for 16 hours. Then, cut the resulting gel material into 3 mm particles and dry it under vacuum at 60°C for 8 hours to obtain porous silica-alumina gel microparticles.

[0030] Step 2: Preparation of epoxy-grafted porous silica-alumina microparticles Weigh out 16.0 g of porous silica-alumina gel microparticles, 6.0 mL of 3-glycidyl etheroxypropyltrimethoxysilane, and 100.0 mL of anhydrous ethanol and add them to a reaction vessel. Stir until the mixture is homogeneous, then add 2.0 mL of deionized water and adjust the pH of the reaction system to 4.5 using glacial acetic acid. Heat the reaction vessel to 55 °C and stir for 2 h. After the reaction is complete, filter and collect the solid. Wash the solid three times with anhydrous ethanol and vacuum dry it in a drying oven at 60 °C for 6 h to obtain epoxy-grafted porous silica-alumina microparticles.

[0031] Step (3): Preparation of zwitterionic grafted porous silica-alumina dispersion Weigh out 20.0 mL of deionized water and 80.0 mL of anhydrous ethanol and mix them to obtain a mixed solvent; Weigh 12.0 g of epoxidized grafted porous silica-alumina microparticles and 80.0 mL of mixed solvent and add them to the reaction vessel. Stir until the dispersion is uniform, then heat the reaction vessel to 45 °C and add 3.0 mL of N,N-dimethyl-1,3-propanediamine. Keep the mixture warm and stir for 2 h, then cool the reaction vessel to 35 °C and add 4.0 g of 1,3-propanesulfonyl lactone. Continue to keep the mixture warm and stir for 6 h. After the reaction is complete, filter and collect the solid. Wash the solid three times with anhydrous ethanol and vacuum dry it in a drying oven at 60 °C for 6 h to obtain zwitterionic grafted porous silica-alumina dispersion.

[0032] Example 2: This example provides a method for preparing zwitterionic grafted porous silica-alumina dispersion, including the following steps: Step 1: Preparation of porous silica-alumina gel microparticles Weigh out 24.0 mL of methyl orthosilicate, 10.0 mL of aluminum isopropoxide, and 100.0 mL of anhydrous ethanol and add them to a reaction vessel. Stir until the mixture is homogeneous, then add 50.0 mL of deionized water and adjust the pH of the reaction system to 10 using saturated ammonia. Heat the reaction vessel to 35°C and stir for 3 hours. Then add 3.0 g of ammonium bicarbonate and stir for 20 minutes. After stirring, pour the resulting sol into a mold and let it stand at 25°C for 20 hours. Then, cut the resulting gel material into 3 mm particles and vacuum dry it at 80°C for 8 hours to obtain porous silica-alumina gel microparticles.

[0033] Step 2: Preparation of epoxy-grafted porous silica-alumina microparticles Weigh 18.0 g of porous silica-alumina gel microparticles, 8.0 mL of 3-glycidyl etheroxypropyltrimethoxysilane, and 100.0 mL of anhydrous ethanol and add them to a reaction vessel. Stir until the mixture is homogeneous, then add 2.0 mL of deionized water and adjust the pH of the reaction system to 5.0 using glacial acetic acid. Heat the reaction vessel to 65 °C and keep it at that temperature for 4 h with stirring. After the reaction is complete, filter and collect the solid. Wash the solid three times with anhydrous ethanol and vacuum dry it in a drying oven at 60 °C for 6 h to obtain epoxy-grafted porous silica-alumina microparticles.

[0034] Step (3): Preparation of zwitterionic grafted porous silica-alumina dispersion Weigh out 20.0 mL of deionized water and 80.0 mL of anhydrous ethanol and mix them to obtain a mixed solvent; Weigh 16.0 g of epoxidized grafted porous silica-alumina microparticles and 100.0 mL of mixed solvent and add them to the reaction vessel. Stir until the dispersion is uniform, then heat the reaction vessel to 55 °C and add 5.0 mL of N,N-dimethyl-1,3-propanediamine. Keep the mixture warm and stir for 3 h, then cool the reaction vessel to 45 °C and add 6.0 g of 1,3-propanesulfonyl lactone. Continue to keep the mixture warm and stir for 8 h. After the reaction is complete, filter and collect the solid, wash it three times with anhydrous ethanol, and vacuum dry it in a drying oven at 60 °C for 8 h to obtain zwitterionic grafted porous silica-alumina dispersion.

[0035] Example 3: This example provides a method for preparing zwitterionic grafted porous silica-alumina dispersion, including the following steps: Step 1: Preparation of porous silica-alumina gel microparticles Weigh out 21.0 mL of methyl orthosilicate, 9.0 mL of aluminum isopropoxide, and 100.0 mL of anhydrous ethanol and add them to a reaction vessel. Stir until the mixture is homogeneous, then add 50.0 mL of deionized water and adjust the pH of the reaction system to 10 using saturated ammonia. Heat the reaction vessel to 35°C and stir for 3 hours. Then add 2.5 g of ammonium bicarbonate and stir for 15 minutes. After stirring, pour the resulting sol into a mold and let it stand at 25°C for 18 hours. Then, cut the resulting gel material into 3 mm particles and vacuum dry it at 70°C for 8 hours to obtain porous silica-alumina gel microparticles.

[0036] Step 2: Preparation of epoxy-grafted porous silica-alumina microparticles Weigh out 17.0 g of porous silica-alumina gel microparticles, 7.0 mL of 3-glycidyl etheroxypropyltrimethoxysilane, and 100.0 mL of anhydrous ethanol and add them to a reaction vessel. Stir until the mixture is homogeneous, then add 2.0 mL of deionized water and adjust the pH of the reaction system to 5.0 using glacial acetic acid. Heat the reaction vessel to 60 °C and stir for 3 h. After the reaction is complete, filter and collect the solid, wash it three times with anhydrous ethanol, and vacuum dry it in a drying oven at 60 °C for 6 h to obtain epoxy-grafted porous silica-alumina microparticles.

[0037] Step (3): Preparation of zwitterionic grafted porous silica-alumina dispersion Weigh out 20.0 mL of deionized water and 80.0 mL of anhydrous ethanol and mix them to obtain a mixed solvent; Weigh 15.0 g of epoxidized grafted porous silica-alumina microparticles and 90.0 mL of mixed solvent and add them to the reaction vessel. Stir until the dispersion is uniform. Then heat the reaction vessel to 50 °C and add 4.0 mL of N,N-dimethyl-1,3-propanediamine. Keep the mixture warm and stir for 3 h. Then cool the reaction vessel to 40 °C and add 5.0 g of 1,3-propanesulfonyl lactone. Continue to keep the mixture warm and stir for 7 h. After the reaction is complete, filter and collect the solid. Wash the solid three times with anhydrous ethanol and dry it under vacuum in a drying oven at 60 °C for 7 h to obtain zwitterionic grafted porous silica-alumina dispersion.

[0038] Example 4: This example provides a method for preparing ettringite-hydroxyapatite whiskers, including the following steps: Step ①: Preparation of needle-shaped ettringite crystal nuclei Weigh out 12.0 g of calcium hydroxide and 200.0 mL of deionized water and add them to the reaction vessel. Stir until a slurry is formed. Heat the reaction vessel to 30 °C and add 24.0 g of aluminum sulfate octahydrate. Keep the temperature and stir for 10 min. Then add 10.0 g of calcium sulfate dihydrate and stir for 1 h. After stirring, cool the reaction vessel to room temperature and age for 8 h. Filter and collect the solid. Wash with anhydrous ethanol until neutral and vacuum dry in a drying oven at 60 °C for 6 h to obtain needle-like ettringite crystal nuclei.

[0039] Step 2: Preparation of ettringite-hydroxyapatite whiskers Weigh 8.0g of needle-shaped ettringite crystal nuclei and 200.0mL of deionized water and add them to the reaction vessel. Stir until the mixture is evenly dispersed. Then, add saturated ammonia water to adjust the pH of the reaction vessel system to 9.5. Heat the reaction vessel to 35℃ and add equal amounts of 10.0g of calcium nitrate and 5.0g of diammonium hydrogen phosphate in 10 batches with an interval of 10min between additions. After the addition is complete and the mixture is kept warm and stirred for 1h, transfer the reaction solution to a hydrothermal reaction vessel. Heat the hydrothermal reaction vessel to 120℃ and keep it warm for 6h. After natural cooling, filter and collect the solid. Wash with anhydrous ethanol until neutral and vacuum dry in a drying oven at 60℃ for 6h to obtain ettringite-hydroxyapatite whiskers.

[0040] Example 5: This example provides a method for preparing ettringite-hydroxyapatite whiskers, including the following steps: Step ①: Preparation of needle-shaped ettringite crystal nuclei Weigh out 18.0 g of calcium hydroxide and 220.0 mL of deionized water and add them to the reaction vessel. Stir until a slurry is formed. Then heat the reaction vessel to 40 °C and add 30.0 g of aluminum sulfate octahydrate. Keep the temperature and stir for 15 min. Then add 15.0 g of calcium sulfate dihydrate and stir for 2 h. After stirring, cool the reaction vessel to room temperature and age for 12 h. Filter and collect the solid. Wash with anhydrous ethanol until neutral and vacuum dry in a drying oven at 60 °C for 8 h to obtain needle-shaped ettringite crystal nuclei.

[0041] Step 2: Preparation of ettringite-hydroxyapatite whiskers Weigh 12.0g of needle-shaped ettringite crystal nuclei and 200.0mL of deionized water and add them to the reaction vessel. Stir until the mixture is evenly dispersed. Then, add saturated ammonia water to adjust the pH of the reaction vessel system to 10.5. Heat the reaction vessel to 45℃ and add equal amounts of 16.0g of calcium nitrate and 8.0g of diammonium hydrogen phosphate in 10 batches with an interval of 10min between additions. After the addition is complete and the mixture is kept warm and stirred for 1h, transfer the reaction solution to a hydrothermal reaction vessel. Heat the hydrothermal reaction vessel to 160℃ and keep it at that temperature for 8h. After natural cooling, filter and collect the solid. Wash with anhydrous ethanol until neutral and vacuum dry in a drying oven at 60℃ for 8h to obtain ettringite-hydroxyapatite whiskers.

[0042] Example 6: This example provides a method for preparing ettringite-hydroxyapatite whiskers, including the following steps: Step ①: Preparation of needle-shaped ettringite crystal nuclei Weigh out 15.0 g of calcium hydroxide and 210.0 mL of deionized water and add them to the reaction vessel. Stir until a slurry is formed. Then heat the reaction vessel to 35 °C and add 27.0 g of aluminum sulfate octahydrate. Keep the temperature and stir for 12 min. Then add 12.0 g of calcium sulfate dihydrate and stir for 2 h. After stirring, cool the reaction vessel to room temperature and age for 10 h. Filter and collect the solid. Wash with anhydrous ethanol until neutral and vacuum dry in a drying oven at 60 °C for 7 h to obtain needle-shaped ettringite crystal nuclei.

[0043] Step 2: Preparation of ettringite-hydroxyapatite whiskers Weigh 10.0g of needle-shaped ettringite crystal nuclei and 200.0mL of deionized water and add them to the reaction vessel. Stir until the mixture is evenly dispersed. Then, add saturated ammonia water to adjust the pH of the reaction vessel system to 10.0. Heat the reaction vessel to 40℃ and add equal amounts of 12.0g of calcium nitrate and 6.0g of diammonium hydrogen phosphate in 10 batches with an interval of 10min between additions. After the addition is complete and the mixture is kept warm and stirred for 1h, transfer the reaction solution to a hydrothermal reaction vessel. Heat the hydrothermal reaction vessel to 150℃ and keep it at that temperature for 7h. After natural cooling, filter and collect the solid. Wash with anhydrous ethanol until neutral and vacuum dry in a drying oven at 60℃ for 7h to obtain ettringite-hydroxyapatite whiskers.

[0044] Example 7: This example provides a method for preparing a permeable material for permeable tree paving bricks, including the following steps: Step 1: Preparation of magnesium silicate gel composite magnesium carbonate dispersion Weigh out 15.0g of magnesium oxide and 200.0mL of deionized water and add them to the reaction vessel. Stir until a slurry is formed. Heat the reaction vessel to 60℃ and add 25.0g of hydrated silica. Keep the mixture warm and stir for 2 hours. Place the reaction system in a curing chamber with 70% humidity for 1 hour. Then, introduce carbon dioxide into the curing chamber and control the temperature of the curing chamber to 20℃ and the pressure to 0.2MPa. Treat the mixture at constant temperature and pressure for 2 hours. After mineralization, filter and collect the solid. Wash the solid with anhydrous ethanol until neutral and vacuum dry it in a drying oven at 60℃ for 6 hours to obtain magnesium silicate gel composite magnesium carbonate dispersion.

[0045] Step 2: Preparation of modified slurry Weigh out 10.0g of zwitterionic grafted porous silica-alumina dispersion prepared in Example 1, 10.0g of magnesium silicate gel composite magnesium carbonate dispersion and 100.0mL of deionized water and add them to a stirring vessel. After mixing evenly, add 20.0g of ettringite composite hydroxyapatite whiskers prepared in Example 4 and continue stirring for 3 minutes to obtain the modified slurry.

[0046] Step 3: Preparation of permeable materials Weigh out 1000.0g of basalt crushed stone with a particle size of 5mm and 50.0g of quartz sand with a particle size of 0.8mm and add them to the mixing tank. After dry mixing for 30s, add 210.0g of P.O42.5 ordinary Portland cement and continue mixing for 30s. Then add 120.0g of modified slurry and mix for 120s to obtain a permeable material.

[0047] Example 8: This example provides a method for preparing a permeable material for permeable tree paving bricks, including the following steps: Step 1: Preparation of magnesium silicate gel composite magnesium carbonate dispersion Weigh out 18.0 g of magnesium oxide and 200.0 mL of deionized water and add them to the reaction vessel. Stir until a slurry is formed. Heat the reaction vessel to 80 °C and add 35.0 g of hydrated silica. Keep the mixture warm and stir for 4 h. Place the reaction system in a curing chamber with 90% humidity for 2 h. Then, introduce carbon dioxide into the curing chamber and control the temperature of the curing chamber to 40 °C and the pressure to 0.4 MPa. Treat the mixture at constant temperature and pressure for 6 h. After mineralization, filter and collect the solid. Wash the solid with anhydrous ethanol until neutral and vacuum dry it in a drying oven at 60 °C for 8 h to obtain magnesium silicate gel composite magnesium carbonate dispersion.

[0048] Step 2: Preparation of modified slurry Weigh out 10.0g of zwitterionic grafted porous silica-alumina dispersion prepared in Example 2, 10.0g of magnesium silicate gel composite magnesium carbonate dispersion and 100.0mL of deionized water and add them to a stirring vessel. After mixing evenly, add 20.0g of ettringite composite hydroxyapatite whiskers prepared in Example 5 and continue stirring for 5min to obtain the modified slurry.

[0049] Step 3: Preparation of permeable materials Weigh out 1000.0g of basalt crushed stone with a particle size of 8mm and 50.0g of quartz sand with a particle size of 1.0mm and add them to the mixing tank. After dry mixing for 60s, add 240.0g of P.O42.5 ordinary Portland cement and continue mixing for 60s. Then add 120.0g of modified slurry and mix for 180s to obtain a permeable material.

[0050] Example 9: This example provides a method for preparing a permeable material for permeable tree paving bricks, including the following steps: Step 1: Preparation of magnesium silicate gel composite magnesium carbonate dispersion Weigh 16.0g of magnesium oxide and 200.0mL of deionized water and add them to the reaction vessel. Stir until a slurry is formed. Heat the reaction vessel to 70℃ and add 30.0g of hydrated silica. Keep the mixture warm and stir for 3 hours. Place the reaction system in a curing chamber with 80% humidity for 2 hours. Then, introduce carbon dioxide into the curing chamber and control the temperature of the curing chamber to 30℃ and the pressure to 0.3MPa. Treat the mixture at constant temperature and pressure for 4 hours. After mineralization, filter and collect the solid. Wash the solid with anhydrous ethanol until neutral and vacuum dry it in a drying oven at 60℃ for 7 hours to obtain magnesium silicate gel composite magnesium carbonate dispersion.

[0051] Step 2: Preparation of modified slurry Weigh out 10.0g of zwitterionic grafted porous silica-alumina dispersion prepared in Example 3, 10.0g of magnesium silicate gel composite magnesium carbonate dispersion and 100.0mL of deionized water and add them to a stirring vessel. After mixing evenly, add 20.0g of ettringite composite hydroxyapatite whiskers prepared in Example 6 and continue stirring for 4min to obtain the modified slurry.

[0052] Step 3: Preparation of permeable materials Weigh out 1000.0g of basalt crushed stone with a particle size of 6mm and 50.0g of quartz sand with a particle size of 0.9mm and add them to the mixing tank. After dry mixing for 45s, add 225.0g of P.O42.5 ordinary Portland cement and continue mixing for 45s. Then add 120.0g of modified slurry and mix for 150s to obtain a permeable material.

[0053] Comparative Example 1: The difference between this comparative example and Example 9 is that the zwitterionic grafted porous silica-alumina dispersion is omitted in step two.

[0054] Comparative Example 2: The difference between this comparative example and Example 9 is that the magnesium silicate gel composite magnesium carbonate dispersion was omitted in step two.

[0055] Comparative Example 3: The difference between this comparative example and Example 9 is that the use of ettringite-hydroxyapatite whiskers was omitted in step two.

[0056] Performance testing: A precast tree surround brick steel mold with dimensions of 200mm×200mm×35mm was selected. The inner wall of the mold was uniformly coated with stearic acid with a thickness of 10μm as a release agent. The permeable materials prepared in Examples 7-9 and Comparative Examples 1-3 were added to the mold at a loading rate of 1.0kg. After loading, the material was leveled and compacted under vibration at a frequency of 40Hz, an amplitude of 0.4mm, and a pressure of 1.0MPa for 25s. The molded green body was then left to stand for curing at 25℃ and 90% relative humidity for 24h before demolding. The demolded tree surround bricks were then cured in a standard environment at 25℃ and 95% relative humidity for 7d, and then transferred to natural curing for 28d to obtain permeable tree surround bricks. The splitting tensile strength, flexural strength, permeability coefficient, frost resistance and abrasion resistance of permeable tree pavers prepared using the permeable materials prepared in Examples 7-9 and Comparative Examples 1-3 were tested in accordance with the standard GB / T 25993-2023 "Permeable Pavement Bricks and Permeable Pavement Panels". Table 1 - Performance Test Data for Each Sample Data Analysis: A comparative analysis of Table 1 reveals that the permeable tree paving bricks prepared using the permeable material obtained in this invention exhibit a splitting tensile strength of 3.9 MPa, a flexural strength of 4.5 MPa, and a permeability coefficient of 2.3 × 10⁻⁶. -2 cm·s -1 Furthermore, after freeze-thaw testing, the average strength loss rate was 7.5%, and after wear testing, the pit length was 24 mm. All data are superior to the comparative example, indicating that: In Comparative Example 1, after step two, the use of zwitterionic grafted porous silica-alumina dispersion was eliminated. The basic structure originally used to build a continuous cementing network in the system was no longer formed, resulting in a lack of a stable and consistent interfacial transition layer on the aggregate surface. During the molding and hardening process, although the remaining components still participated in the system construction, they existed more in the form of local aggregation or discrete distribution, making it difficult to form a continuous structural connection on the overall scale. As a result, the connection between aggregates mainly relied on point or local contact. The interfacial area produced an uneven response when subjected to external forces, and the force path tended to be dispersed. The synergy and consistency of the overall structure were weakened, thus reflecting the change in the response capability of the composite system at the macroscopic level. In Comparative Example 2, because the magnesium silicate gel composite magnesium carbonate dispersion, which was originally located between the cementing phase and the aggregate, was removed in step two, the transition relationship between structures of different scales in the system changed. The continuous structure formed by the zwitterionic grafted porous silica-alumina dispersion directly bears the influence of aggregate scale differences in local areas, and the interface area lacks the conditions for the intermediate layer to regulate deformation and stress distribution. At the same time, although the fibrous structure still participates in local support, it is difficult to effectively compensate for the overall interface coordination, making the system more prone to local structural response differences during molding and service, thus affecting the uniformity of the overall structural behavior. In Comparative Example 3, after step two removed the use of ettringite-hydroxyapatite whiskers, the original spatial constraints and dispersion support mechanisms in the system no longer participated in the overall construction. The structural stability between the cement phase and the aggregate mainly relied on the planar or point connections between particles. During the molding and subsequent use, the stress concentration area and pore boundary lacked effective structural constraints, and local structural changes were more likely to develop along the existing weak paths, resulting in a cumulative structural adjustment. As a result, the system was unable to maintain its original structural distribution under external influences, and the macroscopic composite response changed accordingly. Ultimately, it is demonstrated that when any key structural unit is removed during the preparation process, the original multi-level synergistic structure of the composite system changes accordingly. Specifically, it becomes difficult for different structural elements used to construct continuous bonding, interface transitions, and spatial constraints to form a stable match, causing the connection between aggregates, cementing phases, and pore structures to change from overall coordination to local dominance. During molding and subsequent use, the responses of each structural level to external forces are no longer synchronized, and the stress transmission and structural adjustment processes exhibit obvious discretization characteristics. Local changes are more likely to accumulate and develop along the weak areas of the existing structure. This indicates that the present invention constructs a mutually supportive and mutually constraining composite system through the synergistic configuration of multiple structural units at different scales, and its technical effect is not a simple superposition of the effects of a single material.

[0057] The above description is merely an example and illustration of the structure of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described, or use similar methods to replace them, as long as they do not deviate from the structure of the invention or exceed the scope defined in the claims, all of which should fall within the protection scope of the present invention.

[0058] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0059] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to specific implementations. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a permeable material for permeable tree surround bricks, characterized in that, Includes the following steps: S1. Add zwitterionic grafted porous silica-alumina dispersion, magnesium silicate gel composite magnesium carbonate dispersion and deionized water to a mixing tank and stir. After mixing evenly, add ettringite composite hydroxyapatite whiskers and continue stirring for 3-5 minutes to obtain modified slurry. S2. Add coarse and fine aggregates to the mixing tank, dry mix for 30-60 seconds, then add gel material, continue mixing for 30-60 seconds, then add modified slurry and mix for 120-180 seconds to obtain permeable material.

2. The method for preparing a permeable material for permeable tree surround bricks according to claim 1, characterized in that, In step S1, the ratio of zwitterionic grafted porous silica-alumina dispersion, magnesium silicate gel composite magnesium carbonate dispersion, deionized water and ettringite composite hydroxyapatite whiskers is 1g:1g:10mL:2g; in step S2, the ratio of coarse aggregate, fine aggregate, gel material and modified slurry is 100g:5g:21-24g:12g, wherein the coarse aggregate is basalt crushed stone with a particle size of 5-8mm, the fine aggregate is quartz sand with a particle size of 0.8-1.0mm, and the gel material is P.O42.5 ordinary Portland cement.

3. The method for preparing a permeable material for permeable tree surround bricks according to claim 1, characterized in that, The zwitterionic grafted porous silica-alumina dispersion was prepared by the following method: A1. Add porous silica-alumina gel microparticles, 3-glycidyl etheroxypropyltrimethoxysilane and anhydrous ethanol to a reaction vessel and stir. After mixing evenly, add deionized water and adjust the pH of the reaction system to 4.5-5.0 with glacial acetic acid. Then heat the reaction vessel to 55-65℃ and keep it at that temperature for 2-4 hours. Post-treatment yields epoxy-grafted porous silica-alumina microparticles. A2. Add epoxidized grafted porous silica-alumina microparticles and mixed solvent to a reaction vessel and stir. After uniform dispersion, heat the reaction vessel to 45-55℃ and add N,N-dimethyl-1,3-propanediamine. Keep the temperature and stir for 2-3 hours. Then, cool the reaction vessel to 35-45℃ and add 1,3-propanesulfonyl lactone. Continue to keep the temperature and stir for 6-8 hours. Post-treatment yields zwitterionic grafted porous silica-alumina dispersion.

4. The method for preparing a permeable material for permeable tree surround bricks according to claim 3, characterized in that, In step A1, the ratio of the porous silica-alumina gel microparticles, 3-glycidoxypropyltrimethoxysilane, anhydrous ethanol, and deionized water is 16-18g:6-8mL:100mL:2mL; in step A2, the ratio of the epoxidized grafted porous silica-alumina microparticles, mixed solvent, N,N-dimethyl-1,3-propanediamine, and 1,3-propanesulfonyl lactone is 12-16g:80-100mL:3-5mL:4-6g, wherein the mixed solvent is obtained by mixing deionized water and anhydrous ethanol in a ratio of 1mL:4mL.

5. The method for preparing a permeable material for permeable tree surround bricks according to claim 3, characterized in that, The preparation method of porous silica-alumina gel microparticles is as follows: methyl orthosilicate, aluminum isopropoxide, and anhydrous ethanol are added to a reaction vessel and stirred. After mixing evenly, deionized water is added and saturated ammonia water is used to adjust the pH of the reaction system to 9-10. The reaction vessel is heated to 35℃ and stirred for 2-3 hours. Then, ammonium bicarbonate is added and stirred for 10-20 minutes. After post-treatment, porous silica-alumina gel microparticles are obtained. The ratio of methyl orthosilicate, aluminum isopropoxide, anhydrous ethanol, deionized water, and ammonium bicarbonate is 20-24 mL: 8-10 mL: 100 mL: 50 mL: 2-3 g.

6. The method for preparing a permeable material for permeable tree surround bricks according to claim 1, characterized in that, The ettringite-hydroxyapatite whiskers were prepared by the following method: B1. Add calcium hydroxide and deionized water to the reaction vessel and stir until a slurry is formed. Then, heat the reaction vessel to 30-40℃ and add aluminum sulfate octahydrate. Keep it warm and stir for 10-15 minutes. Then, add calcium sulfate dihydrate and stir to react for 1-2 hours. After post-treatment, needle-shaped ettringite crystal nuclei are obtained. B2. Add needle-shaped ettringite crystal nuclei and deionized water to a reaction vessel and stir. After the mixture is evenly dispersed, add saturated ammonia water to adjust the pH of the reaction vessel system to 9.5-10.

5. Heat the reaction vessel to 35-45℃ and add equal amounts of calcium nitrate and diammonium hydrogen phosphate in 10 batches with an interval of 10 minutes between additions. After the addition is complete and the mixture is kept warm and stirred for 1 hour, transfer the reaction solution to a hydrothermal reaction vessel. Heat the hydrothermal reaction vessel to 120-160℃ and keep it warm for 6-8 hours. The post-treatment yields ettringite composite hydroxyapatite whiskers.

7. The method for preparing a permeable material for permeable tree surround bricks according to claim 6, characterized in that, In step B1, the ratio of calcium hydroxide, deionized water, aluminum sulfate octahydrate, and calcium sulfate dihydrate is 12-18g:200-220mL:24-30g:10-15g; in step B2, the ratio of needle-shaped ettringite nuclei, deionized water, calcium nitrate, and diammonium hydrogen phosphate is 8-12g:200mL:10-16g:5-8g.

8. The method for preparing a permeable material for permeable tree surround bricks according to claim 1, characterized in that, The preparation method of the magnesium silicate gel composite magnesium carbonate is as follows: magnesium oxide and deionized water are added to a reaction vessel and stirred until a slurry is formed. The reaction vessel is then heated to 60-80℃ and hydrated silica is added. After stirring for 2-4 hours, mineralization is carried out, and the magnesium silicate gel composite magnesium carbonate dispersion is obtained through post-treatment.

9. A method for preparing a permeable material for permeable tree surround bricks according to claim 8, characterized in that, In the preparation of magnesium silicate gel composite magnesium carbonate dispersion, the ratio of magnesium oxide, deionized water and hydrated silica is 15-18g:200mL:25-35g.

10. A method for preparing a permeable material for permeable tree surround bricks according to claim 8, characterized in that, The mineralization step is as follows: after the reaction system is placed in a curing chamber with a humidity of 70-90% for 1-2 hours, carbon dioxide is introduced into the curing chamber and the temperature of the curing chamber is controlled at 20-40℃ and the pressure at 0.2-0.4MPa, and the constant temperature and pressure treatment is carried out for 2-6 hours.