Unburned bricks and their manufacturing method

By integrating basic aluminum lactate, sodium aluminate, and phosphate into the refractory mix, the unfired bricks achieve enhanced high-temperature strength and spalling resistance, addressing the limitations of existing unfired bricks and contributing to reduced carbon emissions.

JP7574497B1Active Publication Date: 2024-10-28YOTAI REFRACTORIES
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024117626
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-28
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Existing unfired magnesia-based bricks and alumina-magnesia bricks lack sufficient high-temperature strength and heat spalling resistance, and their production methods do not adequately address carbon dioxide emission reduction.

Method used

Incorporating basic aluminum lactate, sodium aluminate, and phosphate into the refractory raw materials, followed by controlled drying, to form renanite as a binder phase, enhancing high-temperature strength and spalling resistance.

Benefits of technology

The resulting unfired bricks exhibit high compressive and bending strengths at elevated temperatures, reducing carbon dioxide emissions and improving durability and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574497000001
    Figure 0007574497000001
  • Figure 0007574497000002
    Figure 0007574497000002
Patent Text Reader

Abstract

The present invention provides an unfired brick that has excellent hot properties such as high-temperature strength and heat spalling resistance, and contributes to reducing carbon dioxide emissions, and a method for producing the same. [Solution] A method for producing unfired bricks, comprising: a first step of adding 1-2% by mass of an aqueous solution of sodium aluminate by outer percentage to 100% of a refractory raw material containing magnesia or magnesia and spinel as the main component and 1-2% by mass of basic aluminum lactate, and kneading the mixture to obtain a molded body of any shape; and a second step of drying the molded body obtained in the first step to obtain a dried body, characterized in that in the first step, phosphate is added to the main component to which the aqueous solution of sodium aluminate has been added, so that the phosphorus (P) content of the dried body is 0.2-0.6% by mass.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing refractories which can be used, for example, as linings of industrial furnaces such as those used in iron and steel making, non-ferrous metal smelting, lime making, cement making, and glass making. [Background technology]

[0002] Magnesia spinel bricks have excellent heat spalling resistance and volume stability, and are mainly used in rotary kilns that burn cement and lime. Magnesia spinel bricks are fired refractories that are manufactured through a firing process, but from the perspective of reducing carbon dioxide emissions, unfired refractories that do not go through a firing process are superior.

[0003] For example, Patent Document 1 (JP Patent Publication No. 9-87007) proposes "an unfired magnesia brick, characterized in that it contains 0.5 to 10% by weight of a metal powder containing aluminum, 0.5 to 3% by weight of a resin containing carbon converted to fixed carbon, and the remainder being a refractory material mainly composed of magnesia," with the objective of "generating spinel around magnesia particles and forming a structure in which the magnesia particles are bound by the secondarily generated spinel, in order to improve slag penetration of magnesia bricks with excellent slag corrosion resistance."

[0004] In the magnesia unburned brick described in the above Patent Document 1, aluminum reacts with carbon in the resin at a temperature of about 800°C to produce aluminum carbide, and as the temperature rises further, the aluminum carbide reacts with CO in the atmosphere inside the brick to produce alumina and carbon. Alumina reacts with magnesia, the material of the brick, to produce spinel, and this spinel is produced at a temperature of about 1000°C. Therefore, when used to line a molten metal container, the working surface will have a structure mainly composed of magnesia and secondary generated spinel. This secondary generated spinel is highly reactive, so when it comes into contact with slag, the FeO, MnO, and other components in the slag are dissolved in the spinel, suppressing its penetration into the depths of the brick. It is also said that the CaO component in the slag is captured as a CaO·Al2O3 compound by the alumina before the spinel is produced, preventing it from penetrating into the brick.

[0005] Furthermore, Patent Document 2 (JP Patent Publication No. 2000-272956) proposes "an unfired alumina-magnesia brick having a composition of 94.7% by weight Al2O3, 5.3% by weight MgO, 80% by weight of electrofused alumina and 10% by weight of calcined alumina as alumina raw materials, 5% by weight of electrofused magnesia having a particle size of 3.36 to 1.0 mm, and 5% by weight of electrofused spinel having a particle size of 1.0 mm or less as magnesia raw materials," with the objective of "providing an unfired refractory material which has good corrosion resistance and does not crack, peel, open joints, etc. when used to line the inside of the ladle of a secondary refining furnace."

[0006] In the unfired alumina-magnesia brick described in the above Patent Document 2, it is said that the corrosion resistance, expansion amount, and compressive strength can be controlled by setting the magnesia content within an appropriate range, selecting magnesia and spinel as magnesia supply raw materials, and selecting their compounding ratio and particle size. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 9-87007 [Patent Document 2] JP 2000-272956 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, the unfired magnesia brick described in Patent Document 1 and the unfired alumina-magnesia brick described in Patent Document 2 are primarily intended to improve corrosion resistance, and it is difficult to say that their hot properties, such as high-temperature strength, are sufficient.

[0009] In view of the above-mentioned problems in the conventional art, an object of the present invention is to provide an unfired brick which contributes to a reduction in carbon dioxide emissions and which has excellent hot properties such as high-temperature strength and heat spalling resistance, and a method for producing the same. [Means for solving the problem]

[0010] In order to achieve the above object, the present inventors have conducted extensive research into unfired bricks and a method for producing the same, and as a result have discovered that it is extremely effective to incorporate basic aluminum lactate into the refractory raw material, add an aqueous solution of sodium aluminate during kneading, and also add a phosphate, thereby arriving at the present invention.

[0011] That is, the present invention provides: a first step of adding 1 to 2% by mass of an aqueous solution of sodium aluminate in an outer percentage to 100% of a refractory raw material mainly composed of magnesia or magnesia and spinel and containing 1 to 2% by mass of basic aluminum lactate, and kneading the mixture to obtain a molded body of any shape; A second step of drying the molded body obtained in the first step to obtain a dried body, In the first step, a phosphate is added to the main component to which the aqueous sodium aluminate solution has been added, so that the phosphorus (P) content of the dry body is 0.2 to 0.6 mass %; The present invention provides a method for producing an unfired brick, comprising the steps of:

[0012] In the past, no unburned bricks that have not undergone a firing process have been found that exhibit high hot strength in addition to high strength, excellent heat spalling resistance, and volume stability. In contrast, the unburned bricks of the present invention can be imparted with all of these properties by mixing appropriate amounts of basic aluminum lactate, an aqueous solution of sodium aluminate, and a phosphate.

[0013] More specifically, by mixing an appropriate amount of basic aluminum lactate and sodium aluminate, gelation occurs and aluminum lactate is produced. Since aluminum lactate has a moisturizing effect, it is possible to prevent the clay from drying out and obtain a good molded body (first step). Furthermore, by adding phosphate, rhenanite (CaNaPO4: melting point 1830°C), which has a relatively high melting point, is formed as a binding phase, which gives high hot strength to the unfired brick finally obtained through the second step.

[0014] Here, by making the phosphorus (P) content of the dried material after the second process 0.2 mass% or more, the hot strength can be sufficiently improved by the formation of renanilite. On the other hand, by making the phosphorus (P) content of the dried material after the second process 0.6 mass% or less, the effect of adding phosphate on the gelation of basic aluminum lactate can be reduced. In addition, by making the phosphorus (P) content 0.6 mass% or less, the sodium content increased by the addition of phosphate increases, and the formation of a low melting point substance can be suppressed.

[0015] In the unfired brick of the present invention, it is preferable to add at least one of sodium phosphate glass, primary calcium phosphate, potassium phosphate glass, and aluminum phosphate as the phosphate, which can reduce the effect of the addition of the phosphate on the gelation of basic aluminum lactate and can more reliably obtain the effect of improving the hot strength by the formation of rhenanite.

[0016] In the method for producing an unburned brick of the present invention, it is preferable that the Al2O3 solid content concentration of the aqueous sodium aluminate solution is 10 to 20 mass %.

[0017] By adding an aqueous sodium aluminate solution with an Al2O3 solids concentration of 10 to 20 mass% in an outer percentage of 1 to 2 mass% to 100% refractory raw material containing basic aluminum lactate, lactate salts such as sodium lactate decompose during the heating process when used in an actual furnace, and lactic acid evaporates, allowing the highly active aluminum to react with magnesia, allowing the reaction between aluminum and magnesia to form a spinel, which can proceed sufficiently and smoothly.

[0018] Furthermore, the drying temperature in the second step is preferably 200 to 300° C. By setting the drying temperature at 200° C. or higher, the decomposition of sodium lactate and lactic acid can be suppressed while the drying can proceed sufficiently and smoothly, and by setting the drying temperature at 300° C. or lower, the decrease in strength of the unfired bricks can be suppressed and an increase in carbon dioxide emissions related to the drying step can be suppressed.

[0019] The present invention also provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: The main component is magnesia or magnesia and spinel, The phosphorus (P) content is 0.2 to 0.6 mass%; Also provided is an unfired brick characterized by:

[0020] The unfired brick of the present invention is preferably obtained by the manufacturing method of the unfired brick of the present invention, and by setting the phosphorus (P) content to 0.2 to 0.6 mass%, the unfired brick has high strength, high-temperature strength and excellent heat spalling resistance. The main components are magnesia or magnesia and spinel, and the ratio of magnesia to alumina is not particularly limited as long as magnesia is contained.

[0021] In the unfired brick of the present invention, it is preferable that rhenanite (CaNaPO4) is formed. Rhenanite having a high melting point serves as a binding phase, and can provide the unfired brick with excellent high-temperature strength and heat spalling resistance.

[0022] The unfired brick of the present invention preferably has a bending strength of 10 MPa or more at 1200° C. Since the unfired brick has a bending strength of 10 MPa or more at 1200° C., it can be suitably used as an inner lining of industrial furnaces in iron and steel manufacturing, non-ferrous metal smelting, lime manufacturing, cement manufacturing, glass manufacturing, and the like.

[0023] The method for producing unfired bricks of the present invention produces dense molded bodies, which are dried at an appropriate temperature so that lactates such as sodium lactate remain without decomposition. As a result, in the heating process up to 1200°C, lactates such as sodium lactate decompose and lactic acid evaporates, and highly active aluminum reacts with magnesia, allowing the reaction between aluminum and magnesia to form a spinel sufficiently and smoothly. In addition, the addition of phosphoric acid turns rhenanite, which has a high melting point, into a binding phase, allowing the unfired bricks to exhibit high hot strength.

[0024] Furthermore, the unfired brick of the present invention preferably has a compressive strength of 100 MPa or more. The unfired brick has a high compressive strength even at room temperature in addition to excellent hot strength, which can improve the reliability and durability of the unfired brick. Effect of the Invention

[0025] According to the present invention, it is possible to provide an unfired brick which is excellent in hot properties such as high-temperature strength and heat spalling resistance and which contributes to reducing carbon dioxide emissions, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] Representative embodiments of the unfired brick and the method for producing the same according to the present invention will be described in detail below, but the present invention is not limited to these.

[0027] 1. Manufacturing method of unfired bricks The method for producing an unfired brick of the present invention comprises a first step of adding 1-2% by mass of an aqueous solution of sodium aluminate as an outer percentage to 100% of a refractory raw material containing magnesia or magnesia and spinel as a main component and 1-2% by mass of basic aluminum lactate, kneading the mixture, and obtaining a molded body of any shape, and a second step of drying the molded body obtained in the first step to obtain a dried body, characterized in that in the first step, a phosphate is added to the main component to which the aqueous solution of sodium aluminate has been added, so that the phosphorus (P) content of the dried body is 0.2-0.6% by mass. Each step will be described in detail below.

[0028] (1) First step The first step is a step for obtaining a molded body of any shape after adding 1-2 mass% of an aqueous sodium aluminate solution to 100% of a refractory raw material mainly composed of magnesia or magnesia and spinel and containing 1-2 mass% of basic aluminum lactate, and kneading the mixture.The greatest feature of the method for producing an unfired brick of the present invention is that in the first step, a phosphate is further added to the main component to which the aqueous sodium aluminate solution has been added.

[0029] (1-1) Main component The refractory raw material as the main component may be magnesia particles or magnesia particles and spinel particles. The mixing ratio of magnesia particles and spinel particles is not particularly limited as long as it does not impair the effects of the present invention, and may be appropriately adjusted according to the desired properties of the unfired brick. Alternatively, magnesia particles may be used as the main component without using spinel particles.

[0030] It is preferable to mix magnesia particles and spinel particles having different particle sizes, since the mixed raw materials have good heat spalling resistance.

[0031] The type of magnesia raw material is not particularly limited as long as it does not impair the effects of the present invention, but for example, conventionally known electrofused magnesia, seawater magnesia, natural magnesia, etc. In addition, regarding the purity of the magnesia raw material, it is preferable to use a high purity of 95% by weight or more in order to avoid the deterioration of corrosion resistance due to impurities and the influence of over-sintering.

[0032] The type of spinel raw material and the ratio of MgO to Al2O3 are not particularly limited as long as they do not impair the effects of the present invention, and for example, conventionally known alumina-magnesia spinel (MgAl2O4) or magnesia-magnesia spinel can be used. As with the magnesia raw material, it is preferable to use a spinel raw material with a high purity of 95% by weight or more. The spinel raw material is not particularly limited, and electrically fused spinel, fired spinel, etc. can be used.

[0033] (1-2) Essential additives (binders) As an essential additive component, 1 to 2 mass% of basic aluminum lactate is added. Also, 1 to 2 mass% of sodium aluminate aqueous solution is added in an outer percentage to 100% of the refractory raw material containing magnesia and spinel as main components and 1 to 2 mass% of basic aluminum lactate.

[0034] The Al2O3 solid content concentration of the sodium aluminate aqueous solution is preferably 10 to 20 mass%, more preferably 14 to 18 mass%. By adding an aqueous sodium aluminate solution having an Al2O3 solid content concentration of 10 to 20 mass% (outer percentage: 1 to 2 mass%) to 100% of the refractory raw material containing 1 to 2 mass% basic aluminum lactate, the reaction between alumina and magnesia to form a spinel can be sufficiently and smoothly promoted.

[0035] In order to utilize rhenanite having a high melting point as a binder phase, a phosphate is added to the main component to which the sodium aluminate aqueous solution has been added. The type of phosphate to be added is not particularly limited as long as it does not impair the effects of the present invention, but it is preferable to add at least one of sodium phosphate glass, monocalcium phosphate, potassium phosphate glass, and aluminum phosphate. The amount of phosphate added may be adjusted so that the phosphorus (P) content in the finally obtained unfired brick is 0.2 to 0.6 mass%.

[0036] (1-3) Optional additives For example, 1 to 3 mass% of sorbitol can be added as a molding aid to 100% of the refractory raw material. Sorbitol is composed mainly of D-sorbitol and is represented by HOCH2(CHOH)4CH2OH. It is a powder that dissolves easily in water and is generally used as a surfactant or food additive. The addition of sorbitol improves the filling property of the kneaded clay and the lubrication between particles, reduces the change of the clay over time, and inhibits slaking. It is also non-toxic and can obtain a molded body with a high molding density. Additives used as molding aids for fired bricks, such as bittern and magnesium sulfate, can also be used.

[0037] In addition, various conventionally known optional components such as alumina, zirconia and iron oxide used in magnesia bricks and magnesia spinel bricks may be added as long as the effects of the present invention are not impaired.

[0038] (1-4) Mixing and molding The refractory raw material as the main component, the essential additive components, and the optional additive components are kneaded and formed into a desired shape. The kneading and forming methods are not particularly limited, and various conventional methods used in the manufacture of refractories can be applied.

[0039] In the method for producing unfired bricks of the present invention, gelation occurs by mixing appropriate amounts of sodium aluminate and basic aluminum lactate, and aluminum lactate is produced. Since aluminum lactate has a moisturizing effect, drying of the clay is suppressed, and a good molded body can be obtained. Furthermore, the addition of phosphate to such an extent that the phosphorus (P) content in the finally obtained unfired brick is 0.2 to 0.6 mass % does not inhibit gelation caused by mixing appropriate amounts of sodium aluminate and basic aluminum lactate.

[0040] (2)Second process The second step is a step for drying the molded body obtained in the first step to obtain an unfired brick.

[0041] If the molded body obtained in the first step is dried at an appropriate temperature, lactate salts such as sodium lactate remain without being decomposed, and a decrease in strength can be suppressed.

[0042] The drying temperature is preferably 200 to 300° C. By setting the drying temperature at 200° C. or higher, excess water is evaporated and dehydrated, thereby increasing strength. Furthermore, by setting the drying temperature at 300° C. or lower, lactate salts such as sodium lactate remain without being decomposed, suppressing a decrease in strength and suppressing an increase in carbon dioxide emissions related to the drying process.

[0043] The method for drying the molded body is not particularly limited, and various methods conventionally known for use in the production of unfired refractories can be applied.

[0044] The method for producing unburned bricks of the present invention does not preclude the unburned bricks after drying from being fired under appropriate conditions.

[0045] 2. Unfired bricks The unfired brick of the present invention can be suitably obtained by the unfired brick manufacturing method of the present invention, and is characterized in that it contains magnesia or magnesia and spinel as main components and has a phosphorus (P) content of 0.2 to 0.6 mass %.

[0046] The method for measuring the phosphorus (P) content in the unburned brick is not particularly limited, and various conventionally known measuring methods can be used, such as fluorescent X-ray analysis, EPMA measurement, and SEM-EDS measurement.

[0047] In addition, it is preferable that rhenanite (CaNaPO4) is formed in the unfired brick of the present invention. Rhenanite having a high melting point serves as a binding phase, and can provide the unfired brick with excellent high-temperature strength and heat spalling resistance. There is no particular limitation on the method for confirming the formation of rhenanite, but for example, X-ray diffraction measurement or selected area electron diffraction in transmission electron microscope observation can be used.

[0048] The unfired brick of the present invention preferably has a bending strength of 10 MPa or more at 1200° C. Since the unfired brick has a bending strength of 10 MPa or more at 1200° C., it can be suitably used as an inner lining of industrial furnaces in iron and steel manufacturing, non-ferrous metal smelting, lime manufacturing, cement manufacturing, glass manufacturing, and the like.

[0049] The method for measuring the bending strength of an unfired brick at 1200°C is not particularly limited, and various conventionally known measuring methods can be used. For example, a three-point bending test can be performed in an air atmosphere at 1200°C using a hot bending tester. The bending strength of an unfired brick at 1200°C is preferably 10 MPa or more, and more preferably 11 MPa or more.

[0050] The unfired brick of the present invention preferably has a compressive strength of 100 MPa or more. Having a high compressive strength even at room temperature in addition to excellent hot strength can improve the reliability and durability of the unfired brick. The compressive strength is more preferably 110 MPa or more, and most preferably 120 MPa or more.

[0051] Furthermore, the unfired brick of the present invention has excellent corrosion resistance and resistance to structural embrittlement. Specifically, compared with a brick having the same composition but not containing 0.2 to 0.6 mass % of phosphorus (P) (a brick in which rhenanite is not formed), the unfired brick of the present invention has equal to or higher corrosion resistance and resistance to structural embrittlement, and further has extremely excellent hot strength and hot spalling resistance.

[0052] Representative embodiments of the present invention have been described above, but the present invention is not limited to these, and various design modifications are possible, all of which are included in the technical scope of the present invention. EXAMPLES

[0053] Example The raw materials were prepared in the proportions shown in Table 1 as Examples 1 to 5, kneaded in a high-speed mixer, and molded into a shape of 230 x 230 x 85 mm using a hydraulic press. A batch-type dryer was used for drying, and the mixture was kept at 200 to 320°C for 8 hours to obtain unburned bricks as examples of the present invention. The values ​​in Table 1 are shown in mass%, and the amounts of various phosphates, sodium aluminate aqueous solution, sorbitol aqueous solution, and water added are shown as values ​​multiplied by the total amount of magnesia clinker, spinel clinker, and basic aluminum lactate. In addition, the particle size of the magnesia clinker and spinel clinker and the Al2O3 solid content concentration (mass%) of the sodium aluminate aqueous solution are shown.

[0054] Comparative Example Unfired bricks were obtained in the same manner as in the Examples, except that the raw materials were adjusted to the ratios shown in Comparative Examples 1 to 6 in Table 1. Here, only Comparative Example 1 was fired in a tunnel kiln at a maximum temperature of 1750±10°C.

[0055] [Table 1]

[0056] [evaluation] The unfired bricks obtained as the examples and comparative examples were evaluated for corrosion resistance, compressive strength, hot strength, heat spalling resistance, and microstructural embrittlement resistance. In addition, the phosphorus (P) content of each unfired brick was measured.

[0057] (1) Corrosion resistance The corrosion resistance was evaluated by a rotating drum corrosion test. The test method is as follows. The test piece was lined inside the drum, and the test was performed at 1750±50°C using an oxygen-propane burner. A mixture of Portland cement and potassium sulfate in a ratio of 5:1 was added as the corrosion material. After the test was held for 6 hours while changing the corrosion material every hour, the sample was cut in a direction perpendicular to the working surface, and the amount of wear was measured at 8 points to obtain the average amount of wear. The average amount of wear was expressed as an index with the amount of wear in Comparative Example 1 set to 100. The results are shown in Table 2. The smaller the index, the better the corrosion resistance. When the index was 105 or less, it was marked as ◯, when it was more than 105 but less than 115, it was marked as △, and when it was 115 or more, it was marked as ×.

[0058] (2) Compressive strength The compressive strength of a 60mm x 60mm x 60mm test piece was measured using an Amsler strength tester. The results are shown in Table 2. The results were rated as ◯ for 100MPa or more, △ for 70MPa or more but less than 100MPa, and × for less than 70MPa.

[0059] (3) Hot strength The hot strength of a 30mm x 30mm x 120mm test piece was measured using a hot bending tester. Three-point bending (support distance 80mm) was performed in an air atmosphere at 1200℃, and the results are shown in Table 2. Hot bending strength of 10MPa or more was marked as ◯, 5MPa or more but less than 10MPa was marked as △, and less than 5MPa was marked as ×.

[0060] (4) Heat spalling resistance Heat spalling resistance was evaluated using the air cooling method based on JIS R2657. The temperature condition was 1400°C, and heating and cooling were performed a maximum of 10 times. If the specimen spalled during the process, the number of operations at which it spalled was recorded, and if it did not spall until the end, the depth of the crack was measured. The depths of the cracks were compared relatively, with large cracks rated as "large", medium cracks rated as "medium", and small cracks rated as "small". Large cracks were also rated as "x", medium cracks rated as "△", and small cracks rated as "o". The results are shown in Table 2.

[0061] (5) Resistance to structural embrittlement After the heat spalling resistance test, the test piece was cut perpendicular to the working surface, and the surface condition of the cut surface was confirmed. The depth of grain shedding from the heated surface was regarded as the embrittled layer, and the resistance to embrittlement was evaluated. A grain shedding range of 50mm or less was rated as ◯, a grain shedding range of more than 50mm to 60mm was △, and a grain shedding range of more than 60mm was ×. The results are shown in Table 2.

[0062] (6) Phosphorus (P) content The phosphorus (P) content was measured using X-ray fluorescence analysis. The ZSX PrimusIII+ manufactured by Rigaku Corporation was used for the measurement. The results are shown in Table 2.

[0063] [Table 2]

[0064] In the examples of the present invention, all the unfired bricks have a phosphorus (P) content of 0.2 to 0.6 mass%. In addition, all the unfired bricks exhibit high hot strength, with a hot bending strength of 10 MPa or more at 1200°C. In contrast, in the comparative examples, there are no unfired bricks with a hot bending strength of 10 MPa or more at 1200°C, except for the unfired brick of Comparative Example 1, which is a fired material.

[0065] In addition, in the examples of the present invention, the heat spalling resistance of all the unfired bricks was evaluated as ◯. In contrast, in the comparative examples, only the unfired brick of Comparative Example 1, which is a fired material, was evaluated as ◯ in heat spalling resistance. Even when phosphate (sodium phosphate glass) was added, the heat spalling resistance of Comparative Example 5, in which the (P) content of the unfired brick is 0.96 mass%, was evaluated as △, and the heat spalling resistance of Comparative Example 6, in which the (P) content is 1.92 mass%, was evaluated as ×. This is because the phosphorus content increases with the addition of sodium phosphate glass, making it easier for low-melting point substances to be formed.

[0066] Furthermore, in the examples of the present invention, all the unfired bricks were evaluated as "good" in terms of corrosion resistance, resistance to microstructural embrittlement and compressive strength. This shows that the unfired bricks of the present invention are not only excellent in hot properties such as high-temperature strength and heat spalling resistance, but also in corrosion resistance, resistance to microstructural embrittlement and compressive strength.

[0067] In contrast, in Comparative Example 2, in which alumina cement was added without adding phosphate, low melting point substances were easily formed due to the high CaO content, and the hot bending strength and heat spalling resistance were reduced.

[0068] In Comparative Example 3, which uses a carbon bond with the addition of phenolic resin, the hot bending strength is reduced due to oxidation. In Comparative Example 4, which uses powdered sodium silicate, low melting point substances are easily formed due to SiO2 and Na2O, and the hot bending strength and heat spalling resistance are reduced.

[0069] From the above results, it is clear that in order to obtain unfired bricks with excellent hot properties such as high-temperature strength and heat spalling resistance, it is important to add 1 to 2 mass% of an aqueous solution of sodium aluminate in an outer percentage to 100% of a refractory raw material containing magnesia or magnesia and spinel as the main components and 1 to 2 mass% of basic aluminum lactate, and further add a phosphate to adjust the phosphorus (P) content of the dry body to 0.2 to 0.6 mass%.

Claims

1. a first step of adding 1 to 2% by mass of an aqueous solution of sodium aluminate in an outer percentage to 100% of a refractory raw material mainly composed of magnesia or magnesia and spinel and containing 1 to 2% by mass of basic aluminum lactate, and kneading the mixture to obtain a molded body of any shape; A second step of drying the molded body obtained in the first step to obtain a dried body, In the first step, a phosphate is added to the main component to which the sodium aluminate aqueous solution has been added, so that the phosphorus (P) content of the dried body is 0.2 to 0.6 mass %, The aqueous sodium aluminate solution has an Al 2 O 3 solid content concentration of 10 to 20 mass %; A method for producing unfired bricks, comprising the steps of:

2. Adding at least one of sodium phosphate glass, monocalcium phosphate, potassium phosphate glass, and aluminum phosphate as the phosphate; 2. A method for producing an unfired brick according to claim 1, comprising the steps of:

3. The main component is magnesia or magnesia and spinel, The phosphorus (P) content is 0.2 to 0.6 mass %, The compressive strength is 100 MPa or more. An unfired brick characterized by:

4. Renanite (CaNaPO 4 ) is formed, 4. The unfired brick according to claim 3,

5. The bending strength at 1200°C is 10 MPa or more; 5. The unfired brick according to claim 3 or 4,

Citation Information

Patent Citations

  • Flow-in spinnel refractory furnace material and manufacture

    JP1982129878A

  • binder

    JP1983140371A

  • Refractories blended with synthetic binder phase

    JP1984156958A

  • Basic refractory composition

    JP1986068367A

  • Magnesia carbon brick

    JP1993024910A