Metal-ceramic substrate, its manufacturing method and module
The metal-ceramic substrate with a tailored bonding layer of specific metals addresses high temperature and silver migration issues, ensuring a stable and conductive bond between metal and ceramic layers.
Patent Information
- Application Number
- JP2024522664
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-26
- Filing Date
- 2022-11-01
- Publication Date
- 2024-10-28
- Estimated Expiration
- 2042-11-01
AI Technical Summary
Existing methods for producing metal-ceramic substrates face challenges such as high temperature requirements, limited ceramic material compatibility, and issues with silver migration, which affect the stability and conductivity of the bond between the metal and ceramic layers.
A metal-ceramic substrate design featuring a bonding layer composed of metals with specific melting points and compositions, including a metal M1 with a melting point of at least 700°C, metal M2 below 700°C, an active metal M3, and metals M4 like bismuth, gallium, zinc, indium, germanium, or aluminum, with defined weight ratios to ensure a stable bond and high thermal and electrical conductivity without silver migration.
The proposed substrate achieves a stable bond between the metal and ceramic layers with high thermal and electrical conductivity, while minimizing silver migration issues, using a bonding layer with controlled metal compositions.
Smart Images

Figure 2024539042000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal-ceramic substrate, a method for making a metal-ceramic substrate, and a module having a metal-ceramic substrate.
[0002] Metal-ceramic substrates play an important role in the field of power electronics. They are a key element when constructing electronic components, ensuring the rapid dissipation of large amounts of heat during the operation of said components. Metal-ceramic substrates typically consist of a ceramic layer and a metal layer bonded to the ceramic layer.
[0003] Several methods for bonding metal layers to ceramic layers are known from the prior art. In the so-called DCB (direct copper bonding) method, copper is reacted with a reactive gas (usually oxygen) to provide the surface of a copper foil with a copper compound (usually copper oxide) that has a lower melting point than copper. When the copper foil thus treated is applied to a ceramic body and the composite is fired, the copper compound melts and wets the surface of the ceramic body, so that a stable cohesive bond is achieved between the copper foil and the ceramic body. This method is described, for example, in US Pat. No. 3,744,120 (A) or in German Patent No. 2,319,854 (C2).
[0004] Despite the obvious advantages, the DCB method has two main disadvantages. First, the method must be carried out at a relatively high temperature, i.e., slightly below the melting point of copper. Second, the method can only be used for oxide-based ceramics, such as aluminum oxide or superficially oxidized aluminum nitride. Thus, there is a need for an alternative method for producing metal-ceramic substrates under less stringent conditions. In the alternative method, the metal foil can be joined to the ceramic body at a temperature of about 650-1000°C, where a specific solder is used, which contains a metal (usually silver) with a melting point of at least 700°C and an active metal. The role of the active metal is to react with the ceramic material, thus facilitating the joining of the ceramic material to the remaining solder and forming a reaction layer, while the metal with a melting point of at least 700°C serves to join the reaction layer to the metal foil. For example, Japanese Patent No. 4812985(B2) proposes joining copper foil to a ceramic body using a solder containing 50-89% by weight of silver, as well as copper, bismuth and an active metal, which allows the copper foil to be stably attached to the ceramic body.
[0005] To avoid problems related to silver migration, it may be advantageous to use silver-free solders to join the metal foil to the ceramic body. These solders are, for example, based on a high-melting metal (in particular copper), a low-melting metal (such as bismuth, indium or tin) and an active metal (such as titanium). Such a technique is proposed, for example, in DE 102017114893 A1. This technique essentially results in a new and independent class of compounds, since the basis of the solder used is formed by another metal (copper instead of silver), leading to a change in the material properties and to adaptations with regard to other solder components and modified joining conditions. The metal-ceramic substrate thus produced thus comprises, in addition to the metal layer and the ceramic body, a joining layer between the metal layer and the ceramic body containing the active metal.
[0006] The ever-increasing requirements in the field of power electronics also see increasing requirements for the stability of the bond between the metal layer in the metal-ceramic substrate and the ceramic body, as well as the thermal and electrical conductivity of the metal-ceramic substrate. It has been found that the stability of the bond between the metal layer and the ceramic body increases with an increasing content of low melting point metal in the bonding layer. However, there is a problem that a high content of low melting point metal in the bonding layer leads to a high diffusion of the low melting point metal into the metal layer of the metal-ceramic substrate. This effect reduces the thermal and electrical conductivity of the metal-ceramic substrate. Summary of the Invention [Problem to be solved by the invention]
[0007] There is therefore a need for a metal-ceramic substrate which, on the one hand, includes a very stable bond between the metal layer and the ceramic body, and, on the other hand, has high thermal and electrical conductivity. There is also a need for such a metal-ceramic substrate which is at least largely free of silver, in order to avoid the problems associated with silver migration.
[0008] It is therefore an object of the present invention to provide a metal-ceramic substrate which comprises, on the one hand, a very stable bond between the metal layer and the ceramic body, and, on the other hand, has high thermal and electrical conductivity. It is therefore a further object of the present invention to provide such a metal-ceramic substrate which does not have the problems arising in connection with silver migration.
[0009] These objects are achieved by a metal-ceramic substrate according to claim 1. The invention therefore provides (a) a ceramic body; (b) a metal layer; (c) a bonding layer located between the ceramic body and the metal layer, (i) a metal M1 having a melting point of at least 700° C.; (ii) a metal M2 having a melting point below 700° C.; (iii) a metal M3 selected from the group of active metals, and (iv) a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium A bonding layer comprising: A metal-ceramic substrate comprising: The bonding layer has the following characteristics: (c1) M(M2) EDX =10~20% by weight, (c2)15% by weight≦[M(M4) / M(M2)] ICP * 1000wt%+M(M2) EDX ≦100% by weight, and (c3) M(Ag) EDX <10% by weight The present invention is characterized in that During the ceremony, M(M2) EDX is the metal M2 content in the bonding layer, determined using EDX, [M(M4) / M(M2)] ICP is the gold content in the bonding layer, determined using ICP. genus M2 content The content of metal M4 in the bonding layer is the ratio, M(Ag) EDX is the silver content in the bonding layer determined using EDX, A metal-ceramic substrate is provided.
[0010] The present invention further provides a method for producing a metal-ceramic substrate and a module having a metal-ceramic substrate.
[0011] The metal-ceramic substrate according to the present invention includes a ceramic body, a metal layer, and a bonding layer.
[0012] In the metal-ceramic substrate, the bonding layer is located between the ceramic body and the metal layer. Thus, the bonding layer is preferably in contact with the ceramic body and the metal layer. According to a preferred embodiment, the metal-ceramic substrate comprises a ceramic body, a (first) metal layer, a (first) bonding layer in contact with the ceramic body and the first metal layer, a second metal layer, and a second bonding layer in contact with the ceramic body and the second metal layer. According to this embodiment, the (first) bonding layer is preferably located between the ceramic body and the (first metal) layer, and the second bonding layer is preferably located between the ceramic body and the second metal layer. Furthermore, according to this embodiment, the composition of the first bonding layer preferably corresponds to the composition of the second bonding layer.
[0013] The ceramic body preferably comprises a first surface and a second surface. The metal layer preferably comprises the first surface. The second metal layer, if present, preferably comprises the first surface. According to a preferred embodiment, the (first) bonding layer is located in the metal-ceramic substrate between the first surface of the ceramic body and the first surface of the (first) metal layer. According to a further preferred embodiment, the metal-ceramic substrate comprises a second bonding layer in contact with the second surface of the ceramic body and the first surface of the second metal layer. According to this embodiment, the (first) bonding layer is preferably located in the metal-ceramic substrate between the first surface of the ceramic body and the first surface of the (first) metal layer, and the second bonding layer is preferably located between the second surface of the ceramic body and the first surface of the second metal layer. According to a further preferred embodiment, in addition to the bonding layer according to the invention, no further layer is arranged between the ceramic body and the (first) metal layer. According to yet another embodiment, in addition to the bonding layer according to the invention, in case of presence, no further layer is arranged between the ceramic body and the second metal layer.
[0014] The ceramic of the ceramic body is preferably an insulating ceramic. According to a preferred embodiment, the ceramic is selected from the group consisting of oxide ceramics, nitride ceramics, and carbide ceramics. According to a further preferred embodiment, the ceramic is selected from the group consisting of metal oxide ceramics, silicon oxide ceramics, metal nitride ceramics, silicon nitride ceramics, boron nitride ceramics, and boron carbide ceramics. According to a particularly preferred embodiment, the ceramic is selected from the group consisting of aluminum nitride ceramics, silver nitride ceramics, and aluminum oxide ceramics (such as ZTA (zirconia toughened alumina) "zirconia toughened alumina" ceramics). According to yet another very particularly preferred embodiment, the ceramic body comprises (1) at least one element selected from the group consisting of silicon and aluminum, (2) at least one element selected from the group consisting of oxygen and nitrogen, and optionally (3) at least one element selected from the group consisting of (3a) rare earth metals, (3b) metals of group 2 of the periodic table of the elements, (3c) zirconium, (3d) copper, (3e) molybdenum, and (3f) silicon, and optionally (4) unavoidable impurities. According to yet another very particularly preferred embodiment, the ceramic body is free of bismuth, gallium, and zinc.
[0015] The ceramic body preferably has a thickness in the range of 0.05 to 10 mm, more preferably 0.1 to 5 mm, and particularly preferably 0.15 to 3 mm.
[0016] The metal of the metal layer is preferably selected from the group consisting of copper, aluminum and molybdenum. According to a particularly preferred embodiment, the metal of the metal layer is selected from the group consisting of copper and molybdenum. According to a very particularly preferred embodiment, the metal of the metal layer is copper. According to a further very particularly preferred embodiment, the metal layer consists of copper and unavoidable impurities.
[0017] The metal layer preferably has a thickness in the range from 0.01 to 10 mm, particularly preferably in the range from 0.03 to 5 mm and very particularly preferably in the range from 0.05 to 3 mm.
[0018] The bonding layer includes (i) a metal M1 having a melting point of at least 700°C, (ii) a metal M2 having a melting point less than 700°C, (iii) a metal M3 selected from the group of active metals, and (iv) a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum, and magnesium.
[0019] A bonding layer is preferably understood to mean the area of the metal-ceramic substrate which is located between the ceramic body and the metal layer.
[0020] The bonding layer comprises (i) a metal M1 having a melting point of at least 700° C. The metal M1 having a melting point of at least 700° C. preferably has a melting point of at least 850° C., particularly preferably has a melting point of at least 1000° C. According to a preferred embodiment, the metal M1 having a melting point of at least 700° C. is selected from the group consisting of copper, nickel, tungsten and molybdenum. According to a particularly preferred embodiment, the metal M1 having a melting point of at least 700° C. is copper.
[0021] The bonding layer (ii) comprises a metal M2 having a melting point of less than 700° C. The metal M2 having a melting point of less than 700° C. preferably has a melting point of less than 600° C., particularly preferably has a melting point of less than 550° C. According to a particularly preferred embodiment, the metal M2 having a melting point of less than 700° C. is tin.
[0022] The bonding layer comprises (iii) a metal M3 selected from the group of active metals. The metal M3 is therefore preferably a metal which produces a bond with the ceramic by chemical reaction. According to a preferred embodiment, the metal M3 is selected from the group consisting of hafnium, titanium, zirconium, niobium, cerium, tantalum and vanadium. According to a more preferred embodiment, the metal M3 is selected from the group consisting of hafnium, titanium, zirconium, niobium and cerium. According to a particularly preferred embodiment, the metal M3 is selected from the group consisting of hafnium, titanium and zirconium. According to a very particularly preferred embodiment, the metal M3 is titanium.
[0023] The bonding layer comprises (iv) a metal M4. The metal M4 is a metal selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium. According to a particularly preferred embodiment, the metal M4 is selected from the group consisting of bismuth, gallium and zinc. According to a very particularly preferred embodiment, the metal M4 is bismuth.
[0024] The metals M1, M2, M3, and M4 are different metals. Thus, the bonding layer located between the ceramic body and the metal layer includes each of the metals M1, M2, M3, and M4. Thus, the bonding layer located between the ceramic body and the metal layer includes (i) a metal M1 having a melting point of at least 700°C, (ii) a metal M2 having a melting point less than 700°C, (iii) a metal M3 selected from the group of active metals, and (iv) a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum, and magnesium, where the metals M1, M2, M3, and M4 are different. Thus, the metal M2 having a melting point less than 700°C is not selected from the group consisting of bismuth, gallium, zinc, indium, aluminum, and magnesium. Furthermore, the metal M2 is not an active metal. Similarly, the metal M1 having a melting point of at least 700°C is not germanium. Furthermore, the metal M1 having a melting point of at least 700°C is not an active metal.
[0025] According to the invention, the bonding layer has the following properties: (c1) M(M2) EDX =10~20% by weight, (c2)15% by weight≦[M(M4) / M(M2)] ICP * 1000wt%+M(M2) EDX ≦100% by weight, and (c3) M(Ag) EDX <10% by weight having During the ceremony, M(M2) EDX is the content [wt.%] of metal M2 in the bonding layer, determined using EDX; [M(Bi) / M(M2)] ICP is the gold content in the bonding layer, determined using ICP. genus M2 content The content of metal M4 in the bonding layer is the ratio, M(Ag) EDX is the silver content [wt %] in the bonding layer, determined using EDX.
[0026] According to the characteristic (c1), the content of metal M2 in the bonding layer, determined by means of EDX, is 10-20 wt.%. According to a preferred embodiment, the bonding layer has the following characteristics: (c1')M(M2) EDX =10~18wt% has.
[0027] According to a particularly preferred embodiment, the bonding layer has the following properties: (c1'')M(M2) EDX =10~15% by weight has.
[0028] According to the characteristic (c2), there is a relationship between the content of metal M4 and the content of metal M2, so that the bonding layer has the following characteristics: (c2)15% by weight≦[M(M4) / M(M2)] ICP * 1000wt%+M(M2) EDX ≦100% by weight has.
[0029] According to a preferred embodiment, the bonding layer has the following properties: (c2'):15wt%≦[M(M4) / M(M2)] ICP * 1000wt%+M(M2) EDX ≦80% by weight has.
[0030] According to a particularly preferred embodiment, the bonding layer has the following properties: (c2''):15% by weight≦[M(M4) / M(M2)] ICP * 1000wt%+M(M2) EDX ≦70% by weight has.
[0031] Surprisingly, it has been found that by adding small amounts of metal M4, the amount of metal M2 with a melting point below 700 ° C, which is necessary for a particularly stable bond between the ceramic body and the metal layer, can already be reduced, so that the electrical and thermal conductivity of the metal-ceramic substrate is not impaired by the diffusion of metal M2 into the metal layer. Furthermore, it has been found surprisingly that a particularly stable bond is achieved if the content of metal M2 in the bonding layer is within a defined range. The relationship between the proportions of metals M2 and M4 in the bonding layer, which are necessary for this effect, is represented by properties (c1) and (c2). Thus, surprisingly, by adjusting the content of metal M2 with a melting point below 700 ° C and the content of metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium, a metal-ceramic substrate is provided which has a particularly stable bond between the ceramic body and the metal layer on the one hand and high electrical and thermal conductivity on the other hand.
[0032] According to the characteristic (c3), the silver content in the bonding layer is 10 wt% or less as determined by EDX. Thus, the present invention also includes an embodiment in which the bonding layer does not contain silver, i.e., the silver content in the bonding layer is 0 wt% as determined by EDX.
[0033] According to a particularly preferred embodiment, the bonding layer has the following properties: (c3') M(Ag) EDX <5% by weight has.
[0034] According to a very particularly preferred embodiment, the bonding layer has the following properties: (c3'')M(Ag) EDX <1% by weight has.
[0035] The absence of silver or the presence of only small amounts of silver means that undesirable migration of silver at the edges of the bonding layer in the metal-ceramic substrate can be avoided or reduced.
[0036] According to a preferred embodiment, the content of metal M1 in the bonding layer (M(M1) EDX According to a particularly preferred embodiment, the content of the metal M1 in the bonding layer (M(M1) EDX According to a very particularly preferred embodiment, the content of the metal M1 in the bonding layer, determined by means of EDX (M(M1) EDX ) is in the range of 70 to 88% by weight.
[0037] According to a preferred embodiment, the content of metal M3 in the bonding layer, determined by EDX (M(M3) EDX According to a particularly preferred embodiment, the content of the metal M3 in the bonding layer, determined by EDX (M(M3) EDX According to a very particularly preferred embodiment, the content of the metal M3 in the bonding layer, determined by means of EDX (M(M3) EDX ) is in the range of 1 to 14% by weight.
[0038] According to a preferred embodiment, the content of metal M4 in the bonding layer (M(M4)) determined by ICP ICPAccording to a particularly preferred embodiment, the content of the metal M4 in the bonding layer (M(M4) ICP According to a very particularly preferred embodiment, the content of the metal M4 in the bonding layer, determined by means of ICP (M(M4) ICP ) is in the range of 0.1 to 1% by weight.
[0039] Metal-ceramic substrates according to the invention may be manufactured by methods that constitute standard practice in the art.
[0040] According to a preferred embodiment, the method for producing a metal-ceramic substrate according to the invention comprises the steps of: a) a laminate, a1) a ceramic body; a2) a metal foil; a3) a solder material in contact with the ceramic body and the metal foil, (i) a metal M1 having a melting point of at least 700° C.; (ii) a metal M2 having a melting point below 700° C.; (iii) a metal M3 selected from the group of active metals, and (iv) a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium A solder material comprising: providing a laminate comprising: b) heating the laminate to obtain a metal-ceramic substrate; Includes.
[0041] Thus, first, a laminate is preferably provided that includes a ceramic body, a metal foil, and a solder material in contact with the ceramic body and the metal foil.
[0042] Therefore, in the laminate, the solder material is preferably located between the ceramic body and the metal foil. According to a preferred embodiment, the laminate comprises a ceramic body, a (first) metal foil, a (first) solder material in contact with the ceramic body and the first metal foil, a second metal foil, and a second solder material in contact with the ceramic body and the second metal foil. According to this embodiment, the (first) solder material is preferably located between the ceramic body and the (first) metal foil, and the second solder material is preferably located between the ceramic body and the second metal foil. Furthermore, according to this embodiment, the first solder material preferably corresponds to the second solder material.
[0043] The ceramic body, the metal foil and the solder material are preferably designed such that after heating a metal-ceramic substrate according to the invention is produced.
[0044] Thus, the ceramic body and metal foil are preferably designed as described above for the ceramic body and metal layer of the metal-ceramic substrate.
[0045] The solder material preferably comprises (i) a metal M1 having a melting point of at least 700° C., (ii) a metal M2 having a melting point less than 700° C., (iii) a metal M3 selected from the group of active metals, and (iv) a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium. Metals M1, M2, M3 and M4 are preferably designed as described above for the metal-ceramic substrate bonding layer.
[0046] Thus, the metals M1, M2, M3, and M4 are different metals. Thus, the solder material in contact with the ceramic body and the metal layer includes each of the metals M1, M2, M3, and M4. Thus, the solder material in contact with the ceramic body and the metal layer includes i) a metal M1 having a melting point of at least 700°C, (ii) a metal M2 having a melting point less than 700°C, (iii) a metal M3 selected from the group of active metals, and (iv) a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum, and magnesium, where the metals M1, M2, M3, and M4 are different. Thus, the metal M2 having a melting point less than 700°C is not selected from the group consisting of bismuth, gallium, zinc, indium, aluminum, and magnesium. Furthermore, the metal M2 is not an active metal. Similarly, the metal M1 having a melting point of at least 700°C is not germanium. Furthermore, the metal M1 having a melting point of at least 700°C is not an active metal.
[0047] According to a preferred embodiment, (i) metal M1, (ii) metal M2, (iii) metal M3, and (iv) metal M4 are present as constituents of at least one metal component. Thus, the solder material preferably includes at least one metal component including (i) metal M1, (ii) metal M2, (iii) metal M3, and (iv) metal M4. For example, it may be preferable that the solder material includes a metal component (i) containing metal M1, a metal component (ii) containing metal M2, a metal component (iii) containing metal M3, and a metal component (iv) containing metal M4. Furthermore, the solder material comprises a metal component (i) containing a member from the group consisting of (i) metal M1, (ii) metal M2, (iii) metal M3, and (iv) metal M4, and at least one further metal component (ii) containing a member from the group consisting of (i) metal M1, (ii) metal M2, (iii) metal M3, and (iv) metal M4, which may be preferred not to be contained in the metal component (i). The term "metal component" is further not limited. In addition to metals and metal alloys, metal compounds such as intermetallic phases and other compounds (e.g., metal hydrides, etc.) are also included. Thus, according to a preferred embodiment, the metal component is selected from the group consisting of metals, metal alloys, and metal compounds.
[0048] The solder material preferably comprises (i) a metal M1 having a melting point of at least 700° C. According to a preferred embodiment, the solder material comprises a metal component (i) containing a metal M1 having a melting point of at least 700° C. According to a particularly preferred embodiment, the solder material comprises a metal component (i) containing copper. According to a further preferred embodiment, the metal component (i) is copper.
[0049] The solder material preferably comprises (ii) a metal M2 having a melting point of less than 700° C. According to a preferred embodiment, the solder material comprises a metal component (ii) containing a metal M2 having a melting point of less than 700° C. According to a particularly preferred embodiment, the metal component (ii) is an alloy of a metal M2 having a melting point of less than 700° C. with a further metal. The further metal can be selected, for example, from the group consisting of a metal M1 having a melting point of less than 700° C., a metal M2 having a melting point of at least 700° C., a metal M3 selected from the group of active metals, and a metal M4 selected from the group consisting of bismuth, indium, germanium, gallium, and zinc. According to a further preferred embodiment, the metal component (ii) containing a metal M2 having a melting point of less than 700° C. is selected from the group consisting of tin, tin-copper alloys, tin-bismuth alloys, tin-antimony alloys, tin-zinc-bismuth alloys, and indium-tin alloys.
[0050] The solder material preferably comprises a metal M3 selected from the group of active metals. According to a preferred embodiment, the solder material comprises a metal component (iii) containing a metal M3 selected from the group of active metals. According to a particularly preferred embodiment, the metal component (iii) is an active metal alloy or an active metal compound, particularly preferably an active metal hydride. The metal component (iii) is preferably selected from the group consisting of titanium hydride, titanium-zirconium-copper alloy, zirconium hydride and hafnium hydride. According to a particularly preferred embodiment, the metal component (iii) is selected from the group consisting of hafnium hydride, titanium hydride and zirconium hydride. According to a very particularly preferred embodiment, the metal component (iii) is titanium hydride.
[0051] The solder material preferably comprises a metal M4. According to a preferred embodiment, the solder material comprises a metal component (iv) containing a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium. According to a particularly preferred embodiment, the solder material comprises a metal component (iv) containing bismuth. According to a further preferred embodiment, the metal component (iv) is bismuth.
[0052] According to a preferred embodiment, the proportion of metal M1 having a melting point of at least 700 ° C is 65-89 wt.-%, particularly preferably 67-88 wt.-%, very particularly preferably 70-88 wt.-%, based on the total metal weight of the solder material. According to a further preferred embodiment, the proportion of metal M2 having a melting point below 700 ° C is 10-20 wt.-%, particularly preferably 10-18 wt.-%, very particularly preferably 10-15 wt.-%, based on the total metal weight of the solder material. According to yet another preferred embodiment, the proportion of metal M3 selected from the group of active metals is 0.5-15 wt.-%, particularly preferably 0.5-14 wt.-%, very particularly preferably 1-14 wt.-%, based on the total metal weight of the solder material. According to a further preferred embodiment, the proportion of the metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium is 0.01 to 2% by weight, particularly preferably 0.01 to 1.5% by weight, very particularly preferably 0.1 to 1% by weight, based on the total metal weight of the solder material. The solder material is preferably free of silver or low in silver. The proportion of silver is therefore preferably less than 10% by weight, particularly preferably less than 5% by weight, very particularly preferably less than 1% by weight, based on the total metal weight of the solder material.
[0053] The solder material is in contact with the ceramic body and the metal foil. Thus, the solder material is preferably located between the ceramic body and the metal foil. For example, the solder material may be applied to the ceramic body, followed by applying the metal foil to the solder material. The solder material is preferably at least one material selected from the group consisting of pastes, foils and deposits, including a metal M1 having a melting point of at least 700°C, a metal M2 having a melting point of less than 700°C, a metal M3 selected from the group of active metals, and a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium.
[0054] The solder material may be a paste, preferably comprising (a) at least one metal component including a metal M1 having a melting point of at least 700° C., a metal M2 having a melting point less than 700° C., a metal M3 selected from the group of active metals, and a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum, and magnesium, and (b) an organic medium.
[0055] The organic medium is preferably an organic medium commonly used in the related technical field, and preferably contains an organic binder, an organic dispersant, or a mixture thereof.
[0056] The organic binder is preferably removed from the solder material during heating. The organic binder is preferably a thermoplastic or thermosetting material. Examples of organic binders include cellulose derivatives (such as ethyl cellulose, butyl cellulose, and cellulose acetate), polyethers (such as polyoxymethylene), and acrylic resins (such as polymethyl methacrylate and polybutylene methacrylate).
[0057] The organic dispersant is preferably an organic compound that imparts suitable viscosity to the paste and is discharged during drying or heating of the paste.The organic dispersant can be selected from, for example, aliphatic alcohols, terpene alcohols, alicyclic alcohols, aromatic cyclic carboxylic acid esters, alicyclic esters, carbitols and aliphatic polyols.Examples of organic dispersants include octanol, decanol, terpineol (e.g. dihydroterpineol), cyclohexanol, dibutyl phthalate, carbitol, ethyl carbitol, ethylene glycol, butanediol and glycerol.
[0058] The pastes may further contain additives used in standard practice in the art, examples of which include inorganic binders (such as glass frit), stabilizers, surfactants, dispersants, rheology modifiers, wetting aids, defoamers, fillers, and hardeners.
[0059] According to a preferred embodiment, the proportion of at least one metal component including a metal M1 having a melting point of at least 700° C., a metal M2 having a melting point less than 700° C., a metal M3 selected from the group of active metals, and a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium is 20 to 95% by weight, more preferably 30 to 95% by weight, particularly preferably 75 to 95% by weight, based on the total weight of the paste. According to a further preferred embodiment, the proportion of the organic medium is 5 to 80% by weight, more preferably 5 to 70% by weight, particularly preferably 5 to 25% by weight, based on the total weight of the paste.
[0060] According to a further preferred embodiment, the ratio of (a) the total weight of at least one metal component, including a metal M1 having a melting point of at least 700 ° C, a metal M2 having a melting point of less than 700 ° C, a metal M3 selected from the group of active metals, and a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium, to the weight of (b) the organic medium is at least 5: 1, particularly preferably at least 7: 1, very particularly preferably at least 8: 1. According to a preferred embodiment, the ratio of (a) the total weight of at least one metal component, including a metal M1 having a melting point of at least 700 ° C, a metal M2 having a melting point of less than 700 ° C, a metal M3 selected from the group of active metals, and a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium, to the weight of (b) the organic medium is in the range of 1: 1 to 20: 1, particularly preferably in the range of 2: 1 to 20: 1, particularly preferably in the range of 5: 1 to 15: 1.
[0061] To prepare the laminate, the paste is preferably applied to the surface of the ceramic body. The paste can be applied, for example, by a dispersion method or a printing method. Suitable printing methods include, for example, a screen printing process, an inkjet printing method, and an offset printing process. Preferably, the paste is applied to the surface of the ceramic body by a screen printing method.
[0062] After application of the paste, the paste may be pre-dried as necessary. Pre-drying may be performed at room temperature or at an elevated temperature. The conditions for pre-drying may vary depending on the organic medium contained in the paste. The pre-drying temperature may be, for example, within the range of 50 to 180°C, and is preferably within the range of 80 to 150°C. Pre-drying is usually performed for 2 minutes to 2 hours, and preferably for 5 minutes to 1 hour.
[0063] The paste can then be applied to the surface of the metal foil and, if necessary, pre-dried to obtain a laminate.
[0064] The solder material may be a film.
[0065] The film comprises a metal M1 having a melting point of at least 700° C., a metal M2 having a melting point below 700° C., a metal M3 selected from the group of active metals, and a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium. Additionally, the film may comprise further components, such as, for example, a suitable binder.
[0066] The film can be obtained by optionally homogenizing at least one metal component comprising, for example, a metal M1 having a melting point of at least 700° C., a metal M2 having a melting point below 700° C., a metal M3 selected from the group of active metals, and a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium, and a further component being heated to a temperature below the melting points of the metal M1 having a melting point of at least 700° C., the metal M2 having a melting point below 700° C., the active metal M3, and the metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium, but sufficient to form a bond between the metals. This temperature can be, for example, at least 200° C.
[0067] Alternatively, the film can be obtained by mixing at least one metal component comprising, for example, a metal M1 having a melting point of at least 700° C., a metal M2 having a melting point below 700° C., a metal M3 selected from the group of active metals, and a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium, with a binder, forming and heating the mixture to form a shaped body. During heating, the binder can harden and form a matrix in which the metals are distributed.
[0068] To prepare the laminate, a film can be placed, for example, on the ceramic. A surface of a metal foil can then be applied to the film located on the ceramic to obtain the laminate.
[0069] According to a further embodiment, the solder material can be a deposit. The deposit of the solder material can be produced, for example, by galvanic deposition or vapor deposition. Preferably, the solder material deposit is produced on a ceramic body. A metal foil can then be applied to the solder material deposited on the ceramic to obtain a laminate.
[0070] The laminate is heated to obtain a metal-ceramic substrate. According to a preferred embodiment, the heating is performed to obtain a metal-ceramic substrate by a solder material that forms a cohesive bond between the ceramic body and the metal foil. The cohesive bond is preferably formed by a metal M3 being bonded to the ceramic body during heating, with the metal M1 having a melting point of at least 700° C., the metal M2 having a melting point of less than 700° C., the metal M4 being selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium, and the metal of the metal foil being bonded to form an alloy. During the subsequent solidification, a cohesive bond is formed between the ceramic body and the metal foil via the active metal M3 bonded to the ceramic body and the resulting alloy.
[0071] During heating, the laminate is heated to a peak temperature. The peak temperature is not further limited, but is preferably below the melting point of the metal M1, which has a melting point of at least 700 ° C, and below the melting point of the metal of the metal foil. According to a preferred embodiment, the peak temperature is at least 10 ° C, particularly preferably at least 50 ° C, below the melting point of the metal of the metal foil. According to a further preferred embodiment, the peak temperature is at least 700 ° C. The peak temperature is preferably in the range of 700 to 1100 ° C, particularly preferably in the range of 750 to 1050 ° C, very particularly preferably in the range of 800 to 1000 ° C. Peak temperature as used herein refers to the temperature measured at the laminate by a thermocouple. The peak temperature is the maximum temperature measured at the laminate. In order to prevent undesirable effects such as excessive shrinkage or swelling of the molten metal due to excessive fluidity of the molten metal, the skilled person strives to avoid excessively high peak temperatures.
[0072] During heating, the laminate is supplied with heat for a high-temperature heating period. A high-temperature heating period in this specification preferably refers to a period during which the laminate is exposed to a temperature at least equal to the peak temperature of 250°C. Thus, for an exemplary peak temperature of 900°C, the high-temperature heating period corresponds to a period during which the laminate is exposed to a temperature of at least 650°C during heating. According to a preferred embodiment, the high-temperature heating period is not longer than 60 minutes, more preferably not longer than 50 minutes, particularly preferably not longer than 45 minutes, very particularly preferably not longer than 40 minutes. The high-temperature heating period is preferably in the range of 2 to 60 minutes, more preferably in the range of 3 to 50 minutes, particularly preferably in the range of 5 to 45 minutes, very particularly preferably in the range of 10 to 40 minutes.
[0073] The stack is preferably heated with the energy input required for heating starting from the heating zone and proceeding in the direction of the stack. The cohesive bond is preferably formed by bonding with the ceramic body, the metal M3 being selected from the group consisting of metal M1 having a melting point of at least 700° C., metal M2 having a melting point below 700° C., metal M4 having a melting point below 700° C., bismuth, gallium, zinc, indium, germanium, aluminum and magnesium, and the metal of the metal foil to form an alloy. During the subsequent solidification, a cohesive bond is formed between the ceramic body and the metal foil via the active metal M3 bonded to the ceramic body and the alloy.
[0074] According to a particularly preferred embodiment, the laminate is heated in an oven, preferably in a continuous furnace or a chamber furnace.
[0075] A non-oxidizing atmosphere is preferably present in the heating zone. The non-oxidizing atmosphere is preferably an inert gas atmosphere. A nitrogen atmosphere, a helium atmosphere or an argon atmosphere is preferably present in the heating zone. According to a particularly preferred embodiment, a nitrogen atmosphere is present in the heating zone. The proportion of reactive gases, in particular oxygen, in the non-oxidizing atmosphere is preferably less than 1000 ppm, more preferably less than 500 ppm, particularly preferably less than 40 ppm.
[0076] When the laminate is heated, a cohesive bond is preferably formed between the ceramic body and the metal foil via the solder material to obtain a metal-ceramic substrate comprising a ceramic body, a metal layer, and a bonding layer located between the ceramic body and the metal layer. If necessary, the metal-ceramic substrate can be subjected to further processing steps. For example, the exposed surface of the metal-ceramic substrate, preferably the metal layer of the metal-ceramic substrate, can be polished. Preferably, the surface of the metal layer of the metal-ceramic substrate is physically or chemically polished. Further, the metal-ceramic substrate can be constructed. For example, the metal-ceramic substrate can be provided with conductor traces. The conductor traces are preferably produced by etching.
[0077] The metal-ceramic substrates according to the invention can be used in particular for applications in electronics, especially in the field of power electronics.
[0078] The present invention therefore also provides a module comprising a metal-ceramic substrate as described above.
[0079] According to a preferred embodiment, such a module comprises a base plate, which is preferably extensively bonded to the metal layer of the metal-ceramic substrate. According to a further preferred embodiment, the module comprises at least one chip, which is preferably extensively bonded to the metal layer of the at least one metal-ceramic substrate. According to a further preferred embodiment, the module comprises a metal-ceramic substrate comprising a first metal layer and a second metal layer (the first metal layer is preferably on the opposite side to the second metal layer), a base plate and at least one chip, the at least one chip being bonded to the first metal layer of the metal-ceramic substrate and the base plate being bonded to the second metal layer of the metal-ceramic substrate.
[0080] The properties of the metal-ceramic substrate bond layer are preferably determined using the measurement methods described below.
[0081] Measurement method: (i) The content of metals M1, M2, M3 and silver in the bonding layer (characteristic M(M1) EDX , M(M2) EDX , M(M3) EDX and M(Ag) EDX ) is determined as follows: The content of metals M1, M2, M3 and silver in the bonding layer is preferably determined as follows.
[0082] In the first step, 100 mm of the metal-ceramic substrate to be inspected is removed. 2 ~400mm 2A rectangular sample blank with a rectangular base in the range of 0.01 mm to 0.01 mm is cut out by sawing with a diamond saw blade at a low rotational speed with an oil-based lubricant (Buehler) perpendicular to the plane in which the metal layer of the metal-ceramic substrate extends. The sample blank thus has a sample surface that is supplied for inspection. This sample surface thus extends perpendicular to the plane in which the metal layer of the metal-ceramic substrate extends before sawing. The sample blank thus has a portion on the ceramic body, the metal layer and the bonding layer between them. The sample blank is first embedded in a mold containing a low-shrinkage epoxy resin (Epo-Fix, Struers) with the sample surface oriented perpendicular to the mold wall. The epoxy resin is then cured at room temperature. After curing, the sample surface of the sample blank is mechanically polished in an automatic polishing machine (Tegrapole, Struers) to achieve a roughness of 1 μm or less.
[0083] In the second step, the polished sample surface is conductively coated with iridium to a thickness of 1–5 nm using a metal sputtering system (Q150T, Quorum Technologies).
[0084] In a third step, the analysis zone of the sample surface is examined by scanning electron microscope energy dispersive X-ray spectroscopy (SEM-EDX). In SEM-EDX, a focused primary electron beam is guided (screened) point by point on the sample surface. The scattered electrons are detected using a detector and the number of electrons per pixel results in a microscopic image of the sample surface in gray scale. Furthermore, the primary electron beam excites the sample to emit characteristic X-ray radiation and the elements and their weight percentages in the sample can be determined by analyzing the energy spectrum using an EDX detector. For the examination, a scanning electron microscope (JSM-6060 SEM, JEOL Ltd) equipped with a silicon drift EDX detector (NORAN, Thermo Scientific Inc) and analysis software (Pathfinder Mountaineer EDS System, e.g. version 2.8, Thermo Scientific Inc) are used. For the scanning electron microscope, the following settings are used: magnification: 1000x, accelerating voltage = 15 kV, working distance = 10 mm, spot size (50-60) (set to reach 25% + / - 5% of the dead time of the EDX detector).
[0085] In the fourth step, the sample surface is detected using EDX software as an electron micrograph (backscattered electron micrograph). A rectangular field of view of at least 125 μm (horizontal) × 90 μm (vertical) is obtained and an analysis zone is defined using the point analysis function of the EDX software. The analysis zone can be described as follows with reference to Figure 1. a) The sample surface is oriented in the electron micrograph 100 such that the cutout of the ceramic body 120 is at the bottom and the cutout of the metal layer 110 is at the top. In the electron micrograph 100, a transition 5 is visible between the ceramic body (dark) 120 and the bonding or metal layer (light) 110. The rectangular lower boundary 10 of the analysis zone 130 is delineated by a line parallel to said transition 5, which line runs directly through the ceramic body 120 exclusively at said transition 5. b) In this orientation, the sample surface is examined for the presence of metal M2 with a melting point below 700° C. and for the presence of active metal M3. A grayscale image of the electron micrograph 100 within the bonding or metal layer 110 is examined, with metal M2 having the brightest pixels and metal M3 having the darkest pixels (excluding the ceramic body). A line in the electron micrograph 100 parallel to the rectangular lower boundary 10 of the analysis zone 130 passes through the furthest point where either metal M2 or metal M3 with a melting point below 700° C. is detected, forming the rectangular upper boundary 20 of the analysis zone 130. c) The left and right borders 30 and 40 of the rectangle of the analysis zone 130 run parallel to each other at a distance corresponding to the distance of the border of the field of view of the sample surface (preferably 125 μm) and are perpendicular to the lower and upper borders 10 and 20.
[0086] In the fifth step, detect the EDX spectrum using the following settings of the EDX detector: live time = 30 s, speed = auto, low energy cutoff = 100 keV, high energy cutoff = auto (per SEM accelerating voltage).
[0087] In a sixth step, the spectrum is analyzed. For this purpose, the elements to be examined are selected and the elements contained in the ceramic body (whose presence can optionally be determined beforehand by conventional test methods), iridium and the element of the epoxy resin are deselected. The respective amounts of the examined elements are indicated in % by weight, the total amount corresponding to 100%.
[0088] Steps 3 to 6 are repeated 9 times at different points, and then an average value is determined from the values obtained from a total of 10 individual measurements.
[0089] (ii) the ratio of the content of element M4 in the bonding layer to the content of metal M2 in the bonding layer (characteristic [M(M4) / M(M2)] ICP How to determine: Ratio in the bonding layer of metal-ceramic substrate [M(M4) / M(M2)] ICP is preferably determined as follows:
[0090] The metal-ceramic substrate to be examined is transferred to a plastic beaker made of HDPE (high density polyethylene) and mixed with hydrochloric acid (concentration = 30%) and nitric acid (concentration = 65%) with low heat supply. Hydrofluoric acid (concentration = 40%) is added to the digestion to dissolve further insoluble components. For metal-ceramic substrates of conventional dimensions, the following amounts of acid have proven advantageous: 30 mL hydrochloric acid (concentration = 30%), 20 mL nitric acid (concentration = 65%) and 50 μL hydrofluoric acid (concentration = 40%).
[0091] The sample solution thus obtained is transferred to a tared polyethylene bottle. The sample solution is then diluted with water according to the expected value for the content of the element to be examined. An aliquot of the sample solution is transferred to a 100 mL volumetric flask and 10 mL of hydrochloric acid (30 wt%), 10 mL of buffered saline (10 g / L sodium chloride) and a calibration standard (e.g. 1 g / L yttrium solution) are prepared. The measurement solution thus obtained is analyzed by ICP-OES (Inductively Coupled Plasma-Optical Emission Spectroscopy) to determine the ratio [M(M4) / M(M2)] relative to the calibration standard. ICP For this purpose, an ICP optical emission spectrometer iCAP 6500 Duo (Thermo Scientific Inc.) is used, and the following plasma settings are configured for the measurement: purge pump speed (rpm): 35; analysis pump speed (rpm): 35; pump tube type: Tygon Orange / white; HF power: 1150 W; atomizer gas: 0.60 L / min; auxiliary gas: 0.5 L / min.
[0092] The present invention is illustrated by the following illustrative embodiments, which should not be construed as limiting.
[0093] Working Example Preparation of metal-ceramic substrates (Examples 1-8 and Comparative Examples 1-7): In Examples 1 to 8 and Comparative Examples 1 to 7, metal-ceramic substrates with different compositions of the bonding layer were produced. This resulted in respective laminates including a ceramic body, a metal foil, and a solder material in contact with the ceramic body and the metal foil, which were then heated. The metal-ceramic substrates thus obtained were then tested for their bonding strength and their thermal and electrical conductivity.
[0094] For the production of metal-ceramic substrates 1 to 8 according to the invention and comparative examples 1 to 7, pastes according to the compositions shown in Table 1 were first prepared.
[0095] [Table 1]
[0096] For this purpose, tin, titanium hydride and bismuth were successively introduced as powders in the amounts indicated into the indicated amount of organic vehicle containing Texanol and mixed in a static mixer at 35 Hz for 20 minutes until a homogeneous paste was obtained in each case. Copper powder was then added in small portions. The mixture thus produced was stirred until a homogeneous paste was obtained.
[0097] The pastes thus produced were used to bond both sides of a ceramic body to copper foil. For this purpose, a ceramic body having dimensions of 177.8×139.7×0.32 mm (obtained from Toshiba Materials) was used, which had the same front and back sides. Each paste was then sieved through a 165 mesh screen into a ceramic body having dimensions 137×175 mm. 2The paste was screen printed on the back of such a ceramic body in the area of 100 mm and pre-dried at 125° C. for 15 minutes. The paste thickness after pre-drying was 35±5 μm. The device thus produced was then rotated and the paste was printed uniformly on the surface of the ceramic body and pre-dried. The ceramic provided with paste on both sides was then provided with copper foil on both sides, made of oxygen-free highly conductive copper with a purity of 99.99% and dimensions of 174×137×0.3 mm, to obtain a laminate with the following structure: copper foil-pre-dried paste-ceramic-pre-dried paste-copper foil.
[0098] The laminate was then heated in a continuous oven. For this purpose, a silicon carbide plate to which a graphite foil was applied was first placed on the transport chain of the continuous oven. The laminate was placed on the graphite foil, then the laminate was covered with a further graphite foil and the laminate was weighted with a further silicon carbide plate (weight=600 g). The structure was then transported on the transport chain through the heating zone of the continuous oven and heated for 2 minutes starting from 50° C. to a peak temperature of 935° C. (measured on the laminate using a type K thermocouple from Temperatur Messelemente Hettstedt GmbH) within 25 minutes. The temperature of the structure was then cooled again to 50° C. within 25 minutes.
[0099] The metal-ceramic substrate thus obtained was then cooled to room temperature to obtain a metal-ceramic substrate including a ceramic layer bonded to the copper layers on both sides via a bonding layer.
[0100] evaluation: The values according to Table 2 were determined for the metal-ceramic substrates of Examples 1-8 and Comparative Examples 1-7:
[0101] [Table 2]
[0102] Additionally, on the metal-ceramic substrates of Examples 1-8 and Comparative Examples 1-7, the bond strength was determined by peel strength tests, and the electrical conductivity and thermal conductivity were determined.
[0103] The results are shown in Table 3.
[0104] [Table 3] explanation: +++: Adhesion strength of peel strength test > 100N / cm. ++: Adhesion strength of peel strength test = 75<100N / cm. +: Adhesion strength of peel strength test = 40<75N / cm. -: Adhesion strength of peel strength test is <40N / cm.
[0105] Exemplary embodiments depict a metal-ceramic substrate that meets the following criteria: (c1) M(M2) EDX =10~20% by weight, (c2)15% by weight≦[M(M4) / M(M2)] ICP * 1000wt%+M(M2) EDX ≦100% by weight, and (c3) M(Ag) EDX =0~10% by weight
[0106] The bonding layer has a stable bond between the metal layer and the ceramic body and at the same time has high thermal and electrical conductivity. These metal-ceramic substrates do not contain silver, so there are no problems related to silver migration. In comparison, metal-ceramic substrates that do not satisfy conditions (c1) and (c2) result in an unstable bond between the metal layer and the ceramic body, or the resulting metal-ceramic substrate has a comparatively low thermal and electrical conductivity.
[0107] Preparation of metal-ceramic substrates (Examples 9 and 10 and Comparative Example 8): In Examples 9 and 10 and Comparative Example 8, metal-ceramic substrates having different bonding layer compositions were produced in the same manner as in Examples 1 to 8 and Comparative Examples 1 to 7, and then examined for their bonding strength as well as their thermal and electrical conductivity.
[0108] For the preparation of the metal-ceramic substrates, pastes with the compositions shown in Table 4 were used.
[0109] Table 4: evaluation: The values according to Table 2 were determined for the metal-ceramic substrates of Examples 9 and 10 and Comparative Example 8. In addition, the bond strengths on the metal-ceramic substrates of Examples 9 and 10 and Comparative Example 8 were determined by peel strength tests, and the electrical conductivity and thermal conductivity were determined.
[0110] [Table 4] The results are shown in Table 5.
[0111] [Table 5] explanation: +++: Adhesion strength of peel strength test > 100N / cm. ++: Adhesion strength of peel strength test = 75<100N / cm. +: Adhesion strength of peel strength test = 40<75N / cm. -: Adhesion strength of peel strength test is <40N / cm.
[0112] Exemplary embodiments 9 and 10 identify metal-ceramic substrates that meet the following criteria: (c1) M(M2) EDX =10~20% by weight, (c2)15% by weight≦[M(M4) / M(M2)] ICP * 1000wt%+M(M2) EDX ≦100% by weight, and (c3) M(Ag) EDX =0~10% by weight
[0113] The bonding layer has a stable bond between the metal layer and the ceramic body and at the same time has high thermal and electrical conductivity. These metal-ceramic substrates do not contain silver, so there are no problems related to silver migration. In comparison, metal-ceramic substrates that do not satisfy conditions (c1) and (c2) result in an unstable bond between the metal layer and the ceramic body, or the resulting metal-ceramic substrate has a comparatively low thermal and electrical conductivity. [Brief description of the drawings]
[0114] [Figure 1] FIG. 1 is an electron microscope photograph of the bond layer of a metal-ceramic substrate.
Claims
1. (a) a ceramic body; (b) a metal layer; and (c) a bonding layer located between the ceramic body and the metal layer, (i) a metal M1 having a melting point of at least 700° C.; (ii) a metal M2 having a melting point below 700° C.; (iii) a metal M3 selected from the group of active metals, and (iv) a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum, and magnesium; A bonding layer including: A metal-ceramic substrate comprising: The bonding layer has the following characteristics: (c1)M (M2) EDX =10~20 wt%, (c2) 15 wt% ≦ [M (M4) / M (M2)] ICP * 1000 wt% + M (M2) EDX ≦100% by weight, and (c3)M(Ag) EDX <10 wt% The present invention is characterized in that During the ceremony, M (M2) EDX is the content [wt %] of the metal M2 in the bonding layer, determined using EDX; [M(M4) / M(M2)] ICP is the ratio of the content of metal M4 in the bonding layer to the content of metal M2 in the bonding layer, determined using ICP; M(Ag) EDX is the silver content [wt %] in the bonding layer, determined using EDX; Metal-ceramic substrate.
2. 2. The metal-ceramic substrate of claim 1, wherein the ceramic of the ceramic body is selected from the group consisting of aluminum nitride ceramics, silicon nitride ceramics, and aluminum oxide ceramics.
3. 3. The metal-ceramic substrate according to claim 1, wherein the metal of the metal layer is copper.
4. The metal-ceramic substrate according to any one of claims 1 to 3, characterized in that the metal M1 is copper.
5. The metal-ceramic substrate according to any one of claims 1 to 4, characterized in that the metal M2 is tin.
6. The metal-ceramic substrate according to any one of claims 1 to 5, characterized in that the metal M3 is selected from the group consisting of hafnium, titanium, zirconium, niobium, tantalum, vanadium and cerium.
7. A metal-ceramic substrate according to any one of claims 1 to 6, characterized in that the metal M4 is bismuth.
8. The bonding layer has the following characteristics: (c1')M(M2) EDX =10~15wt% The metal-ceramic substrate according to any one of claims 1 to 7, characterized in that it has
9. The bonding layer has the following characteristics: (c2') 15 wt% ≦ [M (M4) / M (M2)] ICP * 1000 wt% + M (M2) EDX ≦70% by weight The metal-ceramic substrate according to any one of claims 1 to 8, characterized in that it has
10. The bonding layer has the following characteristics: (c3')M(Ag) EDX <1% by weight The metal-ceramic substrate according to any one of claims 1 to 9, characterized in that it has
11. 1. A method for producing a metal-ceramic substrate, comprising: a) a laminate, a1) a ceramic body; a2) a metal foil; a3) a solder material in contact with the ceramic body and the metal foil, (i) a metal M1 having a melting point of at least 700° C.; (ii) a metal M2 having a melting point below 700° C.; (iii) a metal M3 selected from the group of active metals, and (iv) a metal M4 selected from the group consisting of bismuth, gallium, zinc, indium, germanium, aluminum and magnesium A solder material comprising: providing a laminate comprising: b) heating the laminate to obtain a metal-ceramic substrate; A method comprising:
12. A module comprising a metal-ceramic substrate according to any one of claims 1 to 10.
Citation Information
Patent Citations
Copper-based interlayer alloy and preparation method thereof, and composite connecting piece of ceramic and oxygen-free copper and welding method thereof
CN113528884A
Kenmazaino metaraizeeshon oyobi korotsuke yogokin
JP1976065056A
Soldering material for active soldering and active soldering method
JP2020527461A
Ductile titanium-indium-copper brazing alloy