Rare earth synergistic flame-retardant asphalt composition and preparation method therefor

By using magnesium hydroxide and nano-lanthanum oxide/cerium oxide synergistic flame retardants in asphalt, the problems of poor compatibility between flame retardants and asphalt and complex preparation processes are solved, achieving efficient flame retardant and smoke suppression effects, and improving improve the construction environment and tunnel safety.

WO2024198547A1PCT designated stage expired Publication Date: 2024-10-03CHONGQING JIAOTONG UNIV

Patent Information

Application Number
PCT/CN2023/139907
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-06
Filing Date
2023-12-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing flame-retardant asphalt products have problems such as poor compatibility between flame retardants and asphalt, poor flame retardant and smoke suppression effects, complex preparation processes and environmental pollution, which limits their application in tunnel asphalt pavements.

Method used

Using a combination of magnesium hydroxide, nano-lanthanum oxide/cerium oxide synergistic flame retardant and asphalt, through the process of stirring, drying, spraying and high-speed shear dispersion, the composite flame retardant is prepared and mixed with asphalt to achieve rare earth Preparation of synergistic flame retardant asphalt.

Benefits of technology

It achieves efficient flame retardant and smoke suppression properties, reduces pollutant emissions during construction, improves the safety of the construction environment in the tunnel, reduces fire losses and casualties, and extends the service life of the highway tunnel pavement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023139907_03102024_PF_FP_ABST
    Figure CN2023139907_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A rare earth synergistic flame-retardant asphalt composition and a preparation method therefor. The rare earth synergistic flame-retardant asphalt composition comprises the following raw materials in parts by weight: 10 parts of a composite flame retardant, and 100 parts of asphalt; wherein the composite flame retardant is composed of magnesium hydroxide, a rare earth synergist, a silane coupling agent KH550, and absolute ethanol; the preparation method comprises the following steps: S100, preparing a composite flame retardant intermediate; S200, preparing a composite flame retardant; and S300, preparing a flame-retardant asphalt. The beneficial effects lie in: the asphalt has efficient flame retardance and smoke suppression performance, and compared with existing flame retardants, also eliminates emission of pollutants in the pavement paving process, and reduces emission of toxic substances in the flame retardant process; the working environment of pavement paving construction in tunnels is improved, the physical health burden of construction personnel is reduced, and also, the fire losses and casualties in highway tunnels can be greatly reduced, driving safety is improved, and the service life of highway tunnel pavements is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Rare earth synergistic flame retardant asphalt composition and preparation method thereof Technical Field

[0001] The present invention relates to the technical field of pavement materials, and in particular to a rare earth synergistic flame-retardant asphalt composition and a preparation method thereof. Background Art

[0002] With the development of land transportation infrastructure, the total mileage of mountain tunnels continues to grow, and my country has entered a period of rapid development in tunnel construction. Asphalt concrete pavements offer excellent driving comfort and are currently the mainstream form of tunnel paving. However, asphalt is primarily composed of hydrocarbons, which are flammable. Tunnel asphalt pavements are semi-enclosed spaces. In the event of a fire, the asphalt in the asphalt mixture burns, producing large amounts of toxic and harmful gases that are difficult to dissipate, posing a threat to the lives and health of tunnel occupants. Flame-retardant asphalt technology has emerged as a necessary step. Its application in tunnel asphalt pavements can reduce the likelihood of tunnel fires, minimizing the resulting casualties and property losses.

[0003] Currently, flame-retardant asphalt products primarily enhance the flame retardancy and smoke suppression properties of asphalt. However, their application is limited by issues such as poor compatibility between the flame retardant and asphalt, poor flame retardancy and smoke suppression, high production costs, and environmental pollution. Chinese invention patent CN 116218028 A discloses an asphalt flame retardant, which comprises the following raw materials, by weight: 30-60 parts metal hydroxide, 5-10 parts montmorillonite, 5-10 parts hydrotalcite, 10-50 parts nitrogen-phosphorus flame retardant, 10-20 parts silicon-based flame retardant, and 1-10 parts surface modifier. The preparation method comprises the following steps: mixing and grinding the raw materials to a mesh size of 1000-2000 mesh, wet-modifying the ground materials, filtering, washing, and drying to obtain the finished product. The wet modification process involves the following steps: the ground raw materials are slurried with deionized water, heated to 60-110°C in a reactor while stirring, and a surface modifier is added. The mixture is stirred and reacted at this temperature for 30-60 minutes. This patent demonstrates flame retardancy and smoke suppression, while controlling the amount of flame retardant added. However, the patent does not demonstrate the effect of the flame retardant on the basic properties of asphalt. Materials such as montmorillonite and hydrotalcite can cause asphalt hardening. Patent CN 116218039 A proposes a novel asphalt composite flame retardant and a preparation method thereof, comprising 10-30 parts of an organic metal phosphate, 20-60 parts of magnesium hydroxide, 2-5 parts of a titanate coupling agent, and 10-30 parts of expandable graphite. The preparation method comprises the following steps: dissolving phenol in an organic solvent, adding phosphorus oxychloride and triethylamine, reacting for a period of time to generate an organic phosphoryl chloride, and then hydrolyzing the organic phosphate ester; sequentially adding the organic phosphate ester and an alkaline substance containing metal ions to the organic solvent to obtain an organic metal phosphate; mixing the titanate coupling agent and the organic solvent to obtain an organic solution, sequentially adding the organic metal phosphate, expandable graphite, and magnesium hydroxide to the organic solution, soaking the organic solution for a period of time, filtering the resulting filter, and drying and cooling the resulting filter to obtain the novel flame retardant. The flame retardant can improve the flame retardancy and smoke suppression properties of asphalt, reduce the fire hazard of asphalt pavement, and enhance the compatibility between the flame retardant and asphalt components. However, the preparation process of this patent is complicated, requires solution immersion, is not environmentally friendly, is difficult to achieve industrial production, and has a general flame retardant effect (the oxygen index value of the F-doped flame retardant in Example 5 is 25.7%).

[0004] The aforementioned patented flame retardant has complex preparation processes, high production costs, and is difficult to apply and promote. Based on this, the present invention proposes a method for preparing rare earth synergistic flame retardant modified asphalt to address the above issues.

[0005] Summary of the Invention

[0006] The purpose of the present invention is to provide a rare earth synergistic flame retardant asphalt composition and a preparation method thereof in order to solve the above problems. The preferred technical solution among the many technical solutions provided by the present invention has the following technical effects: simple preparation process, little impact on the performance of asphalt materials, and good flame retardant and smoke suppression effects, etc., which are described in detail below.

[0007] To achieve the above objectives, the present invention provides the following technical solutions:

[0008] The present invention provides a rare earth synergistic flame retardant asphalt composition, comprising the following raw materials in parts by weight: 10 parts of a composite flame retardant and 100 parts of asphalt;

[0009] The composite flame retardant consists of magnesium hydroxide, rare earth synergist, silane coupling agent KH550 and anhydrous ethanol.

[0010] Preferably, the rare earth synergist is one of lanthanum oxide and cerium oxide.

[0011] Preferably, the mass fractions of the components in the composite flame retardant are: 9 parts of magnesium hydroxide, 1 part of rare earth synergist, 0.09 parts of silane coupling agent KH550 and 0.81 parts of anhydrous ethanol.

[0012] A method for preparing a rare earth synergistic flame-retardant asphalt composition, characterized by comprising the following steps:

[0013] S100: preparing a composite flame retardant intermediate by uniformly stirring 9 parts of magnesium hydroxide and 1 part of lanthanum oxide / cerium oxide at room temperature, and then drying the mixture in an oven to obtain the composite flame retardant intermediate;

[0014] S200: preparing a composite flame retardant by mixing 0.009 parts of a silane coupling agent KH500 with 0.81 parts of anhydrous ethanol to prepare 0.9 parts of a treatment liquid, and then evenly spraying the treatment liquid onto the surface of the composite flame retardant intermediate while stirring to evenly mix the two. After evenly mixing, drying to obtain the composite flame retardant;

[0015] S300: Prepare flame retardant asphalt, add the composite flame retardant into 100 parts of heated asphalt, shear and disperse it through a high-speed shearing machine, and keep it warm for 20 minutes to obtain flame retardant asphalt.

[0016] Preferably, in step S100, the stirring time of magnesium hydroxide and lanthanum oxide / cerium oxide is 5 minutes.

[0017] Preferably, in step S100, the oven temperature is 160°C and the drying time is 30 minutes.

[0018] Preferably, in step S200, the treatment liquid and the composite flame retardant intermediate are mixed evenly and then dried at 65° C. for 1.5 hours.

[0019] Preferably, in step S300, the asphalt is base asphalt or modified asphalt, wherein the heating temperature and the insulation temperature of the base asphalt are both 160°C, and the heating temperature and the insulation temperature of the modified asphalt are both 180°C.

[0020] Preferably, in step S300, the high-speed shearing machine can be replaced by a colloid mill, and the rotation speed of the colloid mill is 4000 r / min.

[0021] In summary, the beneficial effects of the present invention are: by adopting magnesium hydroxide, nano-lanthanum oxide / cerium oxide synergistic flame retardants and fusing them with asphalt, not only can the asphalt have high-efficiency flame retardant and smoke suppression properties, but compared with existing flame retardants, it can also eliminate the emission of pollutants during the pavement paving process, reduce the emission of toxic substances during the flame retardant process, improve the pavement paving construction working environment in the tunnel, reduce the health burden of construction workers, and greatly reduce fire losses and casualties in highway tunnels, improve driving safety, and extend the service life of highway tunnel pavements. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0023] FIG1 is a real picture of the composite flame retardant of the present invention. DETAILED DESCRIPTION

[0024] To make the objectives, technical solutions, and advantages of the present invention more apparent, the technical solutions of the present invention will be described in detail below. Obviously, the embodiments described are only some of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other implementations obtained by those of ordinary skill in the art without inventive effort are within the scope of protection of the present invention.

[0025] The present invention provides a rare earth synergistic flame retardant asphalt composition, comprising the following raw materials in parts by weight: 10 parts of a composite flame retardant, 100 parts of asphalt;

[0026] The composite flame retardant comprises magnesium hydroxide, a rare earth synergist, a silane coupling agent KH550, and anhydrous ethanol. The rare earth synergist is one of lanthanum oxide and cerium oxide. The magnesium hydroxide is industrial grade, with an effective content of Mg(OH)2 of not less than 90%. The mesh size of the magnesium hydroxide is 3000-5000 mesh, the mesh size of the lanthanum oxide and the cerium oxide is 18000 mesh, the concentration of the silane coupling agent KH550 is 97.7wt%, and the concentration of the analytical grade anhydrous ethanol is 95wt%.

[0027] The mass fractions of the components in the composite flame retardant are: 9 parts of magnesium hydroxide, 1 part of rare earth synergist, 0.09 parts of silane coupling agent KH550 and 0.81 parts of anhydrous ethanol.

[0028] A method for preparing a rare earth synergistic flame-retardant asphalt composition, characterized by comprising the following steps:

[0029] S100: preparing a composite flame retardant intermediate by stirring 9 parts of magnesium hydroxide and 1 part of lanthanum oxide / cerium oxide at room temperature for 5 minutes until the mixture is uniform, and then drying the mixture in an oven at 160° C. for 30 minutes to obtain a composite flame retardant intermediate;

[0030] S200: preparing a composite flame retardant by mixing 0.009 parts of a silane coupling agent KH500 with 0.81 parts of anhydrous ethanol to prepare 0.9 parts of a treatment liquid, and then evenly spraying the treatment liquid onto the surface of the composite flame retardant intermediate while stirring to evenly mix the two. After evenly mixing, drying at 65° C. for 1.5 hours to obtain the composite flame retardant;

[0031] S300: preparing flame retardant asphalt, adding the composite flame retardant into 100 parts of heated asphalt, shearing and dispersing it through a high-speed shearing machine (or colloid mill) (4000r / min), and keeping it warm for 20 minutes to obtain the flame retardant asphalt; the asphalt is base asphalt or modified asphalt, wherein the heating temperature and the holding temperature of the base asphalt are both 160°C, and the heating temperature and the holding temperature of the modified asphalt are both 180°C.

[0032] The specific embodiments are as follows:

[0033] Example 1:

[0034] It includes 9 parts of magnesium hydroxide, 1 part of lanthanum oxide, 0.09 parts of silane coupling agent KH550, 0.81 parts of anhydrous ethanol and 100 parts of matrix asphalt;

[0035] Example 2

[0036] It includes 9 parts of magnesium hydroxide, 1 part of cerium oxide, 0.09 parts of silane coupling agent KH550, 0.81 parts of anhydrous ethanol and 100 parts of matrix asphalt;

[0037] Example 3

[0038] It includes 9 parts of magnesium hydroxide, 1 part of cerium oxide, 0.09 parts of silane coupling agent KH550, 0.81 parts of anhydrous ethanol and 100 parts of modified asphalt;

[0039] After setting up three groups of comparative examples, base asphalt, 10% magnesium hydroxide + 90% base asphalt and SBS modified asphalt, the limiting oxygen index test, needle penetration and softening point test were carried out on the comparative examples and the examples respectively. The formula table of the examples is shown in Table 1:

[0040] Table 1

[0041] The experimental results are shown in Table 2:

[0042] Table 2

[0043] As can be seen from Table 2, the limiting oxygen index value of Example 1 (10% ML-SDJZ, rare earth synergistic flame retardant asphalt with added lanthanum oxide) is 26.5%, and the limiting oxygen index value of Example 2 (10% MS-SDJZ, rare earth synergistic flame retardant asphalt with added cerium oxide) is 27.8%, which is much higher than that of Comparative Example 1 (SDJZ, matrix asphalt) and higher than that of Comparative Example 2 (only magnesium hydroxide as flame retardant). The addition of synergistic flame retardants has a significant effect on improving the flame retardant properties of asphalt.

[0044] On the other hand, it can be seen from Table 2 that the softening point of the matrix asphalt is slightly improved after being modified with flame retardants, which indicates that the two flame retardants have a certain improvement effect on the high-temperature stability of asphalt, while the needle penetration is slightly reduced, which indicates that the addition of flame retardants will increase the modulus of asphalt to a certain extent and improve the deformation resistance of asphalt.

[0045] Table 2 also shows that Example 3 (10% ML-SBS, rare earth synergistic flame-retardant SBS-modified asphalt with lanthanum oxide) achieves a high limiting oxygen index of 27.1%, significantly higher than that of Comparative Example 3 (SBS-modified asphalt), demonstrating the excellent flame retardancy of the composite flame retardant. Furthermore, the addition of the composite flame retardant has minimal impact on the basic properties of the SBS-modified asphalt.

[0046] In summary, the flame retardant asphalt prepared by the scheme in this application has excellent flame retardant effect, has no negative impact on the performance of the asphalt itself, and even has a certain positive promotion on the performance of the base asphalt.

[0047] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any modifications or substitutions that can be easily conceived by a person skilled in the art within the technical scope disclosed in the present invention should be included in the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be based on the scope of protection of the claims.

Claims

1. A rare earth synergistic flame retardant asphalt composition, characterized in that: The raw materials include the following parts by weight: 10 parts of composite flame retardant and 100 parts of asphalt; The composite flame retardant consists of magnesium hydroxide, rare earth synergist, silane coupling agent KH550 and anhydrous ethanol.

2. The rare earth synergistic flame retardant asphalt composition according to claim 1, characterized in that: The rare earth synergist is one of lanthanum oxide and cerium oxide.

3. A rare earth synergistic flame retardant asphalt composition according to claim 2, characterized in that: The mass fractions of the components in the composite flame retardant are: 9 parts of magnesium hydroxide, 1 part of rare earth synergist, 0.09 parts of silane coupling agent KH550 and 0.81 parts of anhydrous ethanol.

4. A method for preparing the rare earth synergistic flame retardant asphalt composition according to claim 3, characterized in that: The following steps are involved: S100: preparing a composite flame retardant intermediate, mixing 9 parts of magnesium hydroxide and 1 part of lanthanum oxide / cerium oxide at room temperature, and then drying them in an oven to obtain a composite flame retardant intermediate; S200: preparing a composite flame retardant, taking 0.009 parts of silane coupling agent KH500 and mixing it with 0.81 parts of anhydrous ethanol to prepare 0.9 parts of a treatment liquid, and then spraying the treatment liquid evenly onto the surface of the composite flame retardant intermediate, stirring while spraying to make the two mixed evenly, and drying after mixing evenly to obtain a composite flame retardant; S300: prepare flame retardant asphalt, add the composite flame retardant into 100 parts of heated asphalt, shear and disperse it through a high-speed shearing machine, and keep it warm for 20 minutes to obtain the flame retardant asphalt.

5. A rare earth synergistic flame retardant asphalt composition and a preparation method thereof according to claim 4, characterized in that: In step S100, the stirring time of magnesium hydroxide and lanthanum oxide / cerium oxide is 5 minutes.

6. A rare earth synergistic flame retardant asphalt composition and a preparation method thereof according to claim 4, characterized in that: In step S100, the oven temperature is 160°C and the drying time is 30 minutes.

7. A rare earth synergistic flame retardant asphalt composition and a preparation method thereof according to claim 4, characterized in that: In step S200, the treatment liquid and the composite flame retardant intermediate are mixed evenly and then dried at 65°C for 1.5 hours.

8. The rare earth synergistic flame retardant asphalt composition and preparation method thereof according to claim 4, characterized in that: In step S300, the asphalt is base asphalt or modified asphalt, wherein the heating temperature and the insulation temperature of the base asphalt are both 160°C, and the heating temperature and the insulation temperature of the modified asphalt are both 180°C.

9. A rare earth synergistic flame retardant asphalt composition and a preparation method thereof according to claim 4, characterized in that: In step S300, the high-speed shearing machine can be replaced by a colloid mill, and the rotation speed of the colloid mill is 4000 r / min.

Citation Information

Patent Citations

  • Nano asphalt flame-retardant smoke inhibition modifying agent and preparation thereof

    CN101709123A

  • Flame-retardant modified asphalt and preparation method thereof

    CN103013147A

  • Smoke suppression type asphalt flame retardant and preparation method thereof

    CN108329703A

  • Flame-retardant asphalt and preparation method thereof

    CN109988430A

  • Rare earth synergistic flame-retardant asphalt composition and preparation method thereof

    CN116814087A

Cited By

  • Rare earth hybrid flame retardant as well as preparation method and application thereof

    CN120365631A

  • Warm-mixing flame-retardant composite asphalt modifier as well as preparation and use methods thereof

    CN120422374A

  • A warm mix flame retardant composite asphalt modifier and methods of making and using the same

    CN120422374B

  • Preparation method of additive type nitrogen-phosphorus-lanthanum synergistic flame-retardant polyurethane elastomer

    CN120718243A

  • Preparation process of smoke suppression composite modified asphalt

    CN120795648A