Polyamide oligomer composition and method for producing the same
A controlled depolymerization process for polyamide 66 produces a polyamide oligomer with defined properties, addressing inefficiencies in existing methods by enabling efficient impurity removal and controlled molecular weight, suitable for repolymerization and resource recycling.
Patent Information
- Application Number
- JP2023059838
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-16
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for depolymerizing polyamide 66 to recover monomers are inefficient, produce large amounts of side reactants that are difficult to remove, result in low molecular weight products with high solvent solubility, and have broad molecular weight distributions making impurity separation challenging, limiting their use as repolymerization raw materials.
A polyamide oligomer composition with a specific molecular weight range (250-800), COOH and NH2 group concentrations, and melting point (40-220°C) is produced by mixing polyamide, dicarboxylic acid, and water at controlled temperatures and pressures, allowing for solubility under high pressure and precipitation at normal conditions, thereby reducing impurities.
The method enables the production of a polyamide oligomer suitable for repolymerization with low impurity content, efficient solvent solubility, and controlled molecular weight, facilitating resource recycling and reducing global warming gas emissions.
Smart Images

Figure 2024147066000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyamide oligomer composition, a polyamide using the same, a molded article thereof, a method for producing a polyamide oligomer composition, and a method for producing a polyamide. [Background technology]
[0002] In recent years, interest in global environmental issues has increased, triggered by the marine plastic problem, and awareness of the need to build a sustainable society is spreading. Global environmental issues include global warming, resource depletion, and water shortages, many of which are caused by the rapid increase in resource consumption and greenhouse gas emissions due to human activity since the Industrial Revolution. Therefore, in order to build a sustainable society, technologies related to the recycling of fossil resources such as plastics and the reduction of greenhouse gas emissions are becoming increasingly important.
[0003] In particular, polyamide 66 is used in large quantities in various fields, including automobiles and electrical and electronic applications, and large amounts of greenhouse gases are emitted during the production of the monomer. Therefore, there is a demand for technology to return products containing polyamide 66 to the polymerization raw materials and recycle them.
[0004] As a technique for depolymerizing polyamides composed of diamines and dicarboxylic acids, such as polyamide 66, and returning them to monomers for recycling, a method of hydrolyzing them in the presence of an inorganic base compound, such as sodium hydroxide, at a temperature of, for example, 220°C, which is lower than the melting point of the polyamide, is known (see, for example, Patent Document 1).
[0005] Furthermore, as a method for depolymerizing polyamides consisting of diamines and dicarboxylic acids without using inorganic base compounds, a method has been disclosed in which polyamides are contacted with high-temperature, high-pressure water to recover the diamines and dicarboxylic acids, which are raw material monomers (see, for example, Patent Document 2 and Non-Patent Document 1). A method for depolymerizing using only water has the advantage of being a green recycling method since it does not require a step for removing additives such as sodium hydroxide and does not generate waste materials derived from additives. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Special Publication No. 7-507556 [Patent Document 2] JP 2001-302597 A [Non-patent literature]
[0007] [Non-Patent Document 1] Polymer Degradation and Stability 83 (2004) 389-393 Summary of the Invention [Problem to be solved by the invention]
[0008] However, the method disclosed in Patent Document 1 requires a long reaction time and produces a large amount of by-products (impurities) that are difficult to remove, so the resulting polyamide oligomer could not be used as a raw material for repolymerization.
[0009] Furthermore, in the method disclosed in Patent Document 2, the product obtained has a small average molecular weight and therefore high solubility in solvents, making it difficult to efficiently precipitate and recover the polyamide oligomer from the solution.
[0010] Furthermore, in the method disclosed in Non-Patent Document 1, the polyamide oligomer containing the monomer has a large molecular weight distribution and contains many components with different solvent solubilities, making it difficult to separate impurities or difficult to remove the large amount of by-products produced, and therefore the polyamide oligomer could not be used as a repolymerization raw material. [Means for solving the problem]
[0011] In order to solve the above problems, the present invention has the following configuration. [1] A polyamide oligomer composition comprising a polyamide oligomer represented by chemical formula (I) and having a number average molecular weight of 250 or more and 800 or less. Chemical formula (I):-[-CO-X-CO-NH-Y-NH-] z - (In the formula, X and Y each independently represent a residue containing at least one selected from a divalent aliphatic group having 2 to 20 carbon atoms, a divalent alicyclic group having 3 to 20 carbon atoms, and a divalent aromatic group having 6 to 20 carbon atoms. z is an integer of 1 to 3.) [2] The polyamide oligomer composition according to the above [1], having a COOH group concentration of 2.5 mol / kg or more and 8.0 mol / kg or less. [3] The polyamide oligomer composition according to the above [1], having an NH2 group concentration of 2.5 mol / kg or more and 8.0 mol / kg or less. [4] The polyamide oligomer composition according to [1] above, having a melting point of 40°C or higher and 220°C or lower as measured by differential thermal analysis. [5] A polyamide obtained by using the polyamide oligomer composition according to [1] above as a polymerization raw material. [6] A molded article obtained by molding the polyamide described in [5] above. [7] A method for producing the polyamide oligomer composition according to the above item [1], comprising the step of mixing at least polyamide (A), dicarboxylic acid and / or diamine (B), and solvent (C) at a temperature of 220°C or higher and 300°C or lower and at a pressure of 2 MPa or higher and 30 MPa or lower. [8] The method for producing a polyamide oligomer composition according to the above [7], wherein the solvent (C) is water. [9] The method for producing the polyamide oligomer composition according to the above [7], wherein the polyamide (A) is a polycondensation reaction product of a dicarboxylic acid and a diamine.
[10] The method for producing a polyamide oligomer composition according to the above [7], wherein the dicarboxylic acid and / or diamine (B) is a dicarboxylic acid or diamine constituting the polyamide (A).
[11] A method for producing a polyamide oligomer composition according to the above item [7], wherein when the dicarboxylic acid and / or diamine (B) is either a dicarboxylic acid or a diamine, the molar number of amide groups contained in the polyamide (A): the molar number of dicarboxylic acid or diamine=1:M is 0.45 or more and 0.95 or less.
[12] A method for producing a polyamide oligomer composition according to the above item [7], wherein, in the case where the dicarboxylic acid and / or diamine (B) is both a dicarboxylic acid and a diamine, the number of moles of amide groups contained in the polyamide (A) is the absolute value of the difference between the number of moles of dicarboxylic acid and the number of moles of diamine=1:N, and N is 0.45 or more and 0.95 or less.
[13] The method for producing the polyamide oligomer composition according to [7] above, further comprising a step of recovering the polyamide oligomer composition as a solid by solid-liquid separation.
[14] The method for producing the polyamide oligomer composition according to the above [7], wherein the polyamide (A) is a waste product.
[15] A method for producing a polyamide, comprising the following steps (1) and (2) in this order:
[0012] (1) A step of mixing the polyamide oligomer composition according to claim 1 with a diamine and / or a dicarboxylic acid in a solvent to prepare a salt solution. (2) Polycondensing the salt solution prepared in step (1) Effect of the Invention
[0013] According to the present invention, there can be provided a polyamide oligomer composition which can be suitably used as a raw material for repolymerization, which is compatible with solubility under high temperature and pressure and precipitation under normal temperature and pressure, and which contains few impurities, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will now be described in further detail.
[0015] The polyamide oligomer composition of the present invention contains a polyamide oligomer represented by chemical formula (I) and has a number average molecular weight of 250 or more and 800 or less. Chemical formula (I):-[-CO-X-CO-NH-Y-NH-] z -
[0016] In the formula, X and Y each independently represent a residue containing at least one selected from a divalent aliphatic group having 2 to 20 carbon atoms, a divalent alicyclic group having 3 to 20 carbon atoms, and a divalent aromatic group having 6 to 20 carbon atoms. z is an integer of 1 to 3.
[0017] The polyamide oligomer represented by chemical formula (I) in the present invention has a structure in which a diamine and a dicarboxylic acid are polycondensed.
[0018] The diamine includes an aliphatic diamine, an alicyclic diamine, an aromatic diamine, and the like.
[0019] Examples of the aliphatic diamine include ethylenediamine, trimethylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, tridecanediamine, tetradecanediamine, pentadecanediamine, hexadecanediamine, heptadecanediamine, octadecanediamine, nonadecanediamine, eicosanediamine, 2-methyl-1,5-diaminopentane, 2-methyl-1,8-diaminooctane, and 2,2,4- / 2,4,4-trimethylhexamethylenediamine.
[0020] Examples of alicyclic diamines include cyclohexanediamine, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, bis(4-aminocyclohexyl)methane, bis(3-methyl-4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, bis(aminopropyl)piperazine, and aminoethylpiperazine.
[0021] Examples of the aromatic diamine include metaxylylenediamine and paraxylylenediamine.
[0022] Among these, the diamines preferably include tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, octadecanediamine, and nonadecanediamine.
[0023] Examples of the dicarboxylic acid include an aliphatic dicarboxylic acid, an alicyclic dicarboxylic acid, and an aromatic dicarboxylic acid.
[0024] Examples of the aliphatic dicarboxylic acid include succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, and tetradecanedioic acid.
[0025] Examples of the alicyclic dicarboxylic acid include 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, and 1,3-cyclopentanedicarboxylic acid.
[0026] Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 5-sodium sulfoisophthalic acid, hexahydroterephthalic acid, and hexahydroisophthalic acid.
[0027] Among these, the dicarboxylic acids preferably include adipic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, and terephthalic acid.
[0028] The polyamide oligomer represented by chemical formula (I) in the present invention may contain, as raw materials, in addition to the above diamines and dicarboxylic acids, amino acids such as 6-aminocaproic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, and para-aminomethylbenzoic acid, and lactams such as ε-caprolactam, ω-undecanelactam, and ω-laurolactam, in an amount of 20% by weight or less in the polyamide oligomer composition.
[0029] The polyamide oligomer composition of the present invention has a number average molecular weight of 250 or more and 800 or less. In the present invention, the number average molecular weight of the polyamide oligomer composition is calculated according to formula (II) using the concentration (mol / kg) of the COOH group and the concentration (mol / kg) of the NH2 group, which are the terminal groups of the polyamide oligomer composition in a dry state. Formula (II): [Number average molecular weight] = 1000 / (([COOH group concentration] + [NH2 group concentration]) / 2)
[0030] The COOH group concentration and NH2 group concentration of the polyamide oligomer composition of the present invention are measured by the method described in the Examples. In the method described in the Examples, the polyamide oligomer composition is measured in amounts of 0.010 g and 0.500 g, but the acid solution or alkali solution used in the method is a poor solvent for the polyamide oligomer. Therefore, if the amount of the polyamide oligomer composition used in the terminal group concentration measurement is too large, the polyamide oligomer will precipitate, and the terminal group concentration cannot be measured accurately. For example, it is expected that the polyamide oligomer obtained by depolymerizing polyamide with dicarboxylic acid has a high COOH group concentration. In such a case, the amount of the polyamide oligomer composition used in the terminal group concentration measurement can be reduced to prevent the precipitation of the polyamide oligomer during titration. In this way, for the purpose of accurately measuring the terminal group concentration of the polyamide oligomer composition, the amount of the polyamide oligomer composition used in the terminal group concentration measurement can be changed in the range of 0.010 to 0.500 g.
[0031] A particularly preferred method for using the polyamide oligomer composition of the present invention as a repolymerization raw material is to dissolve the polyamide oligomer composition in a solvent and precipitate the polyamide oligomer from the solution in order to remove impurities contained in the depolymerized polyamide. In order to achieve both of these, the number average molecular weight must be 250 or more and 800 or less. By setting the number average molecular weight in this range, a polyamide oligomer composition with high hot water solubility can be obtained, and the polyamide oligomer composition can be efficiently precipitated from the solution by lowering the temperature. It is preferably 300 or more, more preferably 350 or more. On the other hand, it is preferably 700 or less, more preferably 600 or less, and particularly preferably 550 or less.
[0032] Furthermore, the polyamide oligomer composition of the present invention is preferably represented by chemical formula (III). Chemical formula (III): P-[-CO-X-CO-NH-Y-NH-] z -Q
[0033] In the formula, X and Y each independently represent a residue containing at least one selected from a divalent aliphatic group having from 2 to 20 carbon atoms, a divalent alicyclic group having from 3 to 20 carbon atoms, and a divalent aromatic group having from 6 to 20 carbon atoms; z represents an integer of from 1 to 3; the terminal group structure P is -OH or -NH-Y-NH2; and the terminal group structure Q is -H or -CO-X-COOH.
[0034] The above-mentioned terminal group structure allows efficient precipitation from the solution of the polyamide oligomer composition. Among them, the terminal group structure P is more preferably -OH, and the terminal group structure Q is more preferably -CO-X-COOH. The polyamide oligomer composition may be a mixture of multiple polyamide oligomers having different structures of X and Y as shown in formula (III).
[0035] Therefore, the COOH group concentration and NH2 group concentration of the polyamide oligomer composition of the present invention are not particularly limited as long as they are in a range that satisfies the number average molecular weight of 250 to 800, and can take any value corresponding to the terminal structures P and Q in the chemical formula (III). For example, when the polyamide oligomer having the terminal structure P of -OH and Q of -CO-X-COOH is the main component, the COOH group concentration is preferably 2.5 mol / kg to 8.0 mol / kg. The COOH group concentration and the NH2 group concentration are calculated as the molar equivalent of the COOH group or NH2 group per 1 kg of the polyamide oligomer composition. By setting the concentration in this range, the polyamide oligomer composition can be dissolved in a solvent and precipitated by lowering the temperature, thereby efficiently removing the by-products. It is more preferable that the concentration is 3.0 mol / kg or more, and even more preferable that the concentration is 3.5 mol / kg or more. On the other hand, it is more preferable that the concentration is 7.0 mol / kg or less, and even more preferable that the concentration is 6.0 mol / kg or less.
[0036] In addition, when the main component is a polyamide oligomer having an end structure P of -NH-Y-NH2 and Q of -H, the NH2 group concentration is preferably 2.5 mol / kg or more and 8.0 mol / kg or less. By setting it in this range, the polyamide oligomer composition can be dissolved in a solvent and precipitated by lowering the temperature, thereby efficiently removing by-products. It is more preferably 3.0 mol / kg or more, and even more preferably 3.5 mol / kg or more. On the other hand, it is more preferably 7.0 mol / kg or less, and even more preferably 6.0 mol / kg or less.
[0037] The polyamide oligomer composition of the present invention may contain components other than polyamide oligomers as long as the number average molecular weight is within a range of 250 to 800. Examples of components other than polyamide oligomers include diamines, dicarboxylic acids, lactams, and amino acids. Among them, dicarboxylic acids or diamines, which are components of polyamide oligomers, are preferred. A polyamide oligomer composition containing such dicarboxylic acids or diamines can be used as a polyamide homopolymer raw material because the polyamide produced by providing the composition as a polymerization raw material is a polycondensation product consisting of a single dicarboxylic acid and a single diamine. The content of polyamide oligomer in the polyamide oligomer composition is preferably 50% by weight or more, more preferably 80% by weight or more.
[0038] The melting point of the polyamide oligomer composition of the present invention measured by differential thermal analysis is preferably 40°C or more and 220°C or less. By controlling it within this range, the polyamide oligomer composition can be easily dissolved in a solvent, and by lowering the temperature to precipitate it, it is possible to easily and efficiently remove by-products. The melting point is more preferably 50°C or more, even more preferably 80°C or more, and particularly preferably 100°C or more. On the other hand, the melting point is more preferably 213°C or less, and even more preferably 209°C or less. The melting point of the polyamide oligomer composition is measured by the method described in the Examples.
[0039] The method for producing the polyamide oligomer composition of the present invention is a method for producing the polyamide oligomer composition of the present invention, and includes a step of mixing polyamide (A), dicarboxylic acid and / or diamine (B), and solvent (C) at a temperature of 220°C or higher and 300°C or lower and at a pressure of 2 MPa or higher and 30 MPa or lower.
[0040] In the method for producing a polyamide oligomer composition of the present invention, the polyamide (A) is preferably a polycondensation reaction product of a dicarboxylic acid and a diamine. Here, "a polycondensation reaction product of a dicarboxylic acid and a diamine" means that the content of the structural unit obtained by polycondensing the diamine and the dicarboxylic acid in the total structural units of the polyamide is 50 mol% or more. The content of the structural unit is preferably 80 mol% or more. Representative examples of the dicarboxylic acid and the diamine include the above-mentioned dicarboxylic acid and diamine. Among them, polyamides that are polycondensation reaction products of aliphatic diamines such as tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, octamethylenediamine, nonamethylenediamine, and decamethylenediamine and aliphatic dicarboxylic acids such as adipic acid, sebacic acid, undecanedioic acid, and dodecanedioic acid are particularly preferred for the purpose of increasing the production rate of the polyamide oligomer represented by the chemical formula (I) by depolymerizing the polyamide. In the present invention, two or more kinds of polyamide homopolymers or copolymers, which are polycondensation products of these dicarboxylic acids and diamines, may be blended.
[0041] In addition to the above dicarboxylic acids and diamines, the raw materials for the polyamide (A) in the present invention may include amino acids such as 6-aminocaproic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, and para-aminomethylbenzoic acid, and lactams such as ε-caprolactam, ω-undecanelactam, and ω-laurolactam, in an amount of 20% by weight or less in the polyamide (A).
[0042] Specific examples of polyamide (A) include polyhexamethylene adipamide (nylon 66), polytetramethylene adipamide (nylon 46), polytetramethylene sebacamide (nylon 410), polypentamethylene adipamide (nylon 56), polypentamethylene sebacamide (nylon 510), polyhexamethylene sebacamide (nylon 610), polyhexamethylene dodecamide (nylon 612), polydecamethylene adipamide (nylon 106), polydecamethylene sebacamide (nylon 1 010), Polydecamethylene dodecamide (Nylon 1012), Polycaproamide / Polyhexamethylene adipamide Copolymer (Nylon 6 / 66), Polycaproamide / Polyhexamethylene terephthalamide Copolymer (Nylon 6 / 6T), Polyhexamethylene adipamide / Polyhexamethylene terephthalamide Copolymer (Nylon 66 / 6T), Polyhexamethylene adipamide / Polyhexamethylene isophthalamide Copolymer (Nylon 66 / 6I), Polyhexamethylene terephthalamide / Polyhexamethylene isophthalamide copolymer (nylon 6T / 6I), polyhexamethylene terephthalamide / polydodecanamide copolymer (nylon 6T / 12), polyhexamethylene adipamide / polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (nylon 66 / 6T / 6I), polyxylylene adipamide (nylon XD6), polyxylylene sebacamide (nylon XD10), polyhexamethylene terephthalamide / polypentamethylene terephthalamide Examples of such copolymers include Nylon 6T / 5T, polyhexamethylene terephthalamide / poly-2-methylpentamethylene terephthalamide copolymer (Nylon 6T / M5T), polypentamethylene terephthalamide / polydecamethylene terephthalamide copolymer (Nylon 5T / 10T), polynonamethylene terephthalamide (Nylon 9T), polydecamethylene terephthalamide (Nylon 10T), polydodecamethylene terephthalamide (Nylon 12T), and copolymers thereof. Two or more of these may be blended. Here, " / " indicates a copolymer.
[0043] The polyamide (A) of the present invention may be blended with a polymerization catalyst, other polymers, a filler, various additives, etc., within the scope of not impairing the object of the present invention.
[0044] Examples of the polymerization catalyst include inorganic phosphorus compounds such as phosphoric acid, phosphorous acid, hypophosphorous acid, pyrophosphoric acid, polyphosphoric acid, and alkali metal salts and alkaline earth metal salts thereof.
[0045] Examples of other polymers include polyolefins such as polyethylene and polypropylene, modified polyolefins such as (co)polymers obtained by polymerizing olefin compounds and / or conjugated diene compounds, elastomers such as polyamide elastomers and polyester elastomers, polyesters, polycarbonates, polyphenylene ethers, polyphenylene sulfides, liquid crystal polymers, polysulfones, polyethersulfones, ABS, SAN, polystyrene, polyurethanes, etc. Two or more of these may be blended.
[0046] Examples of the filler include fibrous inorganic fillers such as glass fiber, carbon fiber, potassium titanate whisker, zinc oxide whisker, aluminum borate whisker, aramid fiber, alumina fiber, silicon carbide fiber, ceramic fiber, asbestos fiber, gypsum fiber, and metal fiber, and non-fibrous inorganic fillers such as wollastonite, zeolite, sericite, kaolin, mica, talc, clay, pyrophyllite, bentonite, montmorillonite, asbestos, aluminosilicate, alumina, silicon oxide, magnesium oxide, zirconium oxide, titanium oxide, iron oxide, calcium carbonate, magnesium carbonate, dolomite, calcium sulfate, barium sulfate, magnesium hydroxide, calcium hydroxide, aluminum hydroxide, glass beads, ceramic beads, boron nitride, silicon carbide, and silica. Two or more of these may be blended.
[0047] Various additives include antioxidants and heat stabilizers (hindered phenols, hydroquinones, phosphites and their substitutes, copper halides, iodine compounds, etc.), weathering agents (resorcinols, salicylates, benzotriazoles, benzophenones, hindered amines, etc.), release agents and lubricants (aliphatic alcohols, aliphatic amides, aliphatic bisamides, bisureas, polyethylene wax, etc.), pigments (cadmium sulfide, phthalocyanine, carbon black, etc.), dyes (nigrosine, aniline black, etc.), plasticizers (octyl p-oxybenzoate, N-butyl ether, etc.), and other additives. Examples of suitable antistatic agents include alkylbenzenesulfonamide, antistatic agents (alkyl sulfate-type anionic antistatic agents, quaternary ammonium salt-type cationic antistatic agents, nonionic antistatic agents such as polyoxyethylene sorbitan monostearate, betaine-type amphoteric antistatic agents, etc.), and flame retardants (melamine cyanurate, hydroxides such as magnesium hydroxide and aluminum hydroxide, ammonium polyphosphate, brominated polystyrene, brominated polyphenylene oxide, brominated polycarbonate, brominated epoxy resin, or combinations of these brominated flame retardants with antimony trioxide, etc.). Two or more of these may be blended.
[0048] In the method for producing a polyamide oligomer composition of the present invention, the polyamide (A) may be waste. When the polyamide (A) is waste, fossil resources can be recycled. Furthermore, since there is no need to incinerate the waste, the amount of greenhouse gas emissions can be reduced. Examples of waste include industrial waste generated in the manufacturing process of polyamide products, used waste of polyamide products, etc. Specific examples of industrial waste generated in the manufacturing process of polyamide products include product waste, pellet waste, lump waste, cutting waste during product processing, cutting waste, etc. generated in the manufacturing process of polyamide products. Specific examples of polyamide products include resin molded products such as electric / electronic device parts, automobile parts, and machine parts, fibers such as clothing / industrial materials, and films and sheets such as packaging materials.
[0049] In the method for producing a polyamide oligomer composition of the present invention, products other than the polyamide (A) may be subjected to the method for producing a polyamide oligomer composition of the present invention, as long as the effects of the present invention are not impaired.
[0050] The polyamide oligomer composition of the present invention can be produced, for example, by reacting a depolymerized product of polyamide (A) with a dicarboxylic acid and / or a diamine (B).
[0051] Examples of the dicarboxylic acid or diamine (B) include the dicarboxylic acids and diamines described above.
[0052] In the method for producing a polyamide oligomer composition of the present invention, the dicarboxylic acid and / or diamine (B) is preferably the dicarboxylic acid or diamine constituting the polyamide (A). By using the dicarboxylic acid or diamine constituting the polyamide (A), the produced polyamide oligomer becomes a polycondensation product consisting of a single dicarboxylic acid and a single diamine, and can be used as a polyamide homopolymer raw material.
[0053] In the method for producing a polyamide oligomer composition of the present invention, when the dicarboxylic acid and / or diamine (B) is only one of dicarboxylic acid and diamine, the molar number of amide groups contained in the polyamide (A): the molar number of dicarboxylic acid or diamine (B) = 1:M, M is preferably 0.45 or more and 0.95 or less. By setting M in this range, one of the COOH group concentration and the NH2 group concentration in the system becomes excessive relative to the other, and it becomes easy to avoid high molecular weight due to polycondensation reaction after depolymerization. Therefore, it becomes easy to control the average molecular weight of the obtained polyamide oligomer to 250 or more and 800 or less. M is more preferably 0.50 or more. On the other hand, M is preferably 0.95 or less, more preferably 0.80 or less, even more preferably 0.70 or less, and particularly preferably 0.60 or less.
[0054] In the method for producing a polyamide oligomer composition of the present invention, when the dicarboxylic acid and / or diamine (B) is both a dicarboxylic acid and a diamine, the mole number of amide groups contained in the polyamide (A): the absolute value of the difference between the mole number of dicarboxylic acid and the mole number of diamine = 1:N, N is preferably 0.45 or more and 0.95 or less. By setting N in this range, even when both dicarboxylic acid and diamine are contained, one of the COOH group concentration and the NH2 group concentration in the system can be made excessive relative to the other. Therefore, as in the case where only one of dicarboxylic acid or diamine is contained, it is easy to control the average molecular weight of the obtained polyamide oligomer to 250 or more and 800 or less. N is more preferably 0.50 or more. On the other hand, N is more preferably 0.80 or less, further preferably 0.70 or less, and particularly preferably 0.60 or less.
[0055] The method for producing a polyamide oligomer composition of the present invention includes a step of mixing a solvent (C). The solvent (C) is not particularly limited, but it is particularly preferable that the solvent (C) is water in the method for producing a polyamide oligomer composition of the present invention. By using water as the solvent (C), a polyamide oligomer having a structure in which the terminal group is selected from a COOH group and an NH2 group can be obtained. There is no particular limitation on the water, and any water such as tap water, deionized water, distilled water, and well water may be used. From the viewpoint of suppressing side reactions due to the influence of coexisting salts, it is preferable that the water is deionized water or distilled water.
[0056] The amount of the solvent (C) added is not particularly limited, but is preferably 12 times or less, more preferably 6 times or less, and even more preferably 4 times or less, based on the weight of the polyamide (A). On the other hand, it is preferably 1 time or more, and more preferably 1.5 times or more. By setting the amount of the solvent (C) relative to the weight of the polyamide (A) within the above range, it is possible to achieve both efficient production of the polyamide oligomer and energy saving. In particular, when the solvent (C) is water, it has a larger specific heat capacity (4.3 kJ / kg·K) and heat of vaporization (2,250 kJ / kg) than organic solvents, so setting the amount of water added within the above range can contribute to the recycling of fossil resources and the reduction of greenhouse gas emissions.
[0057] In the method for producing a polyamide oligomer composition of the present invention, the temperature in the step of mixing polyamide (A) and the like is preferably 220°C or higher and 300°C or lower. By mixing at the above temperature, the depolymerization reaction of polyamide (A) is likely to occur. In the present invention, the above temperature may be referred to as the reaction temperature. The reaction temperature refers to the temperature during which polyamide (A), dicarboxylic acid and / or diamine (B), and solvent (C) are reacted for a certain period of time in a temperature-controlled reaction vessel. By setting the reaction temperature at 220°C or higher, particularly when the solvent (C) is water, water can be maintained in a subcritical state, and the efficiency of hydrolysis and depolymerization of polyamide (A) can be improved, while the polycondensation reaction between the depolymerized product and dicarboxylic acid and / or diamine (B) can be rapidly promoted. In addition, by setting the reaction temperature at 300°C or lower, undesirable reactions such as thermal decomposition and side reactions of diamines and dicarboxylic acids can be suppressed. In addition, water preferably used as the solvent (C) is in a state that is neither liquid nor gas when it reaches a pressure of 22.1 MPa and a temperature of 374.2°C. Water in this state is called supercritical water. Supercritical water has the characteristics of having both the solubility of a liquid and the diffusibility of a gas, and is therefore attracting attention as a reaction field for decomposing polymer waste. In addition, hot water in the vicinity of the critical point of a temperature and pressure slightly lower than the critical point of water is called subcritical water. Although subcritical water is water, it has the characteristics of a low dielectric constant and a high ionic product. The dielectric constant and ionic product of subcritical water depend on the temperature and partial pressure of water, and can be controlled. By controlling the dielectric constant low, subcritical water becomes an excellent solvent for organic compounds, despite being water. In addition, by controlling the ionic product high, the hydrogen ion and hydroxide ion concentrations become high, and therefore subcritical water has an excellent hydrolysis effect.
[0058] The reaction temperature may be a constant temperature or may be changed over time. There are no particular limitations on the temperature during the temperature increase process until the reaction temperature is reached or during the cooling process after mixing and reacting at the reaction temperature, as long as the temperature does not exceed the reaction temperature.
[0059] In addition, the pressure in the step of mixing the polyamide (A) and the like, that is, the pressure during the depolymerization reaction of the polyamide (A), is preferably higher than the saturated vapor pressure at the reaction temperature of the solvent (C). By making the pressure higher than the saturated vapor pressure, the solvent can be maintained in a liquid state, and the reaction efficiency can be improved. In the above-mentioned preferred reaction temperature range, in the method for producing a polyamide oligomer composition of the present invention, the pressure in the step of mixing the polyamide (A) and the like is preferably 2 MPa or more and 30 MPa or less. As a method for setting the pressure within this range, for example, a method of pressurizing the inside of a pressure vessel and sealing it can be mentioned. As a method for pressurizing the inside of a pressure vessel, for example, a method of sealing a gas in addition to the polyamide (A), the dicarboxylic acid or diamine (B), and the solvent (C), a method of pressurizing and introducing the solvent (C), and the like can be mentioned. As the gas to be sealed, for example, air, argon, nitrogen, and the like can be mentioned. From the viewpoint of suppressing side reactions such as oxidation reactions, it is preferable to use nitrogen or argon as the gas to be sealed. The degree of gas pressurization is not particularly limited since it is set to the desired pressure, but it can be 0.3 MPa or more. When the solvent (C) is introduced under pressure, it is possible to keep the inside of the pressure vessel free of gas.
[0060] In the method for producing a polyamide oligomer composition of the present invention, the reaction time of polyamide (A), dicarboxylic acid and / or diamine (B), and solvent (C) is not particularly limited, but a preferable lower limit is 0.1 minutes, and a preferable upper limit is 120 minutes. The reaction time here refers to the total time during which polyamide (A), dicarboxylic acid and / or diamine (B), and solvent (C) are mixed in a reaction vessel under conditions of 220°C to 300°C and 2MPa to 30MPa. The reaction time includes the time during which polyamide (A), dicarboxylic acid and / or diamine (B), and solvent (C) are mixed in the reaction vessel at the above temperature range and pressure range, including the temperature and pressure increase process until the desired conditions are reached and the cooling process after the reaction. If the reaction time is not too long, side reactions (such as amino group elimination reaction) of the depolymerized product of polyamide (A) are less likely to proceed, and the depolymerized product is less likely to be converted into a compound that cannot be used as a polyamide raw material, which is preferable. The reaction time is preferably 120 minutes or less, more preferably 60 minutes or less. On the other hand, if the reaction time is 0.1 minutes or more, the hydrolysis depolymerization reaction of the polyamide (A) can be easily carried out sufficiently, and the number average molecular weight of the polyamide oligomer composition can be easily controlled. The reaction time is preferably 0.1 minutes or more, more preferably 1 minute or more, and even more preferably 3 minutes or more.
[0061] In the present invention, the polyamide (A), the dicarboxylic acid and / or diamine (B), and the solvent (C) can be contacted by various known reaction methods such as batch and continuous. For example, in the case of batch, autoclaves, vertical and horizontal reactors, and vertical and horizontal reactors equipped with a stirrer and a heating function as well as a compression mechanism such as a cylinder can be used. In the case of continuous, extruders, tubular reactors, tubular reactors equipped with a mixing mechanism such as a baffle, line mixers, vertical and horizontal reactors, vertical and horizontal reactors equipped with a stirrer, and towers can be used. In addition, the production atmosphere is preferably a non-oxidizing atmosphere, and is preferably carried out under an inert atmosphere such as nitrogen, helium, and argon, and is preferably carried out under a nitrogen atmosphere from the viewpoints of economy and ease of handling.
[0062] There is no particular limitation on the method for recovering the polyamide oligomer composition of the present invention as a solid, and any method can be adopted. For example, when the depolymerization reaction of polyamide (A) is carried out in a batch manner, the depolymerization reaction is discharged after completion of the depolymerization reaction, and a reaction mixture containing a polyamide oligomer, that is, a liquid polyamide oligomer composition, can be obtained. In addition, when the depolymerization reaction is carried out in a continuous manner, a liquid polyamide oligomer composition can be obtained as the reaction proceeds. The liquid polyamide oligomer composition can be obtained in the form of, for example, an aqueous solution, a colloidal liquid, a slurry liquid, a paste liquid, etc., depending on the properties, the content of the polyamide oligomer, and the temperature during recovery. From among them, the solid polyamide oligomer composition can be recovered as a solid by a known method such as solid-liquid separation or extraction after precipitating as a solid component at least at room temperature by cooling.
[0063] In particular, the method for producing the polyamide oligomer composition of the present invention preferably further comprises a step of recovering the polyamide oligomer composition as a solid by solid-liquid separation. The polyamide oligomer composition of the present invention is usually precipitated as a solid component at least at room temperature by cooling, so that it can be recovered as a solid by solid-liquid separation. Examples of the solid-liquid separation method include separation by filtration, centrifugation, and decantation. Note that this series of treatments can be repeated several times as necessary. The liquid phase containing the unreacted dicarboxylic acid and / or diamine (B) separated by solid-liquid separation may be used again to treat the polyamide (A). In order to remove impurities in the polyamide oligomer composition, purification may be performed by a known method such as crystallization.
[0064] The method for producing a polyamide of the present invention includes the following steps (1) and (2) in this order.
[0065] (1) A step of mixing the polyamide oligomer composition of the present invention with a diamine and / or a dicarboxylic acid in a solvent to prepare a salt solution. (2) A step of polycondensing the salt solution prepared in step (1).
[0066] The polyamide of the present invention is made by using the polyamide oligomer composition of the present invention as a polymerization raw material. The polyamide oligomer composition of the present invention is particularly preferably composed of a polyamide oligomer consisting of a dicarboxylic acid structure having COOH groups at both ends, a diamine structure having NH2 groups at both ends, or an amino acid structure having a COOH group at one end and an NH2 group at the other end. Depending on the total COOH group concentration and the total NH2 group concentration in the polyamide oligomer composition containing these, a diamine and / or a dicarboxylic acid are mixed in a solvent to prepare a salt solution in which the molar ratio of the COOH group concentration and the NH2 group concentration contained in the polymerization raw material is adjusted, and the salt solution is polycondensed to produce a polyamide. A plurality of polyamide oligomers having different structures of X and Y represented by formula (I) may be mixed and used as a raw material for the polyamide. The polyamide oligomer composition of the present invention may also be used as a minor component (less than 50% by weight) of the polymerization raw material. The molar ratio of the COOH group concentration to the NH2 group concentration contained in the polymerization raw material is preferably 0.8 to 1.2, more preferably 0.9 to 1.1, and even more preferably 1.0. When the polyamide oligomer composition is produced by depolymerizing polyamide, the obtained polyamide can be an environmentally friendly recycled material that contributes to resource recycling and reduction of greenhouse gas emissions.
[0067] The molded article of the present invention is obtained by molding the polyamide of the present invention. The molded article of the present invention can be obtained by molding the polyamide of the present invention into a desired shape by any melt molding method such as injection molding, extrusion molding, blow molding, vacuum molding, melt spinning, film molding, etc. The molded article of the present invention can be suitably used as, for example, resin molded products such as electric / electronic device parts, automobile parts, and machine parts, fibers such as clothing and industrial materials, and films and sheets such as packaging materials. EXAMPLES
[0068] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0069] The following raw materials were used in each example.
[0070] (A-1) Polyamide 66: "Amilan" (registered trademark) CM3001-N manufactured by Toray Industries, Inc. (A-2) Polyamide 610: "Amilan" (registered trademark) CM2001 manufactured by Toray Industries, Inc. (B-1) Adipic acid: Wako Pure Chemical Industries, Ltd., special grade (B-2) Sebacic acid: manufactured by Tokyo Chemical Industry Co., Ltd. Hexamethylenediamine: Wako Pure Chemical Industries, Ltd., Grade 1.
[0071] Evaluation method (1) COOH group concentration of polyamide oligomer composition The polyamide oligomer composition was precisely weighed out in an amount of 0.010 g, dissolved in 20 ml of benzyl alcohol at 190° C., and titrated with a 0.02 N ethanol solution of potassium hydroxide to determine the molecular weight.
[0072] (2) NH2 group concentration of polyamide oligomer composition The polyamide oligomer composition was precisely weighed out at 0.500 g, dissolved in 25 ml of a phenol-ethanol mixed solvent (volume ratio of 83.5:16.5), and titrated with a 0.02 N aqueous hydrochloric acid solution to determine the content.
[0073] (3) Melting point of polyamide oligomer composition The polyamide oligomer composition was heated under a nitrogen flow from 40°C to 300°C at a heating rate of 10°C / min using a differential thermal analyzer (TG / DTA7200 manufactured by Hitachi High-Tech Science), and the temperature of the endothermic peak that appeared was taken as the melting point. However, when two or more endothermic peaks were detected, the temperature of the endothermic peak detected on the highest temperature side was taken as the melting point.
[0074] (4) Relative viscosity (ηr) The relative viscosity of the polyamide was measured in 98% sulfuric acid at a concentration of 0.01 g / mL at 25° C. using an Ostwald viscometer.
[0075] [Example 1] Into a SUS316L autoclave equipped with a stirrer, 12.02 g of (A-1) polyamide 66, 8.04 g of (B-1) adipic acid, and 58.67 g of deionized water were charged. The number of moles of (B-1) adipic acid was 0.52 times the number of moles of amide groups in (A-1) polyamide 66.
[0076] The reaction vessel was replaced with nitrogen, and the vessel was sealed under a nitrogen pressure of 0.5 MPa, and the reaction was carried out by holding the vessel at 280°C for 15 minutes while stirring at 200 rpm. The pressure in the system during the reaction was 6.2 MPa. The total time for mixing (A-1) polyamide 66, (B-1) adipic acid, and water in the reaction vessel at 250°C or higher was 30 minutes. The mixture was cooled to 80°C, and the entire amount was obtained as a slurry liquid reaction mixture, i.e., a liquid polyamide oligomer composition. The obtained liquid polyamide oligomer composition was subjected to solid-liquid separation by vacuum filtration, and the solid content was washed with warm water at 40°C, to recover the polyamide oligomer composition as a solid.
[0077] The number of carboxyl terminal groups calculated from the terminal group titration of the recovered polyamide oligomer composition was 4.48 mol / kg, the number of amine terminal groups was 0 mol / kg, and the number average molecular weight calculated from formula (II) was 446. The melting point determined from DTA measurement was 205°C.
[0078] [Examples 2 to 6, Comparative Examples 1 to 3] The depolymerization was carried out in the same manner as in Example 1, but the amounts and / or types of polyamide, dicarboxylic acid, and deionized water, the reaction temperature, and the reaction time were changed, and the polyamide was decomposed. In Comparative Examples 1 and 2, a part of the reaction mixture was fixed in the reaction vessel, so only the slurry liquid portion was collected. The reaction conditions, the yield of the reaction product, and the analysis results are shown in Table 1.
[0079] [Table 1]
[0080] From Examples 1 to 6, it was found that mixing polyamide with dicarboxylic acid and water can convert it into a polyamide oligomer composition having a number average molecular weight in the range of 250 to 800. In addition, the obtained polyamide oligomer composition had a COOH group amount in a preferred range, and did not show the melting point (>220°C) of poorly soluble components such as cyclic oligomers and long-chain polyamide oligomers, and therefore was found to be a polyamide oligomer composition with a low impurity content.
[0081] Furthermore, in Examples 1 to 6, the polyamide oligomer composition was uniformly precipitated in the reaction mixture, and the entire reaction mixture was obtained as a slurry liquid. When the polyamide oligomer composition has poor solubility under high temperature and pressure, as in Comparative Examples 1 and 2, it is phase-separated into a mass and then cooled and solidified, so that a part of it is collected in a state of adhering to the wall surface or stirring blade in the reaction vessel, and the entire amount cannot be obtained as a slurry liquid. Therefore, it was determined that Examples 1 to 6 were able to achieve both solubility under high temperature and pressure and precipitation under normal temperature and pressure.
[0082] In Comparative Example 1, in which (A-1) polyamide 66 was contacted with only deionized water, and in Comparative Example 2, in which a small amount of (B-1) adipic acid was added during depolymerization, the number average molecular weight of the obtained polyamide oligomer composition was high, and the hot water solubility was inferior to that of the polyamide oligomer compositions of Examples 1 to 4 and 6. It is presumed that high molecular weight polyamide oligomers with poor hot water solubility solidify while retaining impurities during the cooling process, making it impossible to remove the impurities.
[0083] In Comparative Example 3, in which the reaction was carried out under the same conditions as in Example 1 except that the reaction temperature was changed to 320°C, the recovered solid polyamide oligomer had a high number average molecular weight of 1450, was colored red, and showed a significantly low melting point of 154°C. In Comparative Example 3, since the reaction temperature was high, it is presumed that the repolymerization reaction proceeded in addition to the depolymerization reaction, making it difficult to control the molecular weight. In addition, the amount of oligomer obtained in Comparative Example 3 was clearly smaller than that in Examples 1 to 5. This is considered to be because the acidity of the subcritical water was increased by the reaction at a high temperature, and the polyamide oligomer was further decomposed, resulting in an increase in the proportion of water-soluble components having the structure HO-CO-(-CH2-)4-CO-NH-(-CH2-)6-NH2. In this way, the polyamide oligomer composition, which is high molecular weight by the repolymerization reaction while containing impurities generated by the thermal decomposition reaction, is difficult to separate and remove the impurities, and therefore it is considered impossible to use it for recycling.
[0084] In this way, it was found that by mixing polyamide with dicarboxylic acid and / or diamine, and water at 220°C to 300°C and 2 MPa to 30 MPa, the polyamide can be hydrolyzed to obtain a polyamide oligomer composition with a specific structure.
[0085] [Reference example 1] (B-1) 6.98 g of adipic acid and 5.55 g of hexamethylenediamine were dissolved in 12.5 g of deionized water to prepare a salt solution. The salt solution was transparent. This salt solution was charged into a reaction vessel, sealed, and substituted with nitrogen. The heater on the outer periphery of the reaction vessel was set to a temperature of 290°C, and heating was started. After the pressure inside the vessel reached 1.75 MPa, the pressure inside the vessel was maintained at 1.75 MPa while releasing moisture to the outside of the system, and the temperature inside the vessel was raised to 230°C. After the temperature inside the vessel reached 230°C, the pressure inside the vessel was adjusted to normal pressure over 1 hour (temperature inside the vessel when normal pressure was reached: 270°C). Subsequently, the vessel was maintained for 60 minutes while flowing nitrogen (nitrogen flow) to obtain polyamide 66 (maximum temperature reached: 277°C). The relative viscosity of the obtained polyamide 66 was 2.78, and the melting point was 261°C.
[0086] [Example 7] Polyamide 66 was produced in the same manner as in Reference Example 1, except that 9.95 g of the polyamide oligomer composition obtained in the same manner as in Example 1 and 2.58 g of hexamethylenediamine were used as polymerization raw materials. The relative viscosity of the resulting recycled polyamide 66 was 2.79 and the melting point was 261°C.
[0087] [Comparative Example 4] Polyamide 66 was produced in the same manner as in Reference Example 1, except that 9.56 g of a polyamide oligomer composition obtained in the same manner as in Comparative Example 3 and 0.77 g of hexamethylenediamine were used as polymerization raw materials. The resulting recycled polyamide 66 was colored pale orange, had a relative viscosity of 1.95, and a melting point of 253°C.
[0088] Therefore, from Reference Example 1 and Example 7, it was found that the relative viscosity of the polyamide obtained by repolymerizing the polyamide oligomer composition of the present invention obtained by depolymerizing polyamide was equivalent to that of the polyamide obtained by polymerizing the reagent diamine and the reagent dicarboxylic acid. On the other hand, from Reference Example 1 and Comparative Example 4, the relative viscosity of the polyamide obtained by repolymerizing a composition having a number average molecular weight different from that of the polyamide oligomer composition of the present invention was low. It is presumed that the polymerization was inhibited by impurities. [Industrial Applicability]
[0089] The polyamide oligomer composition of the present invention contains few impurities, and therefore can be suitably used as a raw material for repolymerization of polyamide. In particular, when the polyamide oligomer composition of the present invention is obtained by recycling polyamide, it can contribute to resource recycling and reduction of greenhouse gas emissions.
Claims
1. A polyamide oligomer composition comprising a polyamide oligomer represented by chemical formula (I) and having a number average molecular weight of 250 or more and 800 or less. Chemical formula (I): -[-CO-X-CO-NH-Y-NH-] z - (In the formula, X and Y each independently represent a residue containing at least one selected from a divalent aliphatic group having 2 to 20 carbon atoms, a divalent alicyclic group having 3 to 20 carbon atoms, and a divalent aromatic group having 6 to 20 carbon atoms; and z is an integer of 1 to 3.)
2. The polyamide oligomer composition according to claim 1, having a COOH group concentration of 2.5 mol / kg or more and 8.0 mol / kg or less.
3. N.H. 2 The polyamide oligomer composition according to claim 1 , having a group concentration of 2.5 mol / kg or more and 8.0 mol / kg or less.
4. The polyamide oligomer composition according to claim 1, having a melting point of 40° C. or more and 220° C. or less as measured by differential thermal analysis.
5. A polyamide obtained by using the polyamide oligomer composition according to claim 1 as a polymerization raw material.
6. A molded article obtained by molding the polyamide according to claim 5.
7. 2. A method for producing the polyamide oligomer composition according to claim 1, comprising the step of mixing at least a polyamide (A), a dicarboxylic acid and / or a diamine (B), and a solvent (C) at a temperature of 220° C. or higher and 300° C. or lower and a pressure of 2 MPa or higher and 30 MPa or lower.
8. The method for producing a polyamide oligomer composition according to claim 7, wherein the solvent (C) is water.
9. The method for producing a polyamide oligomer composition according to claim 7, wherein the polyamide (A) is a polycondensation reaction product of a dicarboxylic acid and a diamine.
10. The method for producing a polyamide oligomer composition according to claim 7, wherein the dicarboxylic acid and / or diamine (B) is a dicarboxylic acid or diamine constituting the polyamide (A).
11. 8. The method for producing a polyamide oligomer composition according to claim 7, wherein, in the case where the dicarboxylic acid and / or diamine (B) is only one of a dicarboxylic acid and a diamine, the number of moles of amide groups contained in the polyamide (A) : the number of moles of dicarboxylic acid or diamine = 1:M, M is 0.45 or more and 0.95 or less.
12. 8. The method for producing a polyamide oligomer composition according to claim 7, wherein, in the case where the dicarboxylic acid and / or diamine (B) is both a dicarboxylic acid and a diamine, the number of moles of amide groups contained in the polyamide (A) is expressed as the absolute value of the difference between the number of moles of dicarboxylic acid and the number of moles of diamine=1:N, and N is 0.45 or more and 0.95 or less.
13. The method for producing a polyamide oligomer composition according to claim 7, further comprising a step of recovering the polyamide oligomer composition as a solid by solid-liquid separation.
14. The method for producing a polyamide oligomer composition according to claim 7, wherein the polyamide (A) is a waste product.
15. A method for producing a polyamide, comprising the following steps (1) and (2) in this order: (1) A step of mixing the polyamide oligomer composition according to claim 1 with a diamine and / or a dicarboxylic acid in a solvent to prepare a salt solution. (2) Polycondensing the salt solution prepared in step (1)
Citation Information
Patent Citations
Method for simultaneously producing dicarboxylic acid and diamine from polyamide
JP1995507556A
Method for recovering raw material component from nylon 6, 6
JP2001302597A
Cited By
Depolymerization regeneration method of amido-containing polymer
CN119613281A