Method for manufacturing glass plate, method for chamfering glass plate, and method for manufacturing magnetic disk
Patent Information
- Application Number
- LAP782
- Authority / Receiving Office
- LA · LA
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-11-30
- Filing Date
- 2019-12-02
- Publication Date
- 2023-10-20
AI Technical Summary
The existing methods for manufacturing glass plates for magnetic disks face challenges in precisely shaping the end faces to prevent particle adhesion and ensure accurate assembly, particularly with thin, high-rigidity glass substrates, where ultrashort pulse lasers struggle to maintain target shape consistency and require complex settings.
A method involving irradiation of the glass plate end faces with a laser beam, moving it circumferentially, with a single-mode cross-sectional intensity distribution, controlled power density, and speed to form a chamfered surface, ensuring the end face is processed into a target shape without variations, and maintaining a smooth surface roughness.
This approach allows for efficient and precise shaping of glass plate end faces, preventing particle adhesion and ensuring accurate assembly, while maintaining the rigidity of the glass substrate, thus enhancing the performance and capacity of hard disk drive devices.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Method for manufacturing a glass plate, method for beveling a glass plate, and method for manufacturing a magnetic disk
[0001] The present invention relates to a method for manufacturing a glass plate that processes the shape of the edge surface of a disc-shaped glass plate, a method for chamfering a glass plate to form a chamfered surface on the edge surface of a disc-shaped glass plate by irradiation with laser light, a method for manufacturing a glass plate, or a method for manufacturing a magnetic disk using a chamfering method.
[0002] Hard disk drives for data recording use magnetic disks, which consist of a disc-shaped, non-magnetic glass substrate for magnetic disks with a magnetic layer. When manufacturing glass substrates for magnetic disks, it is preferable to smooth the surface of the disc-shaped glass base plate that forms the basis of the final product, the glass substrate for magnetic disks, to prevent fine particles from adhering to the main surface and adversely affecting the performance of the magnetic disk. Furthermore, it is preferable to align the edge surface of the glass plate to a target shape, both for accurate assembly of the magnetic disk into the HDD device and to make it suitable for gripping by a jig used to hold the outer edge surface of the glass substrate when forming the magnetic film on the main surface of the glass substrate.
[0003] A method for shaping the edge of a glass plate to a target form is known, which involves chamfering the edge of the glass plate using laser light (Patent Document 1). Specifically, an ultrashort pulse laser is used to cut the edge to the desired chamfer shape, and following the ultrashort pulse laser treatment, CO2 is used. 2 The laser is shone on it.
[0004] Special table 2017-511777 publication
[0005] In the edge shaping process described above, which forms a side wall surface and a chamfered surface on the edge of a glass plate, CO2 is used after cutting the edge with an ultrashort pulse laser. 2 The material to be removed is separated by irradiating it with a laser. However, due to the precision of edge cutting by the ultrashort pulse laser, it was not possible to process the end face into the target shape, and the shape of the end face was difficult to achieve, resulting in variations in the shape suitable for gripping with the jig during the magnetic film formation process described above. In addition, the ultrashort laser and CO2 2Because lasers were used in conjunction with other methods to shape the end faces, the shaping process was complicated.
[0006] In recent years, in order to increase the capacity of hard disk drives (HDDs), there has been a trend to thin the glass plates of magnetic disks and increase the number of magnetic disks incorporated into HDDs. In this case, to suppress the vibration of the glass plates that is more likely to occur as the glass substrate becomes thinner, glass materials that increase the rigidity of the glass plates are used. High-rigidity glass materials generally have a high softening point, making them difficult to shape with laser light. Therefore, in order to process the edge face of a thin glass plate with a high softening point into a target shape using laser light, and to suppress the variation of the edge face shape from the target shape, it is necessary to set the laser light irradiation conditions more precisely than before.
[0007] Therefore, the present invention aims to provide a method for manufacturing a glass plate and a magnetic disk that, when shaping the edge surface of a disc-shaped glass plate using laser light, allows the edge surface shape to be processed with simple operation without variation from the target shape.
[0008] One aspect of the present invention is a method for manufacturing a glass plate that processes the shape of the end face of a disc-shaped glass plate. The disc-shaped glass plate has a main surface and an end face perpendicular to the main surface. The manufacturing method includes the step of irradiating the end face with laser light and processing the end face into a target shape while moving the laser light relative to the end face in the circumferential direction of the disc-shaped glass plate, wherein the cross-sectional intensity distribution of the laser light irradiated to the end face is single-mode, and when the width of the luminous beam of the laser light at the irradiation position on the end face in the thickness direction of the glass plate is W1 [mm], the thickness of the glass plate is Th [mm], and the power density of the laser light is Pd, then W1 > Th and Pd × Th is 0.8 to 3.5 [W / mm].
[0009] Another aspect of the present invention is a method for manufacturing a glass plate that processes the shape of the end face of a disc-shaped glass plate. The disc-shaped glass plate has a main surface and an end face perpendicular to the main surface. The manufacturing method includes the step of irradiating the end face with laser light and processing it into a target shape by forming a chamfered surface on the end face while moving the laser light relative to the end face in the circumferential direction of the disc-shaped glass plate, wherein the cross-sectional intensity distribution of the laser light irradiated on the end face is single-mode, and when the width of the luminous beam of the laser light at the irradiation position on the end face in the thickness direction of the glass plate is W1 [mm], the thickness of the glass plate is Th [mm], and the power density of the laser light is Pd, W1 > Th, and when Pd × Th is x, and the moving speed of the laser light moving along the end face is y, the value of Pd × Th and the value of the moving speed are adjusted so that y is within the range of 11.2・x - 4.7 or less.
[0010] Preferably, the laser light is irradiated onto the end face of the glass plate from the direction normal to the end face.
[0011] In the shaping process described above, it is preferable that the irradiation conditions of the laser light are set such that the end face forms a side wall surface perpendicular to the two opposing main surfaces of the glass plate, and a chamfered surface connecting the ends of both sides of the side wall surface and the end of the main surface.
[0012] It is preferable that the irradiation conditions are set such that the ratio (C / Th) of the length C of the chamfered surface along the main surface to the thickness Th is 0.1 to 0.7.
[0013] Preferably, the surface roughness Rz of the end face formed by the laser light is 0.3 μm or less, and the arithmetic mean roughness Ra is 0.03 μm or less.
[0014] Preferably, the laser beam irradiated onto the end face is elliptical in shape, and the ratio of the circumferential length W2 of the laser beam irradiated onto the end face to the diameter D of the glass plate (W2 / D) is 0.03 to 0.3.
[0015] Preferably, the power density Pd is set such that the diameter of the glass plate formed by irradiation with the laser light is greater than the diameter of the glass plate before irradiation with the laser light.
[0016] The speed at which the laser beam moves along the end face is preferably 0.7 to 100 mm / second.
[0017] The Young's modulus of the glass plate is preferably 70 [GPa] or higher.
[0018] The glass plate has a coefficient of thermal expansion of 100 × 10 -7 It is preferable that the value is [1 / K] or less.
[0019] The aforementioned thickness Th is preferably 0.7 mm or less.
[0020] The method for manufacturing the glass plate includes a step of grinding or polishing the main surface of the glass plate that has undergone the shaping process, and it is preferable that, after the shaping process and before grinding or polishing the main surface, the end face is not polished, or if the end face is polished, the amount of material removed by polishing the end face is 5 μm or less.
[0021] Another aspect of the present invention is a method for chamfering a glass plate, in which a chamfered surface is formed on the end face of a disc-shaped glass plate by irradiation with laser light. Before the formation of the chamfered surface, the end face of the glass plate has a surface perpendicular to the main surface at least in the center in the thickness direction of the glass plate. The chamfering method involves irradiating the end face of the glass plate with laser light to soften and / or melt the edge portion of the end face of the glass plate, thereby chamfering the edge portion into a rounded shape, and controlling Pd × Th and the moving speed V, where Th is the thickness of the glass plate, Pd is the power density of the laser light, and V is the moving speed of the laser light moving along the end face, so that a surface perpendicular to the main surface of the glass plate is formed on the end face after the chamfered surface is formed.
[0022] When Pd × Th is x and the moving speed V is y, it is preferable to adjust the value of Pd × Th and the value of the moving speed V so that y is within the range of 11.2・x - 4.7 and 5.4・x - 4.5.
[0023] Yet another aspect of the present invention is a method for manufacturing a glass plate, characterized by performing chamfering on the end face of a disc-shaped glass plate using the chamfering method described above.
[0024] Yet another aspect of the present invention is a method for manufacturing a magnetic disk, characterized by forming a magnetic film on the main surface of a glass plate manufactured by the glass plate manufacturing method described above.
[0025] Another aspect of the present invention is a method for manufacturing a magnetic disk, characterized by forming a magnetic film on the main surface of a glass plate manufactured by the glass plate manufacturing method described above.
[0026] According to the magnetic disk manufacturing method described above, when the edge surface of a disc-shaped glass plate is shaped using laser light, the edge surface shape can be shaped with simple operation without variations in the shape of the edge surface relative to the target shape.
[0027] This figure illustrates the irradiation of laser light in a glass plate manufacturing method according to one embodiment. This figure illustrates an example of the shape of the light beam at the laser light irradiation position. This figure illustrates the light beam and light intensity distribution at the laser light irradiation position. This figure illustrates the shape of the end face after shaping by laser light. Figures (a) to (c) illustrate the difference in the shape of the end face due to differences in laser light irradiation conditions. This figure shows the evaluation results of an experimental example.
[0028] Figure 1 illustrates the irradiation of laser light in a glass plate manufacturing method according to one embodiment. Figure 2 illustrates an example of the shape of the light beam (spot) at the laser light irradiation position. Figure 3 illustrates the light beam and light intensity distribution at the laser light irradiation position. Figure 4 illustrates the shape of the end face after shaping by laser light.
[0029] The glass plate shaped by the glass plate manufacturing method of this embodiment is disc-shaped, with a circular hole drilled at the center of the disc shape, such that an inner circumference is concentric with the outer circumference. To produce a glass plate with an end face aligned to a target shape, or to prevent the connection between the end face and the main surface of the glass plate from becoming a sharp edge, the glass plate is shaped to form a chamfer at the connection between the main surface and the end face. In particular, when manufacturing a disc-shaped glass substrate for magnetic disks with a circular hole, it is desirable that the shape of the end face of the disc-shaped glass plate that forms the basis of the final product, the glass substrate for magnetic disks, be aligned to a target shape in order to accurately incorporate the magnetic disk into the HDD device, and also in order to reliably grip the end face of the glass substrate with a jig when forming a magnetic film on the main surface of the glass substrate. Furthermore, it is desirable to smooth the surface of the end face, where particles are likely to be generated, in order to prevent fine particles from adhering to the main surface and adversely affecting the performance of the magnetic disk. For this purpose, in this embodiment, a laser beam is used to perform the shape processing for chamfering.
[0030] Specifically, as shown in Figure 1, the disc-shaped glass plate 10 with a circular hole 16 has a main surface 12 and an end surface 14. The end surface 14 is perpendicular to the main surface 12. In the example shown in Figure 1, the outer peripheral end surface is used as the end surface 14 for shaping with laser light, but the inner peripheral end surface along the circular hole 16 can also be used for shaping with laser light. In this embodiment, laser light is irradiated onto the end surface 14, and the end surface 14 is shaped into the target shape by moving the laser light L relative to the end surface 14 in the circumferential direction of the disc-shaped glass plate 10. The laser light L is emitted from a laser light source 20 (described later), passed through an optical system 22 including a collimeter to become parallel light, then focused through a focusing lens 24, and the expanded laser light L is irradiated onto the end surface 14. Meanwhile, the glass plate 10 is rotated at a constant speed with its center as the center of rotation. In this way, the laser beam L and the end face 14 are moved relative to each other in the circumferential direction of the disc-shaped glass plate 10, and the laser beam L irradiates the entire circumference of the end face 14 of the glass plate 10. Here, it is preferable that the irradiation of the end face 14 with the laser beam L be performed from the direction normal to the end face 14 being irradiated. In addition to the perfect normal direction (inclination angle of 0 degrees), an inclination angle of 10 degrees or less relative to the normal direction is also an acceptable range for irradiation of the end face 14 with the laser beam L.
[0031] The cross-sectional intensity distribution of the laser beam L irradiated onto the end face 14 is single-mode. That is, the cross-sectional intensity distribution of the laser beam L is a Gaussian distribution. As shown in Figure 2, the width of the light beam at the irradiation position on the end face 14 of such a laser beam L in the thickness direction of the glass plate 10 is W1 [mm], the thickness of the glass plate 10 is Th [mm], and the power density of the laser beam L is Pd [W / mm]. 2When [condition], for the irradiation of the laser beam L, irradiation conditions are used where W1 > Th and Pd × Th is 0.8 to 3.5 [W / mm]. Here, as shown in FIG. 2, the laser beam L is irradiated so as to protrude beyond both sides in the thickness direction of the glass plate 10. Also, by making the widths protruding beyond both sides of the end face equal, chamfers can be evenly performed on both sides in the thickness direction of the glass plate 10, and the shapes of the two chamfer surfaces 14c can be made equal. The power density Pd is a value obtained by dividing the total power P [W] of the laser beam L by the area of the cross-section of the laser beam at the portion irradiated with the laser beam L. When the laser beam L has an elliptical shape (see FIG. 2) with a minor-axis radius of W1 / 2 and a major-axis radius of W2 / 2, the power density Pd is defined as 4 × P / W1 / W2 / π [W / mm 2 (π is the ratio of the circumference of a circle to its diameter).
[0032] Here, as an example of the laser beam L, CO 2 laser beam is used, but any oscillation wavelength with absorption in glass may be used, and it is not limited to the CO 2 laser beam. For example, a CO laser (oscillation wavelength of about 5 μm or 10.6 μm), an Er-YAG laser (oscillation wavelength of about 2.94 μm), etc. can be mentioned. CO 2When using laser light, the wavelength is preferably 3 μm or longer. Furthermore, a wavelength of 11 μm or less is even more preferable. If the wavelength is shorter than 3 μm, the glass will not absorb the laser light well, and the end face 14 of the glass plate 10 may not be heated sufficiently. Also, if the wavelength is longer than 11 μm, it may be difficult to obtain a suitable laser device. The oscillation mode of the laser light source 20 is not particularly limited and may be continuous wave (CW) light, pulsed light, or modulated continuous wave light. However, in the case of pulsed light and modulated continuous wave light, if the relative movement speed of the laser light L is fast, there is a risk of unevenness in the shape of the chamfered surface 14c in the direction of movement. In that case, the oscillation and modulation frequencies are preferably 1 kHz or higher, more preferably 5 kHz or higher, and even more preferably 10 kHz or higher. The width W1 of the light beam and the length W2, which will be described later, can be set by adjusting the irradiation position of the laser light L onto the glass plate 10, for example, using two cylindrical lenses. Furthermore, the width W1 can be determined from the beam profiler, and the length W2 can be determined from the beam shape obtained from the beam profiler and the diameter D of the glass plate.
[0033] By making the width W1 of the laser beam L greater than the thickness Th of the glass plate 10, the laser beam L can be sufficiently irradiated to the side edge of the end face 14 on the main surface 12 side, and a chamfered surface can be formed by softening and / or melting a part of the glass plate 10 with heat. If the ratio Th / W1 of the width W1 of the laser beam L to the thickness of the glass plate 10 is made too large (i.e., Th / W1 approaches 1), the gradient of the laser intensity distribution is affected by a range with a steep slope, so that the heating of the edge portion of the glass plate 10 is weak, and the heating of the central portion in the thickness direction of the end face of the glass plate is strong. As a result, a spherical shape of the end face, as described later, is likely to occur, which is undesirable. Also, if the ratio Th / W1 of the width W1 of the laser beam L to the thickness of the glass plate 10 is made too small, the heating of the end face 14 by the laser beam L may be too small, making it difficult to form a chamfered surface. From the above viewpoint, it is preferable that Th / W1 is in the range of 0.3 to 0.9. On the one hand, if the power density Pd of the laser light L is excessively low, the end face 14 will not be heated sufficiently and a chamfered surface will not be formed. On the other hand, if the power density Pd is excessively high, the entire end face 14 will be rounded into a spherical shape by the heat, and the thickness in the thickness direction of the spherical shape will be greater than the thickness Th of the glass plate 10. For this reason, the irradiation conditions are set to W1 > Th and Pd × Th = 0.8 to 3.5 [W / mm]. Pd × Th is preferably 3.0 [W / mm] or less, more preferably 1.0 to 2.8 [W / mm], and even more preferably 1.2 to 2.3 [W / mm]. Since Pd × Th = 0.8 to 3.5 [W / mm], the thickness Th of the glass plate 10 becomes thinner, and if the irradiation conditions deviate from Pd × Th = 0.8 to 3.5 [W / mm], it means that the power density Pd will be increased. By increasing the power density Pd, the reduced irradiation area of the glass plate 10 by the laser light L can be compensated for by the increased power density Pd, making it possible to form a chamfered surface.
[0034] By using these irradiation conditions, the shape of the end face 14 of the glass plate 10 can be aligned without deviation from the target shape, and a chamfered surface can be formed. Moreover, the surface of the end face 14 can be made smooth.
[0035] In the above embodiment, the chamfered surface 14c can be formed by limiting the range of the Pd × Th value. However, by controlling the Pd × Th value and the moving speed value and irradiating the end face 14 with laser light L, the chamfered surface 14c can be efficiently formed on the end face 14 of the glass plate 10. Furthermore, by controlling the Pd × Th value and the moving speed value in more detail, not only the chamfered surface 14c but also a surface perpendicular to the main surface 12 of the glass plate 10, i.e., a side wall surface 14t, can be formed. This makes it possible to align the shape of the end face 14 without variation relative to the target shape. Moreover, the surface of the end face 14 can be made smooth. In this case, the end face 14 of the glass plate 10 before the chamfered surface 14c is formed has a surface perpendicular to the main surface 12 at least in the center in the thickness direction of the glass plate 10. By irradiating the end face 14 of the glass plate 10 with laser light L, the edges on both sides of the end face 14 in the thickness direction (the boundary portion between the main surface 12 and the end face 14), for example, the corners that are bent at right angles, are softened and / or melted, thereby chamfering the edges of the end face 14 into a rounded shape, and a surface (side wall surface 14t) perpendicular to the main surface 12, sandwiched between the chamfered surfaces 14c on both sides of the glass plate 10 in the thickness direction, can be formed on the chamfered end face 14. In particular, it is preferable that the end face 14 comprises a surface perpendicular to the main surface 12 with a length of at least one-tenth of the thickness Th, and the chamfered surfaces 14c. It is more preferable that the length T (see Figure 4) of the perpendicular surface (side wall surface 14t) is at least one-fifth of the thickness Th. The vertical surface formed together with the chamfered surface 14c by irradiation with the laser light L is, according to one embodiment, a newly formed surface, unlike the surface perpendicular to the main surface 12 of the end face 14 before the chamfered surface 14c is formed by irradiation with the laser light L. Therefore, the surface roughness Rz and arithmetic mean roughness Ra are reduced by irradiation with the laser light L. In addition, the radial distance from the center position of the disc-shaped glass plate 10 to the vertical surface increases. Note that the surface perpendicular to the main surface 12 is a surface whose tolerance range is 90 degrees ± 2 degrees relative to the main surface 12.
[0036] Forming a chamfered surface 14c on the end face 14, as well as a surface perpendicular to the vertical main surface 12 (side wall surface 14t), is preferable because it can suppress variations in the outer diameter (diameter) or inner diameter (diameter of the circular hole 16) of the glass plate 10 with the chamfered surface 14c formed on it, either within a single glass plate 10 or between glass plates 10. For example, if the outer diameter varies, when multiple glass plates 10 are assembled into an HDD device as substrates for magnetic disks and rotated, it can easily disrupt the airflow, potentially increasing problems such as head crashes. Also, when forming a magnetic film using a film deposition device such as a sputtering device, there is a risk of problems such as the glass plate 10 falling due to failure to grip the end face 14 of the glass plate 10. Furthermore, if the inner diameter of the glass plate 10 varies, it may not pass through the spindle when assembled into an HDD device, and the gap between the glass plate 10 and the spindle may become excessively large, potentially disrupting the rotational balance.
[0037] The ability to change the shape of the chamfered surface 14c in various ways by controlling the Pd × Th value and the moving speed value is based on the following idea. That is, if at least the central part in the thickness direction of the end face 14 of the glass plate 10 before irradiation with the laser beam L is a surface perpendicular to the main surface 12 (side wall surface 14t), it has been found that by adjusting the conditions when irradiating with the laser beam L, a surface perpendicular to the main surface 12 (side wall surface 14t) can be formed while simultaneously forming the chamfered surface 14c. Although this mechanism is not entirely clear, it is assumed that there exists a condition in which a perpendicular surface is formed on the end face 14 between the condition in which the chamfering of the end face 14 does not progress (see Figure 5(a)) and the condition in which the entire end face 14 becomes rounded (see Figure 5(b)), and that this condition can be selected by appropriately adjusting Pd × Th and the moving speed. In other words, for example, if the value of Pd × Th is increased while keeping the moving speed constant, it is assumed that the formation of the chamfered surface 14c progresses in the following order: starting from the edge, gradually progressing toward the center in the thickness direction, and finally the entire end face 14 becomes rounded. Here, as the rounding progresses, the length T in the thickness direction of the vertical surface (side wall surface 14t) of the end face 14 gradually decreases.
[0038] A method for manufacturing a glass plate, including the shaping of such a glass plate 10, will be described below using a method for manufacturing a glass substrate for a magnetic disk.
[0039] The glass substrate for magnetic disks is a thin, disc-shaped glass substrate with a circular hole, similar to the glass plate 10 shown in Figure 1(a). The size of the glass substrate for magnetic disks is not specified, but it is typically a nominal diameter of 2.5 inches or 3.5 inches. For a glass substrate with a nominal diameter of 3.5 inches, the outer diameter (nominal value) is, for example, 95 mm to 97 mm. For a glass substrate with a nominal diameter of 2.5 inches, the outer diameter (nominal value) is, for example, 65 mm to 67 mm. The thickness of the glass substrate for magnetic disks is, for example, 0.20 mm to 0.65 mm, preferably 0.30 mm to 0.53 mm. A magnetic layer is formed on the main surface of this glass substrate to create a magnetic disk.
[0040] The glass substrate, like the outer peripheral end of the glass plate 10 shown in Figure 4, includes a pair of main surfaces 12, 12, a side wall surface 14t formed on the end face 14 of the outer peripheral end, chamfered surfaces 14c, 14c interposed between the side wall surface 14t and the main surfaces 12, 12, and the end face of the inner peripheral end also includes a side wall surface (not shown) and a chamfered surface (not shown) interposed between this side wall surface and the main surfaces 12, 12, similar to the end face 14 of the outer peripheral end. The side wall surface 14t is a surface that extends in a direction substantially perpendicular to the main surface 12. "Substantially perpendicular" means that the inclination angle of the side wall surface 14t with respect to the main surface 12 is in the range of 88 to 92 degrees. Let T [mm] be the length of the side wall surface 14t along the thickness direction shown in Figure 4. The chamfered surface 14c is smoothly connected to the main surface 14 and extends toward the side wall surface 14t. The chamfered surface 14c has a curved shape that is convex outward and smoothly connects to the side wall surface 14t. Therefore, the length C [mm] of the chamfered surface 14c shown in Figure 4 along the main surface 12 is the length of the portion that is inclined with respect to the main surface 12 at an angle of more than 2 degrees and less than 88 degrees. In the case where the shape of the end surface 14 is spherical, as shown in Figure 5(c) later, the length C of the chamfered surface 14c is defined as the distance in the direction of the main surface 12 from the thickest point in the thickness direction of the glass plate 10 to the very end.
[0041] Such glass substrates can be prepared, for example, by cutting a glass blank slightly larger than the size of the glass plate 10 from a large pre-fabricated glass plate using a laser beam. The large sheet glass before cutting the glass blank is, for example, a glass plate of a certain thickness produced using the floating method or the down-draw method. Alternatively, it may be a glass plate formed by press-forming a block of glass using a mold. The thickness of the glass plate is thicker than the target thickness when it becomes the final product, a glass substrate for magnetic disks, by the amount of material to be removed by grinding and polishing, for example, several μm to several hundred μm thicker. In addition to the method of cutting the glass blank using a laser beam, a conventional method may also be used, in which notches are formed in the glass plate using a scriber and cracks are generated along the notches by heating or the like to break the plate. Alternatively, the glass blank may be cut by wet etching using an etching solution such as hydrofluoric acid.
[0042] When cutting glass blanks from a large sheet of glass using laser light, solid-state lasers such as YAG lasers or Nd:YAG lasers are used as the laser light source. Therefore, the wavelength of the laser light is, for example, in the range of 1030 nm to 1070 nm. In this case, the laser light is, for example, a pulsed laser, with a pulse width of 10 × 10⁻¹⁰. -12 The pulse duration is less than 10 picoseconds. The light energy of the laser beam can be adjusted as appropriate according to the pulse width and the pulse repetition frequency. By irradiating with this laser beam, defects can be intermittently formed at discrete positions along the boundary line to be cut. After this, the outer and inner parts of the glass plate are separated by heating the outer part more intensely than the inner part, or by heating the outer part. Alternatively, a different type of laser beam may be irradiated along the boundary line so that the defects discretely formed along the boundary line to be cut become linearly continuous. For example, as a different type of laser beam, CO 2A laser can be used. This laser light can be used to form linear defects that connect intermittently formed defects. In this case, the outer and inner parts of the glass plate can be separated by heating the outer part more intensely than the inner part, or by heating the outer part, as needed, with respect to the boundary line. In this way, a disc-shaped glass blank can be cut from the sheet glass. The surface roughness Rz of the end face of the disc-shaped glass blank formed in this way is, for example, 1 to 10 μm, and the arithmetic mean roughness Ra is, for example, 0.1 to 1 μm.
[0043] Furthermore, in order to create concentric circular holes in the cut-out disc-shaped glass blank, the holes are made by laser irradiation, using a scriber, or etching, similar to the method described above. The glass blank with the circular holes becomes the glass substrate when manufacturing a glass substrate for a magnetic disk.
[0044] To form chamfered surfaces 14c on the end faces 14 (the outer and inner end faces) of the disc-shaped glass plate 10 obtained as shown in Figure 1, shaping is performed using a laser beam L. In shaping with a laser beam L, as described above, the laser beam L is irradiated onto the end face 14 of the glass plate 10 (glass base plate), preferably from the direction normal to the end face 14, and the shape of the end face 14 is processed to the target shape while the end face 14 and the laser beam L are moved relative to each other in the circumferential direction of the disc-shaped glass plate 10. The laser beam L is a laser beam having a single-mode cross-sectional intensity distribution, and the irradiation conditions for the laser beam L are set to width W1 > thickness Th, and Pd × Th is 0.8 to 3.5 [W / mm]. This makes it possible to align the shape of the end face 14 of the glass plate 10 with respect to the target shape without variation, and to form chamfered surfaces 14c. Furthermore, by irradiating the end face 14 of the glass plate 10 before chamfering, which has a surface perpendicular to the main surface 12 at least in the center in the thickness direction, with laser light L, the edge portion of the end face 14 of the glass plate 10 is softened and / or melted, and the edge portion of the end face 14 is further chamfered to make it rounded, and in order to form a surface (side wall surface 14t) perpendicular to the main surface of the glass plate 10 on the end face 14 after chamfering, the laser light is irradiated onto the end face 14 by controlling the value of Pd × Th and the value of the moving speed. As a result, the shape of the end face 14 of the glass plate 10 can be made uniform with respect to the target shape, and a surface perpendicular to the main surface 12 and a chamfered surface 14c can be formed.
[0045] In order to form a chamfered surface 14c on the end face 14, according to one embodiment, when W1 > Th, Pd × Th is x, and the moving speed of the laser beam L moving along the end face 14 is y, the values of Pd × Th and the moving speed are adjusted so that y is within the range of 11.2・x - 4.7 or less. Furthermore, as shown in Figure 4, in order for the end face 14 to have a side wall surface 14t which is a surface perpendicular to the main surface 12 in addition to the chamfered surface 14c, according to one embodiment, when W1 > Th, Pd × Th is x, and the moving speed of the laser beam L moving along the end face 14 is y, the values of Pd × Th and the moving speed are adjusted so that y is within the range of 11.2・x - 4.7 or less and 5.4・x - 4.5 or more.
[0046] Figures 5(a) to 5(c) illustrate the differences in the shape of the end face 14 due to differences in the irradiation conditions of the laser beam L. Figures 5(a) to 5(c) show examples of the shape of the end face 14 when the power density Pd is changed to change Pd × Th, while the irradiation conditions are fixed as follows: thickness Th 0.7 mm, width W1 1.0 mm, ratio Th / W1 0.7, length W2 10 mm, and moving speed at the irradiation position 2 mm / second. The glass substrate used before processing had a glass transition temperature Tg of 500°C, a diameter of 95 mm, and the end face was perpendicular to the main surface. The surface roughness Rz of the end face 14 was 5 μm, and the arithmetic mean roughness Ra was 0.5 μm. The laser beam L was irradiated onto the outer edge of the glass substrate. Figure 5(a) shows the state without irradiation of the laser beam L, i.e., Pd = 0 [W / mm 2 This shows an example where Pd = 1.9 [W / mm²]. Figure 5(b) shows Pd = 1.9 [W / mm²]. 2 The irradiation conditions were ] (Pd × Th = 1.33 [W / mm]), and Figure 5(c) shows Pd = 4.0 [W / mm]. 2The shape of the end face 14 under irradiation conditions of ] (Pd × Th = 2.8 [W / mm]) is shown. The portion of the end face 14 shown in Figure 5(c) is spherical, which reduces the outer diameter of the glass plate 10. As a result, the length in the thickness direction of the glass plate 10 becomes longer than the thickness of the glass plate 10 (length between main surfaces), and although a chamfered surface 14c is formed, this is an undesirable shape for a glass substrate with a constant thickness. Therefore, it is preferable that the irradiation conditions with the laser light L be set such that the end face 14 forms a side wall surface 14t perpendicular to the main surface 12, and a chamfered surface 14c connecting both ends of the side wall surface 14t to the end of the main surface 12. To prevent the outer diameter of the glass plate 10 from becoming smaller, or the length in the thickness direction of the spherical shape from becoming longer than the thickness of the glass plate 10 (length between main surfaces), for example, the range of power density Pd should be 1.2 [W / mm]. 2 ]~3.0[W / mm 2 It is preferable to set it to ].
[0047] In one embodiment, it is preferable that the irradiation conditions Pd×Th and the moving speed are set so that the ratio (C / Th) of the length C of the chamfered surface 14c along the main surface 14 to the thickness Th is 0.1 to 0.7. By setting the ratio (C / Th) to 0.1 to 0.7, the chamfered surface 14c can function without corners at the connection portion between the end face 14 and the main surface 12. If the ratio (C / Th) is less than 0.1, the formation of the chamfered surface 14c will be insufficient, and there is a risk that the edges will be easily chipped in subsequent film deposition processes. If the ratio (C / Th) is greater than 0.7, there is a risk that the data recording area on the main surface 14 will be reduced. Therefore, the ratio (C / Th) can be adjusted by adjusting Pd×Th within the range of 0.8 to 3.5 [W / mm], preferably within the range of 1.2 to 2.3 [W / mm], or by adjusting the value of Pd×Th and the value of the moving speed. A ratio (C / Th) of 0.25 to 0.5 is more preferable. According to one embodiment, it is preferable to set the irradiation conditions such that the ratio (T / Th) of the length T [mm] along the thickness direction of the side wall surface 14t to the thickness Th is 0.1 to 0.8. If the ratio (T / Th) is less than 0.1, the formation of the side wall surface 14t will be insufficient, making it difficult to measure the outer or inner diameter of the glass plate 10, which may lead to measurement variations and make production control difficult. Also, if the ratio (C / Th) is greater than 0.8, the formation of the chamfered surface 14c will be insufficient, which may make the edges more prone to chipping in subsequent film formation processes. According to one embodiment, the surface roughness Rz (JIS B0601:2001) of the end face 14 (chamfered surface 14c, side wall surface 14t) formed by the laser light L is preferably 0.3 μm or less, more preferably 0.2 μm or less, and the arithmetic mean roughness Ra (JIS B0601:2001) is preferably 0.03 μm or less, more preferably 0.02 μm or less. The surface roughness Rz and arithmetic mean roughness Ra can be measured, for example, with a laser-type optical microscope. By irradiating the end face 14 with the laser light L under the above irradiation conditions, the chamfered surface 14c and side wall surface 14t can be smoothed.
[0048] Furthermore, as shown in Figure 1, when performing shaping by relatively moving the irradiation position of the laser beam L along the circumferential direction of the disc-shaped glass plate 10, it is preferable to make the circumferential length W2 (see Figure 2) of the disc shape of the glass plate 10 somewhat long, so that the temperature of the end face 14 is gradually increased by heating with the laser beam L, and the end face 14 is effectively heated by the laser beam L so that the maximum temperature is reached at the circumferential center point of the irradiation position. By doing so, the movement speed of the irradiation position of the laser beam L can be increased, and thus the processing time can be shortened. According to one embodiment, the luminous beam of the laser beam L irradiated onto the end face 14 is elliptical in shape, as shown in Figure 2. In this case, it is preferable that the ratio (W2 / D) of the luminous beam of the laser beam L irradiated onto the end face 14 to the diameter D of the glass plate 10 (W2 / D) of the circumferential length W2 of the disc shape of the glass plate 10 is 0.03 to 0.3. If the ratio (W2 / D) is less than 0.03, the length W2 becomes relatively short, making it difficult to gradually increase the temperature of the end face 14 and thus difficult to shorten the processing time. If the ratio (W2 / D) is greater than 0.3, the length W2 becomes relatively long compared to the circumference along the circumferential direction of the glass plate 10. In this case, the irradiation position (position in the irradiation direction of the laser beam L) where the laser beam L irradiates the end face 14 of the glass plate 10 changes greatly depending on the curvature of the glass plate 10. As a result, the light beam spreads out, making it difficult to heat efficiently in the circumferential direction. Furthermore, even when the edge portion of the end face 14 of the glass plate 10 is softened and / or melted by irradiating the end face 14 of the glass plate 10 with laser light to chamfer the edge portion of the end face 14 into a rounded shape, and when the end face 14 is chamfered and a surface perpendicular to the main surface of the glass plate 10 is formed on the chamfered end face 14, the ratio (W2 / D) is preferably 0.03 to 0.3 for the reasons stated above.
[0049] Furthermore, when the end face 14 is irradiated with laser light L, as the power density Pd is gradually increased, the diameter D of the glass plate 10 increases by several tens to several hundreds of micrometers as the shape of the end face 14 rounds. If the power density Pd is further increased, the range of rounding expands, the length in the thickness direction increases, and it becomes spherical, which reduces the diameter D of the glass plate 10. In other words, the diameter D of the glass plate 10 after shaping changes depending on the size of the power density Pd. The example shown in Figure 5(c) is an example where the power density Pd becomes excessively large, causing the end face 14 to become spherical due to excessive heating, and the diameter of the glass plate 10 becomes shorter. A glass plate 10 like the one shown in Figure 5(c) has an outer diameter smaller than the target diameter of the glass plate 10, which is undesirable. Also, excessive heating of the end face 14 makes it easy for the spherical shape to vary, making it impossible to keep the diameter of the glass plate 10 consistent, which is undesirable. Therefore, it is preferable that the power density Pd is set such that the diameter of the glass plate 10 formed by irradiation with the laser light L is greater than the diameter of the glass plate 10 before irradiation with the laser light L.
[0050] The moving speed of the laser beam L as it moves along the end face 14 is preferably 0.7 to 100 [mm / second]. Here, the moving speed is the relative speed to the end face 14. From the viewpoint of processing efficiency, it is preferable that the shaping process by the laser beam L is completed when the laser beam L has completed one full rotation around the glass plate 10. If the moving speed exceeds 100 [mm / second], it becomes difficult to determine the timing for completing the process, and it may become difficult to coincide the start and end points of the process. Also, if the moving speed is lower than 0.7 [mm / second], the shape of the end face changes with even a slight change in Pd × Th, making it difficult to control the shape of the end face. For example, even if a shape with a side wall surface 14t and a chamfered surface 14c as shown in Figure 4 is obtained, even a slight increase in Pd × Th can cause the end face 14 to overheat and easily result in a shape like that shown in Figure 5(c), making stable production difficult. From these points of view, the above-mentioned moving speed is preferably 0.7 to 100 [mm / second]. More preferably, the moving speed is 20 to 100 [mm / second]. When the moving speed is 20 [mm / second] or more, the change in the shape of the end face 14 in response to the change in Pd × Th becomes relatively gentle, and productivity is improved by shortening the processing time. For this reason, a moving speed of 20 to 100 [mm / second] is more preferable.
[0051] Furthermore, in order to promote the formation of a chamfer by the laser beam L, it is preferable to raise the temperature of the glass plate 10 to a temperature higher than room temperature when processing the chamfer shape with the laser beam L. At this time, it is preferable that Tg be 50°C or lower (Tg is the glass transition temperature of the glass plate 10). Moreover, it is even more preferable that the temperature of the glass plate 10 when processing the chamfer shape be in the range of 150 to 400°C. If the temperature of the glass plate 10 is less than 150°C, the formation of the chamfered surface 14c may not be sufficiently obtained. If the temperature of the glass plate 10 is higher than 400°C, the glass plate 10 may deform, making it difficult to irradiate the end face 14 with the laser beam L. As a method of heating the glass plate 10, for example, the glass plate 10 can be heated before performing the chamfering process, or the glass plate 10 can be heated while performing the chamfering process. However, when heating the glass plate 100 while performing the chamfering process, temperature control becomes difficult due to the synergistic effect with heating by the laser beam L, which may result in large variations in the shape of the end face 14. Therefore, when heating the glass plate 10, it is preferable to heat the glass plate 10 prior to chamfering. In this case, it is preferable to appropriately maintain the temperature of the glass plate 10 during the chamfering process.
[0052] After the end face 14 of the glass plate 10 has been shaped in this manner, the end face of the inner circumference is also shaped by laser light L, and then the glass plate 10 undergoes various treatments to have properties suitable for the final product.
[0053] For example, the shaped end face 14 is subjected to end face polishing. In end face polishing, the surface roughness Rz of the chamfered surface 14c and the side wall surface 14t can be reduced to 0.3 μm or less. Therefore, the amount of material removed in end face polishing can be reduced compared to the conventional method of processing the chamfered surface 14c using a full-size grinding wheel, thereby improving production costs and production efficiency. In one embodiment, end face polishing may not be performed at all.
[0054] When manufacturing a glass substrate for a magnetic disk from a glass plate 10, after the edge polishing process described above, the glass plate 10 is treated as an intermediate glass plate before becoming a glass substrate for a magnetic disk, and the main surface 12 of the glass plate 10 is subjected to grinding and polishing. In the grinding and polishing process, the glass plate 10 is ground and then polished. In the grinding process, a double-sided grinding device equipped with a planetary gear mechanism is used to grind the main surface 12 of the glass plate 10. Specifically, the glass plate 10 is held in a holding hole provided in the holding member of the double-sided grinding device, and the main surfaces on both sides of the glass plate 10 are ground. The double-sided grinding device has a pair of upper and lower grinding plates (upper plate and lower plate), and the glass plate 10 is sandwiched between the upper and lower plates. Then, by moving either the upper plate or the lower plate, or both, and supplying coolant, the glass plate 10 and each plate are moved relative to each other, thereby grinding both main surfaces of the glass plate 10. For example, grinding can be performed by mounting a grinding member, which is made of a sheet of fixed abrasive grains in which diamonds are fixed with resin, onto a surface plate.
[0055] Next, the main surface of the glass plate 10 after grinding is subjected to a first polishing process. Specifically, the glass plate 10 is held in a holding hole provided in the polishing carrier of the double-sided polishing device, and the main surfaces on both sides of the glass plate 10 are polished. The purpose of the first polishing is to remove scratches and distortions remaining on the main surface after grinding, or to adjust minute surface irregularities (microwaveness, roughness).
[0056] In the first polishing process, the glass plate 10 is polished using a double-sided polishing device, which has the same configuration as the double-sided grinding device used in the above-mentioned grinding process using fixed abrasive grains, while applying polishing slurry. In the first polishing process, polishing slurry containing free abrasive grains is used. As free abrasive grains used in the first polishing, for example, cerium oxide or zirconia abrasive grains are used. In the double-sided polishing device, as in the double-sided grinding device, the glass plate 10 is sandwiched between a pair of upper and lower platens. Flat polishing pads (for example, resin polishers) that are ring-shaped overall are attached to the upper surface of the lower platen and the bottom surface of the upper platen. Then, by moving either the upper platen or the lower platen, or both, the glass plate 10 is moved relative to each platen, thereby polishing both main surfaces of the glass plate 10. The size of the polishing abrasive grains is preferably in the range of 0.5 to 3 μm in average particle size (d50).
[0057] After the first polishing, the glass plate 10 may be chemically strengthened. In this case, a mixed molten solution of potassium nitrate and sodium nitrate is used as the chemical strengthening solution, and the glass plate 10 is immersed in the chemical strengthening solution. This allows a compressive stress layer to be formed on the surface of the glass plate 10 by ion exchange.
[0058] Next, the glass plate 10 is subjected to a second polishing process. The purpose of the second polishing process is to achieve a mirror finish on the main surface. In the second polishing process, a double-sided polishing apparatus having the same configuration as the double-sided polishing apparatus used in the first polishing process is used. Specifically, the glass plate 10 is held in a holding hole provided in the polishing carrier of the double-sided polishing apparatus, and the main surfaces on both sides of the glass plate 10 are polished. In the second polishing process, the type and particle size of the free abrasive particles and the hardness of the resin polisher differ from those in the first polishing process. It is preferable that the hardness of the resin polisher is lower than that used in the first polishing process. For example, a polishing solution containing colloidal silica as free abrasive particles is supplied between the polishing pad of the double-sided polishing apparatus and the main surface of the glass plate 10, and the main surface of the glass plate 10 is polished. It is preferable that the size of the polishing abrasive particles used in the second polishing process is in the range of 5 to 50 nm in average particle size (d50). The necessity of chemical strengthening treatment can be appropriately selected considering the glass composition and its necessity. In addition to the first and second polishing processes, further polishing processes may be added, or the polishing of the two main surfaces may be completed with a single polishing process. Furthermore, the order of each of the above processes may be changed as appropriate. In this way, the main surface of the glass plate 10 is polished to obtain a glass substrate for a magnetic disk that satisfies the conditions required for a glass plate 10 for a magnetic disk. After this, at least a magnetic layer is formed on the glass plate 10 produced by polishing the main surface to manufacture a magnetic disk.
[0059] In this method for manufacturing the glass plate 10, the main surface 12 of the shaped glass plate 10 is ground or polished. In this case, even if the end face 14 is not polished after shaping the end face 14 but before grinding or polishing the main surface 12, or if the end face 14 is polished, the amount of material removed by polishing the end face 14 can be kept to 5 μm or less. Therefore, the change in the outer diameter of the glass plate 10 can be kept to 10 μm or less. This is because the laser light L can form a chamfered surface 14c and a side wall surface 14t with small surface irregularities.
[0060] In recent years, the demand for increased storage capacity in hard disk drives has become increasingly intense, driven by applications such as big data analysis. Therefore, increasing the number of magnetic disks in a single hard disk drive is being considered. When increasing storage capacity by increasing the number of magnetic disks, it becomes necessary to reduce the thickness of the glass substrate for the magnetic disks, which accounts for the majority of the disk's thickness within the limited space of the drive. However, reducing the thickness of the glass substrate reduces its rigidity, making it more susceptible to large vibrations that are difficult to suppress. Large vibration amplitudes in the glass substrate increase the likelihood of contact with adjacent magnetic disks, and the topmost magnetic disk in a cluster of disks spaced at regular intervals may even come into contact with the ceiling of the hard disk drive's magnetic disk housing. Such contact can cause chipping and particle generation. Therefore, low rigidity of the glass substrate for magnetic disks is undesirable. From this perspective, according to one embodiment, the Young's modulus of the glass plate 10 is preferably 70 [GPA] or higher, more preferably 80 [GPA] or higher, and even more preferably 90 [GPA] or higher. The thickness Th of the glass plate 10 is preferably 0.7 mm or less, and more preferably 0.6 mm or less. This makes it possible to increase the number of magnetic disks mounted in the hard disk drive device by one or two.
[0061] The composition of such a glass plate 10 is not limited, but is preferably as follows.
[0062] (Glass 1) SiO2 56-80 mol%, Li2O 1-10 mol%, B2O3 0-4 mol%, total content of MgO and CaO (MgO + CaO) 9-40 mol%. The specific gravity of Glass 1 is 2.75 g / cm³. 3 Below, the glass transition temperature Tg is 650°C or higher.
[0063] (Glass 2) SiO2 56-80 mol%, Li2O 1-10 mol%, B2O 3 The total content of MgO and CaO (MgO + CaO) is 0-4 mol%, and Al2O 3 The molar ratio of the total content of SiO2 and ZrO2 relative to the total content is ((SiO2 + ZrO2) / Al2O 3 The values are 2 to 13. The specific gravity of glass 2 is 2.50 g / cm³. 3 Below, the glass transition temperature Tg is 500°C or higher, and the specific modulus at 20°C is 30 GPa·cm. 3 It is 1 / g or more.
[0064] (Glass 3) SiO2 expressed in mol% 2 56-65%, Al 2 O 3 5-20%, B 2 O 3 0-4%, MgO 3-28%, Li 2 It contains 1-10% of O, and SiO 2 and Al 2 O 3 Total content (SiO 2 +Al 2 O 3 ) 65-80%, total content of MgO and CaO (MgO + CaO) 11-30%, total content of MgO, CaO, SrO and BaO (MgO + CaO + SrO + BaO) 12-30%, MgO content, 0.7 × CaO content, Li 2 O content, TiO 2 Content and ZrO 2 Sum of contents (MgO+0.7CaO+Li 2 O+TiO 2 +ZrO 2 ) 16% or more, 5 × Li 2 O content, 3×Na 2 O content, 3×K 2 O content, 2×B 2 O 3 content, MgO content, 2×CaO content, 3×SrO content, and BaO content (5Li 2 O+3Na 2 0+3K 2 O+2B 2O 3 +MgO + 2CaO + 3SrO + BaO) 32 - 58%, SiO 2 content, Al 2 O 3 content, B 2 O 3 content, P 2 O 5 content, 1.5×Na 2 O content, 1.5×K 2 O content, 2×SrO content, 3×BaO content and ZnO content sum (SiO 2 +Al 2 O 3 +B 2 O 3 +P 2 O 5 +1.5Na 2 O + 1.5K 2 O + 2SrO + 3BaO + ZnO) 86% or less, and SiO 2 content, Al 2 O 3 content, B 2 O 3 content, P 2 O 5 content, Na 2 O content, K 2 O content, CaO content, 2×SrO content and 3×BaO content sum (SiO 2 +Al 2 O 3 +B 2 O 3 +P 2 O 5 +Na 2 O + K 2 O + CaO + 2SrO + 3BaO) 92% or less, contains, the molar ratio of CaO content to MgO content (CaO / MgO) is 2.5 or less, Li 2 O content to Na 2 O content molar ratio (Na 2 O / Li 2 O) is 5 or less, the molar ratio of Li 2 O content to the total content of MgO and CaO (Li 2 O / (MgO + CaO)) is 0.03 - 0.4, Li 2 O, Na 2 O and K2 The molar ratio of the content of SiO 2 to the total content of O (SiO 2 / (Li 2 O + Na 2 O + K 2 O)) is 4 to 22, the molar ratio of the total content of SiO 2 O 3 to Al 2 and ZrO 2 is (SiO 2 + ZrO 2 ) / Al 2 O 3 is 2 to 10, the molar ratio of the total content of TiO 2 and Al 2 O 3 to the total content of MgO and CaO ((TiO 2 + Al 2 O 3 ) / (MgO + CaO)) is 0.35 to 2, the molar ratio of the total content of MgO and CaO to the total content of MgO, CaO, SrO and BaO ((MgO + CaO) / (MgO + CaO + SrO + BaO)) is 0.7 to 1, the molar ratio of the BaO content to the total content of MgO, CaO, SrO and BaO (BaO / (MgO + CaO + SrO + BaO)) is 0.1 or less, B 2 O 3 , SiO 2 , Al 2 O 3 and P 2 O 5 the molar ratio of the P 2 O 5 content to the total content of B 2 O 5 / (B 2 O<^ 3 + SiO 2 + Al 2 O 3 + P 2 O 5 )) is 0.005 or less, and it is an amorphous oxide glass with a glass transition temperature of 670 °C or higher, a Young's modulus of 90 GPa or higher, a specific gravity of 2.75 or less, and an average linear expansion coefficient in the range of 40 × 10 -7 to 70 × 10 -7 / °C.
[0065] According to one embodiment, the glass plate 10 is preferably made of glass with a glass transition temperature Tg of 500°C or higher, and more preferably with a glass transition temperature Tg of 650°C or higher. The higher the glass transition temperature Tg, the more the thermal shrinkage and deformation caused by thermal shrinkage during heat treatment of the glass plate 10 can be suppressed. Therefore, considering the heat treatment when forming the magnetic film of a magnetic disk or the like on the substrate 1, it is preferable to set the glass transition temperature Tg to 500°C or higher, and more preferably to 650°C or higher.
[0066] According to one embodiment, the glass plate 10 has a coefficient of linear expansion of 100 × 10 -7 It is preferable that the material is composed of a material with a ratio of [1 / K] or less, 95 x 10 -7 It is more preferable that the material be composed of a material with a ratio of [1 / K] or less, 70 x 10 -7 It is even more preferable, and particularly preferable, that the material be composed of a material with a coefficient of thermal expansion of 60 × 10⁻¹⁰ or less. -7 It is less than or equal to [1 / K]. The lower limit of the coefficient of linear expansion of the glass plate 10 is, for example, 40 × 10 -7 The coefficient of linear expansion is [1 / K]. Here, the coefficient of linear expansion is determined by the difference in thermal expansion between 100°C and 300°C. By using such a coefficient of linear expansion, thermal expansion can be suppressed during the heat treatment when forming magnetic films, and when the gripping member of the film-forming apparatus fixes and grips the glass plate 10 at the outer edge, thermal distortion of the glass plate 10 around the gripping portion can be suppressed. For example, the coefficient of linear expansion for a conventional aluminum alloy substrate is 242 × 10 -7 While [1 / K] is the coefficient of linear expansion of the glass plate 10 in one embodiment is 51 × 10 -7 It is [1 / K].
[0067] [Experimental Example] To confirm the effectiveness of the manufacturing method for the glass plate 10 described above, the end face 14 was processed under various conditions of laser beam L irradiation, specifically Pd × Th [W / mm], and the shape of the end face 14 was examined. At that time, the moving speed [mm / second] of the laser beam L as it moved along the end face 14 was also adjusted. After heating the entire glass plate 10 to 350°C before irradiation with the laser beam L, the laser beam L was irradiated onto the end face of the outer edge of the glass plate 10 while maintaining the temperature of the glass plate 10. The laser beam L was irradiated from the direction normal to the end face 14.
[0068] On the other hand, the shape of the end face 14 formed by irradiation with laser light L was visually evaluated in four stages from A to D using magnified photographs obtained with a microscope. Evaluation A: The end face 14 has a surface perpendicular to the main surface 12 (side wall surface 14t) and a chamfered surface 14c, and the length T in the thickness direction of the perpendicular surface (see Figure 4) is one-tenth or more of the thickness Th. Evaluation B: The end face 14 does not have a surface perpendicular to the main surface 12, but only has a chamfered surface 14c, and the length in the thickness direction of the chamfered portion is equal to or shorter than the thickness Th of the original glass plate (length T is less than one-tenth of the thickness Th). Evaluation C: The end face 14 is spherical as shown in Figure 5(c), and the length in the thickness direction of the chamfered portion is longer than the thickness of the original glass plate. Evaluation D: The end face 14 does not have a chamfered surface 14c as shown in Figure 5(a). This is a defective product.
[0069] In Table 1 below, the glass plate 10 used had a diameter of 95 mm and a thickness of 0.7 mm. The glass composition of the glass plate was the glass 1 described above. The luminous beam of the laser light L on the end face 14 was set to an elliptical shape with a width W1 in the thickness direction of 1 mm and a length W2 in the circumferential direction of 10 mm, so that the luminous beam extended evenly to both sides of the end face 14 of the glass plate 10. The power density Pd and the moving speed V of the laser light L were varied.
[0070]
[0071] The glass plates used in Table 2 below were: a glass plate with a diameter of 95 mm and a thickness of 0.7 mm; a glass plate with a diameter of 97 mm and a thickness of 0.7 mm; a glass plate with a diameter of 65 mm and a thickness of 0.7 mm; a glass plate with a diameter of 95 mm and a thickness of 0.6 mm; and a glass plate with a diameter of 95 mm and a thickness of 0.55 mm. The glass composition of the glass plates was the glass 1 described above. For the luminous beam of the laser light L on the end face 14, the width W1 in the thickness direction was set to 1 mm, and the length W2 in the circumferential direction was changed to create an elliptical shape, and the power density Pd of the laser light L was varied in various ways. The moving speed [mm / sec] of the laser light L moving along the end face 14 was fixed at 70 [m / sec]. The shape of the end face 14 was evaluated in four stages from A to D, as in Table 1.
[0072]
[0073] Figure 6 shows the evaluation results shown in Table 1. Figure 6 plots conditions 1 to 40. From Figure 6, it can be seen that the conditions for forming a chamfered surface 14c are that when the moving speed V is 0.7 [mm / sec] or higher, in order to obtain evaluations A to C for forming a chamfered surface 14c, Pd × Th must be at least 0.8 [W / mm]. When the moving speed V is less than 0.7 [mm / sec], the range of Pd × Th that yields evaluations A and B becomes extremely narrow. Therefore, even if a shape with a vertical surface and a chamfered surface 14c is obtained, even a slight increase in Pd × Th can easily cause the end face 14 to overheat, resulting in a shape like that shown in Figure 5(c), making stable production difficult. In this respect, it is preferable that the moving speed V is 0.7 [mm / sec] or higher.
[0074] On the other hand, as shown in Figure 6, when changing the moving speed V, it is preferable to adjust the value of Pd × Th. In this case, when Pd × Th [mm / sec] is x and the moving speed V [mm / sec] is y, the chamfered surface 14c can be formed by setting y to 11.2・x - 4.7 or less. The straight line L1 shown in Figure 6 represents the straight line y = 11.2・x - 4.7. In this case, in order to obtain evaluation A, that is, in order for the end face to have a face perpendicular to the main surface with a length of at least one-tenth of the thickness Th and the chamfered surface 14c, it is preferable to set y to 11.2・x - 4.7 or less and 5.4・x - 4.5 or more. The straight line L2 shown in Figure 6 represents the straight line y = 5.4・x - 4.5. Therefore, when Pd × Th is x and the moving speed V is y, by adjusting the values of Pd × Th and the moving speed V so that y is within the range of 11.2・x - 4.7 and 5.4・x - 4.5, the end face 14 is provided with a surface perpendicular to the main surface 12 (a surface whose length is at least one-tenth of the thickness Th) and a chamfered surface 14c. As a result, as described above, it is possible to suppress variations in the outer diameter (diameter) or inner diameter (diameter of the circular hole 16) of the glass plate 10 within a single glass plate 10 or between glass plates 10. Furthermore, in order to avoid evaluation C and obtain evaluation B, that is, in order to obtain a glass plate 10 (see Figure 5(c)) in which the end face 14 does not have a surface perpendicular to the main surface 12, but only has a chamfered surface 14c, and the length in the thickness direction of the chamfered portion is equal to or shorter than the thickness of the original glass plate, it is preferable to adjust the value of Pd × Th and the value of the moving speed V so that when Pd × Th is x and the moving speed V is y, the range is less than 5.4・x - 4.5 and 3.8・x - 5.6 or greater. The straight line L3 shown in Figure 6 represents the straight line y = 3.8・x - 5.6.
[0075] Furthermore, the results in Table 2 show that even if the diameter, thickness Th, width W1, and length W2 of the glass plate 10 are changed, the evaluation results do not change if the values of Pd × Th and the moving speed V are set within the range of evaluations A to C shown in Figure 6. In the conditions that resulted in evaluations A and B in Tables 1 and 2, the ratio (C / Th) was within the range of 0.1 to 0.7. Also, in all the conditions that resulted in evaluations A to C, the surface roughness Rz was 0.3 μm or less, and the arithmetic mean roughness Ra was 0.03 μm or less. From the above, the effectiveness of the glass plate manufacturing method of this embodiment is clear.
[0076] Although the methods for manufacturing a glass plate, chamfering a glass plate, and manufacturing a magnetic disk of the present invention have been described in detail above, the present invention is not limited to the above embodiments and experimental examples, and various improvements and modifications may be made without departing from the spirit of the present invention.
[0077] 10 Glass plate 12 Main surface 14 End face 14c Chamfered surface 14t Side wall surface 16 Circular hole 20 Laser light source 22 Optical system 24 Focusing lens
Claims
1. A method for manufacturing a glass plate, which processes the shape of an edge surface of a disk-shaped glass plate, wherein the disk-shaped glass plate has a main surface and an edge surface perpendicular to the main surface, and includes the steps of irradiating the edge surface with a laser beam and processing the edge surface into a target shape while moving the laser beam relative to the edge surface in a circumferential direction of the disk-shaped glass plate, wherein the cross-sectional intensity distribution of the laser beam irradiated to the edge surface is single mode, and where W1 [mm] is the width of the laser beam flux at the irradiation position on the edge surface in the thickness direction of the glass plate, Th [mm] is the thickness of the glass plate, and Pd is the power density of the laser beam, W1 > Th and Pd × Th is 0.8 to 3.5 [W / mm].
2. A method for manufacturing a glass plate, which processes the shape of an edge surface of a disk-shaped glass plate, wherein the disk-shaped glass plate has a main surface and an edge surface perpendicular to the main surface, and includes the steps of irradiating the edge surface with a laser beam and moving the laser beam relative to the edge surface in a circumferential direction of the disk-shaped glass plate to form a chamfered surface on the edge surface and process the glass plate into a desired shape, wherein the cross-sectional intensity distribution of the laser beam irradiated on the edge surface is single mode, and where W1 [mm] is the width of the beam of the laser beam at the irradiation position on the edge surface in the thickness direction of the glass plate, Th [mm] is the thickness of the glass plate, and Pd is the power density of the laser beam, W1 > Th, and where Pd × Th is x and y is the speed at which the laser beam moves along the edge surface, the value of Pd × Th and the value of the speed of movement are adjusted so that y is within a range of 11.2 × x - 4.7 or less.
3. The method for manufacturing a glass plate according to claim 1 or 2, wherein the laser light is irradiated onto the end surface of the glass plate from a direction normal to the end surface.
4. A method for manufacturing a glass plate according to any one of claims 1 to 3, wherein the conditions for irradiating the laser light are set so that, in the shaping process, side wall surfaces that are perpendicular to the two opposing main surfaces of the glass plate and chamfered surfaces that connect both ends of the side wall surfaces to the ends of the main surfaces are formed on the end faces.
5. The method for producing a glass plate according to claim 4, wherein the irradiation conditions are set so that a ratio (C / Th) of a length C of the chamfered surface along the main surface to the thickness Th is 0.1 to 0.
7.
6. The method for manufacturing a glass plate according to any one of claims 1 to 5, wherein the surface roughness Rz of the end face formed by the laser beam is 0.3 μm or less, and the arithmetic mean roughness Ra is 0.03 μm or less.
7. The method for manufacturing a glass plate according to any one of claims 1 to 6, wherein the beam of the laser light irradiated onto the end surface has an elliptical shape, and the ratio (W2 / D) of the length W2 in the circumferential direction of the beam of the laser light irradiated onto the end surface to the diameter D of the glass plate is 0.03 to 0.
3.
8. A method for manufacturing a glass plate according to any one of claims 1 to 7, wherein the power density Pd is set so that the diameter of the glass plate formed by the irradiation of the laser light is larger than the diameter of the glass plate before the irradiation of the laser light.
9. The method for manufacturing a glass plate according to any one of claims 1 to 8, wherein the laser light moves along the edge surface at a speed of 0.7 to 100 mm / sec.
10. The method for manufacturing a glass plate according to any one of claims 1 to 9, wherein the glass plate has a Young's modulus of 70 GPa or more.
11. The glass plate has a linear expansion coefficient of 100 x 10 -7 The method for producing a glass plate according to any one of claims 1 to 10, wherein the σ is [1 / K] or less.
12. The method for producing a glass plate according to any one of claims 1 to 11, wherein the thickness Th is 0.7 mm or less.
13. A method for manufacturing a glass plate according to any one of claims 1 to 12, comprising the step of grinding or polishing the main surfaces of the glass plate that has been subjected to the shaping process, wherein after the shaping process and before grinding or polishing the main surfaces, the edge surfaces are not polished, or even if the edge surfaces are polished, the amount of removal by polishing the edge surfaces is 5 μm or less.
14. A method for chamfering a glass plate, in which a chamfered surface is formed on an edge surface of a disk-shaped glass plate by irradiating it with laser light, wherein the edge surface of the glass plate before the formation of the chamfered surface has a surface perpendicular to the main surface at least at the center in the thickness direction of the glass plate, and the edge portion of the edge surface of the glass plate is softened and / or melted by irradiating the edge surface of the glass plate with laser light, and the edge portion is chamfered into a rounded shape, and Pd x Th and moving speed V are controlled so that a surface perpendicular to the main surface of the glass plate is also formed on the edge surface after the chamfered surface is formed, where Th [mm] is the thickness of the glass plate, Pd is the power density of the laser light, and V is the moving speed of the laser light moving along the edge surface.
15. The method for chamfering a glass sheet according to claim 14, wherein the value of Pd×Th and the value of the moving speed are adjusted so that y is within the range of 11.2×x−4.7 or less and 5.4×x−4.5 or more, where x is Pd×Th and y is the moving speed.
16. A method for manufacturing a glass plate, comprising chamfering the edge of a disk-shaped glass plate using the method for chamfering a glass plate according to claim 14 or 15.
17. A method for manufacturing a magnetic disk, comprising forming a magnetic film on the main surface of a glass plate manufactured by the method for manufacturing a glass plate according to any one of claims 1 to 13 and 16.