A reversible adhesive that can quantify adhesion strength through color change and its preparation method.

By preparing a reversible adhesive that can quantify adhesion strength through color changes, the problems of low precision in adhesion strength control and difficulty in real-time monitoring in existing technologies have been solved. This enables temperature-responsive reversible adhesion and visualization of adhesion strength, making it suitable for multiple high-end application scenarios.

CN123107587APending Publication Date: 2026-11-17QUZHOU RES INST OF ZHEJIANG UNIV +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611601566.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing temperature-responsive reversible adhesives suffer from low precision in controlling adhesive strength, difficulty in real-time monitoring, and inability to achieve controllable and monitorable adhesive performance. Furthermore, the synergy between color-changing properties and reversible adhesive performance is poor, and the preparation process is complex and costly, making it difficult to meet the needs of high-end application scenarios.

Method used

By preparing a reversible adhesive that can quantify adhesion strength through color change, a compound with color change and reversible adhesion functions is mixed and reacted with polymerizable monomers, initiators, and crosslinking agents to form a multi-reversible adhesive. Under external temperature stimulation, thermally responsive reversible adhesion and visualized quantitative monitoring of adhesion strength are achieved.

Benefits of technology

It enables visualized and quantitative monitoring of the adhesion strength of reversible adhesives at different temperatures, and has temperature-responsive reversible adhesion properties, making it suitable for reusable devices, flexible electronics, biomedicine, and smart packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107587A_ABST
    Figure CN123107587A_ABST
Patent Text Reader

Abstract

This invention discloses a reversible adhesive that quantifies adhesion strength through color change and its preparation method. The reversible adhesive is prepared by polymerization of a compound with color-changing and reversible adhesion functions in a solution containing a polymerizable monomer, an initiator, and a crosslinking agent. This invention's reversible adhesive, which quantifies adhesion strength through color change, exhibits temperature-responsive reversible adhesion characteristics, strong adhesion, and the ability to quantify adhesion strength based on color changes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of reversible adhesive technology, specifically relating to a reversible adhesive whose adhesion strength can be quantified by color change and its preparation method. Background Technology

[0002] Reversible adhesives, as a class of functional materials that can achieve adhesion-desorption cycles through external stimuli, have significant application value in reusable devices, flexible electronics, biomedicine, and smart packaging. Currently, reversible adhesives based on stimuli such as temperature, pH, and light have become a research hotspot in the materials science field. Among them, temperature-responsive reversible adhesives have particularly prominent application prospects due to their advantages such as simple stimulation methods, fast response speed, and wide applicability. However, existing temperature-responsive reversible adhesives generally suffer from low precision in adhesion strength control and difficulty in real-time monitoring. Most products can only achieve simple switching between adhesion and desorption, failing to accurately reflect changes in adhesion strength at different temperatures, thus failing to meet the stringent requirements of high-end applications for controllable and monitorable adhesion performance.

[0003] Currently, conventional methods for testing adhesive strength mostly rely on offline testing techniques such as shear and tensile tests, which require specialized instruments and equipment, are cumbersome and time-consuming, and cannot achieve real-time in-situ monitoring during adhesive use. Some studies have attempted to achieve visual monitoring of adhesive performance by introducing fluorescent groups and color-changing materials, but existing technologies mostly focus on qualitative judgment of the adhesion state and have failed to establish a quantitative correlation between color change and adhesive strength, making it impossible to accurately quantify the adhesive strength value through apparent color change. Furthermore, the preparation process of existing color-changing-reversible adhesion bifunctional materials is complex, the raw material cost is high, and the synergy between color-changing and reversible adhesion properties is poor, easily leading to problems such as low color-changing sensitivity and poor reversible cycle stability, which limits their industrial application and promotion.

[0004] In existing research, *Advanced Materials*, 2025, DOI: 10.1002 / adma.202507894 reported the development of an amphibious reversible adhesive based on a reversible crosslinking strategy, achieving both high-strength underwater adhesion and erasability. *Advanced Science*, 2025, DOI: 10.1002 / advs.202511818 prepared a robust and reversible supramolecular adhesive material using a dual-terminal molecular strategy, improving the stability of reversible adhesion. *Materials Today*, 2025, DOI: 10.1016 / j.mattod.2025.12.013 developed a thermally hysteretic reversible underwater adhesive, which, while optimizing reversible adhesion performance, still does not solve the core problem of real-time quantitative monitoring of adhesion strength. Patent CN121362533A discloses an acrylic pressure-sensitive adhesive film with bidirectional electronically controlled reversible adhesion function. Although it achieves reversible adhesion control, it does not involve the visualization and quantitative monitoring of adhesion strength.

[0005] Given the shortcomings of the existing technologies, there is an urgent need to develop an adhesive product that combines temperature-responsive reversible adhesion with visualized quantitative monitoring of adhesion strength. Summary of the Invention

[0006] The purpose of this section is to outline some aspects of embodiments of the present invention and to briefly describe some preferred embodiments. Simplifications or omissions may be made in this section, as well as in the abstract and title of this application, to avoid obscuring the purpose of these documents; however, such simplifications or omissions should not be construed as limiting the scope of the invention.

[0007] In view of the problems of reversible adhesion and the inability to visualize and quantitatively monitor the adhesion strength of adhesives in the above and / or prior art, the present invention is proposed.

[0008] One objective of this invention is to provide a reversible adhesive that can quantify adhesion strength through color change, and a compound that has both color change and reversible adhesion functions. Under different external temperature stimuli, the reversible adhesive can achieve thermal response reversible adhesion and visualized quantitative monitoring and quantification of adhesion strength.

[0009] To solve the above-mentioned technical problems, the present invention provides the following technical solution: a reversible adhesive that can quantify the adhesion strength through color change, wherein the reversible adhesive is prepared by polymerization reaction of a compound having color change and reversible adhesion function as shown in Formula I in a solution containing polymerizable monomers, initiators and crosslinking agents; (Formula I); R1 is selected from one of hydroxyl, alkoxy, carboxyl, ester, and phenyl groups, and X is PF6.

[0010] As a preferred embodiment of the reversible adhesive that can quantify adhesion strength through color change according to the present invention, wherein: the preparation method of the compound having color change and reversible adhesion functions as shown in Formula I includes, 4,4'-bipyridine and the compounds shown in Formula II and Formula III were dissolved in acetonitrile, respectively. After mixing, the mixture was reacted at 60-100°C for 6-24 h to obtain a reaction solution. After post-treatment, the compound shown in Formula IV was obtained. The compound shown in Formula IV was subjected to an anion substitution reaction with potassium hexafluorophosphate at a molar ratio of 1:2.5 to obtain a compound with the structure shown in Formula I that has color change and reversible adhesion function. (Formula II); (Formula III); (Formula IV); X1 is one of Cl, Br, or I.

[0011] As a preferred embodiment of the reversible adhesive that allows for quantification of adhesion strength through color change according to the present invention, wherein: the molar ratio of 4,4'-bipyridine to the intermediate product shown in Formula II is 1:0.3 to 0.5, the molar ratio of 4,4'-bipyridine to the intermediate product shown in Formula III is 1:0.3 to 0.5, and the mass amount of acetonitrile, based on the mass amount of 4,4'-bipyridine, is 0.5 to 0.8 g / g.

[0012] As a preferred embodiment of the reversible adhesive of the present invention, which quantifies adhesion strength through color change, wherein: the preparation method of the compound represented by Formula II includes, Imidazole and the compound shown in Formula III were dissolved in anhydrous acetonitrile and mixed thoroughly. The resulting homogeneous solution was reacted at 30-80°C for 6-12 hours under a N2 atmosphere. After the reaction was completed, sodium carbonate was added to the solution and stirred for 1-2 hours. Then, dihalomethane was added and reacted at 0-50°C for 6-12 hours under a N2 atmosphere. The filtrate was obtained by filtration and washed thoroughly with ethyl acetate and anhydrous diethyl ether, respectively, to obtain the compound shown in Formula II.

[0013] As a preferred embodiment of the reversible adhesive that allows for quantification of adhesion strength through color change according to the present invention, wherein: the imidazole and the compound shown in Formula III are added in a molar ratio of 1:1.1; the volume of the acetonitrile is 5-10 mL / g based on the mass of the imidazole; the mass of the sodium carbonate is 0.5-2 g / g based on the mass of the imidazole; and the molar amount of the dihalomethane added is 0.4-0.6 mol / mol based on the molar amount of the imidazole.

[0014] Another object of the present invention is to provide a method for preparing a reversible adhesive that can quantify adhesion strength through color change, wherein the reversible adhesive that can quantify adhesion strength through color change is prepared by the following steps: The compound with color-changing and reversible adhesion functions shown in Formula I, the polymerizable monomer, the initiator, and the crosslinking agent are thoroughly stirred, mixed, and dissolved to obtain a homogeneous and transparent solution. The above-mentioned uniform and transparent solution was injected into a mold, and a reversible adhesive that could quantify the adhesion strength by color change was prepared by photo-initiated polymerization.

[0015] As a preferred embodiment of the method for preparing the reversible adhesive that can quantify the adhesion strength by color change according to the present invention, wherein: the polymerizable monomer is hexyl methacrylate and hydroxyethyl methacrylate, the initiator is photoinitiator 1173, and the crosslinking agent is polyethylene glycol diacrylate.

[0016] As a preferred embodiment of the preparation method of the reversible adhesive that can quantify adhesion strength by color change according to the present invention, wherein: the mass ratio of the polymerizable monomer hexyl methacrylate to hydroxyethyl methacrylate is 1:0.1~10; the amount of the compound with color change and reversible adhesion function as shown in Formula I is 10~50% of the polymerizable monomer by mass; the amount of the photoinitiator is 0.5~5% of the polymerizable monomer by mass; the amount of the crosslinking agent is 0.5~5% of the polymerizable monomer by mass; and the photoinitiated polymerization conditions are a wavelength of 240~330nm and a time of 0.5~3h.

[0017] Compared with the prior art, the present invention has the following beneficial effects: This invention utilizes compounds possessing both color-changing and reversible adhesion functions as thermally responsive reversible units. These compounds are mixed with polymerizable monomers, initiators, and crosslinking agents to prepare multi-reversible adhesives. Under different external temperature stimuli, the thermally responsive reversible adhesion of the adhesives and the visualized quantitative monitoring of adhesion strength are achieved. Therefore, this type of reversible adhesive, whose adhesion strength can be quantified through color changes, has promising application prospects in reusable devices, flexible electronics, biomedicine, and smart packaging. Attached Figure Description

[0018] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Wherein: Figure 1 This is a schematic diagram of the test of the adhesive strength of a reversible adhesive that can quantify the adhesive strength through color change in an embodiment of the present invention. Figure 2 The reversible adhesion properties of the reversible adhesive in Example 6, which can quantify the adhesion strength through color change, change with temperature. Figure 3 The reversible adhesion properties of the reversible adhesive in Example 7, which can quantify the adhesion strength through color change, change with temperature. Figure 4 The reversible adhesion properties of the reversible adhesive in Example 8, which can quantify the adhesion strength through color change, change with temperature. Figure 5 The reversible adhesion properties of the reversible adhesive in Example 9, which can quantify the adhesion strength through color change, change with temperature. Figure 6 The reversible adhesion properties of the reversible adhesive in Example 10, which can quantify the adhesion strength through color change, vary with temperature. Figure 7 This shows the correspondence between the intensity of the absorption peak in a specific band of the ultraviolet absorption spectrum of the reversible adhesive in Example 11 and the shear adhesion strength. Figure 8 This shows the correspondence between the intensity of the absorption peak in a specific band of the ultraviolet absorption spectrum of the reversible adhesive in Example 12 and the shear adhesion strength. Figure 9 This shows the correspondence between the intensity of the absorption peak in a specific band of the ultraviolet absorption spectrum of the reversible adhesive in Example 13 and the shear adhesion strength. Figure 10 This shows the correspondence between the intensity of the absorption peak in a specific band of the ultraviolet absorption spectrum of the reversible adhesive in Example 14 and the shear adhesion strength. Figure 11 This shows the correspondence between the intensity of the absorption peak in a specific band of the ultraviolet absorption spectrum of the reversible adhesive in Example 15 and the shear adhesion strength. Figure 12 The adhesion properties of the adhesive in Comparative Example 1 as a function of temperature; Figure 13 This shows the correspondence between the intensity of the absorption peak in a specific band of the UV absorption spectrum of the adhesive in Comparative Example 2 and the shear adhesion strength. Detailed Implementation

[0019] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the examples in the specification.

[0020] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.

[0021] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that is mutually exclusive with other embodiments.

[0022] Unless otherwise specified, all raw materials used in the examples are commercially available.

[0023] Example 1

[0024] (1) Preparation of intermediate products

[0025]

[0026]

[0027] Imidazole and the starting material (2-bromoethanol) of the compound shown in formula (Ⅱ-Ⅱ) were dissolved in anhydrous acetonitrile and mixed thoroughly. The resulting homogeneous solution was reacted at 50°C for 8 hours in a N2 atmosphere. After the reaction was completed, a solution containing the intermediate product of the structure shown in formula (Ⅱ-Ⅰ) was obtained. Sodium carbonate was added to the solution and stirred for 2 hours. Then dibromomethane was added and reacted at 5°C for 8 hours in a N2 atmosphere. The filtrate was obtained by filtration and washed thoroughly with ethyl acetate and anhydrous diethyl ether, respectively, to obtain the compound shown in formula (Ⅱ).

[0028] In this mixture, imidazole and the compound shown in formula (II-II) were added in a molar ratio of 1:1.1. The volume of acetonitrile used was 6 mL / g based on the mass of imidazole, the mass of sodium carbonate used was 1 g / g based on the mass of imidazole, the molar amount of dibromomethane used was 0.5 mol / mol based on the amount of imidazole, and the washing times were 3 times each with ethyl acetate and anhydrous diethyl ether.

[0029] (2) Synthesis of compounds with color-changing and reversible adhesion functions

[0030]

[0031] 4,4'-bipyridine, the intermediate product shown in formula (II), and the raw material of the compound shown in formula (III) (2-bromoethanol) were dissolved in acetonitrile, respectively. After mixing, the mixture was reacted at 80°C for 12 h to obtain a reaction solution. After post-treatment, the compound (I) with color change and reversible adhesion function was obtained. The molar ratio of 4,4'-bipyridine to the intermediate product shown in formula (II) is 1:0.5, the molar ratio of 4,4'-bipyridine to the compound shown in formula (III) is 1:0.5, and the mass amount of acetonitrile used is 0.6 g / g based on the mass amount of 4,4'-bipyridine. The post-treatment method of the reaction solution is as follows: the cooled reaction solution is filtered under negative pressure, the filter residue is collected and washed multiple times with acetonitrile, the filter residue is washed 3 times with anhydrous diethyl ether, filtered, and thoroughly dried.

[0032]

[0033] The synthesized compound with color-changing and reversible adhesion functions, as shown in formula (Ⅰ), was mixed with potassium hexafluorophosphate in an aqueous solution at a molar ratio of 1:2.5 and stirred at room temperature for 12 h. After the reaction, the mixture was thoroughly washed three times with deionized water to remove unreacted potassium hexafluorophosphate. The mixture was then centrifuged and filtered. The resulting solid product was thoroughly dried in a vacuum oven at 60 °C to obtain the compound with color-changing and reversible adhesion functions as shown in (Ⅰ-Ⅰ), whose anion is hexafluorophosphate.

[0034] Example 2

[0035] This embodiment provides the synthesis of a compound with color-changing and reversible adhesion functions as shown in formula (Ⅰ-Ⅱ). The synthesis and post-processing methods are basically the same as those in Example 1. The difference is that the compounds shown in formula (Ⅱ-Ⅱ) and formula (Ⅲ) are both 2-bromoethyl methyl ether.

[0036]

[0037] Example 3

[0038] This embodiment provides the synthesis of a compound with color-changing and reversible adhesion functions as shown in formula (Ⅰ-Ⅲ). The synthesis and post-processing methods are basically the same as those in Example 1. The difference is that the compounds shown in formula (Ⅱ-Ⅱ) and formula (Ⅲ) are both made of 3-bromopropionic acid.

[0039]

[0040] Example 4

[0041] This embodiment provides the synthesis of a compound with color-changing and reversible adhesion functions as shown in formula (I-IV). The synthesis and post-processing methods are basically the same as those in Example 1. The difference is that the compounds shown in formula (II-II) and formula (III) are all made of methyl 3-bromopropionate.

[0042]

[0043] Example 5

[0044] This embodiment provides the synthesis of a compound with color-changing and reversible adhesion functions as shown in formula (Ⅰ-Ⅴ). The synthesis and post-processing methods are basically the same as those in Example 1. The difference is that the compounds shown in formula (Ⅱ-Ⅱ) and formula (Ⅲ) are both (2-bromoethyl)benzene.

[0045]

[0046] Example 6

[0047] This embodiment provides a method for preparing a reversible adhesive that can quantify adhesion strength through color change, which is obtained through the following steps: The compound with color change and reversible adhesion function shown in formula (Ⅰ-Ⅰ), polymerizable monomer, initiator and crosslinking agent are thoroughly stirred, mixed and dissolved to obtain a homogeneous and transparent solution; The above-mentioned uniform and transparent solution was injected into a mold, and a reversible adhesive that could quantify the adhesion strength by color change was prepared by photo-initiated polymerization.

[0048] The polymerizable monomers are hexyl methacrylate and hydroxyethyl methacrylate in a mass ratio of 1:0.8; the compound with color change and reversible adhesion function shown in formula (Ⅰ-Ⅰ) accounts for 20% of the polymerizable monomers by mass; the photoinitiator is photoinitiator 1173, accounting for 1% of the polymerizable monomers by mass; the crosslinking agent is polyethylene glycol diacrylate, accounting for 1% of the polymerizable monomers by mass; and the photoinitiated polymerization conditions are a wavelength of 250 nm and a time of 1 h.

[0049] The above-mentioned test method for the adhesive strength of reversible adhesives, which can quantify adhesive strength through color change, is as follows: A certain amount of the prepared reversible adhesive was placed between two pieces of ordinary transparent glass, fixed with clips, and then heated to the test temperature of 30°C. After holding at the temperature for 5 minutes, it was cooled to room temperature, and its shear adhesion strength was tested. The above heating and cooling steps were repeated when testing the adhesion strength at the next temperature point (40, 50, 60, 70, 80°C and 70, 60, 50, 40, 30°C respectively).

[0050] From the appendix Figure 1 Test diagram and appendix Figure 2The results of the reversible adhesion performance show that the reversible adhesive, which contains the compound shown in formula (Ⅰ-Ⅰ) and has color-changing and reversible adhesion functions, exhibits adhesion strength that can be quantified by color change. The adhesion strengths after heating and then cooling at 30, 40, 50, 60, 70, and 80℃ are 0.43, 0.71, 0.89, 1.08, 1.34, and 1.57 MPa, respectively, showing a gradually increasing trend. Furthermore, the adhesion strengths after heating and then cooling at 70, 60, 50, 40, and 30℃ are 1.39, 0.99, 0.92, 0.75, and 0.48 MPa, respectively, which are basically consistent with the corresponding adhesion strengths tested at higher temperatures. This indicates that the reversible adhesive, which contains the compound shown in formula (Ⅰ-Ⅰ) and has color-changing and reversible adhesion functions, exhibits temperature-responsive reversible adhesion performance.

[0051] Example 7

[0052] This embodiment provides a method for preparing a reversible adhesive that can quantify adhesion strength through color change. It is basically the same as that in Example 6, except that it uses a compound with color change and reversible adhesion function as shown in formula (I-II).

[0053] From the appendix Figure 1 Test diagram and appendix Figure 3 The results of the reversible adhesion performance show that the reversible adhesive with color-changing and reversible adhesion functions, which includes the compound shown in formula (Ⅰ-Ⅱ), has an adhesion strength that can be quantified by color change. The adhesion strengths after heating and then cooling at 30, 40, 50, 60, 70, and 80℃ are 0.39, 0.58, 0.74, 0.87, 1.12, and 1.29 MPa, respectively, showing a gradually increasing trend. Then, the adhesion strengths after heating and then cooling at 70, 60, 50, 40, and 30℃ are 1.19, 0.92, 0.78, 0.63, and 0.41 MPa, respectively, which are basically consistent with the corresponding adhesion strengths tested at higher temperatures. This indicates that the reversible adhesive with color-changing and reversible adhesion functions, which includes the compound shown in formula (Ⅰ-Ⅱ), has temperature-responsive reversible adhesion performance.

[0054] Example 8

[0055] This embodiment provides a method for preparing a reversible adhesive that can quantify adhesion strength through color change. It is basically the same as that in Example 6, except that it uses a compound with color change and reversible adhesion function as shown in formula (I-III).

[0056] From the appendix Figure 1 Test diagram and appendix Figure 4The results of the reversible adhesion performance show that the reversible adhesive with color-changing and reversible adhesion functions, which includes the compound shown in formula (I-III), has an adhesion strength that can be quantified by color change. The adhesion strengths after heating and then cooling at 30, 40, 50, 60, 70, and 80℃ are 0.62, 0.94, 1.15, 1.39, 1.58, and 1.76 MPa, respectively, showing a gradually increasing trend. Then, the adhesion strengths after heating and then cooling at 70, 60, 50, 40, and 30℃ are 1.61, 1.42, 1.19, 0.96, and 0.65 MPa, respectively, which are basically consistent with the corresponding adhesion strengths tested at higher temperatures. This indicates that the reversible adhesive with color-changing and reversible adhesion functions, which includes the compound shown in formula (I-III), has temperature-responsive reversible adhesion performance.

[0057] Example 9

[0058] This embodiment provides a method for preparing a reversible adhesive that can quantify adhesion strength through color change. It is basically the same as that in Example 6, except that it uses a compound with color change and reversible adhesion function as shown in formula (I-IV).

[0059] From the appendix Figure 1 Test diagram and appendix Figure 5 The results of the reversible adhesion performance show that the reversible adhesive with color-changing and reversible adhesion functions, which includes the compound shown in formula (I-IV), has an adhesion strength that can be quantified by color change. The adhesion strengths after heating and then cooling at 30, 40, 50, 60, 70, and 80℃ are 0.77, 1.05, 1.26, 1.54, 1.79, and 2.05 MPa, respectively, showing a gradually increasing trend and exceeding 2 MPa at the highest. Then, the adhesion strengths after heating and then cooling at 70, 60, 50, 40, and 30℃ are 1.78, 1.59, 1.31, 1.11, and 0.79 MPa, respectively, which are basically consistent with the corresponding adhesion strengths tested at higher temperatures. This indicates that the reversible adhesive with color-changing and reversible adhesion functions, which includes the compound shown in formula (I-IV), has temperature-responsive reversible adhesion performance.

[0060] Example 10

[0061] This embodiment provides a method for preparing a reversible adhesive that can quantify adhesion strength through color change. It is basically the same as that in Example 6, except that it uses a compound with color change and reversible adhesion function with the structure shown in formula (I-V).

[0062] From the appendix Figure 1 Test diagram and appendix Figure 6The results of the reversible adhesion performance show that the reversible adhesive with color-changing and reversible adhesion functions, which includes the compound shown in formula (I-V), has an adhesion strength that can be quantified by color change. The adhesion strengths after heating and then cooling at 30, 40, 50, 60, 70, and 80℃ are 0.51, 0.79, 0.92, 1.13, 1.47, and 1.72 MPa, respectively, showing a gradually increasing trend. Then, the adhesion strengths after heating and then cooling at 70, 60, 50, 40, and 30℃ are 1.52, 1.21, 0.96, 0.83, and 0.56 MPa, respectively, which are basically consistent with the corresponding adhesion strengths tested at higher temperatures. This indicates that the reversible adhesive with color-changing and reversible adhesion functions, which includes the compound shown in formula (I-V), has temperature-responsive reversible adhesion performance.

[0063] Example 11

[0064] This embodiment provides a method for quantifying the adhesion strength of a reversible adhesive that can be quantified by color change, specifically as follows: Based on the correspondence between the absorption peak intensity of a specific band in the ultraviolet absorption spectrum of the adhesive film and the absorption peak intensity of a specific band in the preset ultraviolet absorption spectrum and the adhesion strength at different temperatures, the adhesion strength of the reversible adhesive that can be quantified by color change is quantitatively calculated.

[0065] The relationship between the absorption peak intensity of a specific band in the preset ultraviolet absorption spectrum and the adhesion strength at different temperatures can be obtained as follows: The reversible adhesive prepared in Example 6 was placed between two pieces of ordinary transparent glass and fixed with clips. The initial absorption peak intensity of the specific wavelength band (450 nm) of the ultraviolet absorption spectrum of the reversible adhesive was measured. The reversible adhesive was heated to the test temperature of 30°C, kept at that temperature for 5 minutes, and then cooled to room temperature. Its shear adhesion strength and the absorption peak intensity of the specific wavelength band (450 nm) of the ultraviolet absorption spectrum were tested. The shear adhesion strength and the absorption peak intensity of the specific wavelength band (450 nm) of the ultraviolet absorption spectrum of the reversible adhesive were measured at different test heating temperatures (40, 50, 60, 70, 80°C). Based on the correspondence between the shear adhesion strength and the corresponding absorption peak intensity of the specific wavelength band of the ultraviolet absorption spectrum at different test heating temperatures, the correspondence between the absorption peak intensity of the specific wavelength band of the ultraviolet absorption spectrum and the shear adhesion strength of the tested reversible adhesive were quantitatively determined.

[0066] From the appendix Figure 1 Test diagram and appendix Figure 7The results of the correlation between the absorption peak intensity of a specific band of the ultraviolet absorption spectrum and the adhesion strength at different temperatures show that the reversible adhesive with color-changing and reversible adhesion functions, which includes the compound shown in formula (Ⅰ-Ⅰ), has an adhesion strength that can be quantified by color change. The adhesion strength after heating and then cooling at 30, 40, 50, 60, 70, and 80℃ is 0.43, 0.71, 0.89, 1.08, 1.34, and 1.57 MPa, respectively, showing a gradually increasing trend. At the same time, the absorption peak intensity of the specific band (450 nm) of the ultraviolet absorption spectrum at the corresponding temperatures is 0.05 (25℃), 0.07 (30℃), 0.11 (40℃), 0.25 (50℃), 0.33 (60℃), 0.46 (70℃), and 0.59 (80℃), respectively, also showing an increasing trend, and the increasing trend is basically synchronized with the adhesion strength. The above results indicate that the adhesive strength of the reversible adhesive, which contains the structure shown in formula (Ⅰ-Ⅰ) and has color-changing and reversible adhesion functions, can be quantified by its apparent color change at different response temperatures.

[0067] Example 12

[0068] This embodiment provides a method for quantifying the adhesion strength of a reversible adhesive that can be quantified by color change. It is basically the same as that in Example 11, except that it uses a compound with color change and reversible adhesion function as shown in formula (I-II).

[0069] From the appendix Figure 1 Test diagram and appendix Figure 8 The results of the correlation between the absorption peak intensity of a specific band of the ultraviolet absorption spectrum and the adhesion strength at different temperatures show that the reversible adhesive with color-changing and reversible adhesion functions, which includes the compound shown in formula (Ⅰ-Ⅱ), has an adhesion strength that can be quantified by color change. The adhesion strength after heating and then cooling at 30, 40, 50, 60, 70, and 80℃ is 0.39, 0.58, 0.74, 0.87, 1.12, and 1.29 MPa, respectively, showing a gradually increasing trend. At the same time, the absorption peak intensity of the specific band (450nm) of the ultraviolet absorption spectrum at the corresponding temperatures is 0.04 (25℃), 0.09 (30℃), 0.17 (40℃), 0.28 (50℃), 0.36 (60℃), 0.43 (70℃), and 0.54 (80℃), respectively, also showing an increasing trend, and the increasing trend is basically synchronized with the adhesion strength. The above results indicate that the adhesive strength of the reversible adhesive, which contains the structure shown in formula (Ⅰ-Ⅱ) and has color-changing and reversible adhesion functions, can be quantified by its apparent color change at different response temperatures.

[0070] Example 13

[0071] This embodiment provides a method for quantifying the adhesion strength of a reversible adhesive that can be quantified by color change. It is basically the same as that in Example 11, except that it uses a compound with color change and reversible adhesion function as shown in formula (I-III).

[0072] From the appendix Figure 1 Test diagram and appendix Figure 9 The results of the correlation between the absorption peak intensity of a specific band of the ultraviolet absorption spectrum and the adhesion strength at different temperatures show that the reversible adhesive with color-changing and reversible adhesion functions, which includes the compounds shown in formulas (Ⅰ-Ⅲ), has an adhesion strength that can be quantified by color change. The adhesion strength after heating and then cooling at 30, 40, 50, 60, 70, and 80℃ is 0.62, 0.94, 1.15, 1.39, 1.58, and 1.76 MPa, respectively, showing a gradually increasing trend. At the same time, the absorption peak intensity of the specific band (450 nm) of the ultraviolet absorption spectrum at the corresponding temperatures is 0.04 (25℃), 0.09 (30℃), 0.28 (40℃), 0.37 (50℃), 0.56 (60℃), 0.68 (70℃), and 0.73 (80℃), respectively, also showing an increasing trend, and the increasing trend is basically synchronized with the adhesion strength. The above results indicate that the adhesive strength of the reversible adhesive, which contains the structure shown in formulas (I-III) and has color-changing and reversible adhesion functions, can be quantified by its apparent color change at different response temperatures.

[0073] Example 14

[0074] This embodiment provides a method for quantifying the adhesion strength of a reversible adhesive that can be quantified by color change. It is basically the same as that in Example 11, except that it uses a compound with color change and reversible adhesion function as shown in formula (I-IV).

[0075] From the appendix Figure 1 Test diagram and appendix Figure 10The results of the correlation between the absorption peak intensity of a specific band of the ultraviolet absorption spectrum and the adhesion strength at different temperatures show that the reversible adhesive with color-changing and reversible adhesion functions, which includes the compounds shown in formulas (I-IV), exhibits adhesion strength that can be quantified by color change. The adhesion strengths after heating and then cooling at 30, 40, 50, 60, 70, and 80℃ are 0.77, 1.05, 1.26, 1.54, 1.79, and 2.05 MPa, respectively, showing a gradually increasing trend. Simultaneously, the absorption peak intensities of the specific band (450 nm) of the ultraviolet absorption spectrum at the corresponding temperatures are 0.05 (25℃), 0.12 (30℃), 0.35 (40℃), 0.48 (50℃), 0.68 (60℃), 0.72 (70℃), and 0.89 (80℃), respectively, also showing an increasing trend, and this increasing trend is basically synchronized with the adhesion strength. The above results indicate that the adhesive strength of the reversible adhesive, which contains the structure shown in formulas (I-IV) and has color-changing and reversible adhesion functions, can be quantified by its apparent color change at different response temperatures.

[0076] Example 15

[0077] This embodiment provides a method for quantifying the adhesion strength of a reversible adhesive that can be quantified by color change. It is basically the same as that in Example 11, except that it uses a compound with color change and reversible adhesion function as shown in formula (I-V).

[0078] From the appendix Figure 1 Test diagram and appendix Figure 11 The results of the correlation between the absorption peak intensity of a specific band of the ultraviolet absorption spectrum and the adhesion strength at different temperatures show that the reversible adhesive with color-changing and reversible adhesion functions, which includes the compound shown in formula (Ⅰ-Ⅴ), has an adhesion strength that can be quantified by color change. The adhesion strength after heating and then cooling at 30, 40, 50, 60, 70, and 80℃ is 0.51, 0.79, 0.92, 1.13, 1.47, and 1.72 MPa, respectively, showing a gradually increasing trend. At the same time, the absorption peak intensity of the specific band (450 nm) of the ultraviolet absorption spectrum at the corresponding temperatures is 0.04 (25℃), 0.08 (30℃), 0.19 (40℃), 0.28 (50℃), 0.36 (60℃), 0.49 (70℃), and 0.61 (80℃), respectively, also showing an increasing trend, and the increasing trend is basically synchronized with the adhesion strength. The above results indicate that the adhesive strength of the reversible adhesive, which contains the structure shown in formula (I-V) and has color-changing and reversible adhesion functions, can be quantified by its apparent color change at different response temperatures.

[0079] The test data shows that all reversible adhesives containing compounds with color-changing and reversible adhesion functions, whose adhesive strength can be quantified by color change, exhibit temperature-responsive reversible adhesion properties. Among them, the reversible adhesives containing compounds with color-changing and reversible adhesion functions, whose adhesive strength can be quantified by color change, exhibit relatively superior temperature-responsive reversible adhesion properties. The reversible adhesive containing compounds with color-changing and reversible adhesion functions, whose adhesive strength can be quantified by color change, has the highest adhesive strength, reaching 2.05 MPa after being heated to 80°C and then cooled to room temperature, far exceeding the other embodiments. On the other hand, the adhesive strength of reversible adhesives containing compounds with color-changing and reversible adhesion functions, including those with structures shown in formulas (Ⅰ-Ⅰ), (Ⅰ-Ⅱ), (Ⅰ-Ⅲ), (Ⅰ-Ⅳ), and (Ⅰ-Ⅴ), can be quantified by their apparent color changes at different response temperatures. Taking Example 14 as an example, the absorption peak intensity of the reversible adhesive containing compounds with color-changing and reversible adhesion functions, including those with structures shown in formula (Ⅰ-Ⅳ), in a specific band (450nm) of the ultraviolet absorption spectrum at different temperatures shows an increasing trend, and the increasing trend is basically synchronized with the adhesive strength, showing a large correlation between the two.

[0080] Comparative Example 1

[0081] This comparative example provides a method for preparing an adhesive that is essentially the same as that of Examples 6 and 11, except that no compounds with color-changing and reversible adhesion functions are added.

[0082] From the appendix Figure 1 Test diagram and appendix Figure 12 The adhesion performance results show that the adhesive without any color-changing and reversible adhesion functional compounds exhibits adhesion strengths of 0.05, 0.06, 0.06, 0.07, 0.07, and 0.08 MPa after heating and cooling at 30, 40, 50, 60, 70, and 80℃, respectively, which are essentially unchanged with increasing temperature. Furthermore, the adhesion strengths after heating and cooling at 70, 60, 50, 40, and 30℃ are 0.07, 0.07, 0.07, 0.06, and 0.06 MPa, respectively, which are basically consistent with the corresponding adhesion strengths tested at higher temperatures. This indicates that the adhesive without any color-changing and reversible adhesion functional compounds does not possess temperature-responsive reversible adhesion properties.

[0083] From the appendix Figure 1 Test diagram and appendix Figure 13The results of the correlation between the absorption peak intensity of a specific band of the ultraviolet absorption spectrum and the adhesion strength at different temperatures show that the adhesion strength of the adhesive without any color-changing and reversible adhesion functional compounds after heating and then cooling at 30, 40, 50, 60, 70, and 80℃ is 0.05, 0.06, 0.06, 0.07, 0.07, and 0.08 MPa, respectively. At the same time, the absorption peak intensity of the specific band (450 nm) of the ultraviolet absorption spectrum at the corresponding temperatures is 0.04 (25℃), 0.04 (30℃), 0.05 (40℃), 0.04 (50℃), 0.05 (60℃), 0.05 (70℃), and 0.05 (80℃), respectively, with basically no change in absorption peak intensity. The above results indicate that adhesives without any color-changing and reversible adhesion compounds do not exhibit temperature-responsive reversible adhesion properties at different response temperatures, and their adhesion strength cannot be quantified by their apparent color changes.

[0084] Comparative Example 2

[0085] This comparative example provides a method for preparing an adhesive, which is basically the same as that of Examples 6 and 11, except that the structure of the added adhesive compound is shown in formula (I-VI).

[0086] The synthesis and post-processing methods of the compounds shown in formulas (Ⅰ-Ⅵ) are basically the same as those in Example 1, except that the compounds shown in formulas (Ⅱ-Ⅱ) are 2-bromoethanol and the compounds shown in formula (Ⅲ) are bromoethane.

[0087]

[0088] The reversible adhesion performance test results show that the reversible adhesive of the compound containing the structure shown in formula (Ⅰ-Ⅵ) exhibits gradually increasing adhesion strengths after being heated and then cooled at 30, 40, 50, 60, 70, and 80℃, respectively. Furthermore, the adhesion strengths after being heated and then cooled at 70, 60, 50, 40, and 30℃ are 1.28, 0.97, 0.81, 0.65, and 0.39 MPa, respectively, which are basically consistent with the corresponding adhesion strengths tested at higher temperatures. This indicates that the adhesive of the compound containing the structure shown in formula (Ⅰ-Ⅵ) has temperature-responsive reversible adhesion properties.

[0089] The results of the correlation between the absorption peak intensity of a specific band of the ultraviolet absorption spectrum and the adhesion strength at different temperatures show that the reversible adhesive containing the compound with reversible adhesion function of the structure shown in formula (Ⅰ-Ⅵ) has an adhesion strength of 0.38, 0.62, 0.77, 0.95, 1.26 and 1.31 MPa after heating and then cooling at 30, 40, 50, 60, 70 and 80℃, respectively, showing a gradually increasing trend. At the same time, the absorption peak intensity of the specific band (450nm) of the ultraviolet absorption spectrum at the corresponding temperatures is 0.06 (25℃), 0.05 (30℃), 0.05 (40℃), 0.05 (50℃), 0.04 (60℃), 0.05 (70℃) and 0.05 (80℃), respectively, and the absorption peak intensity remains basically unchanged. The above results indicate that the adhesive of the compound containing the structure shown in formula (I-VI) with reversible adhesion function has temperature-responsive reversible adhesion properties, but the corresponding adhesive strength at the corresponding temperature is lower compared with Examples 6 and 11. The correlation between the absorption peak intensity of a specific band of a specific ultraviolet absorption spectrum and the adhesive strength at different temperatures indicates that the reversible adhesive of the compound containing the structure shown in formula (I-VI) with reversible adhesion function does not have the ability to quantify its adhesive strength through apparent color changes.

[0090] Comparative Example 3

[0091] This comparative example provides a method for preparing an adhesive, which is basically the same as that of Examples 6 and 11, except that the structure of the added functional compound is shown in formula (I-VII).

[0092] The synthesis and post-processing methods of the compounds shown in formulas (Ⅰ-Ⅶ) are basically the same as those in Example 1, except that the compounds shown in formulas (Ⅱ-Ⅱ) are bromoethane and the compounds shown in formula (Ⅲ) are 2-bromoethanol.

[0093]

[0094] The reversible adhesion performance test results show that the reversible adhesive of the compound containing the structure shown in formula (Ⅰ-Ⅶ) with reversible adhesion function has an adhesion strength of 0.08, 0.09, 0.08, 0.1, 0.09 and 0.09 MPa after being heated and then cooled at 30, 40, 50, 60, 70 and 80℃, respectively, which is basically unchanged with temperature. Then, the adhesion strength after being heated and then cooled at 70, 60, 50, 40 and 30℃ is 0.09, 0.09, 0.09, 0.08 and 0.08 MPa, respectively, which is basically consistent with the corresponding adhesion strength tested when the temperature is increased. This indicates that the adhesive of the functional compound containing the structure shown in formula (Ⅰ-Ⅶ) does not have temperature-responsive reversible adhesion performance.

[0095] The results of the correlation between the absorption peak intensity of a specific band of the ultraviolet absorption spectrum and the adhesion strength at different temperatures show that the adhesion strength of the reversible adhesive containing the compound with reversible adhesion function, which has the structure shown in formula (Ⅰ-Ⅶ), after being heated and then cooled at 30, 40, 50, 60, 70, and 80℃, is 0.08, 0.09, 0.08, 0.1, 0.09, and 0.09 MPa, respectively. At the same time, the absorption peak intensities of the specific band (450 nm) of the ultraviolet absorption spectrum at the corresponding temperatures are 0.04 (25℃), 0.05 (30℃), 0.09 (40℃), 0.19 (50℃), 0.31 (60℃), 0.48 (70℃), and 0.57 (80℃), respectively. The absorption peak intensity increases with increasing temperature. The above results indicate that the adhesive containing the functional compound shown in formula (I-VII) has temperature-responsive color change properties, but it does not have temperature-responsive reversible adhesion properties compared to Examples 6 and 11.

[0096] Comparative Example 4

[0097] This comparative example provides a method for preparing an adhesive, which is basically the same as that of Examples 6 and 11, except that the structure of the added functional compound is shown in formula (I-VIII).

[0098] The synthesis and post-processing methods of the compounds shown in formulas (Ⅰ-Ⅷ) are basically the same as those in Example 1, except that the compounds shown in formulas (Ⅱ-Ⅱ) and (Ⅲ) are all made of bromoethane.

[0099]

[0100] The reversible adhesion performance test results show that the adhesive containing the functional compound of formula (I-VIII) exhibits adhesion strengths of 0.07, 0.06, 0.08, 0.08, 0.09, and 0.08 MPa after being heated and then cooled at 30, 40, 50, 60, 70, and 80℃, respectively, which are essentially unchanged with temperature. Furthermore, the adhesion strengths after being heated and then cooled at 70, 60, 50, 40, and 30℃ are 0.08, 0.09, 0.09, 0.08, and 0.08 MPa, respectively, which are basically consistent with the corresponding adhesion strengths tested at higher temperatures. This indicates that the adhesive containing the functional compound of formula (I-VIII) does not possess temperature-responsive reversible adhesion properties.

[0101] The results of the correlation between the absorption peak intensity of a specific band of the ultraviolet absorption spectrum and the adhesion strength at different temperatures show that the adhesion strength of the reversible adhesive containing the compound with reversible adhesion function, which includes the structure shown in formula (Ⅰ-Ⅷ), after being heated and then cooled at 30, 40, 50, 60, 70, and 80℃, is 0.07, 0.06, 0.08, 0.08, 0.09, and 0.08 MPa, respectively. At the same time, the absorption peak intensity of the specific band (450nm) of the ultraviolet absorption spectrum at the corresponding temperatures is 0.07 (25℃), 0.06 (30℃), 0.06 (40℃), 0.06 (50℃), 0.06 (60℃), 0.05 (70℃), and 0.07 (80℃), respectively, and the absorption peak intensity remains basically unchanged. The above results indicate that the adhesive containing the functional compound of formula (I-VIII) does not have temperature-responsive reversible adhesion properties, nor does it have the ability to quantify its adhesive strength through apparent color changes.

[0102] Comparative Example 5

[0103] This comparative example provides a method for preparing an adhesive, which is basically the same as that of Examples 6 and 11, except that the structure of the added functional compound is shown in formula (I-IX).

[0104]

[0105] The preparation method of this compound is as follows:

[0106] (1) Preparation of intermediate products

[0107]

[0108]

[0109] Imidazole and the starting material (2-bromoethanol) of the compound shown in formula (Ⅱ-Ⅱ) were dissolved in anhydrous acetonitrile and mixed thoroughly. The resulting homogeneous solution was reacted at 50°C for 8 hours in a N2 atmosphere. After the reaction was completed, a solution containing the intermediate product of the structure shown in formula (Ⅱ-Ⅰ) was obtained. Sodium carbonate was added to the solution and stirred for 2 hours. Then dibromomethane was added and reacted at 5°C for 8 hours in a N2 atmosphere. The filtrate was obtained by filtration and washed thoroughly with ethyl acetate and anhydrous diethyl ether, respectively, to obtain the compound shown in formula (Ⅱ). Among them, imidazole and the compound shown in formula (II-II) were added in a molar ratio of 1:1.1, the volume of acetonitrile was 6 mL / g based on the mass of imidazole, the mass of sodium carbonate was 1 g / g based on the mass of imidazole, the molar amount of dibromomethane was 0.5 mol / mol based on the amount of imidazole, and the washing times of ethyl acetate and anhydrous diethyl ether were 3 times each.

[0110]

[0111] The synthesized compound with color-changing and reversible adhesion structure shown in formula (II) was mixed with potassium hexafluorophosphate in an aqueous solution at a molar ratio of 1:2.5 and stirred at room temperature for 12 h. After the reaction, the mixture was thoroughly washed three times with deionized water to remove unreacted potassium hexafluorophosphate. Then, the mixture was centrifuged and filtered to obtain the compound shown in formula (II-a).

[0112] (2) Synthesis of compounds with color-changing and reversible adhesion functions

[0113]

[0114] 4,4'-bipyridine, the intermediate product shown in formula (II-a), and the starting material of the compound shown in formula (III) (2-bromoethanol) were dissolved in acetonitrile, respectively. After mixing, the mixture was reacted at 80°C for 12 h to obtain a reaction solution. After post-treatment, the compound (I-IX) with color change and reversible adhesion function was obtained.

[0115] Wherein, X1 is Br, the molar ratio of 4,4'-bipyridine to the intermediate shown in formula (II) is 1:0.5, the molar ratio of 4,4'-bipyridine to the intermediate shown in formula (III) is 1:0.5, and the mass amount of acetonitrile is 0.6 g / g based on the mass amount of 4,4'-bipyridine. The post-treatment method of the reaction solution is as follows: the cooled reaction solution is filtered under negative pressure, the filter residue is collected and washed multiple times with acetonitrile, the filter residue is washed 3 times with anhydrous diethyl ether, filtered, and thoroughly dried.

[0116] The reversible adhesion performance test results show that the adhesive containing the functional compound of formula (Ⅰ-Ⅸ) exhibits gradually increasing adhesion strengths after being heated and then cooled at 30, 40, 50, 60, 70, and 80℃, respectively. Furthermore, the adhesion strengths after being heated and then cooled at 70, 60, 50, 40, and 30℃ are 1.22, 0.96, 0.83, 0.66, and 0.35 MPa, respectively, which are basically consistent with the corresponding adhesion strengths tested at higher temperatures. This indicates that the adhesive containing the functional compound of formula (Ⅰ-Ⅸ) possesses temperature-responsive reversible adhesion properties.

[0117] The results of the correlation between the absorption peak intensity of a specific band of the ultraviolet absorption spectrum and the adhesion strength at different temperatures show that the reversible adhesive containing the compound with reversible adhesion function of the structure shown in formula (Ⅰ-Ⅸ) has an adhesion strength of 0.33, 0.6, 0.78, 0.92, 1.21 and 1.39 MPa after heating and then cooling at 30, 40, 50, 60, 70 and 80℃, respectively, showing a gradually increasing trend. At the same time, the absorption peak intensity of the specific band (450nm) of the ultraviolet absorption spectrum at the corresponding temperatures is 0.04 (25℃), 0.28 (30℃), 0.39 (40℃), 0.09 (50℃), 0.06 (60℃), 0.69 (70℃) and 0.27 (80℃), respectively, showing an irregular increase and decrease in absorption peak intensity. The above results indicate that the reversible adhesive of the functional compound containing formula (I-IX) exhibits temperature-responsive reversible adhesion properties. However, compared to Examples 6 and 11, the corresponding adhesive strength at the corresponding temperatures is lower. The correlation between the absorption peak intensity of a specific band of a specific ultraviolet absorption spectrum and the adhesive strength at different temperatures shows that the color of the reversible adhesive of the functional compound containing formula (I-IX) changes irregularly with temperature, and it does not have the ability to quantify its adhesive strength through apparent color changes.

[0118] Comparative Example 6

[0119] This comparative example provides a method for preparing a reversible adhesive, which is basically the same as that of Examples 6 and 11, except that the structure of the added compound with reversible adhesion function is shown in formula (I-X).

[0120]

[0121] The preparation method of this compound is as follows:

[0122]

[0123]

[0124] Imidazole and the starting material (2-bromoethanol) of the compound shown in formula (Ⅱ-Ⅱ) were dissolved in anhydrous acetonitrile and mixed thoroughly. The resulting homogeneous solution was reacted at 50°C for 8 h in a N2 atmosphere. After the reaction was completed, a solution containing the intermediate product of the structure shown in formula (Ⅱ-Ⅰ) was obtained. Sodium carbonate was added to the solution and stirred for 2 h. Then bromomethane was added and reacted at 5°C for 8 h in a N2 atmosphere. The filtrate was obtained by filtration and washed thoroughly with ethyl acetate and anhydrous diethyl ether, respectively, to obtain the compound shown in formula (Ⅱ-b). Among them, imidazole and the compound shown in formula (II-II) were added in a molar ratio of 1:1.1, the volume of acetonitrile was 6 mL / g based on the mass of imidazole, the mass of sodium carbonate was 1 g / g based on the mass of imidazole, the molar amount of bromomethane was 0.5 mol / mol based on the amount of imidazole, and the washing times of ethyl acetate and anhydrous diethyl ether were 3 times each.

[0125]

[0126] The synthesized compound with color-changing and reversible adhesion functions, as shown in formula (Ⅱ-b), was mixed with potassium hexafluorophosphate in an aqueous solution at a molar ratio of 1:2.5 and stirred at room temperature for 12 h. After the reaction, the mixture was thoroughly washed three times with deionized water to remove unreacted potassium hexafluorophosphate. Then, the mixture was centrifuged and filtered to obtain the compound shown in formula (Ⅰ-Ⅹ).

[0127] The reversible adhesion performance test results show that the reversible adhesive of the compound containing the structure shown in formula (I-X) exhibits gradually increasing adhesion strengths after being heated and then cooled at 30, 40, 50, 60, 70, and 80℃, respectively. Furthermore, the adhesion strengths after being heated and then cooled at 70, 60, 50, 40, and 30℃ are 1.15, 0.86, 0.74, 0.52, and 0.28 MPa, respectively, which are basically consistent with the corresponding adhesion strengths tested at higher temperatures. This indicates that the reversible adhesive of the compound containing the structure shown in formula (I-X) possesses temperature-responsive reversible adhesion properties.

[0128] The results of the correlation between the absorption peak intensity of a specific band of the ultraviolet absorption spectrum and the adhesion strength at different temperatures show that the reversible adhesive containing the compound with reversible adhesion function of the structure shown in formula (Ⅰ-Ⅹ) exhibits an adhesion strength of 0.25, 0.48, 0.71, 0.83, 1.11 and 1.27 MPa after heating and then cooling at 30, 40, 50, 60, 70 and 80℃, respectively, showing a gradually increasing trend. At the same time, the absorption peak intensity of the specific band (450nm) of the ultraviolet absorption spectrum at the corresponding temperatures is 0.04 (25℃), 0.06 (30℃), 0.05 (40℃), 0.04 (50℃), 0.05 (60℃), 0.05 (70℃) and 0.06 (80℃), respectively, with the absorption peak intensity remaining basically unchanged. The above results indicate that the reversible adhesive of the compound containing the structure shown in formula (I-X) has reversible adhesion function and exhibits temperature-responsive reversible adhesion properties. However, compared with Examples 6 and 11, the corresponding response adhesion strength at the corresponding temperature is lower, and it does not have the ability to quantify its adhesion strength through apparent color changes.

[0129] Comparative Example 7

[0130] This comparative example provides a method for preparing a color-changing gel, which is basically the same as that of Examples 6 and 11, except that the structure of the added color-changing compound is shown in formula (I-XI).

[0131]

[0132] The preparation method of this compound is as follows:

[0133]

[0134] 4,4'-bipyridine, the compound raw material shown in formula (II) (bromomethane), and the compound raw material shown in formula (III) (2-bromoethanol) were dissolved in acetonitrile, respectively. After mixing, the mixture was reacted at 80°C for 12 h to obtain a reaction solution. After post-treatment, the compound (I-a) with color change and reversible adhesion function was obtained.

[0135] The molar ratio of 4,4'-bipyridine to the compound shown in formula (II) is 1:0.5, the molar ratio of 4,4'-bipyridine to the compound shown in formula (III) is 1:0.5, and the mass amount of acetonitrile used is 0.6 g / g based on the mass amount of 4,4'-bipyridine. The post-treatment method of the reaction solution is as follows: the cooled reaction solution is filtered under negative pressure, the filter residue is collected and washed multiple times with acetonitrile, the filter residue is washed 3 times with anhydrous diethyl ether, filtered, and thoroughly dried.

[0136]

[0137] The synthesized compound with color-changing and reversible adhesion functions, as shown in formula (Ⅰ-a), was mixed with potassium hexafluorophosphate in an aqueous solution at a molar ratio of 1:2.5 and stirred at room temperature for 12 h. After the reaction, the mixture was thoroughly washed three times with deionized water to remove unreacted potassium hexafluorophosphate. The mixture was then centrifuged and filtered. The resulting solid product was thoroughly dried in a vacuum oven at 60 °C to obtain the compound with color-changing and reversible adhesion functions, as shown in formula (Ⅰ-Ⅺ), whose anion is hexafluorophosphate.

[0138] The adhesion performance test results show that the gel containing the color-changing compound of the structure shown in formula (Ⅰ-Ⅺ) exhibits adhesion strengths of 0.06, 0.06, 0.08, 0.08, 0.09, and 0.09 MPa after being heated and then cooled at 30, 40, 50, 60, 70, and 80℃, respectively, which are basically unchanged with temperature. Furthermore, the adhesion strengths after being heated and then cooled at 70, 60, 50, 40, and 30℃ are 0.09, 0.09, 0.09, 0.07, and 0.07 MPa, respectively, which are basically consistent with the corresponding adhesion strengths tested during temperature increase. This indicates that the gel containing the compound of formula (Ⅰ-Ⅺ) does not possess temperature-responsive reversible adhesion properties.

[0139] The results of the correlation between the absorption peak intensity of a specific band of the specific ultraviolet absorption spectrum and the adhesion strength at different temperatures show that the reversible adhesive of the compound with reversible adhesion function containing the structure shown in formula (Ⅰ-Ⅺ) has an adhesion strength of 0.06, 0.06, 0.08, 0.08, 0.09 and 0.09 MPa after being heated and then cooled at 30, 40, 50, 60, 70 and 80℃, respectively. At the same time, the absorption peak intensities of the specific band (450nm) of the ultraviolet absorption spectrum at the corresponding temperatures are 0.04 (25℃), 0.06 (30℃), 0.98 (40℃), 0.19 (50℃), 0.57 (60℃), 0.36 (70℃) and 0.24 (80℃), respectively. The absorption peak intensity changes with temperature, but does not show a linear relationship. The above results indicate that the gel of the compound containing the structure shown in formula (I-XI) with color-changing function has temperature-responsive color-changing function. However, compared with Examples 6 and 11, the intensity of the corresponding absorption peak at the corresponding temperature is inconsistent and does not change linearly with temperature. Moreover, its adhesion strength does not have temperature-responsive reversible adhesion properties at different response temperatures.

[0140] Comparative Example 8

[0141] This comparative example provides a method for preparing an adhesive with temperature-responsive color change and reversible adhesion properties, which is basically the same as that of Example 6 and Example 11. The difference is that the added compounds with reversible adhesion and color change functions have the structures shown in Formula (I-X) and Formula (I-XI), respectively.

[0142]

[0143] The reversible adhesion performance test results show that the adhesive strength of the compound containing the structures shown in formulas (I-X) and (I-XI), which has reversible adhesion function and color change, is 0.27, 0.46, 0.72, 0.86, 1.12, and 1.29 MPa after heating and then cooling at 30, 40, 50, 60, 70, and 80℃, respectively, showing a gradually increasing trend. Then, the adhesive strength after heating and then cooling at 70, 60, 50, 40, and 30℃ is 1.13, 0.85, 0.74, 0.49, and 0.27 MPa, respectively, which is basically consistent with the corresponding adhesive strength tested at the temperature rise. This indicates that the adhesive containing the compounds shown in formulas (I-X) and (I-XI), which has reversible adhesion function and color change, has temperature-responsive reversible adhesion performance.

[0144] The results of the correlation between the absorption peak intensity of specific ultraviolet absorption spectra in specific bands and the adhesion strength at different temperatures show that the adhesives containing the structures shown in formulas (I-X) and (I-XI) with reversible adhesion function and color change have adhesion strengths of 0.27, 0.46, 0.72, 0.86, 1.12, and 1.29 MPa after being heated and then cooled at 30, 40, 50, 60, 70, and 80 °C, respectively. At the same time, the absorption peak intensities of the specific band (450 nm) of the ultraviolet absorption spectrum at the corresponding temperatures are 0.05 (25 °C), 0.06 (30 °C), 0.88 (40 °C), 0.29 (50 °C), 0.47 (60 °C), 0.33 (70 °C), and 0.58 (80 °C), respectively. The absorption peak intensity changes with temperature, but does not show a linear relationship. The above results indicate that the adhesive containing the compounds shown in formulas (I-X) and (I-XI) has reversible adhesion function and color change, and possesses temperature-responsive reversible adhesion properties. However, the intensity of the absorption peak in a specific band of the ultraviolet absorption spectrum at the corresponding temperature varies and does not change linearly with temperature. Simply superimposing the two cannot achieve the purpose of quantifying its adhesive strength ability through apparent color change.

[0145] The adhesive provided by this invention can achieve stable reversible adhesion cycles with temperature changes. At the same time, it can intuitively reflect the real-time changes in adhesion strength through changes in apparent color, establish a precise correspondence between color parameters and adhesion strength, and achieve rapid quantification of adhesion strength without the need for complex instruments. This meets the application needs of high-performance reversible adhesive materials in fields such as flexible electronics and smart devices, and promotes the further development and industrial application of reversible adhesive technology.

[0146] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. A reversible adhesive that quantifies adhesion strength through color change, characterized in that: The reversible adhesive is prepared by polymerization of a compound with color-changing and reversible adhesion functions, as shown in Formula I, in a solution containing polymerizable monomers, initiators, and crosslinking agents. The amount of the compound with color-changing and reversible adhesion functions as shown in Formula I is 10-50% of the polymerizable monomer by mass, the amount of the initiator is 0.5-5% of the polymerizable monomer by mass, and the amount of the crosslinking agent is 0.5-5% of the polymerizable monomer by mass. The polymerizable monomers are hexyl methacrylate and hydroxyethyl methacrylate; Formula I; R1 is selected from one of hydroxyl, alkoxy, carboxyl, ester, and phenyl groups, and X is PF6.

2. The reversible adhesive that can quantify adhesion strength through color change as described in claim 1, characterized in that: The method for preparing the compound with color-changing and reversible adhesion functions as shown in Formula I includes, 4,4'-bipyridine and the compounds shown in Formula II and Formula III were dissolved in acetonitrile, respectively. After mixing, the mixture was reacted at 60-100°C for 6-24 h to obtain a reaction solution. After post-treatment, the compound shown in Formula IV was obtained. The compound shown in Formula IV was subjected to an anion substitution reaction with potassium hexafluorophosphate at a molar ratio of 1:2.5 to obtain a compound with the structure shown in Formula I that has color change and reversible adhesion function. Formula II; Formula III; Formula IV; X1 is one of Cl, Br, or I.

3. The reversible adhesive that can quantify adhesion strength through color change as described in claim 2, characterized in that: The molar ratio of 4,4'-bipyridine to the intermediate product shown in Formula II is 1:0.3 to 0.5, the molar ratio of 4,4'-bipyridine to the intermediate product shown in Formula III is 1:0.3 to 0.5, and the mass amount of acetonitrile, based on the mass amount of 4,4'-bipyridine, is 0.5 to 0.8 g / g.

4. The reversible adhesive that can quantify adhesion strength through color change as described in claim 2, characterized in that: The method for preparing the compound represented by Formula II includes, Imidazole and the compound shown in Formula III were dissolved in anhydrous acetonitrile and mixed thoroughly. The resulting homogeneous solution was reacted at 30-80°C for 6-12 hours under a N2 atmosphere. After the reaction was completed, sodium carbonate was added to the solution and stirred for 1-2 hours. Then, dihalomethane was added and reacted at 0-50°C for 6-12 hours under a N2 atmosphere. The filtrate was obtained by filtration and washed thoroughly with ethyl acetate and anhydrous diethyl ether, respectively, to obtain the compound shown in Formula II.

5. The reversible adhesive that can quantify adhesion strength through color change as described in claim 4, characterized in that: The imidazole and the compound shown in Formula III are added in a molar ratio of 1:1.1; the volume of the acetonitrile is 5-10 mL / g based on the mass of the imidazole; the mass of the sodium carbonate is 0.5-2 g / g based on the mass of the imidazole; and the molar amount of the dihalomethane added is 0.4-0.6 mol / mol based on the amount of imidazole.

6. A method for preparing a reversible adhesive that can quantify adhesion strength through color change, characterized in that: The reversible adhesive that allows for the quantification of adhesion strength through color change is prepared through the following steps: The compound with color-changing and reversible adhesion function as shown in Formula I, the polymerizable monomer, the initiator, and the crosslinking agent are thoroughly stirred, mixed and dissolved to obtain a homogeneous and transparent solution; The above-mentioned uniform and transparent solution was injected into a mold, and a reversible adhesive that could quantify the adhesion strength by color change was prepared by photo-initiated polymerization.

7. The method for preparing the reversible adhesive that can quantify adhesion strength through color change as described in claim 6, characterized in that: The polymerizable monomers are hexyl methacrylate and hydroxyethyl methacrylate, the initiator is photoinitiator 1173, and the crosslinking agent is polyethylene glycol diacrylate.

8. The method for preparing the reversible adhesive that can quantify adhesion strength through color change as described in claim 7, characterized in that: In the polymerizable monomer, the mass ratio of hexyl methacrylate to hydroxyethyl methacrylate is 1:0.1~1.

9. The method for preparing a reversible adhesive that can quantify adhesion strength by color change as described in any one of claims 6 to 8, characterized in that: The amount of the compound with color-changing and reversible adhesion functions as shown in Formula I is 10-50% of the polymerizable monomer by mass, the amount of the photoinitiator is 0.5-5% of the polymerizable monomer by mass, and the amount of the crosslinking agent is 0.5-5% of the polymerizable monomer by mass.

10. The method for preparing the reversible adhesive that can quantify adhesion strength by color change as described in claim 9, characterized in that: The conditions for photoinitiated polymerization are a wavelength of 240–330 nm and a time of 0.5–3 h.

Citation Information

Patent Citations

  • Acrylic acid pressure-sensitive adhesive film with bidirectional electric control reversible adhesion function and preparation method of acrylic acid pressure-sensitive adhesive film

    CN121362533A