Method for producing crystalline film, vapor phase growth device, and β-gallium oxide crystalline film

The vapor phase growth method combining trimethyl gallium, oxygen, and silicon dopant in argon, within a controlled temperature range, addresses the challenge of achieving high-purity β-Ga2O3 films, enabling the production of high-purity β-Ga2O3 crystal films with enhanced mobility for high-voltage power devices.

WO2024242090A1PCT designated stage expired Publication Date: 2024-11-28NIPPON SANSO CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018607
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2024-05-21
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional MOCVD methods face difficulties in obtaining high-purity crystalline β-Ga2O3 films necessary for high-voltage power devices due to impurity incorporation and thermal stability issues.

Method used

A vapor phase growth method involving the combination of trimethyl gallium, oxygen, and silicon dopant in argon, heated to 850-1100°C, is used to form a β-gallium oxide crystal film, with a vapor phase growth apparatus designed to prevent impurity incorporation by controlling gas flow and temperature, resulting in a crystal film with low carbon, hydrogen, and nitrogen content and high mobility.

Benefits of technology

The method produces high-purity β-Ga2O3 crystal films with low impurity content and high electron mobility, suitable for high-voltage power devices, by effectively suppressing unintentional impurity incorporation and maintaining optimal growth temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018607_28112024_PF_FP_ABST
    Figure JP2024018607_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a method for producing a crystalline film, wherein multiple feedstock gases are converged at a convergence position to obtain a mixed gas having trimethylgallium, oxygen, and a silicon dopant contained in argon, the temperature at the convergence position is set to be 850-1100°C so as to heat the obtained mixed gas from the convergence position, the heated mixed gas is guided onto the surface of a substrate 2, and a β-gallium oxide crystalline film is grown on the surface of the substrate 2.
Need to check novelty before this filing date? Find Prior Art

Description

Crystalline film manufacturing method, vapor phase growth apparatus, and β-gallium oxide crystal film

[0001] The present invention relates to a method for producing a crystalline film, a vapor phase growth apparatus, and a β-gallium oxide crystalline film. This application claims priority to Japanese Patent Application No. 2023-084641, filed on May 23, 2023, the contents of which are incorporated herein by reference.

[0002] Vapor deposition is a thin-film formation method in which thin-film raw materials are supplied in a gaseous state onto a substrate and deposited on the substrate surface through a chemical reaction. For example, gallium nitride semiconductor thin films, which are used to make blue light-emitting diodes, green light-emitting diodes, and violet laser diodes, are manufactured by MOCVD (Metal Organic Chemical Vapor Deposition), which uses organic metals as raw materials.

[0003] An example of a vapor phase growth apparatus for forming a semiconductor thin film using a vapor phase growth method is disclosed in Patent Document 1. The vapor phase growth apparatus in Patent Document 1 heats the area near the substrate, but cools the source gas flow path with a cooling device to prevent the source gas from forming a film in the flow path before reaching the substrate. In addition, a heat insulating plate separates the source gas flow path from the area near the substrate, preventing the source gas flow path from being heated together with the area near the substrate.

[0004] In recent years, gallium oxide has been attracting attention as a new semiconductor material. Gallium oxide has different crystal structures, which are designated as α, β, γ, δ, and ε types. Of these, the β type is considered to be the most thermally stable. β-gallium oxide (β-Ga 2 O 3 ) has excellent physical properties, such as a band gap of approximately 5 eV and a breakdown field of approximately 8 MV / cm, and is expected to be applied to high-voltage power devices. Non-Patent Document 1 reports that β-gallium oxide crystals were formed into a film by MOCVD.

[0005] Patent No. 4542860

[0006] F.Alema,B.Hertog,A.Osinsky,P.Mukhopadhyay,M.Toporkov,and WVSchoenfeld,J.Cryst.Growth 475(2017)77-82

[0007] To realize high-voltage power devices, high-purity β-Ga 2 O 3 However, it is difficult to grow high-purity β-Ga films by conventional MOCVD. 2 O 3 The present invention has been made in view of the above circumstances, and provides a method for producing a crystalline film of high purity β-Ga. 2 O 3 A method for producing a crystal film, a vapor phase growth apparatus, and a β-gallium oxide crystal film are provided.

[0008] In order to achieve the above-mentioned objects, the present invention employs the following configurations. [1] A method for producing a crystalline film, comprising: joining a plurality of source gases at a joining position to obtain a mixed gas containing trimethylgallium, oxygen, and a silicon dopant in argon; heating the obtained mixed gas from the joining position; then directing the heated mixed gas to a substrate surface and growing a β-gallium oxide crystalline film on the substrate surface. [2] The method for producing a crystalline film according to [1], wherein heating is performed so that the temperature at the joining position becomes 850 to 1100°C. [3] The method for producing a crystalline film according to [1] or [2], wherein the plurality of source gases comprises a first source gas containing trimethylgallium and a silicon dopant in argon, and a second source gas containing oxygen in argon. [4] A vapor phase growth apparatus for forming a β-gallium oxide crystal film by vapor phase growth by supplying a mixed gas containing trimethylgallium, oxygen, and a silicon dopant in argon to a substrate placed in a reactor, the vapor phase growth apparatus comprising: a source gas flow path for directing each of multiple source gases to a confluence position; and a mixed gas flow path for directing the mixed gas obtained at the confluence position from the confluence position to the substrate surface and then discharging it; and a heating device for heating the temperature at the confluence position to 850 to 1100°C. [5] The vapor phase growth apparatus according to [4], wherein the heating device is disposed around a portion of the reactor surrounding the confluence position. [6] The vapor phase growth apparatus according to [4] or [5], wherein the source gas flow path comprises a flow path for a first source gas containing trimethylgallium and a silicon dopant in argon and a flow path for a second source gas containing oxygen in argon. [7] A vapor phase growth apparatus according to [4] or [5], wherein the source gas flow path comprises a flow path for a first source gas containing trimethylgallium and a silicon dopant in argon and a flow path for a second source gas containing oxygen in argon. 17 cm -3 [8] A β-gallium oxide crystal film having a donor concentration N d and the acceptor concentration N a The difference between [N d -N a ] is 10 15 cm -3 10 above 19 cm -3 [9] The β-gallium oxide crystal film according to [7], having a mobility of 30 cm or less. 2The β-gallium oxide crystal film according to [7] or [8], wherein Vs is 0.1V or more.

[0009] According to the method for producing a crystal film and the vapor phase growth apparatus of the present invention, high purity β-Ga 2 O 3 Furthermore, the β-gallium oxide crystal film of the present invention is highly pure and is expected to be used in high-voltage power devices.

[0010] Fig. 1 is a schematic configuration diagram of a vapor phase growth apparatus according to a first embodiment, as viewed from the front; Fig. 2 is a schematic configuration diagram of a vapor phase growth apparatus according to the first embodiment, as viewed from above; Fig. 3 is a schematic configuration diagram of a vapor phase growth apparatus according to a second embodiment, as viewed from the front; Fig. 4 is a diagram showing the results of Experimental Example 1; Fig. 5 is a diagram showing the results of Experimental Example 5; Fig. 6 is a diagram showing the results of Experimental Example 6; Fig. 7 is a diagram showing the results of Experimental Example 7; Fig. 8 is a diagram showing the results of Experimental Example 9; Fig. 9 is a diagram showing the results of Experimental Example 10; Fig. 11 is a diagram showing the results of Experimental Example 11; Fig. 12 is a diagram showing the results of Experimental Example 12; Fig. 13 is a diagram showing the results of Experimental Example 13; Fig. 14 is a diagram showing the results of Experimental Example 14; Fig. 15 is a diagram showing the results of Experimental Example 15; Fig. 16 is a diagram showing the results of Experimental Example 16; Fig. 17 is a diagram showing the results of Experimental Example 17; Fig. 18 is a diagram showing the results of Experimental Example 18; Fig. 19 is a diagram showing the results of Experimental Example 19; Fig. 20 is a diagram showing the results of Experimental Example 20; Fig. 21 is a diagram showing the results of Experimental Example 21; Fig. 22 is a diagram showing the results of Experimental Example 22; Fig. 23 is a diagram showing the results of Experimental Example 23; Fig. 24 is a diagram showing the results of Experimental Example 24; Fig. 25 is a diagram showing the results of Experimental Example 25; Fig. 26 is a diagram showing the results of Experimental Example 26; Fig. 27 is a diagram showing the results of Experimental Example 27; Fig. 28

[0011] 1 and 2 show a vapor phase growth apparatus according to a first embodiment of the present invention. The vapor phase growth apparatus in Fig. 1 is an apparatus for forming a β-gallium oxide crystal film by vapor phase growth, and includes a reaction tube 1 in which a substrate 2 is placed, and a zone heater 10 for heating the reaction tube 1. In this embodiment, the zone heater 10 corresponds to the heating device of the present invention. Furthermore, the reaction tube 1 corresponds to the reactor of the present invention.

[0012] Formed within reaction tube 1 are upstream flow channel 20, intermediate flow channel 26, and downstream flow channel 29. Upstream flow channel 20 corresponds to the source gas flow path of the present invention, which guides multiple source gases to a joining position. Meanwhile, intermediate flow channel 26 and downstream flow channel 29 are flow paths that guide the mixed gas from the joining position to the substrate surface and then discharge it, and correspond to the mixed gas flow path of the present invention.

[0013] Three flow paths are formed in the upstream flow channel 20, in order from top to bottom: a top channel 21, a middle channel 22, and a bottom channel 23. The middle channel 22 serves as a source gas flow path for supplying a first source gas to the substrate 2, and the top channel 21 and the bottom channel 23 serve as source gas flow paths for supplying a second source gas to the substrate 2.

[0014] 1 and 2, the vertical cross section of upstream flow channel 20 of this embodiment decreases in diameter from upstream to downstream, and the horizontal cross section increases in diameter from upstream to downstream. At the downstream end, the channel has a flattened shape that expands horizontally, and the first source gas flows out from the vertical center, and the second source gas flows out from above and below.

[0015] Intermediate flow channel 26 is connected to the downstream side of upstream flow channel 20, and this connection point, i.e., the upstream end of intermediate flow channel 26, corresponds to the confluence position of the present invention where multiple source gases converge. At the confluence position, the first source gas flowing out of middle channel 22 and the second source gas flowing out of top channel 21 and bottom channel 23 converge, and the resulting mixed gas flows through intermediate flow channel 26. Point A, indicated by a black circle in the figure, is the center of the confluence position.

[0016] An upper opening 27 is formed in the upper pipe wall of the intermediate flow channel 26, and a hanging-type substrate holder 3 is fitted into this upper opening 27. The hanging-type substrate holder 3 has a plurality of claws for supporting the substrate 2 on its underside facing the interior of the intermediate flow channel 26. By placing the substrate 2 on this hanging-type substrate holder 3, the lower surface of the substrate 2 is exposed to the mixed gas in the intermediate flow channel 26. By using a so-called "face-down" configuration in which the lower surface of the substrate 2 is exposed to the mixed gas, it is easy to avoid unexpected particle adhesion, etc.

[0017] The downstream flow channel 29 is connected to the downstream side of the intermediate flow channel 26 , and the mixed gas that has passed through the intermediate flow channel 26 is discharged from the downstream side of the downstream flow channel 29 to the outside of the reaction tube 1 .

[0018] A source gas supply pipe is connected to the upstream side of the upstream flow channel 20. Specifically, a first source gas supply pipe 31 is connected to the middle channel 22 and supplies a first source gas to the middle channel 22. A second source gas supply pipe 32a is connected to the top channel 21 and supplies a second source gas to the top channel 21. A second source gas supply pipe 32b is connected to the bottom channel 23 and supplies a second source gas to the bottom channel 23.

[0019] The zone heater 10 is provided in an annular shape along the outer wall of the reaction tube 1. The zone heater 10 is composed of an upstream heater 11, an intermediate heater 12, and a downstream heater 13, and the temperatures of the upstream heater 11, the intermediate heater 12, and the downstream heater 13 can be set individually.

[0020] The upstream heater 11 is disposed within the outer wall of the reaction tube 1 around a portion surrounding point A so as to heat the vicinity of point A where the first and second source gases join (the upstream portion of the intermediate flow channel 26). The intermediate heater 12 is disposed within the outer wall of the reaction tube 1 around a portion surrounding the location where the upper surface opening 27 of the intermediate flow channel 26 is provided so as to heat the location where the substrate 2 is disposed, i.e., the location where the substrate 2 is disposed. The downstream heater 13 is disposed within the outer wall of the reaction tube 1 around a portion surrounding the location where the upper surface opening 27 is provided so as to heat the downstream side of the location where the upper surface opening 27 of the intermediate flow channel 26 is provided and the downstream flow channel 29.

[0021] The downstream side of upstream flow channel 20 (near point A) is covered with a heat insulating box 5. Heat insulating box 5 can be constructed, for example, by sealing an alumina heat insulating material inside a hollow annular box made of quartz. By providing heat insulating box 5, it is possible to prevent the source gas from thermally decomposing in upstream flow channel 20 and gallium and the like from adhering to the inside of upstream flow channel 20.

[0022] Instead of the insulating box 5, an insulating mat or the like may be wrapped around the downstream side of the upstream flow channel 20. When the insulating box 5 is used, it can be moved in the direction of the flow of the raw material gas while maintaining its overall shape, making it easier to adjust the temperature near point A.

[0023] [Method for manufacturing a crystal film] To manufacture a crystal film using the vapor phase growth apparatus of the first embodiment, the substrate 2 is suspended by the hanging substrate holder 3, and a mixed gas is brought into contact with the lower surface of the substrate 2 under predetermined heating conditions.

[0024] The substrate 2 is not particularly limited as long as it is plate-shaped and can support a crystal film, and may be a known substrate. It may be an insulating substrate, a conductive substrate, or a semiconductor substrate. In this embodiment, the substrate is preferably a crystal substrate.

[0025] The crystalline substrate is not particularly limited as long as it is a substrate containing a crystalline substance as a main component, and may be a known substrate. It may be an insulating substrate, a conductive substrate, or a semiconductor substrate. It may be a single crystal substrate or a polycrystalline substrate. Examples of crystalline substrates include substrates containing a crystalline substance having a corundum structure as a main component, substrates containing a crystalline substance having a β-gallia structure as a main component, and substrates having a hexagonal crystal structure. The "main component" refers to a substrate containing the crystalline substance in a composition ratio of 50% or more, preferably 70% or more, and more preferably 90% or more.

[0026] Examples of substrates containing a crystalline substance having a corundum structure as a main component include a sapphire substrate and an α-type gallium oxide substrate. Examples of substrates containing a crystalline substance having a β-gallium structure as a main component include a β-Ga 2 O 3 Substrate, or β-Ga 2 O 3 and Al 2 O 3Examples of the substrate having a hexagonal crystal structure include a SiC substrate, a ZnO substrate, and a GaN substrate. Examples of other crystal substrates include a Si substrate.

[0027] In this embodiment, the crystal substrate is preferably a sapphire substrate. Examples of sapphire substrates include c-plane sapphire substrates, m-plane sapphire substrates, and a-plane sapphire substrates. In this embodiment, the crystal substrate is preferably a c-plane sapphire substrate. In addition, in this embodiment, the crystal substrate is also preferably an m-plane sapphire substrate, and the sapphire substrate may have an off-angle. The off-angle is not particularly limited, but is preferably 0° to 15° toward the a-axis or m-axis, or a direction including both of them. The thickness of the crystal substrate is not particularly limited, but is preferably 50 to 2000 μm, and more preferably 200 to 800 μm.

[0028] The mixed gas contains vaporized trimethylgallium, oxygen, and silicon dopant gas in argon gas. Trimethylgallium is the source of gallium atoms, oxygen (oxygen molecules) is the source of oxygen atoms, and argon is the carrier. Silicon dopants include monosilane, tetramethylsilane, and tetraethylsilane.

[0029] It is preferable that the trimethylgallium and oxygen contained in the mixed gas are supplied separately up to the joining point. This prevents the trimethylgallium and oxygen from reacting with each other before the gases join. It is also preferable that the trimethylgallium and silicon dopant are supplied to the joining point in a pre-mixed state. This allows for stable control of the supply ratio of silicon dopant to trimethylgallium.

[0030] In this embodiment, the first source gas is a gas containing trimethylgallium and silicon dopant in argon, and can be supplied to the joining position via the middle channel 22. The second source gas is a gas containing oxygen in argon, and can be supplied to the joining position via the top channel 21 and the bottom channel 23.

[0031] The supply ratio of silicon dopant to trimethylgallium can be adjusted depending on the amount of silicon to be doped in the crystal film. -9 ~10 -4 According to this embodiment, it is possible to prevent silicon from being unintentionally contained in the mixed gas as an impurity, and therefore it is easy to adjust the amount of silicon to be doped by adjusting the supply ratio of the silicon dopant to trimethylgallium.

[0032] The growth temperature, i.e., the temperature of the mixed gas when it comes into contact with the surface of the substrate 2, is preferably 575 to 1100°C. By keeping the growth temperature at or above the preferred lower limit, the concentration of impurities incorporated into the crystal film can be reduced. The growth temperature is preferably approximately constant over the entire range of the upstream and downstream surfaces of the substrate 2.

[0033] The temperature at point A is preferably 850 to 1100°C, more preferably 870 to 1080°C, even more preferably 890 to 1060°C, and particularly preferably 900 to 1050°C. When the temperature at point A is equal to or higher than the preferred lower limit, the concentration of impurities incorporated into the crystal film can be reduced. When the temperature at point A is equal to or lower than the preferred upper limit, it can be avoided that the temperature exceeds the appropriate growth temperature before contacting the surface of the substrate 2.

[0034] The temperature of the mixed gas before contacting the surface of substrate 2, including point A, is preferably equal to or lower than the growth temperature, and more preferably lower than the growth temperature. This prevents the mixed gas from thermally decomposing before reaching the surface of substrate 2, and prevents gallium, gallium oxide, and the like from adhering to the interior of upstream flow channel 20 or the upstream side of intermediate flow channel 26. It is preferable that the temperature of the mixed gas gradually increase from point A until it contacts the most upstream side of the surface of substrate 2.

[0035] The temperature inside the intermediate flow channel 26 at point A or the like can be confirmed by inserting a thermocouple 4 into the flow path. When measuring the temperature at point A, the tip of the thermocouple 4 is inserted until it reaches the position of point A. When measuring the temperature at point B (the position indicated by the white circle in the figure), the tip of the thermocouple 4 is inserted until it reaches the position of point B. Figures 1 and 2 show a state in which the tip of the thermocouple 4 is retracted slightly downstream of point B.

[0036] However, if the thermocouple 4 is inserted during the actual film formation, problems such as the adhesion of a gallium oxide film to the thermocouple 4 occur. Therefore, nitrogen containing no trimethylgallium, no silicon dopant, or no oxygen is flowed during measurement using the thermocouple 4. Then, the thermocouple 4 is pulled out from the reaction tube 1 during film formation.

[0037] Second Embodiment Fig. 3 shows a vapor phase growth apparatus according to a second embodiment of the present invention. The vapor phase growth apparatus of Fig. 3 is similar to that of the first embodiment, except that it is a so-called "face-up type" in which the upper surface of the substrate 2 is exposed to the mixed gas. In Fig. 3, the same components as those of the first embodiment are denoted by the same reference numerals as in Fig. 1, and detailed description thereof will be omitted.

[0038] Since the vapor phase growth apparatus of this embodiment is a so-called face-up type, a bottom opening 28 is formed in the lower pipe wall of the intermediate flow channel 26, and a top-mounted substrate holder 6 is fitted into this bottom opening 28. A recess for placing the substrate 2 on the top-mounted substrate holder 6 is formed on the top surface, and by placing the substrate 2 on this top-mounted substrate holder 6, the top surface of the substrate 2 is exposed to the mixed gas in the intermediate flow channel 26. The method for producing a crystal film using the vapor phase growth apparatus of this embodiment is the same as the method for producing a crystal film using the vapor phase growth apparatus of the first embodiment, except that the substrate 2 is placed on the top-mounted substrate holder 6.

[0039] In the above-described embodiments, the upstream flow channel 20 is configured to include the middle channel 22 for supplying the first source gas and the top channel 21 and bottom channel 23 for supplying the second source gas. However, the upstream flow channel 20 may be configured to include a fourth channel for supplying a third source gas. In this case, the silicon dopant is not contained in the first source gas, and a gas containing a silicon dopant in argon may be used as the third source gas.

[0040] Furthermore, both the hanging type substrate holder 3 and the over-mounted type substrate holder 6 may be attached to the intermediate flow channel 26 to form an apparatus capable of simultaneously depositing films by two methods, face-down type and face-up type. In addition, various modifications are possible within the scope of the present invention.

[0041] <Mechanism of Action> According to each of the above embodiments, a β-gallium oxide crystal film with few impurities can be efficiently obtained. The reason for this is believed to be as follows: First, in the above embodiments, trimethylgallium is used as the gallium source.

[0042] When triethylgallium is used as the gallium source instead of trimethylgallium, triethylgallium, which has a low decomposition temperature, easily reacts with silicon dioxide contained in the materials (quartz, etc.) of components that come into contact with the source gas, such as flow channels. As a result, there is a problem that a large amount of thermally decomposed silicon is incorporated into the crystalline film. In addition, triethylgallium has a low vapor pressure, making it difficult to supply high-concentration gallium to the reactor.

[0043] In the above embodiment, trimethylgallium, which has a high decomposition temperature and is not susceptible to self-thermal decomposition, is used as the gallium source, which suppresses reaction with quartz, etc., and reduces the amount of silicon unintentionally incorporated into the crystalline film. In addition, because trimethylgallium has a high vapor pressure, it is possible to supply a high concentration of gallium to the reactor, making it possible to grow a crystalline film at high speed.

[0044] Furthermore, when an organic metal is used as a metal source, carbon and hydrogen derived from hydrocarbon groups tend to be incorporated into the crystal film. In each of the above embodiments, the mixed gas is sufficiently heated from the confluence point, so that the hydrocarbons generated by the decomposition of trimethylgallium can be sufficiently combusted with oxygen before reaching the substrate. As a result, the incorporation of carbon and hydrogen derived from hydrocarbon groups into the crystal film can be suppressed.

[0045] In the above embodiment, argon was used as the carrier. If nitrogen gas were used as the carrier, nitrogen would be incorporated into the film and form acceptors. Argon does not form donors or acceptors in the film.

[0046] In this manner, the above embodiment can reduce the amount of impurities unintentionally mixed into the β-gallium oxide crystal film, and as a result, by adjusting the supply ratio of silicon dopant to trimethylgallium, it is possible to stably control the electron concentration in the crystal film.

[0047] Conventionally, the source gas flow path has been cooled by a cooling device to prevent the source gas from forming a film in the flow path before reaching the substrate. In contrast, in the above embodiment, not only is cooling not performed, but the mixed gas is intentionally heated from the confluence point, and film formation in the flow path is sufficiently suppressed for practical use. This is thought to be because the hydrocarbon group portion reacts more easily with oxygen than the gallium derived from trimethylgallium. The crystal film obtained in the above embodiment will be described in detail below.

[0048] <Crystalline Film> The crystalline film of this embodiment is a β-type gallium oxide crystalline film. The crystalline film of this embodiment has a total content of carbon, hydrogen, and nitrogen of 2×10 17 cm -3 The total content of carbon, hydrogen, and nitrogen is 10 17 cm -3 Preferably, it is 10 or less. 16 cm -3 In this specification and claims, the unit of the numerical value indicating the content of each atom contained in the crystal film is "cm -3" This unit means the number of atoms per cubic centimeter, and is expressed as "atoms / cm 3 The same applies to the electron concentration shown in FIG.

[0049] The carbon content is 10 17 cm -3 Preferably, it is 10 or less. 16 cm -3 More preferably, it is 10 15 cm -3 It is more preferable that the hydrogen content is 10 17 cm -3 Preferably, it is 10 or less. 16 cm -3 More preferably, it is 10 15 cm -3 It is more preferable that the nitrogen content is 10 or less. 17 cm -3 Preferably, it is 10 or less. 16 cm -3 More preferably, it is 10 15 cm -3 It is even more preferable that:

[0050] The content of silicon not contained as a dopant, i.e., not derived from an intentionally used silicon dopant, is 10 16 cm -3 Preferably, it is 10 or less. 15 cm -3 It is more preferable that the content of each of carbon, hydrogen, nitrogen and silicon is the average value of the concentration in the range of 1 to 3 μm from the film surface, measured by secondary ion mass spectrometry (SIMS).

[0051] The crystal film of this embodiment is doped with silicon to be of n-type. d and the acceptor concentration N a The difference between [N d -N a ] is 10 15 cm -3 10 above 19 cm -3 The difference [Nd -N a ] is the average value of the values ​​in the range of 2 to 3 μm from the film surface calculated by capacitance-voltage (CV) measurement using a mercury probe. d -N a ] is 10 15 cm -3 10 above 19 cm -3 It is preferable that:

[0052] The crystal film of this embodiment has a mobility of 30 cm 2 / Vs or more, and 2 / Vs or more, and more preferably 100 cm 2 / Vs or more is more preferable. High mobility can suppress power loss during operation of the semiconductor device. The thickness of the crystal film of this embodiment is preferably 0.5 to 100 μm.

[0053] The crystalline film of this embodiment can be particularly suitably used in semiconductor devices, and is particularly useful in power devices. Examples of semiconductor devices formed using the crystalline film of this embodiment include transistors such as MIS and HEMT, TFTs, Schottky barrier diodes using semiconductor-metal junctions, PN or PIN diodes combined with other P layers, and light-emitting / receiving elements. The crystalline film of this embodiment may be used in semiconductor devices as is, as formed on a substrate, or may be applied to semiconductor devices after being peeled off from the substrate by known means. The semiconductor device can be further suitably used as a power module, inverter, or converter by known means, and further suitably used in semiconductor systems using, for example, power supplies.

[0054] <Substrate> The following substrates were used in the following experimental examples: Substrate A: (010) surface, thickness 0.50 mm, Sn-doped Ga 2 O 3 Substrate (manufactured by Novel Crystal Technology Co., Ltd.) Substrate B: (0001) plane, thickness 0.43 mm, m-axis off-angle 0.15°, sapphire substrate (manufactured by Orbray Corporation).

[0055] <Raw Materials> The following raw materials were used in the following experimental examples: TMGa: trimethylgallium (manufactured by Taiyo Nippon Sanso Corporation). 2 : Oxygen (manufactured by Taiyo Nippon Sanso Corporation) Ar: Argon (manufactured by Taiyo Nippon Sanso Corporation) TMSi: Tetramethylsilane (manufactured by Taiyo Nippon Sanso Corporation).

[0056] <Measurement method> The content of each of the impurities, carbon, hydrogen, and nitrogen, was measured at 64 points every 0.031 μm in the range of 1 to 3 μm from the film surface using a secondary ion mass spectrometer IMS-6f manufactured by CAMECA. The content was calculated as the average of the 64 measurement results. The silicon content was measured at 53 points every 0.038 μm in the range of 1 to 3 μm from the film surface using the same device as used to measure carbon, hydrogen, and nitrogen. The content was calculated as the average of the 53 measurement results.

[0057] Difference [N d -N a ] was measured at six points every 0.2 μm in the range of 2 to 3 μm from the film surface using a MATERIALS DEVELOPMENT CORPORATION (CV) measuring device Model 802B equipped with a mercury probe. The average of the six measurement results was calculated as the difference [N d -N a The electron concentration and mobility were determined by AC Hall measurement (alternating current electromagnetic field method) using ResiTest 8300 manufactured by Toyo Corporation.

[0058] Ar, O 2 The gas flow rates of , , and TMGa were measured using Fujikin FCST1030MZDTC-4J1-F5L-AR-R6-D28, FCST1005MZDTC-4J1-F1L-O2-R5-D28, and FCST1005MZDTC-4J1-F1L-AR-R4-D28, respectively. The pressure after merging was measured using a diaphragm vacuum gauge. The flow rate of the mixed gas was calculated from the temperature and pressure after merging and the mixed gas flow rate.

[0059] Experimental Example 1: The temperature distribution was confirmed for the same device as in Figure 1, except that an alumina insulating material with a volume similar to that of the insulating box was wrapped around the upstream flow channel 20 instead of the insulating box 5. The distance from point A to point B was 200 mm. The height and width of the intermediate flow channel 26 were 10 mm and 80 mm, respectively.

[0060] In order to check the temperature distribution using the thermocouple 4, N 2 The N 2 gas supplied from the first source gas supply pipe 31, the second source gas supply pipe 32a, and the second source gas supply pipe 32b is introduced only into the first source gas supply pipe 31. 2 The flow rates of the respective gases were 3.0 L / min, the total flow rate was 9.0 L / min, and the pressure after merging was 1.4 kPa. As a result, the flow rate of the mixed gas at a temperature of 1000°C was 63.2 m / sec, and the time it took for the mixed gas to reach the center of the substrate holder from point A was 0.0019 sec.

[0061] The set temperatures of the zone heaters 10 were 600°C for the upstream heater 11 and 960°C for the intermediate heater 12 and downstream heater 13. As a result, the temperature distribution shown in Figure 4 was obtained. As shown in Figure 4, the temperature at point A was 903°C, and the temperature near the substrate was maintained at a constant temperature of approximately 1000°C.

[0062] Experimental Example 2 Using the same apparatus as in Experimental Example 1, a β-Ga film with a thickness of 5 μm was formed on the substrate A. 2 O 3 A crystalline film was grown. The thermocouple 4 was not used. The gas supplied from the first source gas supply pipe 31 was a gas containing TMGa in Ar, and the gas supplied from the second source gas supply pipes 32a and 32b was a gas containing O in Ar. 2 The gas used was a gas containing TMSi. TMSi was not used as a dopant.

[0063] The supply rate of TMGa was 182 μmol / min, and O 2The supply rate of the mixed gas was set to 178,571 μmol / min (2.0 L / min). The supply ratio of oxygen to trimethylgallium at this time was 981, expressed as a molar ratio of oxygen molecules to trimethylgallium. The growth time was 60 minutes. The set temperature of the zone heater 10 was the same as in Experimental Example 1. The total flow rate of the mixed gas (total flow rate after merging), the pressure after merging, the flow rate of the mixed gas at a temperature of 1,000°C, and the time it took for the mixed gas to reach the center of the substrate holder from point A were 8.4 L / min, 2.4 kPa, 34.4 m / sec, and 0.0035 sec, respectively.

[0064] The impurity concentration in the resulting crystal film was measured, and the carbon concentration was found to be 3×10 16 cm -3 , hydrogen concentration is 7×10 16 cm -3 , nitrogen concentration is 9 × 10 15 cm -3 , silicon concentration is 1×10 15 cm -3 All of these showed extremely low values ​​equivalent to the background level of SIMS measurement. The total content of carbon, hydrogen, and nitrogen was 2 × 10 17 cm -3 The difference [N d -N a ] is 2 x 10 15 cm -3 This confirmed that the impurity concentration could be kept extremely low when the temperature at the joining point was set to 903°C.

[0065] Experimental Example 3 Using the same apparatus as in Experimental Example 1, a β-Ga film having a thickness of 5 μm was formed on the substrate shown in Table 1. 2 O 3 A crystalline film was grown. The thermocouple 4 was not used. The gas supplied from the first source gas supply pipe 31 was a gas containing TMGa in Ar, and the gas supplied from the second source gas supply pipes 32a and 32b was a gas containing O in Ar. 2 The gas used was a gas containing TMSi. TMSi was not used as a dopant.

[0066] The supply rate of TMGa was 182 μmol / min, and O 2The supply rate of trimethylgallium was set to 178571 μmol / min (2.0 L / min). The supply ratio of oxygen to trimethylgallium at this time, expressed as the molar ratio of oxygen molecules to trimethylgallium, was 981. The growth time was 60 minutes.

[0067] The total flow rate, pressure, and flow rate of the mixed gas at a temperature of 1000°C, as well as the time it takes for the mixed gas to reach the center of the substrate holder from point A, were changed for each example as shown in Table 1. The set temperature of the zone heater 10 was the same as in Experimental Example 1.

[0068] The carbon concentration in the resulting crystal film was measured, and the results shown in Table 1 were obtained. From this, it was confirmed that, under the condition that the temperature at the confluence point was 903°C, the impurity concentration could be further reduced by reducing the flow rate of the mixed gas and lengthening the time it took for the gas to reach the center of the substrate from point A.

[0069]

[0070] Experimental Example 4 Using the same apparatus as in Experimental Example 1, a β-Ga film having a thickness of 5 μm was formed on the substrate shown in Table 1. 2 O 3 A crystalline film was grown. The thermocouple 4 was not used. The gas supplied from the first source gas supply pipe 31 was a gas containing TMGa and TMSi in Ar, and the gas supplied from the second source gas supply pipes 32a and 32b was a gas containing O in Ar. 2 The gas contained

[0071] The supply rate of TMGa was fixed at 182 μmol / min, and the supply rate of TMSi was changed to change the TMSi / TMGa supply ratio (the supply molar ratio of tetramethylsilane to trimethylgallium) in the first source gas to 9.97×10 -5 From 4.98 x 10 -7 It has changed up to.

[0072] O 2The supply rate of trimethylgallium was set to 178,571 μmol / min (2.0 L / min). The supply ratio of oxygen to trimethylgallium was 981, expressed as a molar ratio of oxygen molecules to trimethylgallium. The growth time was 60 minutes. The total flow rate of the mixed gas, the pressure, the flow rate of the mixed gas at a temperature of 1,000°C, the time required for the mixed gas to reach the center of the substrate holder from point A, and the set temperature of the zone heater 10 were the same as in Experimental Example 1.

[0073] The results of measuring the electron concentration of the obtained crystal film are shown in Figure 5. As shown in Figure 5, the electron concentration changed linearly depending on the TMSi / TMGa supply ratio. This confirms that, under the condition that the temperature at the joining point was 903°C, the influence of impurities could be suppressed and the electron concentration could be stably controlled by changing the TMSi / TMGa supply ratio.

[0074] Experimental Example 5: The temperature distribution was confirmed using the same apparatus as in Figure 1 (the position of the insulating box 5 was also the same as in Figure 1). The distance from point A to point B was set to 200 mm. The height and width of the intermediate flow channel 26 were set to 10 mm and 80 mm, respectively.

[0075] In order to check the temperature distribution using the thermocouple 4, N 2 The N 2 gas supplied from the first source gas supply pipe 31, the second source gas supply pipe 32a, and the second source gas supply pipe 32b is introduced only into the first source gas supply pipe 31. 2 The flow rates of the respective gases were 3.0 L / min, the total flow rate was 9.0 L / min, and the pressure after merging was 1.4 kPa. As a result, the flow rate of the mixed gas at a temperature of 1000°C was 63.2 m / sec, and the time it took for the mixed gas to reach the center of the substrate holder from point A was 0.0019 sec.

[0076] Regarding the set temperature of the zone heater 10, the upstream heater 11 was set to 600°C in Experimental Example 5-1 and 960°C in Experimental Example 5-2. The intermediate heater 12 and downstream heater 13 were set to 960°C in both Experimental Example 5-1 and Experimental Example 5-2. As a result, the temperature distribution shown in Figure 6 was obtained. As shown in Figure 6, the temperature at point A was 923°C in Experimental Example 5-1 and 939°C in Experimental Example 5-2. The temperature near the substrate was able to be kept constant at approximately 1000°C in both Experimental Example 5-1 and Experimental Example 5-2.

[0077] Experimental Example 6 Using the same apparatus as in Experimental Example 1, a β-Ga film with a thickness of 5 μm was formed on the substrate A. 2 O 3 A crystalline film was grown. The thermocouple 4 was not used. The gas supplied from the first source gas supply pipe 31 was a gas containing TMGa in Ar, and the gas supplied from the second source gas supply pipes 32a and 32b was a gas containing O in Ar. 2 The gas used was a gas containing TMSi. TMSi was not used as a dopant.

[0078] The supply rate of TMGa was 182 μmol / min, and O 2 The supply rate of the mixed gas was set to 178,571 μmol / min (2.0 L / min). The supply ratio of oxygen to trimethylgallium at this time was 981, expressed as the molar ratio of oxygen molecules to trimethylgallium. The growth time was 60 minutes. The set temperature of the zone heater 10 was the same as in Experimental Example 5-1 for Experimental Example 6-1, and the same as in Experimental Example 5-2 for Experimental Example 6-2. The total flow rate of the mixed gas (total flow rate after merging), the pressure after merging, the flow rate of the mixed gas at a temperature of 1,000°C, and the time it took for the mixed gas to reach the center of the substrate holder from point A were 8.4 L / min, 1.4 kPa, 59.0 m / sec, and 0.0020 sec, respectively.

[0079] When the carbon concentration in the obtained crystal film was measured, the carbon concentration in Experimental Example 6-1 was 6×10 17 cm -3 , the carbon concentration in Experimental Example 6-2 is 1×10 17 cm -3From this, it was confirmed that the carbon concentration could be kept lower by increasing the temperature at point A from 923°C to 939°C.

[0080] REFERENCE SIGNS LIST 1 Reaction tube 2 Substrate 3 Hanging type substrate holder 4 Thermocouple 5 Heat insulating box 6 Top type substrate holder 10 Zone heater 11 Upstream heating heater 12 Intermediate heating heater 13 Downstream heating heater 20 Upstream flow channel 21 Top channel 22 Middle channel 23 Bottom channel 26 Intermediate flow channel 27 Top opening 28 Bottom opening 29 Downstream flow channel 31 First source gas supply pipe 32a Second source gas supply pipe 32b Second source gas supply pipe

Claims

1. A method for producing a crystal film, comprising: joining a plurality of source gases at a joining point to obtain a mixed gas containing trimethylgallium, oxygen, and a silicon dopant in argon; heating the mixed gas obtained at the joining point; and then directing the heated mixed gas to a substrate surface to grow a β-gallium oxide crystal film on the substrate surface.

2. The method for producing a crystal film according to claim 1, wherein heating is performed so that the temperature at the joining point is 850 to 1100°C.

3. The method for producing a crystal film according to claim 1 or 2, wherein the plurality of source gases are a first source gas containing trimethylgallium and a silicon dopant in argon, and a second source gas containing oxygen in argon.

4. A vapor phase growth apparatus for supplying a mixed gas containing trimethylgallium, oxygen, and a silicon dopant in argon to a substrate placed in a reaction furnace to form a β-gallium oxide crystal film by vapor phase growth, the vapor phase growth apparatus comprising: a source gas flow path for leading a plurality of source gases to a junction position; and a mixed gas flow path for leading the mixed gas obtained at the junction position from the junction position to the substrate surface and then discharging the gas; and a heating device for heating the junction position to a temperature of 850 to 1100°C.

5. The vapor phase growth apparatus according to claim 4, wherein the heating device is disposed around a portion of the reaction furnace surrounding the joining position.

6. The vapor phase growth apparatus according to claim 4 or 5, wherein the source gas flow passage comprises a flow passage for a first source gas containing trimethylgallium and a silicon dopant in argon, and a flow passage for a second source gas containing oxygen in argon.

7. The total content of carbon, hydrogen, and nitrogen is 2 x 10 17 cm -3 and is doped with silicon.

8. Donor concentration N d and the acceptor concentration N a The difference between [N d -N a ] is 10 15 cm -3 More than 10 19 cm -3 The β-gallium oxide crystal film according to claim 7, wherein:

9. Mobility is 30 cm 2 The β-gallium oxide crystal film according to claim 7 or 8, wherein Vs is 0.1 V or more.

Citation Information

Patent Citations

  • Tablet half splitter

    JP2023084641A

  • Vapor phase growth apparatus

    JP4542860B2

  • Method for manufacturing light-emitting element and light-emitting element

    JP2012142512A

  • Crystal laminate structure

    JP2020100560A

  • Atomic layer deposition and vapor deposition reactor with in-chamber microplasma source