现有铝合金板材均匀化处理工艺存在均匀化不彻底、晶粒不均、炉温差异影响品质、处理效率低、产品一致性差的问题。
By employing techniques such as low-order preheating gradient heating, multi-point temperature measurement array closed-loop control, and segmented gradient slow cooling, combined with high-temperature precise homogenization and low-frequency micro-vibration synergistic treatment, the coarse crystal clusters are broken up with the assistance of low-frequency micro-vibration, promoting uniform diffusion of alloying elements, eliminating local micro-segregation, and achieving uniform performance of the entire batch.
It significantly improves the uniformity of the microstructure of aluminum alloy sheets, shortens the heat treatment cycle, reduces energy consumption, improves the quality and yield of finished products, and ensures the dimensional accuracy and service life of the sheets.
Abstract
Description
Technical Field
[0001] This invention relates to the field of aluminum alloy sheet processing technology, and specifically to a method for homogenizing aluminum alloy ingots. Background Technology
[0002] Aluminum alloys, with their advantages of low density, high specific strength, corrosion resistance, and excellent processing performance, are widely used in aerospace, automotive manufacturing, rail transportation, precision instruments, and many other fields, making them an indispensable lightweight core material in industrial production. Aluminum alloy sheets are mostly produced through ingot rolling processes. During the solidification and crystallization of the ingot, factors such as uneven cooling rates, differences in crystallization sequence, and varying diffusion rates of alloying elements can easily lead to severe dendritic segregation and compositional segregation problems. Simultaneously, a large number of low-melting-point non-equilibrium eutectic structures and coarse second-phase particles are formed, and significant casting internal stresses remain inside the ingot. These as-cast structural defects significantly increase the deformation resistance of aluminum alloy sheets, reduce the material's thermoplasticity and subsequent rolling, stamping, and other forming and processing properties, easily leading to quality problems such as cracking and uneven deformation during sheet processing. Furthermore, it results in poor mechanical property stability and significant anisotropy in the finished sheet, drastically reducing the product's dimensional accuracy and service life.
[0003] Existing homogenization processes mostly employ single-stage constant-temperature long-term holding or two-stage heating and holding modes, which have the following technical defects: First, conventional constant-temperature high-temperature holding easily causes abnormal local grain growth, resulting in a mixed coarse and fine microstructure of the sheet, which easily leads to edge burrs, waviness, thickness differences, and anisotropy of mechanical properties during subsequent hot rolling; Second, traditional processes do not consider the temperature differences before and after the heating furnace, or between the upper and lower temperature zones, resulting in poor uniformity of the microstructure of batch sheets both internally and externally, and between the upper and lower parts, leading to low batch stability; Third, relying solely on thermal diffusion to achieve homogenization results in low dissolution efficiency of coarse and hard second phases, large segregation residues, long heat treatment cycles, and high energy consumption; Fourth, the fixed cooling rate during the cooling stage easily generates new precipitation segregation, weakening the homogenization effect. Existing published patents mostly focus on two-stage and three-stage temperature superposition holding, resulting in severe process homogenization. They lack systematic innovations such as actively dispersing grains, dynamically correcting furnace temperatures, gradient dissolution and phase elution, and segmented temperature control and shaping, and cannot fundamentally improve the overall microstructure uniformity of aluminum alloy sheets.
[0004] In summary, existing homogenization processes for aluminum alloy sheets suffer from problems such as incomplete homogenization, uneven grain size, quality issues due to furnace temperature differences, low processing efficiency, and poor product consistency. Summary of the Invention
[0005] This invention addresses the problems of incomplete homogenization, uneven grain size, quality issues caused by furnace temperature differences, low processing efficiency, and poor product consistency in existing homogenization processes for aluminum alloy sheets. It proposes a homogenization method for aluminum alloy ingots.
[0006] The present invention provides a method for homogenizing aluminum alloy ingots, the specific method of which is as follows:
[0007] Step 1: Place the aluminum alloy ingot into the furnace for pretreatment;
[0008] Step 2: By controlling the furnace temperature and raising it in a low-level preheating gradient, the stress inside the pretreated aluminum alloy ingot is eliminated.
[0009] Step 3: Perform medium-temperature isothermal melting pretreatment on the stress-relieved aluminum alloy ingot;
[0010] Step 4: Then, the aluminum alloy ingot is subjected to high-temperature precision homogenization combined with low-frequency micro-vibration synergistic treatment.
[0011] Step 5: Perform segmented gradient slow cooling and shaping;
[0012] Step 6: After cooling, the aluminum alloy ingot is removed from the furnace and obtained with uniform structure, no obvious segregation, and refined grains. It can be directly put into the hot rolling process to complete the processing of the aluminum alloy ingot.
[0013] Furthermore, the specific steps for pre-treating the aluminum alloy ingot in step one, which involves placing it in a furnace, are as follows:
[0014] Step 1: Mill the surface of the cast aluminum alloy ingot to remove oxide scale and surface defects;
[0015] Step 1 and Step 2: Arrange aluminum alloy ingots in layers at intervals in the heating furnace. Set up a multi-point temperature measurement array in the furnace to collect the real-time temperature of the upper, middle, lower, left and right temperature zones in the furnace and establish a closed-loop control model for furnace temperature difference.
[0016] Furthermore, in step two, the furnace temperature is controlled to rise at a rate of 8–12°C / min until it reaches 320–360°C, and the constant temperature holding time is controlled to be 1.5–2.5 hours.
[0017] Furthermore, in step three, when performing medium-temperature isothermal melting pretreatment on the aluminum alloy ingot, the temperature inside the furnace is controlled to rise at 5-8℃ / min until it reaches 420-450℃, and the isothermal holding time is controlled to be 3-5h.
[0018] Furthermore, the medium-temperature isothermal dissolution pretreatment in step three involves dissolving the low-melting-point non-equilibrium eutectic phase at low temperature first, breaking up shallow dendritic segregation, and avoiding the local phase agglomeration and coarseness caused by direct high-temperature heat preservation.
[0019] Furthermore, the technical parameters for the high-temperature precise homogenization and low-frequency micro-vibration synergistic processing in step four are as follows: the furnace temperature is controlled to continue to rise slowly at 3-5℃ / min to 490-530℃, and the constant temperature is finely adjusted according to the aluminum alloy grade, with the constant temperature holding time controlled at 4-6 hours; the low-frequency micro-vibration homogenization auxiliary device in the furnace is activated throughout the holding process, with a vibration frequency of 15-25Hz and a micro-amplitude of 0.1-0.3mm; at the same time, the heating power of each zone is dynamically corrected based on the multi-point temperature measurement array data, so that the temperature difference throughout the furnace is controlled within ±2℃.
[0020] Furthermore, the segmented gradient slow cooling and shaping process in step five specifically includes:
[0021] First stage: 490℃~400℃, slow cooling rate 3~5℃ / min;
[0022] Second stage: 400℃~300℃, slow cooling rate 5~8℃ / min;
[0023] The third stage: the furnace is allowed to cool naturally to room temperature below 300℃.
[0024] Compared with the prior art, the present invention has the following advantages:
[0025] 1. This invention overcomes the shortcomings of existing technologies by incorporating high-temperature precision homogenization and low-frequency micro-vibration synergistic treatment into the aluminum alloy ingot processing method. Specifically, the furnace temperature is slowly increased to 490-530℃ at a rate of 3-5℃ / min, and the constant temperature is finely adjusted according to the aluminum alloy grade, with the holding time controlled at 4-6 hours. Throughout the holding process, a low-frequency micro-vibration homogenization auxiliary device is activated in the furnace, with a vibration frequency of 15-25Hz and a micro-amplitude of 0.1-0.3mm. Simultaneously, the heating power of each zone is dynamically corrected based on multi-point temperature measurement array data, controlling the temperature difference throughout the furnace to within ±2℃. This process breaks away from the industry's inherent thinking of relying solely on temperature diffusion for homogenization. By using low-frequency micro-vibration to assist in breaking up coarse crystal clusters and promoting uniform diffusion of alloy elements, it completely eliminates local micro-segregation that cannot be removed by conventional processes, improving the uniformity of the microstructure by more than 40%.
[0026] 2. This invention establishes a closed-loop temperature difference control model by arranging a multi-point temperature measurement array inside the furnace to collect real-time temperatures in the upper, middle, lower, left, and right temperature zones of the furnace. Essentially, it solves the common industry problem of "inconsistent quality of furnace core, furnace opening, and upper and lower layer plates" in traditional batch heat treatment by dynamically correcting the temperature difference in the furnace zone through multi-point array temperature measurement, and achieves a high degree of uniformity in the performance of the entire batch.
[0027] 3. This invention adopts an integrated process of gradient heating and segmented slow cooling. First, stress is relieved at low temperature, impurities are dissolved at medium temperature, homogenization is carried out at high temperature, and gradient shaping is performed. The microstructure is improved step by step, and secondary precipitation and segregation are eliminated. Compared with the traditional two-stage heat preservation process, the grains are finer and there are no abnormal grain growth.
[0028] 4. Under the premise of ensuring a significant improvement in homogenization effect, this invention shortens the overall heat treatment cycle by 15% to 25%, reduces heating energy consumption, and significantly reduces the defects such as local hard spots, uneven edge structure, and burrs in subsequent hot-rolled plates. The shortened processing cycle reduces energy consumption and greatly improves the quality and yield of subsequent rolled products. Detailed Implementation
[0029] Specific Implementation Method 1: The homogenization treatment method for aluminum alloy ingots described in this implementation method is as follows:
[0030] Step 1: Place the aluminum alloy ingot into the furnace for pretreatment;
[0031] Step 2: By controlling the furnace temperature and raising it in a low-level preheating gradient, the stress inside the pretreated aluminum alloy ingot is eliminated.
[0032] Step 3: Perform medium-temperature isothermal melting pretreatment on the stress-relieved aluminum alloy ingot;
[0033] Step 4: Then, the aluminum alloy ingot is subjected to high-temperature precision homogenization combined with low-frequency micro-vibration synergistic treatment.
[0034] Step 5: Perform segmented gradient slow cooling and shaping;
[0035] Step 6: After cooling, the aluminum alloy ingot is removed from the furnace and obtained with uniform structure, no obvious segregation, and refined grains. It can be directly put into the hot rolling process to complete the processing of the aluminum alloy ingot.
[0036] This specific implementation method incorporates high-temperature precision homogenization and low-frequency micro-vibration synergistic treatment into the aluminum alloy ingot processing method, breaking the industry's inherent thinking of relying solely on temperature diffusion for homogenization. By using low-frequency micro-vibration to assist in breaking coarse crystal clusters and promoting uniform diffusion of alloy elements, it completely eliminates local micro-segregation that cannot be removed by conventional processes, improving the uniformity of the structure by more than 40%.
[0037] Specific Implementation Method Two: This implementation method further defines the processing method described in Specific Implementation Method One. The specific steps of the homogenization treatment method for aluminum alloy ingots described in this implementation method, specifically placing the aluminum alloy ingot into the furnace for pretreatment in step one, are as follows:
[0038] Step 1: Mill the surface of the cast aluminum alloy ingot to remove oxide scale and surface defects;
[0039] Step 1 and Step 2: Arrange aluminum alloy ingots in layers at intervals in the heating furnace. Set up a multi-point temperature measurement array in the furnace to collect the real-time temperature of the upper, middle, lower, left and right temperature zones in the furnace and establish a closed-loop control model for furnace temperature difference.
[0040] This specific implementation method involves arranging a multi-point temperature measurement array inside the furnace to collect real-time temperatures in the upper, middle, lower, left, and right temperature zones of the furnace, and establishing a closed-loop temperature difference control model for the furnace. Essentially, it uses multi-point array temperature measurement to dynamically correct the temperature difference in the furnace zone, solving the common industry problem of "inconsistent quality between the furnace core, furnace opening, and upper and lower layers of plates" in traditional batch heat treatment, and achieving a high degree of uniformity in the performance of the entire batch.
[0041] Specific Implementation Method 3: This implementation method is a further limitation of the processing method described in Specific Implementation Method 2. In the homogenization treatment method for aluminum alloy ingots described in this implementation method, in step 2, the furnace temperature is controlled to rise at a rate of 8-12℃ / min until it reaches 320-360℃, and the constant temperature holding time is controlled to be 1.5-2.5h.
[0042] In this specific embodiment, the furnace temperature is controlled to rise at a rate of 8-12°C / min until it reaches 320-360°C, and the constant temperature holding time is controlled at 1.5-2.5h. This forms a low-level preheating gradient temperature rise in the furnace, thereby slowly releasing the internal stress of the aluminum alloy ingot through low-temperature gradient temperature rise, avoiding grain boundary cracking and microstructure distortion caused by rapid temperature rise, and forming a preliminary stable crystal lattice structure.
[0043] Specific Implementation Method Four: This implementation method is a further limitation of the processing method described in Specific Implementation Method Three. In the homogenization treatment method for aluminum alloy ingots described in this implementation method, in step three, when performing medium-temperature constant-temperature melting pretreatment on the aluminum alloy ingots, the temperature inside the furnace is controlled to rise at 5-8℃ / min until it reaches 420-450℃, and the constant-temperature holding time is controlled to be 3-5h.
[0044] Specific Implementation Method 5: This implementation method is a further limitation of the processing method described in Specific Implementation Method 4. In the homogenization treatment method for aluminum alloy ingots described in this implementation method, the medium-temperature isothermal dissolution pretreatment in step three dissolves the low-melting-point non-equilibrium eutectic phase at low temperature first, disperses shallow dendritic segregation, and avoids local phase agglomeration and coarsening caused by direct high-temperature heat preservation.
[0045] Specific Implementation Method Six: This implementation method further defines the processing method described in Specific Implementation Method One. The homogenization treatment method for aluminum alloy ingots described in this implementation method has the following technical parameters in step four: The furnace temperature is controlled to continue slowly increasing at 3-5℃ / min to 490-530℃. The constant temperature is fine-tuned according to the aluminum alloy grade, and the constant temperature holding time is controlled to be 4-6 hours. Throughout the holding process, the low-frequency micro-vibration homogenization auxiliary device in the furnace is activated, with a vibration frequency of 15-25Hz and a micro-amplitude of 0.1-0.3mm. Simultaneously, the heating power of each zone is dynamically corrected based on multi-point temperature measurement array data to control the temperature difference throughout the furnace within ±2℃.
[0046] In this specific embodiment, micro-vibration-assisted lattice slip breaks up local coarse crystal clusters and accumulated precipitates, overcoming the limitations of traditional homogeneity relying solely on thermal diffusion, significantly improving element diffusion uniformity, and completely eliminating dendritic segregation and grain boundary enrichment phases.
[0047] Specific Implementation Method Seven: This implementation method further defines the processing method described in Specific Implementation Method One. The homogenization treatment method for aluminum alloy ingots described in this implementation method, specifically the segmented gradient slow cooling and shaping process in step five, is as follows:
[0048] First stage: 490℃~400℃, slow cooling rate 3~5℃ / min;
[0049] Second stage: 400℃~300℃, slow cooling rate 5~8℃ / min;
[0050] Third stage: The furnace is allowed to cool naturally to room temperature below 300℃;
[0051] In this specific implementation, by using graded temperature control cooling, secondary precipitation and segregation caused by rapid cooling are avoided, and the uniform and refined grain structure is locked in, ensuring that the structure, hardness, and ductility of the entire plate are highly consistent.
[0052] Specific Implementation Method Eight: This implementation method further defines the processing method described in Specific Implementation Method One. This implementation method provides a homogenization treatment method for aluminum alloy ingots, optimizing process parameters for commonly used 6-series, 5-series, and 7-series industrial aluminum alloys.
[0053] 6061 / 6063 series: High temperature homogenization temperature 500~510℃, vibration frequency 18~22Hz;
[0054] 5052 / 5083 series: High temperature homogenization temperature 490~500℃, vibration frequency 15~20Hz;
[0055] 7075 high-strength aluminum alloy: high temperature homogenization temperature 510~525℃, vibration frequency 20~25Hz, extended heat preservation to 5.5~6h.
[0056] Specific Implementation Method Nine: This implementation method further defines the processing method described in Specific Implementation Method One. The homogenization treatment method for aluminum alloy ingots described in this implementation method, taking 6061 aluminum alloy ingots as an example, involves the following specific steps:
[0057] S1. Mill and clean the surface of the 6061 ingot, load it into the furnace at even intervals, and turn on multi-point temperature monitoring.
[0058] S2. Increase the temperature to 340℃ at a rate of 10℃ / min and hold for 2 hours;
[0059] S3. Increase the temperature to 435℃ at a rate of 6℃ / min and hold for 4 hours;
[0060] S4. Heat to 505℃ at 4℃ / min, hold for 5 hours, with 20Hz micro-vibration and 0.2mm amplitude throughout, and control the furnace temperature within ±2℃.
[0061] S5, three-stage gradient slow cooling to room temperature;
[0062] After treatment, the ingot is free of dendrite segregation, and the grains are uniform and refined, resulting in a smooth surface and uniform and stable mechanical properties in the subsequent hot-rolled sheet.
[0063] Specific Implementation Method Ten: This implementation method further defines the processing method described in Specific Implementation Method One. The homogenization treatment method for aluminum alloy ingots described in this implementation method, taking 5052 aluminum alloy ingots as an example, involves the following specific steps:
[0064] S1. Ingot cleaning and furnace loading;
[0065] S2, heat to 330℃ at 10℃ / min, and hold for 2 hours;
[0066] S3, heat to 425℃ at 6℃ / min, and hold for 3.5h;
[0067] S4, heat to 495℃ at 4℃ / min, hold for 4.5h, and homogenize with 18Hz micro-vibration;
[0068] S5, Gradient slow cooling and shaping;
[0069] The tensile strength and bending consistency of the sheet metal are significantly improved, and the burrs and wavy defects on the rolled edge are greatly reduced.
[0070] Specific Implementation Method Eleven: This implementation method further defines the processing method described in Specific Implementation Method One. The homogenization treatment method for aluminum alloy ingots described in this implementation method, taking a 7075 aluminum alloy ingot as an example, involves the following specific steps:
[0071] S1. Precision milling of ingots before loading into the furnace;
[0072] S2, heat to 350℃ at 9℃ / min, and hold for 2.5h;
[0073] S3, heat to 445℃ at 5℃ / min, and hold for 5 hours;
[0074] S4, heat up to 520℃ at 3℃ / min, hold for 6h, and homogenize with 22Hz high-frequency micro-vibration;
[0075] S5, Strict gradient slow cooling;
[0076] Completely eliminates the problem of coarse second phase enrichment in high-strength alloys, and the microstructure uniformity meets the standards for use in high-end aerospace and precision sheet metal.
Claims
1. A method for homogenizing aluminum alloy ingots, characterized in that: The specific method is as follows: Step 1: Place the aluminum alloy ingot into the furnace for pretreatment; Step 2: By controlling the furnace temperature and raising it in a low-level preheating gradient, the stress inside the pretreated aluminum alloy ingot is eliminated. Step 3: Perform medium-temperature isothermal melting pretreatment on the stress-relieved aluminum alloy ingot; Step 4: Then, the aluminum alloy ingot is subjected to high-temperature precision homogenization combined with low-frequency micro-vibration synergistic treatment. Step 5: Perform segmented gradient slow cooling and shaping; Step 6: After cooling, the aluminum alloy ingot is removed from the furnace and obtained with uniform structure, no obvious segregation, and refined grains. It can be directly put into the hot rolling process to complete the processing of the aluminum alloy ingot.
2. The homogenization treatment method for aluminum alloy ingots according to claim 1, characterized in that: The specific steps for pre-treating the aluminum alloy ingot in step one, which involves placing it in a furnace, are as follows: Step 1: Mill the surface of the cast aluminum alloy ingot to remove oxide scale and surface defects; Steps 1 and 2: Arrange aluminum alloy ingots in layers at intervals inside the heating furnace. Set up a multi-point temperature measurement array inside the furnace to collect the real-time temperature of the upper, middle, lower, left, and right temperature zones inside the furnace and establish a closed-loop control model for furnace temperature difference.
3. The homogenization treatment method for aluminum alloy ingots according to claim 2, characterized in that: In step two, the furnace temperature is controlled to rise at a rate of 8-12℃ / min until it reaches 320-360℃, and the constant temperature holding time is controlled to be 1.5-2.5h.
4. The homogenization treatment method for aluminum alloy ingots according to claim 3, characterized in that: In step three, during the medium-temperature isothermal melting pretreatment of the aluminum alloy ingot, the temperature inside the furnace is controlled to rise at 5-8℃ / min until it reaches 420-450℃, and the isothermal holding time is controlled to be 3-5 hours.
5. The homogenization treatment method for aluminum alloy ingots according to claim 4, characterized in that: The intermediate-temperature isothermal dissolution pretreatment in step three involves dissolving the low-melting-point non-equilibrium eutectic phase at low temperature to break up shallow dendritic segregation.
6. The homogenization treatment method for aluminum alloy ingots according to claim 1, characterized in that: The technical parameters for the high-temperature precise homogenization and low-frequency micro-vibration synergistic processing in step four are as follows: the furnace temperature is controlled to continue to rise slowly at 3-5℃ / min to 490-530℃, and the constant temperature is finely adjusted according to the aluminum alloy grade, and the constant temperature holding time is controlled to be 4-6 hours; the low-frequency micro-vibration homogenization auxiliary device in the furnace is activated throughout the holding process, with a vibration frequency of 15-25Hz and a micro-amplitude of 0.1-0.3mm; at the same time, the heating power of each zone is dynamically corrected based on the multi-point temperature measurement array data, and the temperature difference in the entire furnace is controlled within ±2℃.
7. The homogenization treatment method for aluminum alloy ingots according to claim 1, characterized in that: The segmented gradient slow cooling and shaping process in step five is specifically as follows: First stage: 490℃~400℃, slow cooling rate 3~5℃ / min; Second stage: 400℃~300℃, slow cooling rate 5~8℃ / min; The third stage: the furnace is allowed to cool naturally to room temperature below 300℃.