Ultra-high molecular weight polyethylene powder and molded article
By controlling the entanglement of ultra-high molecular weight polyethylene powder and employing specific processing methods, high-strength fibers with minimal molecular weight reduction are produced, addressing the challenge of entanglement-related strength and moldability issues in ultra-high molecular weight polyethylene powders.
Patent Information
- Application Number
- PCT/JP2024/023800
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-07-11
- Filing Date
- 2024-07-01
- Publication Date
- 2025-01-16
AI Technical Summary
Ultra-high molecular weight polyethylene powders face challenges in achieving high-strength fibers with minimal molecular weight reduction during kneading, as excessive entanglement leads to decreased strength and poor moldability due to insufficient disentanglement of molecular chains.
Control the entanglement of ultra-high molecular weight polyethylene powder in liquid paraffin by adjusting intrinsic viscosity, motility index, and degree of entanglement within specific ranges, and employing a method involving slurry formation, gelation, and controlled extrusion processes to produce high-strength fibers.
The approach results in high-strength fibers with minimal molecular weight reduction and improved moldability, achieving uniform gel formation and enhanced mechanical properties.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Ultra-high molecular weight polyethylene powder and moldings
[0001] The present invention relates to an ultra-high molecular weight polyethylene powder and a molded article.
[0002] Polyethylene is used in a wide variety of applications, including films, sheets, microporous membranes, fibers, foams, and pipes. Polyethylene is used because it is easy to melt-process, and the resulting molded articles have high mechanical strength and excellent chemical resistance and rigidity. Among these, ultra-high molecular weight polyethylene has a large molecular weight, which gives it greater mechanical strength, excellent sliding properties and abrasion resistance, as well as excellent chemical stability and long-term reliability.
[0003] Ultra-high molecular weight polyethylene has low fluidity even when melted at temperatures above its melting point. Therefore, a common method is to add a solvent such as liquid paraffin or decalin to ultra-high molecular weight polyethylene powder to form a slurry and process it.
[0004] From the viewpoint of improving the extrusion processability of ultra-high molecular weight polyethylene and improving the strength of molded bodies, methods such as those disclosed in Patent Document 1 have been disclosed. Patent Document 1 discloses that by controlling the pore volume and pore size of polyethylene powder, which has a large particle size and exhibits little change in molecular weight under specific kneading conditions, within appropriate ranges, molded bodies that are easy to process and have high strength can be obtained.
[0005] WO2019 / 187727 publication
[0006] To improve the stretchability of ultra-high molecular weight polyethylene and obtain high-strength molded products, it is necessary to sufficiently disentangle the molecular chains. If the molecular chains are not sufficiently disentangled, the shear forces during kneading will cause the molecular chains to break, resulting in a decrease in molecular weight. Although high orientation is achieved, there is a problem of a decrease in strength.
[0007] The polyethylene powder described in Patent Document 1 focuses on untangling molecular chains by adjusting the pore volume and pore diameter of polyethylene powder with a large particle diameter within an appropriate range. However, there is no description of improving the strength of the yarn by reducing the amount of entanglement of the polyethylene powder itself, regardless of the particle diameter, and there is room for improvement.
[0008] The present invention has been made in view of the above circumstances, and aims to provide, in gel spinning of ultra-high molecular weight polyethylene powder, high-strength fibers that undergo little molecular weight reduction and are less susceptible to yarn breakage even when wound at high speed.
[0009] As a result of intensive research into solving the above problems, the present inventors have found that the above problems can be solved by controlling the entanglement (mobility) of ultra-high molecular weight polyethylene powder in liquid paraffin, and have thus completed the present invention.
[0010] That is, the present invention is as follows. [1] An ultra-high molecular weight polyethylene powder having an intrinsic viscosity IV of 12.0 dL / g or more and 35.0 dL / g or less, and a mobility index calculated from the following formula (I) of 57 ms or more and 73 ms or less, [Mobility Index]=Tα×Rα / (Rα+Rβ)+Tβ×Rβ / (Rα+Rβ) (Formula I), wherein Tα is the relaxation time (ms) of the low mobility component α, Rα is the abundance ratio of the low mobility component α, Tβ is the relaxation time (ms) of the intermediate component β, and Rβ is the abundance ratio of the intermediate component β, and Tα, Rα, Tβ, and Rβ are values obtained by approximating a free induction decay curve obtained by the Carr-Purcell-Meiboom-Gill method using pulsed NMR to three components, namely, the low mobility component α, the intermediate component β, and the high mobility component γ. [2] The ultra-high molecular weight polyethylene powder according to [1], wherein the degree of entanglement calculated from the following formula (II) is 0.6 or more and 2.8 or less: [degree of entanglement]=Rβ / Rα (formula II) [wherein Rβ and Rα are as defined in claim 1]. [3] The ultra-high molecular weight polyethylene powder according to [1] or [2], wherein the relationship of the following formula (formula III) is satisfied: [Mobility index]>-0.2×[intrinsic viscosity IV]+62 (formula III). [4] 13
[0023] The ultra-high molecular weight polyethylene powder according to any one of [1] to [3], wherein the content of structural units derived from olefin copolymerizable with ethylene is 0.1 mol% or less as measured by C-NMR. [5] The ultra-high molecular weight polyethylene powder according to any one of [1] to [4], wherein the D50 measured by a laser diffraction particle size analyzer is 40 μm or more and 400 μm or less. [6] The ultra-high molecular weight polyethylene powder according to any one of [1] to [5], wherein the intrinsic viscosity IV is 17.0 dL / g or more and 33.0 dL / g or less. [7] The ultra-high molecular weight polyethylene powder according to any one of [1] to [6], wherein the mobility index is 64 ms or more and 73 ms or less. [8] The ultra-high molecular weight polyethylene powder according to any one of [1] to [7], wherein the titanium (Ti) content is 10 ppm or less and the aluminum (Al) content is 10 ppm or less. [9] The ultra-high molecular weight polyethylene powder according to any one of [1] to [8], which is for use in high-strength fibers.
[10] A molded product of the ultra-high molecular weight polyethylene powder according to any one of [1] to [9].
[11] The molded product according to
[10] , which is a fiber.
[12] A method for producing a polyethylene terephthalate dispersion comprising: a slurrying step of mixing an ultra-high molecular weight polyethylene powder with a first liquid paraffin and stirring the mixture at a temperature equal to or lower than the melting point of the ultra-high molecular weight polyethylene powder to obtain a slurry; a gelling step of mixing the slurry with a second liquid paraffin at a temperature equal to or higher than 150°C and equal to or lower than 300°C to obtain a gel for a raw yarn at a temperature equal to or higher than 140°C and equal to or lower than 200°C; an extrusion step of extruding the gel for a raw yarn to obtain a raw yarn; an extraction step of extracting the first liquid paraffin and the second liquid paraffin from the raw yarn to obtain a raw yarn for drawing; and a raw yarn drawing step of heating and drawing the raw yarn for drawing, wherein the intrinsic viscosity IV of the ultra-high molecular weight polyethylene powder is equal to or higher than 12.0 dL / g and equal to or lower than 35.0 dL / g, and the mobility index of the ultra-high molecular weight polyethylene powder calculated from the following (formula I) is equal to or higher than 57 ms and equal to or lower than 73 ms. [Mobility index]=Tα×Rα / (Rα+Rβ)+Tβ×Rβ / (Rα+Rβ) (Formula I) [wherein Tα is the relaxation time (ms) of the low mobility component α, Rα is the abundance ratio of the low mobility component α, Tβ is the relaxation time (ms) of the intermediate component β, and Rβ is the abundance ratio of the intermediate component β, and Tα, Rα, Tβ, and Rβ are values obtained by approximating a free induction decay curve obtained by the Carr Purcell Meiboom Gill method using pulsed NMR to three components: the low mobility component α, the intermediate component β, and the high mobility component γ.]
[13] A method for producing a high strength fiber according to
[12] , comprising a kneading step of kneading the yarn gel before the extrusion step.
[14] The method for producing a high-strength fiber according to
[12] or
[13] , wherein in the slurry step, the stirring temperature is 25°C or higher and 120°C or lower, and in the gelling step, the polyethylene concentration of the yarn gel is 3% by mass or higher and 20% by mass or lower.
[15] The method for producing a high-strength fiber according to
[13] or
[14] , wherein in the kneading step, the temperature is 140°C or higher and 200°C or lower, the time is 5 minutes or higher and 180 minutes or lower, and the rotation speed is 3 rpm or higher and 50 rpm or lower.
[16] The method for producing a high-strength fiber according to any one of
[12] to
[15] , further comprising a quenching step after the extrusion step, wherein the time from the extrusion step to the quenching step is from 0 to 10 seconds, and the temperature in the quenching step is from 5 to 30°C.
[17] The method for producing a high-strength fiber according to any one of
[12] to
[16] , further comprising an extrusion preparation step before the extrusion step, wherein the temperature in the extrusion preparation step is from 140 to 200°C, and the time in the extrusion preparation step is from 5 to 90 minutes.
[18] The method for producing a high-strength fiber according to any one of
[12] to
[17] , further comprising: in the extrusion step, an extrusion speed of from 5 to 20 mm / min, a take-up speed of from 200 to 1600 mm / min, a throughput of from 0.2 g / min to 1.5 g / min, and a spinning orifice diameter of from 0.8 mm to 1.5 mm.
[19] The method for producing a high-strength fiber according to any one of
[12] to
[18] , wherein an extraction solvent is used in the extraction step, the extraction solvent is hexane or dichloromethane, and the extraction time is 3 hours or more and 24 hours or less.
[20] The method for producing a high-strength fiber according to any one of
[12] to
[19] , wherein the raw yarn drawing step involves multi-stage drawing.
[21] The method for producing a high-strength fiber according to
[20] , wherein the multi-stage drawing is two-stage drawing.
[22] The method for producing a high-strength fiber according to
[21] , wherein the two-stage drawing includes a first drawing step and a second drawing step, and in the first drawing step, the let-off speed is 50 mm / min or more and 200 mm / min or less, the take-up speed is 1000 mm / min or more and 4000 mm / min or less, and the temperature is 110°C or more and 155°C or less, and in the second drawing step, the let-off speed is 50 mm / min or more and 200 mm / min or less, the take-up speed is 100 mm / min or more and 500 mm / min or less, and the temperature is 130°C or more and 155°C or less.
[0011] According to the present invention, it is possible to provide an ultra-high molecular weight polyethylene powder that undergoes little molecular weight reduction during kneading and allows the production of a uniform gel, thereby providing fibers with good stretchability and high strength.
[0012] Hereinafter, a mode for carrying out the present invention (hereinafter also referred to as "the present embodiment") will be described in detail. Note that the present invention is not limited to the present embodiment, and various modifications can be made within the scope of the gist of the present invention.
[0013] [Ultra-High Molecular Weight Polyethylene Powder] The ultra-high molecular weight polyethylene powder of this embodiment (hereinafter also simply referred to as "polyethylene powder" or "powder") has an intrinsic viscosity IV of 12.0 dL / g or more and 35.0 dL / g or less, preferably 17.0 dL / g or more and 33.0 dL / g or less, and more preferably 20.9 dL / g or more and 31.0 dL / g or less.
[0014] In this embodiment, the intrinsic viscosity IV refers to the intrinsic viscosity calculated from the specific viscosity of the polymer solution.
[0015] The ultra-high molecular weight polyethylene powder of the present embodiment has an intrinsic viscosity IV of not less than the lower limit, thereby further improving the strength, and has an intrinsic viscosity IV of not more than the upper limit, thereby further improving the moldability.
[0016] The ultra-high molecular weight polyethylene powder of the present embodiment is preferably a powder made of an ethylene homopolymer and / or a copolymer of ethylene and an olefin copolymerizable with ethylene (hereinafter also referred to as a "comonomer") (hereinafter also referred to as an "ethylene-based polymer").
[0017] The olefin copolymerizable with ethylene is not particularly limited, but specific examples thereof include α-olefins having 3 to 15 carbon atoms, cyclic olefins having 3 to 15 carbon atoms, olefins represented by the formula CH 2 = CHR 1 (where R 1 is an aryl group having 6 to 12 carbon atoms. ) and at least one comonomer selected from the group consisting of linear, branched, or cyclic dienes having from 3 to 15 carbon atoms. Among these, α-olefins having from 3 to 15 carbon atoms are preferred.
[0018] The α-olefin is not particularly limited, but examples thereof include propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, and 1-tetradecene.
[0019] In the ultra-high molecular weight polyethylene powder of this embodiment, 13 The comonomer content measured by C-NMR is preferably 0.1 mol% or less, more preferably 0.05 mol% or less, and even more preferably 0.02 mol% or less. When the comonomer content in the ultra-high molecular weight polyethylene powder of this embodiment is within the above range, decomposition tends to be suppressed, and the strength of molded articles obtained by molding the ultra-high molecular weight polyethylene powder tends to be improved. The method for measuring the comonomer content is as described in the Examples below.
[0020] The ultra-high molecular weight polyethylene powder according to the present embodiment may be made from ethylene produced from biomass-derived naphtha or biomass-derived ethanol. For example, the biomass-derived ultra-high molecular weight polyethylene powder can be produced by a cracking method using biomass-derived naphtha as a raw material.
[0021] [Intrinsic Viscosity IV] The intrinsic viscosity IV of the ultra-high molecular weight polyethylene powder of this embodiment is as described above.
[0022] The method for controlling the intrinsic viscosity IV within the above range is not particularly limited, but for example, it can be achieved by changing the polymerization temperature of the reactor when homopolymerizing ethylene or copolymerizing ethylene with a copolymerizable olefin. The intrinsic viscosity IV tends to decrease as the polymerization temperature increases, and tends to increase as the polymerization temperature decreases. Another method for adjusting the intrinsic viscosity IV within the above range is not particularly limited, but for example, it can be achieved by changing the type of organometallic compound used as a co-catalyst when homopolymerizing ethylene or copolymerizing ethylene with a copolymerizable olefin. Another method for adjusting the intrinsic viscosity IV within the above range is not particularly limited, but for example, it can be achieved by adding a chain transfer agent when homopolymerizing ethylene or copolymerizing ethylene with a copolymerizable olefin.
[0023] The chain transfer agent is not particularly limited, but includes hydrogen, ethylene, α-olefin, etc. By adding a chain transfer agent, the intrinsic viscosity (IV) of the ultra-high molecular weight polyethylene produced tends to be lowered even at the same polymerization temperature.
[0024] In this embodiment, the intrinsic viscosity IV can be determined by the method described in the examples below.
[0025] [Mobility Index and Degree of Entanglement of Ultra-High Molecular Weight Polyethylene Powder] A known index for estimating the entanglement of molecular chains in a polyethylene powder is the evaluation of dynamic viscoelasticity.
[0026] In evaluating dynamic viscoelasticity, the degree of entanglement is evaluated from the response when stress is applied to the resin, so it is possible to determine the average degree of entanglement for the entire resin. However, when simultaneously controlling multiple physical properties such as mechanical properties and moldability, it is preferable to treat the multiple entangled components present in the resin separately, so the average degree of entanglement alone is insufficient as an indicator. In addition, since dynamic viscoelasticity is generally measured using press-molded products, it is not suitable for evaluating the entanglement of polyethylene powder.
[0027] Furthermore, as the name suggests, ultra-high molecular weight polyethylene powder has an extremely high molecular weight and strong entanglement of molecular chains. When the intrinsic viscosity IV is 12.0 dL / g or higher, as in the ultra-high molecular weight polyethylene powder of this embodiment, the strength of entanglement of molecular chains tends to be remarkable. If the entanglement of molecular chains is too strong, melt processing becomes difficult, so a solvent is added to the polyethylene powder to form a slurry, which is then molded.
[0028] Therefore, in order to identify a raw material suitable for moldings with well-controlled physical properties such as mechanical properties and moldability, the present inventors discovered that accurate evaluation is possible by measuring the degree of entanglement of polyethylene powder in liquid paraffin under the <Slurry Motility Measurement Conditions> described below using the slurry mobility index (hereinafter also referred to as the "mobility index") calculated from pulse NMR measurement of a polyethylene slurry at 150°C as an index for evaluating the entanglement components of polyethylene powder in a solvent. Furthermore, they discovered that calculating the degree of entanglement of the slurry (hereinafter also referred to as the "degree of entanglement") together with the mobility index enables a more accurate evaluation of the degree of entanglement of polyethylene powder in liquid paraffin.
[0029] For pulsed NMR measurements, the Carr Purcell Meiboom Gill method is used, which is a measurement method suitable for evaluating the mobility of polymers (such as rubbery state) in which the molecular chains are actively moving.
[0030] As a result, when the free induction decay curve obtained by the Carr-Purcell-Meiboom-Gill method using pulsed NMR was approximated to three components, namely, a low mobility component α, an intermediate component β, and a high mobility component γ, it was found that a polyethylene powder slurry in which the relaxation time T and component ratio R of each component satisfy the following mobility index is surprisingly suitable as a raw material for fibers (e.g., high-strength fibers):
[0031] <Conditions for measuring slurry mobility> Measurement device: TD-NMR device manufactured by Bruker (model: minispec mq20) Heating conditions: 10°C / min temperature increase, 23 minutes at 60°C, temperature retention 10°C / min temperature increase, 23 minutes at 90°C, temperature retention 10°C / min temperature increase, 23 minutes at 105°C, temperature retention 10°C / min temperature increase, 23 minutes at 120°C, temperature retention 5°C / min temperature increase, 26 minutes at 130°C, temperature retention 5°C / min temperature increase, 26 minutes at 140°C, temperature retention 5°C / min temperature increase, 10 minutes at 150°C, temperature retention (motility was then measured)
[0032] The temperatures above are the values measured by a thermocouple at the internal temperature of the sample. The set temperature of the device is corrected by creating calibration lines (Equation A) and (Equation B) to take into account any deviation from the target temperature (actual temperature) of the sample. Round off any decimal points. (For temperatures between 0°C and 100°C): y = 1.0984x + 260.88 (Equation A) (For temperatures greater than 100°C and less than 200°C): y = 1.1729x + 252.21 (Equation B) x = target temperature (°C), y = set temperature (K)
[0033] Slurry preparation conditions: When the total of polyethylene powder and liquid paraffin (liquid paraffin manufactured by MORESCO Corporation (product name: Smoil P-350P)) is 100 parts by mass, 30 parts by mass of polyethylene powder, 70 parts by mass of liquid paraffin, and 1 part by mass of antioxidant (antioxidant manufactured by ADEKA Corporation (ADEKA STAB AO-60G)) are mixed. After preparation, the sample is left to soak for 20 hours, and then measurements are carried out.
[0034] The liquid paraffin used in measuring the slurry mobility is liquid paraffin manufactured by MORESCO Corporation (product name: Smoil P-350P), and its representative properties are density at 15°C: 0.866 g / cm 3 , pour point: -10°C, kinematic viscosity at 40°C: 68.00 mm2 / s (cSt), kinematic viscosity at 100°C: 9.188 mm2 / s (cSt), ring analysis Cn: 30%, Cp: 70%, average molecular weight: 489 g / mol.
[0035] (Motility index) = Tα × Rα / (Rα + Rβ) + Tβ × Rβ / (Rα + Rβ) (Equation I) Tα: relaxation time (ms) of low mobility component α Rα: proportion of low mobility component α Tβ: relaxation time (ms) of intermediate component β Rβ: proportion of intermediate component β
[0036] The specific method for measuring the motility index is as described in the Examples below.
[0037] The liquid paraffin used in the molding process may be any liquid paraffin that functions as a plasticizer and that, when kneaded with the ultra-high molecular weight polyethylene powder, can form a homogeneous solution at or above the melting point of the ultra-high molecular weight polyethylene powder.
[0038] The antioxidant used during molding is not particularly limited, but is preferably, for example, a phenolic compound or a phenolic phosphate compound. Specific examples include phenolic antioxidants such as 2,6-di-t-butyl-4-methylphenol (dibutylhydroxytoluene), n-octadecyl-3-(4-hydroxy-3,5-di-t-butylphenyl)propionate, and tetrakis(methylene(3,5-di-t-butyl-4-hydroxyhydrocinnamate))methane; phenolic phosphorus antioxidants such as 6-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenzo[d,f][1,3,2]dioxaphosphepine; and phosphorus antioxidants such as tetrakis(2,4-di-t-butylphenyl)-4,4′-biphenylene-diphosphonite, tris(2,4-di-t-butylphenyl)phosphite, and cyclic neopentanetetraylbis(2,4-t-butylphenylphosphite).
[0039] The low-mobility component α in the slurry of the polyethylene powder of this embodiment is composed of tightly entangled molecular chains that are difficult to dissolve when dissolved in a solvent, and is considered to be a component that is likely to be subject to strong shear as physical crosslinking points during the molding process.
[0040] The intermediate component β in the polyethylene powder slurry of this embodiment corresponds to the portion where the dissolved molecular chains are weakly entangled, and is thought to be a component that is easily disentangled during the molding process. Furthermore, the stronger the entanglement of the components and the lower the mobility, the shorter the relaxation time T. The highly mobile component γ in the polyethylene powder slurry of this embodiment is thought to correspond to the terminal portion of the polyethylene molecular chains that are not entangled with liquid paraffin.
[0041] The mobility index of a slurry is expressed as the ratio of each component and the relaxation time when the polymer is dissolved in liquid paraffin, and is an index for evaluating the degree of entanglement and mobility of the entire molecular chain.
[0042] The ultra-high molecular weight polyethylene powder of this embodiment has a mobility index of 57 ms or more and 73 ms or less, preferably 60 or more and 69 or less, and more preferably 64 ms or more and 68 ms or less, under the slurry mobility measurement conditions.
[0043] A mobility index of 57 ms or more at 150°C results in a moderate amount of strong entanglement of molecular chains, reducing stress during molding and processing, thereby minimizing the decrease in molecular weight. Furthermore, since the molecular chains are smoothly unraveled, fibers that are less susceptible to yarn breakage even when drawn at high speeds tend to be obtained.
[0044] On the other hand, when the mobility index at 150°C is 73 ms or less, the molecular chains have a moderate amount of weak entanglement components, there are sufficient entanglement points, and stress is transmitted uniformly during drawing, making it easier to obtain high-strength yarn.
[0045] Generally, when the degree of entanglement of molecular chains is strong, the mobility of the molecular chains is low, resulting in a high kneading share, a decrease in molecular weight, and the molecular chains do not move smoothly during stretching, resulting in poor molding processability and unevenness.
[0046] On the other hand, when the degree of entanglement of the polymer is weak, the mobility of the molecular chains is high, resulting in excellent stretchability and a high degree of orientation, resulting in a high-strength thread. However, since there are not enough entanglement points, stress does not propagate uniformly, which is thought to result in unevenness. This unevenness creates areas with weak mechanical strength, which become the starting point for fracture.
[0047] The polyethylene powder of this embodiment has a well-controlled degree of entanglement, which makes it possible to improve both the mechanical strength and molding processability of the fiber.
[0048] In order to control the mobility index of the 150° C. slurry of the ultra-high molecular weight polyethylene powder of this embodiment within the above range, it is necessary to appropriately reduce the entanglement of the polyethylene powder. There are no particular limitations on the method for reducing entanglement, but possible methods include suppressing entanglement formation in the early stages of polymerization and polymerizing an unbranched linear polymer.
[0049] One way to reduce entanglement in polyethylene powder is to suppress entanglement formation in the early stages of polymerization. Entanglement formation in the early stages of polymerization occurs mainly when the active sites are close to each other and polymer chains growing from nearby sites become entangled. Therefore, it is thought that entanglement due to polymerization can be reduced by reducing the active site density on the catalyst surface and increasing the distance between active sites.
[0050] For example, there are a method of reducing the active site density of the catalyst, a method of using a co-catalyst used in polymerization that is bulkier than the distance between adjacent catalytic active sites, a method of simultaneously adding titanium tetrachloride and a specific organomagnesium when supporting active sites on a carrier, and a method of using a mixture of two or more types of co-catalysts for polymerization.
[0051] A specific method for reducing the active site density of a catalyst is to reduce the amount of titanium supported on the catalyst by adjusting the molar ratio of raw materials during synthesis. The molar ratio of titanium to magnesium atoms in the support (Ti / Mg) is preferably 1 / 4 or less, more preferably 1 / 8 or less, more preferably 1 / 16 or less, and even more preferably 1 / 32 or less. Another method is to perform a surface treatment with organoaluminum after supporting titanium on the support, thereby liberating excess titanium compounds.
[0052] Titanium tetrachloride is known to form an agglomerated structure on the support, and polymer chains grow from the agglomerated active sites while becoming entangled. By reducing the active site density on the catalyst surface, the number of agglomerated active sites can be reduced, and the entanglement at the initial stage of polymerization can be reduced.
[0053] It is also possible to use a co-catalyst that is bulkier than the distance between adjacent catalytic active sites. Due to steric hindrance from the bulky co-catalyst, active sites that are closer than the size of the co-catalyst are not activated, and the distance between active sites participating in the polymerization appears to be greater. This makes it difficult for the polymer chains growing during polymerization to entangle with each other, resulting in a polyethylene powder with minimal entanglement.
[0054] Furthermore, after extensive research, the inventors discovered that polyethylene powder with less entanglement can also be obtained by using an organomagnesium to carry out a vigorous reaction when supporting active sites on a support. While the reason why polyethylene powder with less entanglement can be obtained using the above method is unclear, it is believed that when titanium tetrachloride and a highly reactive organomagnesium are added simultaneously, a vigorous reaction occurs, generating catalyst fine particles in the solvent rather than on the support surface. Each catalyst fine particle is independently supported on the support, thereby increasing the distance between active sites. For example, the organomagnesium may be a mixture of dialkylmagnesium and trialkylaluminum, and it is preferable that the proportion of dialkylmagnesium is higher than that of trialkylaluminum.
[0055] The degree of entanglement of the slurry of the ultra-high molecular weight polyethylene powder of this embodiment, as calculated by the following formula (II), is 0.6 or more and 2.8 or less, preferably 1.0 or more and 2.7 or less, and more preferably 1.2 or more and 2.6 or less, under the above-mentioned conditions for measuring the slurry mobility: (degree of entanglement)=Rβ / Rα (formula II)
[0056] As described above, Rα and Rβ in (Equation II) are the abundance ratio of the low-mobility component α and the abundance ratio of Rβ:intermediate component β, respectively.
[0057] Rα is preferably 9 or more and 24 or less, and more preferably 10 or more and 23 or less.
[0058] Rβ is preferably 12 or more and 27 or less, and more preferably 13 or more and 26 or less.
[0059] When Rα and Rβ are within the above ranges, the entanglement points are well balanced, and excellent stretchability and strength tend to be obtained.
[0060] The degree of entanglement is indicated by the proportion of low-mobility component α and the proportion of intermediate component β in liquid paraffin, and indicates the number of entanglement points that act like physical crosslinking points that restrain molecular chains.
[0061] When the degree of entanglement of the slurry of the ultra-high molecular weight polyethylene powder is 0.6 or more, the number of entanglement points does not become too large, and sufficient lamellar crystals can be obtained without lowering the polymer concentration and kneading, which results in better drawability during gel spinning processing and tends to make the yarn less susceptible to breakage.
[0062] Furthermore, by setting the degree of entanglement of the slurry to 2.8 or less, there are sufficient entanglement points that are responsible for the propagation of the drawing stress, which allows the stress to be propagated uniformly, promotes the orientation of molecular chains, enables drawing at a higher magnification, and tends to enable the production of yarn with higher strength.
[0063] One possible method for controlling the degree of entanglement of the ultra-high molecular weight polyethylene powder of this embodiment in a 150°C slurry within the above range is to polymerize a non-branched linear polymer. The absence of branches makes the molecular chains more slippery, and the entanglements formed during polymerization can be dissolved during the dissolution process, resulting in a polyethylene powder with a low degree of entanglement in liquid paraffin.
[0064] Specifically, one method involves using a mixture of two or more types of co-catalysts for polymerization. It is generally known that a chain transfer reaction results in the production of macromonomers with terminal double bonds through beta hydrogen elimination. Because macromonomers are incorporated into molecular chains during polymerization, they form long-chain branches, which inhibit the unraveling of molecular chains and increase entanglement. Therefore, by using a mixture of two or more types of co-catalysts, it is possible to promote chain transfer of the co-catalyst and suppress branching, resulting in a polyethylene powder with reduced entanglement during the dissolution process.
[0065] Generally, the higher the molecular weight of the ultra-high molecular weight polyethylene powder, the stronger the entanglement. This relationship is prominent in the molecular weight range where the intrinsic viscosity is below 12.0 dL / g. At 12.0 dL / g or above, the decrease in mobility begins to reach an upper limit, but a relationship between the intrinsic viscosity and the mobility index can be established. The ultra-high molecular weight polyethylene powder of this embodiment preferably satisfies the following (Formula III), more preferably the following (Formula III-A), and even more preferably the following (Formula III-B): [Mobility Index] > -0.2 x [Intrinsic Viscosity IV] + 62 (Formula III) [Mobility Index] > -0.2 x [Intrinsic Viscosity IV] + 65 (Formula III-A) [Mobility Index] > -0.2 x [Intrinsic Viscosity IV] + 69 (Formula III-B)
[0066] [Titanium and Aluminum Contents in Ultra-High Molecular Weight Polyethylene Powder] The titanium (Ti) content in the ultra-high molecular weight polyethylene powder of this embodiment is preferably 10 ppm or less, more preferably 0 ppm or more and 8 ppm or less, and even more preferably 0 ppm or more and 5 ppm or less. The aluminum (Al) content in the ultra-high molecular weight polyethylene powder of this embodiment is preferably 10 ppm or less, more preferably 0 ppm or more and 8 ppm or less, and even more preferably 0 ppm or more and 5 ppm or less.
[0067] In the ultra-high molecular weight polyethylene powder of the present embodiment, by adjusting the titanium and aluminum contents to fall within these ranges, the amount of metal eluted into a liquid can be reduced. For example, contamination of the filtrate in filter applications is suppressed, and the safety of medical fibers used in living organisms tends to be improved.
[0068] It is generally known that polyethylene degradation occurs when a large amount of metals derived from catalyst residues remains in the ultra-high molecular weight polyethylene powder. The Ti and Al contents in the ultra-high molecular weight polyethylene powder can be controlled by the productivity of ethylene homopolymer or ethylene-based polymer per unit catalyst. The productivity of ethylene homopolymer or ethylene-based polymer can be controlled by the polymerization temperature, polymerization pressure, and slurry concentration of the reactor during production. That is, methods for increasing the productivity of the ethylene homopolymer or ethylene-based polymer used in this embodiment are not particularly limited, but include, for example, increasing the polymerization temperature, increasing the polymerization pressure, and / or increasing the slurry concentration. Other methods for controlling the aluminum content include changing the catalyst composition during polymerization of the ethylene homopolymer or ethylene-based polymer, selecting the type of co-catalyst component, reducing the co-catalyst component concentration, or washing the ethylene homopolymer or ethylene-based polymer with an acid or alkali. In this embodiment, the Ti and Al contents can be measured by the method described in the Examples below.
[0069] [Average Particle Diameter D50] The average particle diameter D50 of the polyethylene powder of this embodiment measured with a laser particle size distribution analyzer is preferably 40 μm or more and 400 μm or less, more preferably 50 μm or more and 350 μm or less, and even more preferably 60 μm or more and 300 μm or less.
[0070] The polyethylene powder of this embodiment has an average particle diameter D50 of 40 μm or more, which makes it easier to handle and tends to reduce problems during the molding process. The average particle diameter D50 of 400 μm or less improves the solubility in a solvent (e.g., liquid paraffin), resulting in a gel with a more uniform distribution of molecular chains and a high degree of orientation, which tends to enable the production of high-strength fibers with excellent mechanical strength.
[0071] The method for controlling the average particle diameter D50 within the above range is not particularly limited, but for example, there is a method for appropriately adjusting the conditions in the polymerization system (polymerization temperature, ethylene pressure, etc.) Specifically, there is a method for increasing the polymerization temperature and / or polymerization pressure.
[0072] In this embodiment, D50 can be determined by the method described in the examples below.
[0073] [Catalyst] The catalyst used in the production of the polyethylene powder according to this embodiment is not particularly limited, and examples thereof include general Ziegler-Natta catalysts. The Ziegler-Natta catalyst is preferably a catalyst comprising a solid catalyst [A] and an organometallic compound component [B], wherein the solid catalyst [A] is an olefin polymerization catalyst produced by reacting an organomagnesium compound (hereinafter also referred to as "(A-1)") soluble in an inert hydrocarbon solvent and represented by the following formula 1 with a titanium compound (hereinafter also referred to as "(A-2)") represented by the following formula 2:
[0074] (A-1): (M 1 ) α (Mg) β (R 2 ) a (R 3 ) b (Y 1 ) c ...Formula 1 (wherein, M 1 is a metal atom belonging to the group consisting of Groups 12, 13, and 14 of the periodic table, and R 2 and R 3 is a hydrocarbon group having 2 to 20 carbon atoms, and Y 1 represents an alkoxy group, a siloxy group, an aryloxy group, an amino group, an amide group, -N=C-R 4 , R 5 , -SR 6 (where R 4 , R 5 and R 6 represents a hydrocarbon group having 1 to 20 carbon atoms. When c is 2, Y 1 may be different from each other), and a β-keto acid residue, and α, β, a, b, and c are real numbers that satisfy the following relationships: 0≦α, 0<β, 0≦a, 0≦b, 0≦c, 0<a+b, 0≦c / (α+β)≦2, nα+2β=a+b+c (where n is M 1 Represents the valence of
[0075] (A-2):Ti(OR 7 ) d X 1 (4-d) ...Equation 2 (where d is a real number between 0 and 4, and R 7 is a hydrocarbon group having 1 to 20 carbon atoms, and X 1 is a halogen atom.)
[0076] The inert hydrocarbon solvent used in the reaction of (A-1) and (A-2) is not particularly limited, but specific examples include aliphatic hydrocarbons such as pentane, hexane, and heptane; aromatic hydrocarbons such as benzene and toluene; and alicyclic hydrocarbons such as cyclohexane and methylcyclohexane.
[0077] First, (A-1) will be explained. (A-1) is shown in the form of an organomagnesium complex compound soluble in an inert hydrocarbon solvent, and includes all dihydrocarbylmagnesium compounds and complexes of these compounds with other metal compounds. The relational formula nα+2β=a+b+c between the symbols α, β, a, b, and c indicates the stoichiometry of the valence of the metal atom and the substituent.
[0078] In Formula 1, R 2 and R 3 The hydrocarbon group having 2 to 20 carbon atoms is not particularly limited, but specifically includes an alkyl group, a cycloalkyl group, or an aryl group, such as an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, an octyl group, a decyl group, a cyclohexyl group, and a phenyl group. Among these, an alkyl group is preferred. When α>0, the metal atom M 1 As the metal atom, a metal atom belonging to the group consisting of Groups 12, 13 and 14 of the periodic table can be used, such as zinc, boron, aluminum, etc. Among these, aluminum and zinc are preferred.
[0079] metal atom M 1 The ratio β / α of magnesium to R is not particularly limited, but is preferably 0.1 or more and 30 or less, and more preferably 0.5 or more and 10 or less. When a predetermined organomagnesium compound with α=0 is used, for example, R2 When R is 1-methylpropyl or the like, it is soluble in an inert hydrocarbon solvent, and such a compound also gives preferable results in this embodiment. 2 , R 3 It is recommended that the following satisfy one of the following three groups: (1), (2), and (3).
[0080] Group (1): R 2 , R 3 At least one of R is a secondary or tertiary alkyl group having 4 to 6 carbon atoms, preferably R 2 , R 3 and R are both alkyl groups having 4 to 6 carbon atoms, and at least one of them is a secondary or tertiary alkyl group. 2 and R 3 and are alkyl groups having different numbers of carbon atoms, preferably R 2 is an alkyl group having 2 or 3 carbon atoms, and R 3 is an alkyl group having 4 or more carbon atoms. 2 , R 3 At least one of R is a hydrocarbon group having 6 or more carbon atoms, and preferably R 2 , R 3 The alkyl group must have a total of 12 or more carbon atoms.
[0081] Specific examples of these groups are shown below. Specific examples of the secondary or tertiary alkyl group having 4 to 6 carbon atoms in group (1) include a 1-methylpropyl group, a 2-methylpropyl group, a 1,1-dimethylethyl group, a 2-methylbutyl group, a 2-ethylpropyl group, a 2,2-dimethylpropyl group, a 2-methylpentyl group, a 2-ethylbutyl group, a 2,2-dimethylbutyl group, and a 2-methyl-2-ethylpropyl group. Of these, a 1-methylpropyl group is particularly preferred.
[0082] Furthermore, in group (2), specific examples of alkyl groups having 2 or 3 carbon atoms include ethyl, 1-methylethyl, and propyl groups. Of these, the ethyl group is particularly preferred. Furthermore, the alkyl group having 4 or more carbon atoms is not particularly limited, but specific examples include butyl, pentyl, hexyl, heptyl, and octyl groups. Of these, the butyl and hexyl groups are particularly preferred.
[0083] Furthermore, the hydrocarbon group having 6 or more carbon atoms in group (3) is not particularly limited, but specific examples include a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a phenyl group, a 2-naphthyl group, etc. Among the hydrocarbon groups, an alkyl group is preferred, and among the alkyl groups, a hexyl group and an octyl group are particularly preferred.
[0084] Generally, as the number of carbon atoms contained in the alkyl group increases, the compound tends to be more soluble in an inert hydrocarbon solvent, but the viscosity of the solution tends to increase. Therefore, it is preferable to use an alkyl group with a moderate chain length for ease of handling. The organomagnesium compound can be used after being diluted with an inert hydrocarbon solvent, but it can also be used without any problems even if a trace amount of Lewis basic compounds such as ethers, esters, and amines is contained or remains in the solution.
[0085] Next, Y 1 In formula 1, Y 1 represents an alkoxy group, a siloxy group, an aryloxy group, an amino group, an amide group, -N=C-R 4 , R 5 , -SR 6 (where R 4 , R 5 and R 6 each independently represents a hydrocarbon group having from 2 to 20 carbon atoms, or a β-keto acid residue.
[0086] In Formula 1, R 4 , R 5 and R 6The hydrocarbon group represented by the formula (I) is preferably an alkyl group or aryl group having from 1 to 12 carbon atoms, and particularly preferably an alkyl group or aryl group having from 3 to 10 carbon atoms. Examples of the hydrocarbon group include, but are not limited to, a methyl group, an ethyl group, a propyl group, a 1-methylethyl group, a butyl group, a 1-methylpropyl group, a 1,1-dimethylethyl group, a pentyl group, a hexyl group, a 2-methylpentyl group, a 2-ethylbutyl group, a 2-ethylpentyl group, a 2-ethylhexyl group, a 2-ethyl-4-methylpentyl group, a 2-propylheptyl group, a 2-ethyl-5-methyloctyl group, an octyl group, a nonyl group, a decyl group, a phenyl group, and a naphthyl group. Of these, a butyl group, a 1-methylpropyl group, a 2-methylpentyl group, and a 2-ethylhexyl group are particularly preferred.
[0087] Also, in formula 1, Y 1 is preferably an alkoxy group or a siloxy group. The alkoxy group is not particularly limited, but specific examples include a methoxy group, an ethoxy group, a propoxy group, a 1-methylethoxy group, a butoxy group, a 1-methylpropoxy group, a 1,1-dimethylethoxy group, a pentoxy group, a hexoxy group, a 2-methylpentoxy group, a 2-ethylbutoxy group, a 2-ethylpentoxy group, a 2-ethylhexoxy group, a 2-ethyl-4-methylpentoxy group, a 2-propylheptoxy group, a 2-ethyl-5-methyloctoxy group, an octoxy group, a phenoxy group, and a naphthoxy group. Of these, a butoxy group, a 1-methylpropoxy group, a 2-methylpentoxy group, and a 2-ethylhexoxy group are more preferred. The siloxy group is not particularly limited, but specifically preferred examples include hydrodimethylsiloxy, ethylhydromethylsiloxy, diethylhydrosiloxy, trimethylsiloxy, ethyldimethylsiloxy, diethylmethylsiloxy, and triethylsiloxy groups. Of these, hydrodimethylsiloxy, ethylhydromethylsiloxy, diethylhydrosiloxy, and trimethylsiloxy groups are more preferred.
[0088] In this embodiment, the synthesis method of (A-1) is not particularly limited. For example, 2 MgX 1 , and formula R2 Mg(R 2 has the above meaning, and X 1 is a halogen atom; and an organomagnesium compound of the formula M 1 R 3 n and M 1 R 3 (n-1) H (M 1 , and R 3 has the same meaning as above, and n is M 1 ) in an inert hydrocarbon solvent at a temperature of 25°C to 150°C, and if necessary, subsequently reacting with an organometallic compound of formula Y 1 -H(Y 1 has the same meaning as above, or Y 1 Among these, the compound can be synthesized by reacting an organomagnesium compound and / or an organoaluminum compound having a functional group represented by the formula Y 1 When reacting a compound represented by —H with a compound represented by formula Y, the order of the reactions is not particularly limited. 1 -H, a method of adding a compound represented by formula Y 1 Either a method of adding the organomagnesium compound to the compound represented by --H or a method of adding both simultaneously can be used.
[0089] In this embodiment, Y relative to all metal atoms in (A-1) 1 The molar composition ratio c / (α+β) of Y to all metal atoms is 0≦c / (α+β)≦2, and preferably 0≦c / (α+β)<1. 1 When the molar composition ratio of (A-1) is 2 or less, the reactivity of (A-1) with (A-2) tends to be improved.
[0090] Next, (A-2) will be explained. (A-2) is a titanium compound represented by formula 2. (A-2): Ti(OR 7 ) d X 1 (4-d)...Equation 2 (where d is a real number between 0 and 4, and R 7 is a hydrocarbon group having 1 to 20 carbon atoms, and X 1 is a halogen atom.)
[0091] In the above formula 2, d is preferably 0 or more and 1 or less, and more preferably 0. 7 The hydrocarbon group represented by the formula (I) is not particularly limited, but specific examples include aliphatic hydrocarbon groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, 2-ethylhexyl, heptyl, octyl, decyl, and aryl groups; alicyclic hydrocarbon groups such as cyclohexyl, 2-methylcyclohexyl, and cyclopentyl groups; and aromatic hydrocarbon groups such as phenyl and naphthyl groups. Of these, aliphatic hydrocarbon groups are preferred. X 1 Examples of halogen atoms represented by the formula (I) include chlorine, bromine, and iodine. Among these, chlorine is preferred. In this embodiment, it is particularly preferred that (A-2) is titanium tetrachloride. In this embodiment, two or more compounds selected from the above can be used in combination.
[0092] Next, the reaction between (A-1) and (A-2) will be described. The reaction is preferably carried out in an inert hydrocarbon solvent, and more preferably in an aliphatic hydrocarbon solvent such as hexane or heptane. The molar ratio of (A-1) to (A-2) in the reaction is not particularly limited, but the molar ratio of Ti atoms contained in (A-2) to Mg atoms contained in (A-1) (Ti / Mg) is preferably 0.1 or more and 10 or less, and more preferably 0.3 or more and 3 or less. The reaction temperature is not particularly limited, but is preferably carried out in the range of -80°C or more and 150°C or less, and more preferably -40°C or more and 100°C or less. The order of addition of (A-1) and (A-2) is not particularly limited, and any of the following methods is possible: adding (A-1) followed by (A-2), adding (A-2) followed by (A-1), or adding (A-1) and (A-2) simultaneously. However, the method of adding (A-1) and (A-2) simultaneously is preferred. In this embodiment, the solid catalyst [A] obtained by the above reaction is used as a slurry solution using an inert hydrocarbon solvent.
[0093] Another example of the Ziegler-Natta catalyst used in the present embodiment is preferably an olefin polymerization catalyst comprising a solid catalyst [C] and an organometallic compound component [B], wherein the solid catalyst [C] is produced by supporting an organomagnesium compound soluble in an inert hydrocarbon solvent represented by formula 5 (hereinafter also referred to as "(C-4)") and a titanium compound represented by formula 6 (hereinafter also referred to as "(C-5)") on a carrier (hereinafter also referred to as "(C-3)") prepared by reacting an organomagnesium compound soluble in an inert hydrocarbon solvent represented by formula 3 (hereinafter also referred to as "(C-1)") with a chlorinating agent represented by formula 4 (hereinafter also referred to as "(C-2)").
[0094] (C-1): (M 2 ) γ (Mg) δ (R 8 ) e (R 9 ) f (OR 10 ) g ...Formula 3 (wherein, M 2is a metal atom belonging to the group consisting of Groups 12, 13, and 14 of the periodic table, and R 8 , R 9 and R 10 are hydrocarbon groups having 2 to 20 carbon atoms, and γ, δ, e, f, and g are real numbers that satisfy the following relationships: 0≦γ, 0<δ, 0≦e, 0≦f, 0≦g, 0<e+f, 0≦g / (γ+δ)≦2, kγ+2δ=e+f+g (where k is M 2 Represents the valence of
[0095] (C-2): H h SiCl i R 11 (4-(h+i)) ...Formula 4 (wherein, R 11 is a hydrocarbon group having 1 to 12 carbon atoms, and h and i are real numbers that satisfy the following relationship: 0<h, 0<i, 0<h+i≦4).
[0096] (C-4): (M 1 ) α (Mg) β (R 2 ) a (R 3 ) b Y 1 c ...Formula 5 (wherein, M 1 is a metal atom belonging to the group consisting of Groups 12, 13, and 14 of the periodic table, and R 2 and R 3 is a hydrocarbon group having 2 to 20 carbon atoms, and Y 1 is alkoxy, siloxy, aryloxy, amino, amido, -N=C-R 4 , R 5 , -SR 6 (where R 4 , R 5 and R 6 represents a hydrocarbon group having 1 to 20 carbon atoms. When c is 2, Y 1 may be different from each other), and a β-keto acid residue, and α, β, a, b, and c are real numbers that satisfy the following relationships: 0≦α, 0<β, 0≦a, 0≦b, 0≦c, 0<a+b, 0≦c / (α+β)≦2, nα+2β=a+b+c (where n is M 1 Represents the valence of
[0097] (C-5):Ti(OR 7 ) d X 1 (4-d) ...Equation 6 (where d is a real number between 0 and 4, and R 7 is a hydrocarbon group having 1 to 20 carbon atoms, and X 1 is a halogen atom.)
[0098] First, (C-1) will be explained. (C-1) is shown in the form of an organomagnesium complex compound soluble in an inert hydrocarbon solvent, but it encompasses all dihydrocarbylmagnesium compounds and complexes of these compounds with other metal compounds. The relationship kγ+2δ=e+f+g between the symbols γ, δ, e, f, and g in Formula 3 indicates the stoichiometry of the valence of the metal atom and the substituent.
[0099] In the above formula, R 8 Or R 9 The hydrocarbon group represented by is not particularly limited, but specifically, it is an alkyl group, a cycloalkyl group, or an aryl group, and examples thereof include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, an octyl group, a decyl group, a cyclohexyl group, and a phenyl group. Among these, R 8 and R 9 are each an alkyl group. When α>0, the metal atom M 2 As the metal atom, a metal atom belonging to the group consisting of Groups 12, 13 and 14 of the periodic table can be used, such as zinc, boron, aluminum, etc. Among these, aluminum and zinc are particularly preferred.
[0100] metal atom M 2 The ratio δ / γ of magnesium to R is not particularly limited, but is preferably 0.1 or more and 30 or less, and more preferably 0.5 or more and 10 or less. When a predetermined organomagnesium compound with γ=0 is used, for example, R 8 When R is 1-methylpropyl or the like, it is soluble in an inert hydrocarbon solvent, and such a compound also gives preferable results in this embodiment. 8 , R 9It is recommended that the be one of the following three groups: (1), (2), and (3).
[0101] Group (1): R 8 , R 9 At least one of R is a secondary or tertiary alkyl group having 4 to 6 carbon atoms, and preferably R 8 , R 9 and R each have 4 to 6 carbon atoms, and at least one of them is a secondary or tertiary alkyl group. 8 and R 9 and are alkyl groups having different carbon numbers, preferably R 8 is an alkyl group having 2 or 3 carbon atoms, and R 9 is an alkyl group having 4 or more carbon atoms. 8 , R 9 At least one of R is a hydrocarbon group having 6 or more carbon atoms, and preferably R 8 , R 9 The sum of the carbon atoms contained in the alkyl group is 12 or more.
[0102] Specific examples of these groups are shown below. Specific examples of the secondary or tertiary alkyl group having 4 to 6 carbon atoms in group (1) include a 1-methylpropyl group, a 2-methylpropyl group, a 1,1-dimethylethyl group, a 2-methylbutyl group, a 2-ethylpropyl group, a 2,2-dimethylpropyl group, a 2-methylpentyl group, a 2-ethylbutyl group, a 2,2-dimethylbutyl group, and a 2-methyl-2-ethylpropyl group. Of these, a 1-methylpropyl group is particularly preferred.
[0103] In addition, in group (2), examples of the alkyl group having 2 or 3 carbon atoms include ethyl, 1-methylethyl, and propyl groups. Of these, an ethyl group is particularly preferred. In addition, the alkyl group having 4 or more carbon atoms is not particularly limited, but specific examples include a butyl group, a pentyl group, a hexyl group, a heptyl group, and an octyl group. Of these, a butyl group and a hexyl group are particularly preferred.
[0104] Furthermore, the hydrocarbon group having 6 or more carbon atoms in group (3) is not particularly limited, but specific examples include a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a phenyl group, a 2-naphthyl group, etc. Among the hydrocarbon groups, an alkyl group is preferred, and among the alkyl groups, a hexyl group and an octyl group are particularly preferred.
[0105] Generally, as the number of carbon atoms contained in the alkyl group increases, the compound tends to be more soluble in an inert hydrocarbon solvent, and the viscosity of the solution tends to increase. Therefore, it is preferable to use an alkyl group with a moderate chain length for ease of handling. The organomagnesium compound is used as an inert hydrocarbon solution, but it can be used without any problems even if a trace amount of Lewis basic compounds such as ethers, esters, and amines is contained or remains in the solution.
[0106] Next, the alkoxy group (OR 10 ) will be explained. 10 The hydrocarbon group represented by R is preferably an alkyl group or aryl group having 1 to 12 carbon atoms, and particularly preferably an alkyl group or aryl group having 3 to 10 carbon atoms. 10 Although not particularly limited, specific examples include a methyl group, an ethyl group, a propyl group, a 1-methylethyl group, a butyl group, a 1-methylpropyl group, a 1,1-dimethylethyl group, a pentyl group, a hexyl group, a 2-methylpentyl group, a 2-ethylbutyl group, a 2-ethylpentyl group, a 2-ethylhexyl group, a 2-ethyl-4-methylpentyl group, a 2-propylheptyl group, a 2-ethyl-5-methyloctyl group, an octyl group, a nonyl group, a decyl group, a phenyl group, a naphthyl group, etc. Among these, a butyl group, a 1-methylpropyl group, a 2-methylpentyl group, and a 2-ethylhexyl group are particularly preferred.
[0107] In this embodiment, the synthesis method of (C-1) is not particularly limited, but a compound represented by the formula R 8 MgX 1 and formula R 8 Mg(R 8 has the above meaning, and X 1 is a halogen atom; and an organomagnesium compound of the formula M 2 R9 k and formula M 2 R 9 (k-1) H (M 2 , R 9 and k has the same meaning as above) in an inert hydrocarbon solvent at a temperature of 25° C. to 150° C., and if necessary, subsequently reacting with an organometallic compound belonging to the group consisting of R 9 (R 9 has the same meaning as above.) R soluble in an alcohol or an inert hydrocarbon solvent having a hydrocarbon group represented by 9 A method of reacting the compound with an alkoxy magnesium compound and / or an alkoxy aluminum compound having a hydrocarbon group represented by the following formula is preferred.
[0108] Among these, when an organomagnesium compound soluble in an inert hydrocarbon solvent is reacted with an alcohol, the order of the reaction is not particularly limited, and any of a method of adding the alcohol to the organomagnesium compound, a method of adding the organomagnesium compound to the alcohol, or a method of adding both simultaneously can be used. In this embodiment, the reaction ratio of the organomagnesium compound soluble in an inert hydrocarbon solvent and the alcohol is not particularly limited, but it is preferable that the molar composition ratio g / (γ+δ) of alkoxy groups to all metal atoms in the alkoxy group-containing organomagnesium compound obtained as a result of the reaction is 0≦g / (γ+δ)≦2, and 0≦g / (γ+δ)<1.
[0109] Next, (C-2) will be explained. (C-2) is a silicon chloride compound represented by formula 4, which has at least one Si—H bond. (C-2): H h SiCl i R 11 (4-(h+i)) ...Formula 4 (wherein, R 11 is a hydrocarbon group having 1 to 12 carbon atoms, and h and i are real numbers that satisfy the following relationship: 0<h, 0<i, 0<h+i≦4).
[0110] In Formula 4, R 11The hydrocarbon group represented by the formula (I) is not particularly limited, but specific examples include aliphatic hydrocarbon groups, alicyclic hydrocarbon groups, and aromatic hydrocarbon groups, such as methyl, ethyl, propyl, 1-methylethyl, butyl, pentyl, hexyl, octyl, decyl, cyclohexyl, and phenyl groups. Among these, alkyl groups having 1 to 10 carbon atoms are preferred, and alkyl groups having 1 to 3 carbon atoms, such as methyl, ethyl, propyl, and 1-methylethyl, are more preferred. Furthermore, h and i are numbers greater than 0 that satisfy the relationship h+i≦4, and it is preferred that i be 2 to 3.
[0111] These compounds are not particularly limited, but specific examples include HSiCl 3 , HSiCl 2 CH 3 , HSiCl 2 C 2 H 5 , HSiCl 2 (C 3 H 7 ), HSiCl 2 (2-C 3 H 7 ), HSiCl 2 (C 4 H 9 ), HSiCl 2 (C 6 H 5 ), HSiCl 2 (4-Cl-C 6 H 4 ), HSiCl 2 (CH=CH 2 ), HSiCl 2 (CH 2 C 6 H 5 ), HSiCl 2 (1-C 10 H 7 ), HSiCl 2 (CH 2 CH=CH 2 ), H 2 SiCl(CH 3 ), H 2 SiCl(C 2 H 5 ), HSiCl(CH 3 )2 , HSiCl(C 2 H 5 ) 2 , HSiCl(CH 3 ) (2-C 3 H 7 ), HSiCl(CH 3 ) (C 6 H 5 ), HSiCl(C 6 H 5 ) 2 Silicon chloride compounds consisting of these compounds or mixtures of two or more selected from these compounds are used. Among these, HSiCl 3 , HSiCl 2 CH 3 , HSiCl(CH 3 ) 2 , HSiCl 2 (C 3 H 7 ) is preferred, and HSiCl 3 , HSiCl 2 CH 3 is more preferred.
[0112] Next, the reaction between (C-1) and (C-2) will be described. During the reaction, it is preferable to dilute (C-2) in advance with an inert hydrocarbon solvent, a chlorinated hydrocarbon such as 1,2-dichloroethane, o-dichlorobenzene, or dichloromethane; an ether-based medium such as diethyl ether or tetrahydrofuran; or a mixture thereof. Among these, an inert hydrocarbon solvent is more preferable in terms of catalyst performance. The reaction ratio between (C-1) and (C-2) is not particularly limited, but the ratio of silicon atoms contained in (C-2) to 1 mol of magnesium atoms contained in (C-1) is preferably 0.01 mol or more and 100 mol or less, and more preferably 0.1 mol or more and 10 mol or less.
[0113] The method for reacting (C-1) and (C-2) is not particularly limited, and any of the following methods can be used: a simultaneous addition method in which (C-1) and (C-2) are simultaneously introduced into a reactor and reacted; a method in which (C-2) is previously charged into a reactor and then (C-1) is introduced into the reactor; or a method in which (C-1) is previously charged into a reactor and then (C-2) is introduced into the reactor. Among these, the method in which (C-2) is previously charged into a reactor and then (C-1) is introduced into the reactor is preferred. The support (C-3) obtained by the above reaction is preferably separated by filtration or decantation, and then thoroughly washed with an inert hydrocarbon solvent to remove unreacted materials, by-products, etc.
[0114] The reaction temperature between (C-1) and (C-2) is not particularly limited, but is preferably 25°C or higher and 150°C or lower, more preferably 30°C or higher and 120°C or lower, and even more preferably 40°C or higher and 100°C or lower. In a simultaneous addition method in which (C-1) and (C-2) are simultaneously introduced into a reactor and reacted, it is preferable to adjust the temperature of the reactor to a predetermined temperature in advance, and then adjust the temperature inside the reactor to a predetermined temperature while performing the simultaneous addition, thereby adjusting the reaction temperature to a predetermined temperature. In a method in which (C-2) is previously charged into a reactor and then (C-1) is introduced into the reactor, it is preferable to adjust the temperature of a reactor charged with the silicon chloride compound to a predetermined temperature, and then adjust the temperature inside the reactor to a predetermined temperature while introducing the organomagnesium compound into the reactor, thereby adjusting the reaction temperature to a predetermined temperature. In the method in which (C-1) is charged into a reactor in advance and then (C-2) is introduced into the reactor, it is preferable to adjust the temperature of the reactor into which (C-1) has been charged to a predetermined temperature, and then adjust the temperature inside the reactor to a predetermined temperature while introducing (C-2) into the reactor, thereby adjusting the reaction temperature to a predetermined temperature.
[0115] Next, the organomagnesium compound (C-4) will be explained. As (C-4), the compound represented by the above-mentioned formula 5 (C-4) is preferred.
[0116] (C-4): (M 1 ) α (Mg) β (R 2) a (R 3 ) b Y 1 c ...Formula 5 (wherein, M 1 is a metal atom belonging to the group consisting of Groups 12, 13, and 14 of the periodic table, and R 2 and R 3 is a hydrocarbon group having 2 to 20 carbon atoms, and Y 1 is alkoxy, siloxy, aryloxy, amino, amido, -N=C-R 4 , R 5 , -SR 6 (where R 4 , R 5 and R 6 represents a hydrocarbon group having 1 to 20 carbon atoms. When c is 2, Y 1 may be different from each other), and a β-keto acid residue, and α, β, a, b, and c are real numbers that satisfy the following relationships: 0≦α, 0<β, 0≦a, 0≦b, 0<a+b, 0≦c / (α+β)≦2, nα+2β=a+b+c (where n is M 1 Represents the valence of
[0117] The amount of (C-4) used is preferably 0.1 or more and 10 or less, more preferably 0.5 or more and 5 or less, in terms of the molar ratio of magnesium atoms contained in (C-4) to titanium atoms contained in (C-5).
[0118] The temperature for the reaction of (C-4) and (C-5) is not particularly limited, but is in the range of -80°C or higher and 150°C or lower, preferably -40°C or higher and 100°C or lower, and more preferably -40°C or higher and 10°C or lower.
[0119] The concentration of (C-4) when used is not particularly limited, but is preferably 0.1 mol / L or more and 2 mol / L or less, and more preferably 0.5 mol / L or more and 1.5 mol / L or less, based on the titanium atoms contained in (C-4). Note that an inert hydrocarbon solvent is preferably used to dilute (C-4).
[0120] The order of addition of (C-4) and (C-5) to (C-3) is not particularly limited, and any of the following methods is possible: adding (C-4) followed by (C-5), adding (C-4) followed by (C-5), or adding (C-4) and (C-5) simultaneously. Among these, from the viewpoint of reducing entanglement, a simultaneous addition method is preferred in which (C-3) is previously charged into a reactor, and then (C-4) and (C-5) are simultaneously introduced into the reactor and reacted. It is preferable to use a mixture of dialkyl magnesium and triethyl aluminum for (C-4). The mixing ratio of (C-4) is preferably a molar ratio (Mg / Al) relative to aluminum of 1 or more and 100 or less, more preferably 4 or more and 10 or less. The dispersibility of the organic magnesium is improved by mixing organic aluminum.
[0121] The reason why the molecular mobility index can be controlled by adding (C-4) and (C-5) simultaneously is that the precipitation of the fine particle catalyst occurs not on the surface of the carrier but in the inert hydrocarbon solvent, and each fine particle catalyst is independently supported on the surface of the carrier, thereby suppressing the aggregation of active sites.
[0122] Furthermore, it is believed that the use of dialkyl magnesium in (C-4) makes the reaction more vigorous, resulting in a more fine particle catalyst. A method in which (C-4) and (C-5) are added simultaneously is preferred. The reaction temperature of (C-4) and (C-5) is preferably between -40°C and 10°C. Within the above temperature range, the generation of by-products is suppressed and uniformity is maintained during the generation of the fine particle catalyst, even during a vigorous reaction.
[0123] The reaction of (C-4) with (C-5) is carried out in an inert hydrocarbon solvent, preferably an aliphatic hydrocarbon solvent such as hexane, heptane, etc. The catalyst thus obtained is used as a slurry solution using an inert hydrocarbon solvent.
[0124] Next, (C-5) will be described. In this embodiment, (C-5) is a titanium compound represented by the above formula 6. (C-5): Ti(OR 7 ) d X 1 (4-d) ...Equation 6 (where d is a real number between 0 and 4, and R 7is a hydrocarbon group having 1 to 20 carbon atoms, and X 1 is a halogen atom.)
[0125] In Formula 6, R 7 The hydrocarbon group represented by the formula (I) is not particularly limited, but specific examples include aliphatic hydrocarbon groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, 2-ethylhexyl, heptyl, octyl, decyl, and aryl groups; alicyclic hydrocarbon groups such as cyclohexyl, 2-methylcyclohexyl, and cyclopentyl groups; and aromatic hydrocarbon groups such as phenyl and naphthyl groups. Of these, aliphatic hydrocarbon groups are preferred. X 1 The halogen atom represented by the formula (C-5) is not particularly limited, but specific examples include chlorine, bromine, and iodine. Among these, chlorine is preferable. The (C-5) selected from the above may be used alone or in combination of two or more.
[0126] The amount of titanium compound (C-5) used is not particularly limited, but from the viewpoint of increasing the distance between active sites, the molar ratio of titanium to magnesium atoms (Ti / Mg) contained in the support (C-3) is preferably 1 / 4 or less, more preferably 1 / 8 or less, more preferably 1 / 16 or less, and even more preferably 1 / 32 or less. It is preferable for the molar ratio of titanium to magnesium atoms (Ti / Mg) contained in the support to be below the upper limit, because this reduces the active site density on the catalyst surface, reduces the number of active sites that form an aggregate structure, and reduces entanglement at the initial stage of polymerization. On the other hand, a ratio of 1 / 64 or more is preferable in terms of catalyst activity.
[0127] The reaction temperature of (C-5) is not particularly limited, but is preferably −80° C. or higher and 150° C. or lower, more preferably −40° C. or higher and 100° C. or lower, and even more preferably −20° C. or higher and 60° C. or lower.
[0128] In the present embodiment, the method for supporting (C-5) on (C-3) is not particularly limited. A method of reacting (C-3) with an excess of (C-5) or a method of efficiently supporting (C-5) by using a third component may be used, but a method of supporting (C-5) by reacting (C-5) with an organomagnesium compound (C-4) is preferred.
[0129] [Treatment of Solid Catalyst Surface] Another preferred example of the Ziegler-Natta catalyst used in this embodiment is an olefin polymerization catalyst which comprises a solid catalyst [C] and an organometallic compound component [B], and is produced by treating the surface of the solid catalyst by reacting (hereinafter also referred to as "surface treatment") the solid catalyst [C] with an organoaluminum compound (C-6) represented by formula 7, which is soluble in an inert hydrocarbon solvent. (C-6): AlR 12 j Z 1 (3-j) ...Formula 7 (wherein, R 12 is a hydrocarbon group having 1 to 20 carbon atoms; Z 1 is a group belonging to the group consisting of a hydrogen atom, a halogen atom, an alkoxy group, an aryloxy group, and a siloxy group, and j is a number of 2 or more and 3 or less.
[0130] In the above formula 7, R 12The hydrocarbon group having 1 to 20 carbon atoms represented by the formula (I) is not particularly limited, but specifically includes aliphatic hydrocarbons, aromatic hydrocarbons, and alicyclic hydrocarbons. Preferred examples include trialkylaluminums such as trimethylaluminum, triethylaluminum, tripropylaluminum, tributylaluminum, tri(2-methylpropyl)aluminum (or triisobutylaluminum), tripentylaluminum, tri(3-methylbutyl)aluminum, trihexylaluminum, trioctylaluminum, and tridecylaluminum; aluminum halide compounds such as diethylaluminum chloride, ethylaluminum dichloride, bis(2-methylpropyl)aluminum chloride, ethylaluminum sesquichloride, and diethylaluminum bromide; alkoxyaluminum compounds such as diethylaluminum ethoxide and bis(2-methylpropyl)aluminum butoxide; siloxyaluminum compounds such as dimethylhydrosiloxyaluminum dimethyl, ethylmethylhydrosiloxyaluminum diethyl, and ethyldimethylsiloxyaluminum diethyl; and mixtures thereof. Of these, trialkylaluminum compounds, diethylaluminum chloride, ethylaluminum dichloride, and ethylaluminum sesquichloride are particularly preferred.
[0131] The amount of (C-6) used is preferably 0.1 or more and 10 or less, more preferably 0.5 or more and 5 or less, in terms of the molar ratio of aluminum atoms contained in (C-6) to titanium atoms contained in the solid catalyst [C].
[0132] The temperature for the reaction of (C-6) with the solid catalyst [C] is not particularly limited, but is in the range of -80°C or higher and 150°C or lower, preferably -40°C or higher and 100°C or lower, and more preferably 0°C or higher and 60°C or lower.
[0133] The concentration of (C-6) when used is not particularly limited, but is preferably 0.1 mol / L or more and 2 mol / L or less, and more preferably 0.5 mol / L or more and 1.5 mol / L or less, based on the aluminum atoms contained in (C-6). Note that it is preferable to use an inert hydrocarbon solvent to dilute (C-6).
[0134] There are no particular limitations on the method for adding (C-6) to the solid catalyst [C], but from the viewpoint of workability, it is preferable to charge the solid catalyst [C] in advance into a reactor and then add (C-6).
[0135] By treating the solid catalyst [C] with an organoaluminum compound, it reacts with the titanium compound supported on the catalyst surface, and not only acts as a reduction reaction to change the valence, but also liberates excess titanium compound.
[0136] From the viewpoint of controlling entanglement, it is preferable to treat the surface with an organoaluminum compound (C-6), since this reduces the density of active sites on the catalyst surface and makes it possible to increase the distance between active sites.
[0137] In this embodiment, it is preferable to perform washing (decantation) after catalyst synthesis four or more times. By performing decantation four or more times, unreacted raw materials tend to be reduced, and scale during polymerization tends to be reduced.
[0138] [Co-catalyst] Next, the organometallic compound component [B] used in this embodiment will be described. The solid catalyst [A] or solid catalyst [C] used in this embodiment becomes a highly active polymerization catalyst when combined with the organometallic compound component [B]. The organometallic compound component [B] is sometimes called a "co-catalyst." The organometallic compound component [B] is preferably a compound containing a metal belonging to the group consisting of Groups 1, 2, 12, and 13 of the periodic table, and is particularly preferably an organoaluminum compound and / or an organomagnesium compound.
[0139] As the organoaluminum compound, it is preferable to use a compound represented by the following formula 7 alone or in combination: AlR 12 j Z 1 (3-j) ...Formula 7 (wherein, R 12 is a hydrocarbon group having 1 to 20 carbon atoms; Z 1 is a group belonging to the group consisting of a hydrogen atom, a halogen atom, an alkoxy group, an aryloxy group, and a siloxy group, and j is a number of 2 or more and 3 or less.
[0140] In the above formula 7, R 12 The hydrocarbon group having 1 to 20 carbon atoms represented by the formula (I) is not particularly limited, but specifically includes aliphatic hydrocarbons, aromatic hydrocarbons, and alicyclic hydrocarbons, and a trialkylaluminum compound is particularly preferred.
[0141] As the organomagnesium compound, an organomagnesium compound soluble in an inert hydrocarbon solvent represented by the above formula 3 is preferred. (M 2 ) γ (Mg) δ (R 8 ) e (R 9 ) f (OR 10 ) g ...Formula 3 (wherein, M 2 is a metal atom belonging to the group consisting of Groups 12, 13, and 14 of the periodic table, and R 8 , R 9 and R 10 are hydrocarbon groups having 2 to 20 carbon atoms, and γ, δ, e, f, and g are real numbers that satisfy the following relationships: 0≦γ, 0<δ, 0≦e, 0≦f, 0≦g, 0<e+f, 0≦g / (γ+δ)≦2, kγ+2δ=e+f+g (where k is M 2 Represents the valence of
[0142] The organomagnesium compound is shown in the form of an organomagnesium complex compound soluble in an inert hydrocarbon solvent, but it also includes dialkylmagnesium compounds and complexes of these compounds with other metal compounds. 2 , R 8 , R 9 , OR 10 As already mentioned, it is preferable that the organomagnesium compound has high solubility in an inert hydrocarbon solvent, and therefore, δ / γ is preferably in the range of 0.5 to 10. 2 More preferred are compounds in which is aluminum.
[0143] From the viewpoint of apparently widening the distance between active sites involved in polymerization, it is preferable to use, as the bulky organometallic compound component [B], an organoaluminum compound represented by the following formula 8, either alone or in combination: AlR 12 j R 13 k Z 1 (3-(j+k)) ...Formula 8 (wherein, R 12 is a hydrocarbon group having 1 to 20 carbon atoms, R 13 is a bulky hydrocarbon group, and Z 1 is a group belonging to the group consisting of a hydrogen atom, a halogen atom, an alkoxy group, an aryloxy group, and a siloxy group, and j and k are real numbers that satisfy the following relationship: 0<j, 0<k, 0<j+k≦3).
[0144] In the above formula 8, R 13 The bulky hydrocarbon group represented by the formula (I) is not particularly limited, but specifically includes 2,6-di-tertbutylphenoxy, 2,6-di-tertbutyl-4-methylphenoxy, 2,6-di-tertbutyl-4-ethylphenoxy, 2,4,6-tri-tertbutylphenoxy, 2,6-diisopropylphenoxy, 2,6-di-sec-butylphenoxy, 2,6-dicyclohexylphenoxy, and 2,6-diphenylphenoxy groups. The steric hindrance of the bulky cocatalyst increases the distance between activated active sites. (2,6-di-tertbutyl-4-methylphenoxy)diethylaluminum is particularly preferred as a bulky cocatalyst.
[0145] Alternatively, it is also preferred to mix the organoaluminum compound of formula 7 with dibutylhydroxytoluene (BHT) dissolved in an inert hydrocarbon solvent in a molar ratio to aluminum (BHT / Al) of 0.9 to 1.9.
[0146] The combination ratio of the solid catalyst [A] or the solid catalyst [C] and the organometallic compound component [B] is not particularly limited, but it is preferable that the organometallic compound component [B] is 1 mmol or more and 3,000 mmol or less per 1 g of the solid catalyst [A] or the solid catalyst [C].
[0147] The method for adding the organometallic compound component [B] to the polymerization system under polymerization conditions is not particularly limited, and the organometallic compound component [B] may be added to the polymerization system separately from the catalyst component, or may be reacted with the catalyst component in advance and then added to the polymerization system.
[0148] The concentration of the organometallic compound component [B] in the polymerization system is not particularly limited, but from the viewpoint of completely capturing impurities and the amount of residual metal in the polymer, it is preferably from 0.001 mmol / L to 10 mmol / L, more preferably from 0.01 mmol / L to 5 mmol / L, and even more preferably from 0.05 mmol / L to 2 mmol / L.
[0149] On the other hand, in order to obtain the ultra-high molecular weight polyethylene powder of this embodiment, it is preferable that the molecular chain has a structure that is easy to slide, and a method of polymerizing an unbranched linear polymer is exemplified. Specifically, it is preferable to use a mixture of two or more types of organometallic compound component [B].
[0150] [Method for Polymerizing Ultra-High Molecular Weight Polyethylene Powder] The polymerization method for producing the ultra-high molecular weight polyethylene powder of the present embodiment is not limited to the following, but examples thereof include a slurry polymerization method, a gas phase polymerization method, a solution polymerization method, etc. Among these, the slurry polymerization method is preferred because it can efficiently remove the heat of polymerization.
[0151] In the slurry polymerization method, an inert hydrocarbon medium can be used as the medium, and further, olefin itself can also be used as the medium.The inert hydrocarbon medium is not limited to the following, but examples thereof include aliphatic hydrocarbons such as propane, butane, isobutane, pentane, isopentane, hexane, heptane, octane, decane, dodecane, kerosene, etc.; alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclopentane, etc.; aromatic hydrocarbons such as benzene, toluene, xylene, etc.; halogenated hydrocarbons such as ethyl chloride, chlorobenzene, dichloromethane, etc.; and mixtures thereof.
[0152] The polymerization reaction in the method for producing polyethylene powder of this embodiment can be carried out in any of a batch system, a semi-continuous system, and a continuous system.
[0153] It is also possible to carry out the polymerization in two or more stages with different reaction conditions.
[0154] In the method for producing a polyethylene powder of the present embodiment, the polymerization temperature range of the ethylene polymer is preferably 30°C or higher and 100°C or lower, more preferably 35°C or higher and 95°C or lower, and even more preferably 40°C or higher and 90°C or lower.
[0155] A polymerization temperature of 30° C. or higher enables industrially efficient production, while a polymerization temperature of 100° C. or lower can suppress the formation of massive scale caused by partial melting of the polymer, enabling continuous and stable production without clogging of pipes.
[0156] In the method for producing a polyethylene powder of the present embodiment, the polymerization pressure for the ethylene polymer is preferably in the range of normal pressure or more and 2 MPaG or less, more preferably 0.2 MPaG or more and 1.5 MPaG or less, and even more preferably 0.3 MPaG or more and 0.9 MPaG or less.
[0157] A polymerization pressure of atmospheric pressure or higher enables industrially efficient production, while a polymerization pressure of 2 MPaG or lower tends to enable stable production without generating massive scale due to rapid polymerization in the polymerization reactor.
[0158] The molecular weight of the ethylene polymer can be adjusted by making hydrogen present in the polymerization system or by changing the polymerization temperature, as described in German Patent Application Publication No. 3127133.
[0159] By adding hydrogen as a chain transfer agent to the polymerization system, the molecular weight can be controlled within an appropriate range. When hydrogen is added to the polymerization system, the molar fraction of hydrogen is preferably in the range of 0 mol% to 30 mol%, more preferably 0 mol% to 25 mol%.
[0160] Alternatively, hydrogen can be brought into contact with the catalyst beforehand and then added to the polymerization system through the catalyst introduction line. Immediately after the catalyst is introduced into the polymerization system, the catalyst concentration near the outlet of the introduction line becomes high, which causes rapid polymerization and increases the possibility of localized high temperature conditions. On the other hand, by bringing hydrogen into contact with the catalyst before being introduced into the polymerization system, the initial activity of the catalyst can be suppressed, and the generation of clumped scale due to rapid polymerization and the deactivation of the catalyst at high temperatures can be suppressed.
[0161] In general, when polymerizing an ethylene polymer, an antistatic agent such as Stadis or STATSAFE manufactured by Innospec (distributor: Maruwa Bussan) can be used to suppress static adhesion of the polymer to a polymerization reactor.
[0162] Antistatic agents such as Stadis and STATSAFE can also be diluted in an inert hydrocarbon medium and added to a polymerization reactor by a pump, etc. In this case, the amount added is preferably 1 ppm or more and 500 ppm or less, more preferably 10 ppm or more and 100 ppm or less, relative to the amount of ethylene polymer produced per unit time, by adding the antistatic agent to a solid catalyst in advance or by adding the antistatic agent to a polymerization reactor.
[0163] In this embodiment, in addition to the components described above, other components (additives, etc.) that are useful for producing (polymerizing) polyethylene can be used.
[0164] The solvent separation method in the polymerization step of the polyethylene powder of this embodiment can be any of decantation, centrifugation, filter filtration, etc., but filter filtration is preferred because it allows for easy separation of the ethylene polymer and the solvent.
[0165] The method for deactivating the catalyst used in the polymerization step of the ethylene polymer constituting the polyethylene powder of the present embodiment is not particularly limited, but the catalyst is preferably deactivated after separating the ethylene polymer from the solvent.
[0166] By introducing an agent for deactivating the catalyst after separating the polyethylene powder from the solvent, it is possible to suppress the precipitation of low-molecular-weight components, catalyst components, and the like contained in the solvent in the ethylene-based polymer.
[0167] The agent for deactivating the catalyst is not particularly limited, but examples thereof include oxygen, water, alcohols, glycols, phenols, carbon monoxide, carbon dioxide, ethers, carbonyl compounds, and alkynes.
[0168] In the method for producing a polyethylene powder according to the present embodiment, a drying step is preferably carried out after separating the ethylene polymer from the solvent. In the drying step, a rotary kiln method, a paddle method, a fluidized bed dryer, or the like is preferably used. The drying temperature is preferably 30° C. or higher and 150° C. or lower.
[0169] It is also effective to introduce an inert gas such as nitrogen into the dryer to accelerate drying. In this case, it is even more effective to use steam or the like as a catalyst deactivator.
[0170] After drying the ethylene polymer constituting the polyethylene powder of the present embodiment, it may be sieved to remove coarse particles.
[0171] The polyethylene powder of the present embodiment may be a mixture of multiple polyethylene powders containing ethylene polymers obtained by the above-mentioned production method.
[0172] If necessary, the ink may be used in combination with known additives such as slip agents, neutralizing agents, antioxidants, light stabilizers, antistatic agents, and pigments.
[0173] The slip agent or neutralizing agent is not particularly limited, but examples thereof include aliphatic hydrocarbons, higher fatty acids, higher fatty acid metal salts, fatty acid esters of alcohols, waxes, higher fatty acid amides, silicone oils, rosins, etc. Specific examples of suitable additives include stearates such as calcium stearate, magnesium stearate, and zinc stearate. The content of the slip agent or neutralizing agent is not particularly limited, but is preferably 5000 ppm or less, 4000 ppm or less, or 3000 ppm or less.
[0174] The antioxidant is not particularly limited, but for example, a phenol-based compound or a phenol-phosphate-based compound is preferable. Specific examples include phenolic antioxidants such as 2,6-di-t-butyl-4-methylphenol (dibutylhydroxytoluene), n-octadecyl-3-(4-hydroxy-3,5-di-t-butylphenyl)propionate, and tetrakis(methylene(3,5-di-t-butyl-4-hydroxyhydrocinnamate))methane; phenolic phosphorus antioxidants such as 6-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenzo[d,f][1,3,2]dioxaphosphepine; and phosphorus antioxidants such as tetrakis(2,4-di-t-butylphenyl)-4,4'-biphenylene-diphosphonite, tris(2,4-di-t-butylphenyl)phosphite, and cyclic neopentanetetraylbis(2,4-t-butylphenylphosphite). The content of the antioxidant is not particularly limited, but is 5% or less, preferably 3% or less, and more preferably 1% or less. When the content of the antioxidant is 5% or less, deterioration of polyethylene is suppressed, and embrittlement, discoloration, deterioration of mechanical properties, etc. are less likely to occur, resulting in superior long-term stability.
[0175] The light resistance stabilizer is not particularly limited, but examples thereof include benzotriazole-based light resistance stabilizers such as 2-(5-methyl-2-hydroxyphenyl)benzotriazole and 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole; and hindered amine-based light resistance stabilizers such as bis(2,2,6,6-tetramethyl-4-piperidine)sebacate and poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}]. The content of the light resistance stabilizer is not particularly limited, but is 5,000 ppm or less, preferably 3,000 ppm or less, and more preferably 2,000 ppm or less.
[0176] The antistatic agent is not particularly limited, but examples thereof include aluminosilicate, kaolin, clay, natural silica, synthetic silica, silicates, talc, diatomaceous earth, and glycerin fatty acid esters.
[0177] [Uses] The ultra-high molecular weight polyethylene powder of this embodiment can be used as a raw material for various molded articles such as microporous films, fibers, particularly high-strength fibers, sintered bodies, press-molded bodies, and ram-pressed bodies.
[0178] The polyethylene powder of this embodiment is particularly suitable as a raw material for high-strength fibers.
[0179] [Molded Product] The molded product of this embodiment is a molded product of the ultra-high molecular weight polyethylene powder of this embodiment described above.
[0180] The method for producing the molded body is not particularly limited, but examples thereof include a molding method that uses a wet extrusion method and involves steps of extruding a resin, stretching, extracting, and drying.
[0181] The method for producing fibers (e.g., high-strength fibers) is not particularly limited, but examples thereof include a method in which liquid paraffin and the above-mentioned ultra-high molecular weight polyethylene powder are kneaded and spun, followed by heating and drawing. Specific examples thereof include, but are not particularly limited to, a production method under the following general swelling conditions:
[0182] Ultra-high molecular weight polyethylene powder, liquid paraffin, and, if necessary, additives such as antioxidants are blended and stirred at a temperature at least 30°C lower than the melting point (Tm2) of the ultra-high molecular weight polyethylene powder to prepare a slurry liquid. Next, the slurry liquid is charged into a kneader and kneaded at a constant temperature. After that, the mixture is passed through a spinneret attached to the tip of the extruder and spun. Next, the discharged yarn containing liquid paraffin is wound at a location away from the spinneret. Next, to remove the liquid paraffin from the wound yarn, the yarn is immersed in hexane for extraction, and then dried.
[0183] The obtained yarn is first drawn in a thermostatic bath, and then secondly drawn in the thermostatic bath until the yarn breaks, thereby obtaining a high-strength fiber (drawn yarn).
[0184] [High-Strength Fiber] Specific examples of the method for producing high-strength fiber include a production method including a slurry process, a gelling process, an optional kneading process, an optional extrusion preparation process, an extrusion process, an optional quenching process, an extraction process, and a raw yarn drawing process.
[0185] (Slurry Step) The slurry step is a step of mixing the ultra-high molecular weight polyethylene powder and first liquid paraffin, and stirring the mixture at a temperature equal to or lower than the melting point of the ultra-high molecular weight polyethylene powder to obtain a slurry.
[0186] The stirring temperature is preferably 25°C or higher and 120°C or lower, more preferably 50°C or higher and 115°C or lower, even more preferably 80°C or higher and 110°C or lower, and particularly preferably 90°C or higher and 105°C or lower. By setting the stirring temperature to 25°C or higher, the liquid paraffin can be efficiently impregnated into the pores of the ultra-high molecular weight polyethylene powder. Furthermore, by setting the temperature to 120°C or lower, melting of the surface of the ultra-high molecular weight polyethylene powder is suppressed and fusion of the powder particles is prevented, thereby obtaining a uniform gel in which molecular chain entanglements are untangled.
[0187] (Gelling step) The gelling step is a step of mixing the slurry with a second liquid paraffin at a temperature of 150°C or higher and 300°C or lower to obtain a gel for raw yarn at a temperature of 140°C or higher and 200°C or lower. By setting the temperature of the gel for raw yarn at 140°C or higher, a uniform gel in which entanglements of molecular chains are disentangled can be obtained in a short time. Furthermore, by setting the temperature at 200°C or lower, a significant decrease in molecular weight due to thermal decomposition can be suppressed.
[0188] The temperature of the second liquid paraffin is preferably 150°C or higher and 250°C or lower, more preferably 150°C or higher and 200°C or lower, and even more preferably 150°C or higher and 180°C or lower.
[0189] The temperature of the yarn gel is preferably 140°C or higher and 190°C or lower, more preferably 140°C or higher and 180°C or lower, and even more preferably 140°C or higher and 170°C or lower.
[0190] The polyethylene concentration of the yarn gel is preferably 3% by mass or more and 20% by mass or less, more preferably 3% by mass or more and 15% by mass or less, even more preferably 3% by mass or more and 10% by mass or less, and particularly preferably 3% by mass or more and 8% by mass or less. By making the polyethylene concentration of the yarn gel 3% by mass or more, yarn with little unevenness in yarn diameter can be stably spun. Furthermore, by making it 20% by mass or less, yarn with untangled molecular chains can be obtained.
[0191] (Kneading Step) The kneading step is a step of kneading the yarn gel.
[0192] The kneading temperature is preferably 140° C. or higher and 200° C. or lower, more preferably 140° C. or higher and 180° C. or lower, even more preferably 140° C. or higher and 170° C. or lower, and particularly preferably 150° C. or higher and 160° C. or lower. By setting the kneading temperature to 140° C. or higher, a uniform gel in which the entanglement of molecular chains is untangled can be obtained. Furthermore, by setting the kneading temperature to 200° C. or lower, a significant decrease in molecular weight due to thermal decomposition can be suppressed.
[0193] The kneading time is preferably 5 minutes or more and 180 minutes or less, more preferably 10 minutes or more and 150 minutes or less, even more preferably 15 minutes or more and 90 minutes or less, and particularly preferably 30 minutes or more and 60 minutes or less. By kneading for 5 minutes or more, a uniform gel in which the entanglement of molecular chains is disentangled can be obtained. Furthermore, by kneading for 180 minutes or less, a significant decrease in molecular weight due to thermal decomposition can be suppressed.
[0194] The kneading rotation speed is preferably 3 rpm or more and 50 rpm or less, more preferably 3 rpm or more and 30 rpm or less, even more preferably 3 rpm or more and 20 rpm or less, and particularly preferably 3 rpm or more and 10 rpm or less. By setting the kneading rotation speed to 3 rpm or more, a uniform gel in which the entanglement of molecular chains is untangled can be obtained. Furthermore, by setting the kneading rotation speed to 50 rpm or less, a significant decrease in molecular weight due to thermal decomposition can be suppressed.
[0195] (Extrusion Preparation Step) The extrusion preparation step is a step of preparing the yarn gel before extruding it. Specific examples of the extrusion preparation include temperature adjustment and degassing the yarn gel.
[0196] The temperature in the extrusion preparation step is preferably 140°C or higher and 200°C or lower, more preferably 140°C or higher and 190°C or lower, even more preferably 140°C or higher and 180°C or lower, and particularly preferably 150°C or higher and 180°C or lower. By setting the temperature in the extrusion preparation step to 140°C or higher, it is possible to prevent the outflow of liquid paraffin from the gel for raw yarn and suppress fluctuations in gel concentration, thereby enabling stable production of raw yarn. Furthermore, by setting the temperature to 200°C or lower, it is possible to suppress a significant decrease in molecular weight due to thermal decomposition.
[0197] The time for the extrusion preparation step (e.g., the degassing time) is preferably 5 minutes or more and 90 minutes or less, more preferably 5 minutes or more and 60 minutes or less, even more preferably 15 minutes or more and 60 minutes or less, and particularly preferably 30 minutes or more and 60 minutes or less. By setting the time for the extrusion preparation step to 5 minutes or more, the gel for raw yarn can be sufficiently degassed, and raw yarn can be obtained stably. Furthermore, by setting the time to 90 minutes or less, a significant decrease in molecular weight due to thermal decomposition can be suppressed.
[0198] (Extrusion Step) The extrusion step is a step of extruding the yarn gel to obtain yarn.
[0199] The extrusion speed is preferably 5 mm / min or more and 20 mm / min or less, more preferably 5 mm / min or more and 15 mm / min or less, even more preferably 7.5 mm / min or more and 12 mm / min or less, and particularly preferably 7.5 mm / min or more and 10 mm / min or less. By setting the extrusion speed to 5 mm / min or more, the raw yarn can be recovered without applying tension, and can be drawn to a high ratio in the raw yarn drawing step, resulting in a highly oriented (high-strength) yarn. Furthermore, by setting the extrusion speed to 20 mm / min or less, the extrusion rate can be stabilized, and a raw yarn with little unevenness in yarn diameter can be stably obtained.
[0200] The take-up speed is preferably 200 mm / min or more and 1600 mm / min or less, more preferably 200 mm / min or more and 1400 mm / min or less, even more preferably 250 mm / min or more and 1000 mm / min or less, and particularly preferably 500 mm / min or more and 800 mm / min or less. By setting the take-up speed to 200 mm / min or more, the raw yarn can be recovered without applying tension, and can be drawn to a high ratio in the raw yarn drawing step, resulting in a highly oriented (high-strength) yarn. Furthermore, by setting the take-up speed to 1600 mm / min or less, the discharge rate can be stabilized, and a raw yarn with little unevenness in yarn diameter can be stably obtained.
[0201] The discharge rate is preferably 0.2 g / min or more and 1.5 g / min or less, more preferably 0.2 g / min or more and 1.2 g / min or less, even more preferably 0.2 g / min or more and 1.0 g / min or less, and particularly preferably 0.3 g / min or more and 0.8 g / min or less. By setting the discharge rate to 0.2 g / min or more, the raw yarn can be recovered without applying tension, and can be drawn to a high ratio in the raw yarn drawing step, thereby obtaining a highly oriented (high-strength) yarn. Furthermore, by setting the discharge rate to 1.5 g / min or less, melt fracture can be suppressed, and a raw yarn with little unevenness in yarn diameter can be stably obtained.
[0202] The spinning hole diameter is preferably 0.8 mm or more and 1.5 mm or less, more preferably 0.8 mm or more and 1.2 mm or less, even more preferably 0.8 mm or more and 1.0 mm or less, and particularly preferably 0.9 mm or more and 1.0 mm or less. By setting the spinning hole diameter to 0.8 mm or more, the raw yarn diameter after liquid paraffin extraction can be adjusted to a certain thickness, and by drawing to a high ratio in the raw yarn drawing step, a highly oriented (high-strength) yarn can be obtained. Furthermore, by setting the diameter to 1.5 mm or less, the time required to extract liquid paraffin from the raw yarn can be shortened, and the extraction process can be completed efficiently.
[0203] (Quenching Step) The quenching step is a step of rapidly cooling the raw yarn. The quenching method is not particularly limited, but may be, for example, a method of passing the raw yarn through a water bath.
[0204] The time from the extrusion step to the quenching step (for example, the time until the extruded yarn enters the water bath) is preferably 0 to 10 seconds, more preferably 0 to 5 seconds, and even more preferably 0 to 2 seconds. By setting the time from the extrusion step to the quenching step to 10 seconds or less, the molten yarn can be rapidly cooled and solidified, and unevenness in the yarn diameter can be minimized.
[0205] When the yarn is passed through a water bath in the quenching step, the distance from the spinneret to the water surface of the water bath is preferably 0 cm or more and 10 cm or less, more preferably 1 cm or more and 8 cm or less, even more preferably 1 cm or more and 5 cm or less, and particularly preferably 1 cm or more and 3 cm or less. By setting the distance from the spinneret to the water surface of the water bath to 10 cm or less, the molten yarn can be rapidly cooled and solidified, and unevenness in the yarn diameter can be minimized.
[0206] The temperature in the quenching step is preferably 5° C. or higher and 30° C. or lower, more preferably 5° C. or higher and 25° C. or lower, even more preferably 5° C. or higher and 20° C. or lower, and particularly preferably 5° C. or higher and 15° C. or lower. By setting the temperature in the quenching step to 5° C. or higher, cooling costs can be reduced and production can be performed efficiently. Furthermore, by setting the temperature to 30° C. or lower, the molten raw yarn can be rapidly cooled and solidified, and unevenness in the raw yarn diameter can be minimized.
[0207] (Extraction Step) The extraction step is a step of extracting the first liquid paraffin and the second liquid paraffin from the raw yarn to obtain a raw yarn for drawing.
[0208] To extract the liquid paraffin, it is preferable to use an extraction solvent, which includes, but is not limited to, hexane and dichloromethane.
[0209] The extraction method is not particularly limited, but may be, for example, a method in which the raw yarn is immersed in an extraction solvent.
[0210] The extraction time is preferably 3 hours or more and 24 hours or less, more preferably 3 hours or more and 20 hours or less, even more preferably 5 hours or more and 20 hours or less, and particularly preferably 10 hours or more and 20 hours or less. By setting the extraction time to 3 hours or more, it is possible to extract liquid paraffin to a level that does not pose a problem for use as a raw yarn for drawing. If a large amount of liquid paraffin remains in the raw yarn for drawing, when heat is applied in the raw yarn drawing step, the molecular chain mobility is high and it is easy to become highly oriented, but on the other hand, it is difficult to maintain this state (it tends to return to the state before high orientation). Therefore, it is difficult to obtain a high-strength yarn. Furthermore, by setting the extraction time to 24 hours or less, it is possible to efficiently obtain a raw yarn for drawing without reducing productivity.
[0211] (Yarn Drawing Step) The yarn drawing step is a step of heating and drawing the yarn to be drawn.
[0212] The stretching is preferably multi-stage stretching, more preferably two-stage stretching, which preferably includes a first stretching step and a second stretching step.
[0213] ((Primary Stretching Step)) The delivery speed is preferably 50 mm / min or more and 200 mm / min or less, more preferably 50 mm / min or more and 150 mm / min or less, even more preferably 50 mm / min or more and 120 mm / min or less, and particularly preferably 50 mm / min or more and 100 mm / min or less.
[0214] The take-up speed is preferably 1000 mm / min to 4000 mm / min, more preferably 1000 mm / min to 3500 mm / min, still more preferably 1500 mm / min to 3500 mm / min, and particularly preferably 2000 mm / min to 3000 mm / min. The draw ratio is controlled by adjusting the delivery speed and take-up speed, and is set in consideration of productivity.
[0215] The drawing temperature is preferably 110°C or higher and 155°C or lower, more preferably 110°C or higher and 150°C or lower, even more preferably 115°C or higher and 145°C or lower, and particularly preferably 120°C or higher and 140°C or lower. By setting the drawing temperature to 110°C or higher, drawing can be performed in a state where the mobility of molecular chains is high, thereby achieving high orientation. Furthermore, by setting the temperature to 155°C or lower, drawing can be performed without melting the raw yarn to be drawn.
[0216] (Secondary Stretching Step) The delivery speed is preferably 50 mm / min or more and 200 mm / min or less, more preferably 50 mm / min or more and 150 mm / min or less, even more preferably 50 mm / min or more and 120 mm / min or less, and particularly preferably 50 mm / min or more and 100 mm / min or less.
[0217] The take-up speed is preferably 100 mm / min to 500 mm / min, more preferably 100 mm / min to 450 mm / min, even more preferably 150 mm / min to 400 mm / min, and particularly preferably 200 mm / min to 300 mm / min. The draw ratio is controlled by adjusting the delivery speed and take-up speed, and is set in consideration of productivity.
[0218] The drawing temperature is preferably 130°C or higher and 155°C or lower, more preferably 130°C or higher and 150°C or lower, even more preferably 135°C or higher and 150°C or lower, and particularly preferably 140°C or higher and 150°C or lower. By setting the drawing temperature to 130°C or higher, drawing can be performed in a state where the mobility of molecular chains is high, thereby achieving high orientation. Furthermore, by setting the temperature to 155°C or lower, drawing can be performed without melting the primarily drawn yarn.
[0219] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples. Unless otherwise specified, various operations were carried out at room temperature.
[0220] In the present application, the ethylene and hexane used in the examples and comparative examples were dehydrated using MS-3A (manufactured by Showa Union), and hexane was further deoxygenated by degassing under reduced pressure using a vacuum pump before use.
[0221] The physical properties of the ultra-high molecular weight polyethylene powders of the Examples and Comparative Examples were measured by the following methods.
[0222] (1) Intrinsic Viscosity IV The intrinsic viscosity IV of the polyethylene powders obtained in the Examples and Comparative Examples was measured in accordance with ISO 1628-3 (2010). The solvent used was 20 mL of decahydronaphthalene (to which 1 g / L of 2,6-di-t-butyl-4-methylphenol had been added), which had been degassed using a vacuum pump and substituted with nitrogen. A Cannon-Fenske viscometer (Shibata Scientific Instruments Co., Ltd.: Product No. -100) was used as the viscosity tube. The measurement was repeated three times, and the average of the three values obtained was used.
[0223] (2) Motility Index and Entanglement Degree of Slurry Containing Ultra-High Molecular Weight Polyethylene Powder The mobility index and entanglement degree of the ultra-high molecular weight polyethylene powder obtained in the Examples and Comparative Examples were measured using pulse NMR. A small sample tube with a diameter of 7 mm and a height of 45 mm was filled with 0.12 g of polyethylene powder, 0.28 g of liquid paraffin (product name: Smoil P-350P, manufactured by MORESCO Corporation), and 0.004 g of antioxidant (antioxidant (ADEKA STAB AO60G), manufactured by ADEKA Corporation) to prepare a slurry. The small sample tube containing the slurry was placed in a measurement sample tube with a diameter of 9 mm and a height of 180 mm and left to stand for 20 hours in a thermostatic chamber controlled at a temperature of 22°C and a humidity of 60%, allowing sufficient time for impregnation to produce a sample. The measurement sample tube was placed in a Bruker TD-NMR device (model: minispec mq20) set to an internal temperature of 30°C, and the sample was heated according to the <heating conditions> shown below.
[0224] The liquid paraffin used in measuring the slurry mobility is liquid paraffin manufactured by MORESCO Corporation (product name: Smoil P-350P), and its representative properties are density at 15°C: 0.866 g / cm 3 , pour point: -10°C, kinematic viscosity at 40°C: 68.00 mm2 / s (cSt), kinematic viscosity at 100°C: 9.188 mm2 / s (cSt), ring analysis Cn: 30%, Cp: 70%, average molecular weight: 489 g / mol.
[0225] The temperatures shown in the <Temperature Rise Conditions> below are the values measured by a thermocouple at the internal temperature of the sample. <Temperature Rise Conditions> 10°C / min temperature rise 23 minutes at 60°C, hold temperature 10°C / min temperature rise 23 minutes at 90°C, hold temperature 10°C / min temperature rise 23 minutes at 105°C, hold temperature 10°C / min temperature rise 23 minutes at 120°C, hold temperature 5°C / min temperature rise 26 minutes at 130°C, hold temperature 5°C / min temperature rise 26 minutes at 140°C, hold temperature 5°C / min temperature rise 10 minutes at 150°C, hold temperature
[0226] The set temperature of the device was corrected using the calibration lines (Equation A) and (Equation B) to take into account any discrepancy with the target temperature (actual temperature) of the sample. Decimals were rounded off. (For temperatures between 0°C and 100°C): y = 1.0984x + 260.88 (Equation A) (For temperatures between 100°C and 200°C): y = 1.1729x + 252.21 (Equation B) x = target temperature (°C), y = set temperature (K)
[0227] After the temperature increase was completed by the above procedure, the spin-spin relaxation time (T2, sometimes simply referred to as "relaxation time" in this specification) of the sample at 150°C was measured according to the <Measurement conditions> shown below. <Measurement conditions> Magnetic field strength: 0.47 T Measurement nuclide: 1H (20 MHz) Measurement method: Carr Purcell Meiboom Gill method Number of accumulations: 256 Repetition time: 3 seconds Interval (τ) between the first 90° pulse and the 180° pulse: 0.04 milliseconds Total number of echo signals: 6400 Heater power: 5%
[0228] The free induction decay (FID) obtained by the measurement was subjected to curve fitting using the analysis program TD-NMR-A manufactured by Bruker (fitting range: full range, i.e., t = 0.10032 to 567.8196). For fitting, the function shown in the following <Equation 1> was used.
[0229] <Equation 1> f(t) = Rαexp(-t / Tα) + Rβexp(-t / Tβ) + Rγexp(-t / Tγ) (where Rα + Rβ + Rγ = 100) t: variable (time) Tα: relaxation time (ms) of low mobility component α Rα: abundance ratio of low mobility component α Tβ: relaxation time (ms) of intermediate component β Rβ: abundance ratio of intermediate component β Tγ: relaxation time (ms) of high mobility component γ Rγ: abundance ratio of high mobility component γ
[0230] Finally, the mobility index (ms) and the degree of entanglement were calculated from each relaxation time T and each abundance ratio R obtained by curve fitting of the free induction decay and the following (Equation I) and (Equation II). This procedure was repeated five times, and the maximum and minimum values were excluded to calculate the average values of the three points, from which the final mobility index and degree of entanglement were calculated.
[0231] (Motility index) = Tα × Rα / (Rα + Rβ) + Tβ × Rβ / (Rα + Rβ) (Equation I) (Entanglement degree) = Rβ / Rα (Equation II)
[0232] Temperature Calibration Method <Calibration Method> 1. The heater power of the device was set to 5%, and the calibration lines (Equation A) and (Equation B) were obtained using the following procedure. A measurement sample tube with a diameter of 9 mm and a height of 180 mm was filled with polyethylene powder to a height of 1 cm from the bottom, and a thermocouple was inserted. 2. The measurement sample tube was placed into a Bruker TD-NMR device (model: minispec mq20) with the device temperature set to 0°C. 3. The thermocouple value was recorded 5 minutes after placement. 4. After 10 minutes or more had passed since placement, the set temperature was set to 10°C and heating was initiated. 5. The thermocouple value was recorded 5 minutes after heating was complete (device temperature = set temperature). 6. After 10 minutes or more had passed since heating was complete, the set temperature was set to 20°C and heating was initiated. 7. Thereafter, steps (5) and (6) are repeated at 10°C intervals up to 200°C. 8. Plot the recorded thermocouple temperature on the horizontal axis and the set temperature on the vertical axis, and perform a linear approximation.
[0233] (3) 13 Comonomer content measured by C-NMR in polyethylene powder 13 The comonomer (olefin copolymerizable with ethylene) content measured by C-NMR was measured according to the method disclosed in G. J. Ray et al., Macromolecules, 10, 773 (1977), 13 The signal intensity of methylene carbon observed in the C-NMR spectrum was used to calculate the nucleus. 13 C Observation frequency: 100.53 MHz Pulse width: 45° (7.5 μsec) Pulse program: single pulse dec PD: 5 s Measurement temperature: 130°C Number of accumulations: 30,000 or more Reference: PE (-eee-) signal, 29.9 ppm Solvent: orthodichlorobenzene-d4 Sample concentration: 5 to 10 wt% Dissolution temperature: 130 to 140°C
[0234] (4) Ti Content and Al Content The Ti and Al contents of the polyethylene powders obtained in the examples and comparative examples were evaluated by high-frequency plasma mass spectrometry in accordance with JIS K 0133. Samples were prepared by pressure decomposition with nitric acid using a microwave decomposition apparatus (model ETHOS TC, manufactured by Milestone General Co., Ltd.). The elemental concentrations of titanium (Ti) and aluminum (Al) of the prepared samples were measured by the internal standard method using an ICP-MS (inductively coupled plasma mass spectrometer, model X Series X7, manufactured by Thermo Fisher Scientific Co., Ltd.), and these were taken as the Ti content and Al content, respectively.
[0235] (5) D 10 , D 50 and D 90 The particle sizes of the ultra-high molecular weight polyethylene powders obtained in the Examples and Comparative Examples were measured using a laser diffraction particle size distribution analyzer (Mastersizer 3000 manufactured by Malvern Panalytical). Based on the measurements, a cumulative particle size distribution was created from the small particle size side, and the particle sizes at 10%, 50%, and 90% of the cumulative size were designated as D. 10 , D 50 and D 90 The measurement was repeated three times, and the average value of the three measurements was used. Dispersion medium: soapy water (purified water containing 1 wt% of IGEPAL (registered trademark) CO-630)
[0236] <Method 1 for producing high-strength fiber> [Swelling step] A high-strength fiber was produced using ultra-high molecular weight polyethylene powder as follows. When the total amount of the ultra-high molecular weight polyethylene powder and liquid paraffin was 100 parts by mass, 15 parts by mass of the ultra-high molecular weight polyethylene powder, 85 parts by mass of liquid paraffin (liquid paraffin (product name: Smoil P-350P) manufactured by MORESCO Corporation), and 1 part by mass of an antioxidant (antioxidant (ADEKA STAB AO-60G) manufactured by ADEKA Corporation) were blended together to obtain a mixture having a melting point (T m2 ) and stirred for 60 minutes at a temperature 35°C lower than that of the starting temperature to prepare a slurry liquid.
[0237] [Kneading Step] Next, the slurry liquid was poured into liquid paraffin (liquid paraffin manufactured by MORESCO Corporation (product name: Smoil P-350P)) at 160°C and stirred for 2 minutes to produce a gel with a polymer concentration of 5 parts by mass. The obtained gel was poured into a Labo Plastomill manufactured by Toyo Seiki Seisaku-sho (main body model: 4C150-01) and kneaded at a constant temperature of 150°C for 180 minutes with a screw rotation speed of 10 rpm to produce a kneaded gel.
[0238] [Spinning Process] Next, spinning was performed using a Capilograph 1D (main unit model: PMD-C) manufactured by Toyo Seiki Co., Ltd. An orifice with a hole diameter of 1.0 mm, a length of 66 mm, and an inlet angle of 90° was used. The kneaded gel was introduced into a furnace set at 180°C, and degassing was performed for 60 minutes. The extrusion speed was then set to 7.5 mm / min so that the discharge rate was 0.35 g / min. The raw yarn was passed through a water bath directly below the tip of the orifice and collected at a winding speed of 2.8 m / min. The distance from the tip of the orifice to the water bath surface was 8 cm, and the temperature of the water bath was set to 20°C. The wound raw yarn was then immersed in hexane for extraction to remove liquid paraffin, followed by drying for 24 hours to obtain a raw yarn.
[0239] [Drawing step] The raw yarn thus obtained was subjected to a first drawing at a speed of 20 mm / min in a thermostatic oven at 120°C, and then a second drawing at a speed of 10 mm / min in a thermostatic oven at 140°C until just before the yarn broke, thereby obtaining a high-strength fiber (drawn yarn). The temperature in the thermostatic oven was measured at the center of the thermostatic oven with a thermometer.
[0240] <Method 2 for producing high-strength fiber> A high-strength fiber was produced using ultra-high molecular weight polyethylene powder as follows. When the total amount of the ultra-high molecular weight polyethylene powder and liquid paraffin was 100 parts by mass, 15 parts by mass of the ultra-high molecular weight polyethylene powder, 85 parts by mass of liquid paraffin (liquid paraffin (product name: Smoil P-350P) manufactured by MORESCO Corporation), and 1 part by mass of an antioxidant (tetrakis[methylene(3,5-di-t-butyl-4-hydroxy-hydrocinnamate)]methane (product name: ANOX20) manufactured by Great Lakes Chemical Japan Co., Ltd.) were blended together to obtain a fiber having a melting point (T m2) for 60 minutes at a temperature 35°C lower than the initial temperature, thereby preparing a slurry liquid. Next, the slurry liquid was poured into liquid paraffin (liquid paraffin manufactured by MORESCO Corporation (product name: Smoil P-350P)) at 180°C and stirred for 2 minutes to produce a gel with a polymer concentration of 5 parts by mass. The obtained gel was poured into a Labo Plastomill manufactured by Toyo Seiki Co., Ltd. (main unit model: 4C150-01) and kneaded at a constant temperature of 150°C for 180 minutes at a screw rotation speed of 10 rpm to produce a kneaded gel. Next, a spinning operation was carried out using a Capilograph 1D manufactured by Toyo Seiki Co., Ltd. (main unit model: PMD-C). An orifice with a hole diameter of 1.0 mm, a length of 66 mm, and an inlet angle of 90° was used, and the kneaded gel was poured into a furnace set at 180°C, after which degassing was carried out for 60 minutes. The extrusion speed was then set to 10 mm / min to achieve a discharge rate of 0.45 g / min. The raw yarn was passed through a water bath directly below the orifice tip and collected at a take-up speed of 0.8 m / min. The distance from the orifice tip to the water bath surface was 8 cm, and the water bath temperature was set to 20°C. The wound raw yarn was then immersed in hexane for extraction to remove liquid paraffin, followed by drying for 24 hours. The resulting raw yarn was subjected to a primary drawing in a thermostatic bath at 120°C with a let-off speed of 100 mm / min and a take-up speed of 3000 mm / min, followed by a secondary drawing in a thermostatic bath at 140°C with a let-off speed of 100 mm / min and a take-up speed just before the yarn breakage, thereby obtaining a high-strength fiber (drawn yarn). The drawing process was performed using a heated drawing apparatus (main unit model: IMC-3F08) manufactured by Imoto Machinery Co., Ltd. The temperature inside the thermostatic chamber is the temperature at the center of the thermostatic chamber measured with a thermometer.
[0241] <High-strength fiber manufacturing method 3> A high-strength fiber was obtained in the same manner as described above (High-strength fiber manufacturing method 2), except that the kneading time in a Laboplastomill (main body model: 4C150-01) manufactured by Toyo Seiki Co., Ltd. was set to 0 minutes (no kneading in the Laboplastomill).
[0242] [Decomposition rate of gel after kneading] The intrinsic viscosity IV of the raw yarn obtained by the above method was calculated by the method specified above. The intrinsic viscosity of the dried molded product (raw yarn) was calculated and designated as IV(A). The intrinsic viscosity of the ultra-high molecular weight polyethylene powder before kneading was calculated and designated as IV. The decomposition rate was calculated from the calculated intrinsic viscosity IV and intrinsic viscosity IV(A) using the following formula. The gel decomposition rate was evaluated according to the following criteria. Calculation of decomposition rate: Decomposition rate = {IV - IV(A)} / IV
[0243] (Evaluation criteria) ◎: Decomposition rate 0% or more and less than 21% ○: Decomposition rate 21% or more and less than 51% △: Decomposition rate 51% or more and less than 81% ×: Decomposition rate 81% or more
[0244] [Tensile Breaking Strength of High-Strength Fiber] 10 m of high-strength fiber (drawn yarn) spun by the method described above was cut at 1 m intervals, and 10 of the obtained fibers were pulled until they broke at room temperature, and the average breaking strength was calculated. The breaking strength was calculated by dividing the maximum load applied to the yarn by the fineness. Here, fineness refers to the ratio of the number of fibers per 1 × 10 4 The weight (g) per meter was calculated from the weight of 10 m of high-strength fiber. The fineness is expressed in dtex. A balance capable of measuring to the nearest 0.1 mg was used to measure the weight. The tensile breaking strength of the high-strength fiber was evaluated according to the following criteria.
[0245] (Evaluation criteria) ☆: Breaking strength 43 cN / dtex or more ◎: Breaking strength 30 cN / dtex or more, less than 43 cN / dtex ○: Breaking strength 25 cN / dtex or more, less than 30 cN / dtex △: Breaking strength 20 cN / dtex or more, less than 25 cN / dtex ×: Breaking strength less than 20 cN / dtex
[0246] [Evaluation of high-speed winding properties of high-strength fiber] The gel kneaded by the method described above was spun using a Capilograph 1D (main body model: PMD-C) manufactured by Toyo Seiki Co., Ltd. The orifice used had a hole diameter of 0.5 mm, a length of 5 mm, and an inlet angle of 90°. The spinning conditions were fixed at a temperature of 200°C and an extrusion speed of 20 mm / min, and the winding speed was increased from 3 m / min to 19.7 m / min. 2The speed at which the film broke was measured as the high winding speed while gradually increasing the winding speed, and the film was evaluated based on the average value of five measurements and the following evaluation criteria.
[0247] (Evaluation criteria) ☆: High-speed winding speed is 900 m / min or more. ◎: High-speed winding speed is 700 m / min or more and less than 900 m / min. ○: High-speed winding speed is 400 m / min or more and less than 700 m / min. △: High-speed winding speed is 200 m / min or more and less than 400 m / min. ×: High-speed winding speed is less than 200 m / min.
[0248] [Catalyst synthesis method] (1) Synthesis of raw material [a-2] 6[Mg(C 4 H 9 ) 2 ] Al(C 2 H 5 ) 3 2,000 mmol of raw material [a-1] was charged and diluted with hexane. Then, while stirring at 50°C, a hexane solution of 800 mmol of n-butanol was added dropwise over 3 hours, and after completion of the reaction, the line was washed with 300 mL of hexane. Stirring was continued for another 2 hours at 50°C. After the reaction was completed, the mixture was cooled to room temperature and used as raw material [a-2]. Raw material [a-2] had a total concentration of magnesium and aluminum of 1.0 mol / L.
[0249] (2) Synthesis of Raw Material [a-3] 2,000 mL of [a-1] (corresponding to 2,000 mmol of magnesium and aluminum) was placed in an 8 L stainless steel autoclave that had been thoroughly purged with nitrogen, and 240 mL of a hexane solution of 8.33 mol / L methylhydrogenpolysiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.) was pressure-fed while stirring at 80°C, and stirring was continued for another 2 hours at 80°C. After the reaction was completed, the mixture was cooled to room temperature and used as Raw Material [a-3]. Raw Material [a-3] had a total concentration of magnesium and aluminum of 0.786 mol / L.
[0250] (3) Synthesis of [A-1] Support: 1,000 mL of a 1 mol / L hexane solution of trichlorosilane was placed in an 8 L stainless steel autoclave that had been thoroughly purged with nitrogen, and a hexane solution of the raw material [a-2] organomagnesium compound equivalent to 943 mmol of magnesium was added dropwise over 3 hours at 65°C. The reaction was continued for another 1 hour with stirring at 65°C. After completion of the reaction, the supernatant was removed and the support was washed four times with 1,800 mL of hexane to obtain [A-1] support. Analysis of this support revealed that the magnesium content per 1 g of solid was 7.5 mmol.
[0251] (4) Preparation of catalyst [c-1] To 1,970 ml of hexane slurry containing 110 g of the above [A-1] carrier, 103 mL of a 1 mol / L hexane solution of titanium tetrachloride and 131 ml of raw material [a-3] were added simultaneously over 3 hours while stirring at 10°C. After the addition, the reaction was continued for 1 hour at 10°C. After completion of the reaction, the supernatant was removed, and the unreacted raw material components were removed by washing four times with hexane, thereby preparing solid catalyst component [c-1].
[0252] (5) Preparation of catalyst [c-2] 23 mL of a hexane solution of 1 mol / L titanium tetrachloride and 29 mL of raw material [a-3] were simultaneously added over 3 hours to 1,970 mL of hexane slurry containing 110 g of the above [A-1] carrier while stirring at 10°C. After the addition, the reaction was continued for 1 hour at 10°C. After the reaction was completed, the supernatant was removed and the mixture was washed four times with hexane to remove unreacted raw material components. After the reaction was completed, 23 mL of a hexane solution of 1 mol / L triethylaluminum (hereinafter also referred to as TEA) was added over 1 hour while stirring at 40°C. After the addition, the reaction was continued for 1 hour at 40°C. After the reaction was completed, the supernatant was removed and the components in the supernatant were removed by washing four times with hexane to prepare solid catalyst component [c-2].
[0253] (6) Preparation of catalyst [c-3] 103 mL of a hexane solution of 1 mol / L titanium tetrachloride and 103 mL of raw material [a-1] were simultaneously added over 3 hours to 1,970 mL of hexane slurry containing 110 g of the above [A-1] carrier while stirring at 5°C. After the addition, the reaction was continued for 1 hour at 5°C. After the reaction was completed, the supernatant was removed and the mixture was washed four times with hexane to remove unreacted raw material components. After the reaction was completed, 103 mL of a hexane solution of 1 mol / L ethylaluminum dichloride (hereinafter also referred to as EADC) was added over 1 hour while stirring at 40°C. After the addition, the reaction was continued for 1 hour at 40°C. After the reaction was completed, the supernatant was removed and the components in the supernatant were removed by washing four times with hexane to prepare solid catalyst component [c-3].
[0254] (7) Preparation of catalyst [c-4] 23 mL of a hexane solution of 1 mol / L titanium tetrachloride and 23 mL of raw material [a-1] were simultaneously added over 3 hours to 1,970 mL of hexane slurry containing 110 g of the above [A-1] carrier while stirring at 5°C. After the addition, the reaction was continued for 1 hour at 5°C. After the reaction was completed, the supernatant was removed and the mixture was washed four times with hexane to remove unreacted raw material components. After the reaction was completed, 23 mL of a hexane solution of 1 mol / L ethylaluminum dichloride (hereinafter also referred to as EADC) was added over 1 hour while stirring at 40°C. After the addition, the reaction was continued for 1 hour at 40°C. After the reaction was completed, the supernatant was removed and the components in the supernatant were removed by washing four times with hexane to prepare solid catalyst component [c-4].
[0255] The changes made during catalyst synthesis are summarized below.
[0256] (8) Synthesis of Cocatalyst [b-2] In a 300 mL glass vessel thoroughly purged with nitrogen, 180 mL of a 1.0 mol / L hexane solution [b-1] of triisobutylaluminum and diisobutylaluminum hydride (9:1 mixture) was charged, and 30 mL of a 1.0 mol / L hexane solution of TEA was added dropwise over 30 minutes while stirring at 30°C. After the dropwise addition, the reaction was continued for 30 minutes. Cocatalyst [b-2] was obtained.
[0257] (9) Synthesis of Cocatalyst [b-3] In a 300 mL glass vessel thoroughly purged with nitrogen, 100 mL of a 1.0 mol / L TEA hexane solution was charged, and 90 mL of a 1.0 mol / L dibutylhydroxytoluene hexane solution was added dropwise over 30 minutes while stirring at 0°C. After the dropwise addition, the reaction was continued for 30 minutes. A bulky cocatalyst [b-3] was obtained.
[0258] Example 1 Polymerization of Polyethylene Powder Polyethylene powder was polymerized using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen, according to the method described below. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 75°C, and 0.5 mmol / L of organometallic compound component (b-2) was added as a cocatalyst. Next, ethylene was added to the reactor so that the internal pressure reached 0.397 MPa, and hydrogen was then added to the reactor so that the internal pressure reached 0.400 MPa. Furthermore, 10.0 mg of the catalyst [c-4] was added. The internal temperature was maintained at 75°C, and polymerization was carried out for 90 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, ethylene was supplied as needed to maintain the internal pressure at 0.400 MPa. After polymerization, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. The polymer slurry was filtered through a 500 mesh (26 μm mesh) filter to obtain polyethylene powder. The obtained polyethylene powder was dried at 40°C for 24 hours. The polymerization activity in the polymerization reactor was 6,000 g per 1 g of catalyst. Scale and extremely coarse particles were removed using a sieve with 425 µm openings, and the physical properties of the polyethylene powder were evaluated.
[0259] The polyethylene powder (A) and the fibers of the polyethylene powder (A) produced by the above-mentioned <Production methods 1 to 3 of high-strength fibers> were subjected to the various evaluations described above, and the results are shown in Table 3.
[0260] (Examples 2 to 15 and Comparative Examples 1, 2, and 4) Polyethylene powder and fibers thereof were produced in the same manner as in Example 1, except that the polymerization conditions were changed as shown in Tables 2 and 4, and the above-mentioned various evaluations were carried out. The results are shown in Tables 3 and 5. In Examples 14 and 15, 1-butene was copolymerized as the comonomer (represented as "CM" in the tables).
[0261] Example 16 Polymerization of Polyethylene Powder (B) Hexane, ethylene, and a catalyst were continuously supplied to a 300-L vessel-type polymerization reactor equipped with three swept-back impellers and three baffles. The polymerization pressure was 0.4 MPa. The polymerization temperature was maintained at 60°C by jacket cooling. Hexane was supplied from the bottom of the polymerization reactor at 40 L / h, with an average residence time of 120 minutes. Catalyst [c-3] was used as the polymerization catalyst and was supplied so that the polyethylene powder production rate was 10.0 kg / h. Cocatalyst component [b-1] (triisobutylaluminum and diisobutylaluminum hydride (9:1 mixture)) was used and was supplied at 10 mmol / h. Hydrogen was not supplied. STATSAFE 3000 (90 g / L) diluted with normal hexane was added as the polymerization catalyst in an amount of 25 ppm by mass relative to the polyethylene powder production rate. The stirring speed was 230 rpm. The polymerization slurry in the polymerization reactor was introduced into an intermediate flash tank at a pressure of 0.05 MPaG and a temperature of 40°C to maintain a constant level in the polymerization reactor, and unreacted ethylene was separated. The polymerization slurry was continuously pumped from the flash tank to a centrifuge to separate the polymer and solvent. The separated polyethylene powder was then sent to a rotary kiln-type dryer controlled at 70°C and dried while being blown with nitrogen. During this drying process, steam was sprayed onto the polyethylene powder to deactivate the catalyst and cocatalyst. The resulting polyethylene powder was sieved through a 425 μm mesh sieve to remove any material that did not pass through the sieve, yielding a polyethylene powder. The polymerization activity in the polymerization reactor was 21,000 g per gram of catalyst. The results are shown in Tables 4 and 5.
[0262] Comparative Example 3 Preparation of Catalyst [c-5] Using a 1.5 L autoclave, 20 g of catalyst [c-1] was prepolymerized. 800 mL of normal hexane was used as the solvent, and 0.4 mmol of [b-1] (a 9:1 mixture of triisobutylaluminum and diisobutylaluminum hydride) was used as the cocatalyst component. 20 mol % (molar ratio: hydrogen / (ethylene + hydrogen)) of hydrogen was supplied. The polymerization temperature was 20°C, and ethylene was supplied so that 5 g of polyethylene was polymerized per 1 g of catalyst [c-1]. After completion of the polymerization, the supernatant was removed, and the mixture was washed four times with hexane to remove unreacted raw material components, thereby preparing catalyst [c-5]. Polyethylene powder was polymerized using a 300 L vessel-type polymerization reactor equipped with three swept-back impellers and three baffles. Normal hexane was supplied as a solvent at a flow rate of 40 L / hour, the total liquid volume was adjusted so that the slurry concentration was 30% by mass, and the stirring speed was 550 rpm. Ziegler-Natta catalyst [c-5] was used as the polymerization catalyst and was supplied so that the polyethylene powder production rate was 9 kg / hour. STATSAFE 3000 (90 g / L) diluted with normal hexane was added as the polymerization catalyst in an amount of 20 ppm by mass relative to the polyethylene powder production rate. [b-1] (triisobutylaluminum and diisobutylaluminum hydride (9:1 mixture)) was used as the cocatalyst component and was supplied at a rate of 10 mmol / hour. Hydrogen was supplied at 1.0 mol% (molar ratio: hydrogen / (ethylene + hydrogen)). The polymerization temperature was 78°C, the polymerization pressure was 0.3 MPaG, and the average residence time was 3.0 hours. The polymerization slurry in the polymerization reactor was introduced into a flash tank at a pressure of 0.05 MPaG and a temperature of 70°C so that the level in the polymerization reactor was kept constant, and unreacted ethylene and hydrogen were separated. Next, the polymerization slurry was continuously pumped from the flash tank to a centrifuge to separate the polymer and solvent, and the separated polyethylene powder was then sent to a rotary kiln-type dryer controlled at 90°C and dried while nitrogen was blown in. Note that during this drying process, steam was sprayed onto the polyethylene powder to deactivate the catalyst and cocatalyst. The results are shown in Tables 4 and 5.
[0263]
[0264] The polyethylene powder of the present invention has industrial applicability as a raw material for various molded articles, microporous membranes, battery separators, and fibers.
Claims
1. An ultra-high molecular weight polyethylene powder having an intrinsic viscosity IV of 12.0 dL / g or more and 35.0 dL / g or less, and a mobility index calculated from the following formula (I) of 57 ms or more and 73 ms or less, [Mobility Index] = Tα x Rα / (Rα + Rβ) + Tβ x Rβ / (Rα + Rβ) (Formula I) (wherein Tα is the relaxation time (ms) of the low mobility component α, Rα is the abundance ratio of the low mobility component α, Tβ is the relaxation time (ms) of the intermediate component β, Rβ is the abundance ratio of the intermediate component β, and the Tα, Rα, Tβ, and Rβ are values obtained by approximating a free induction decay curve obtained by the Carr Purcell Meiboom Gill method using pulse NMR to three components, the low mobility component α, the intermediate component β, and the high mobility component γ).
2. The ultra-high molecular weight polyethylene powder according to claim 1, wherein the degree of entanglement calculated from the following formula (II) is 0.6 or more and 2.8 or less: [degree of entanglement]=Rβ / Rα (formula II) [wherein Rβ and Rα are as defined in claim 1].
3. The following relationship (Equation III) is satisfied: [Mobility Index]>-0.2×[Intrinsic Viscosity IV]+62 (Equation III) The ultra-high molecular weight polyethylene powder according to claim 1 or 2.
4. 13 3. The ultra-high molecular weight polyethylene powder according to claim 1, wherein the content of structural units derived from olefins copolymerizable with ethylene, as measured by C-NMR, is 0.1 mol % or less.
5. The ultra-high molecular weight polyethylene powder according to claim 1 or 2, wherein D50 measured by a laser diffraction particle size distribution measuring device is 40 μm or more and 400 μm or less.
6. The ultra-high molecular weight polyethylene powder according to claim 1 or 2, having an intrinsic viscosity IV of 17.0 dL / g or more and 33.0 dL / g or less.
7. The ultra-high molecular weight polyethylene powder according to claim 1 or 2, having a mobility index of 64 ms or more and 73 ms or less.
8. The ultra-high molecular weight polyethylene powder according to claim 1 or 2, wherein the titanium (Ti) content is 10 ppm or less, and the aluminum (Al) content is 10 ppm or less.
9. The ultra-high molecular weight polyethylene powder according to claim 1 or 2, which is for use in high-strength fibers.
10. A molded body of the ultra-high molecular weight polyethylene powder according to claim 1 or 2.
11. The molded article according to claim 10, wherein the molded article is a fiber.
12. A method for producing a polyethylene powder for stretching, comprising: a slurrying step of mixing ultra-high molecular weight polyethylene powder with a first liquid paraffin and stirring the mixture at a temperature equal to or lower than the melting point of the ultra-high molecular weight polyethylene powder to obtain a slurry; a gelling step of mixing the slurry with a second liquid paraffin having a temperature of 150°C or higher and 300°C or lower to obtain a gel for raw yarn having a temperature of 140°C or higher and 200°C or lower; an extrusion step of extruding the gel for raw yarn to obtain raw yarn; an extraction step of extracting the first liquid paraffin and the second liquid paraffin from the raw yarn to obtain raw yarn for stretching; and a raw yarn stretching step of heating and stretching the raw yarn for stretching, wherein the intrinsic viscosity IV of the ultra-high molecular weight polyethylene powder is 12.0 dL / g or higher and 35.0 dL / g or lower, and the mobility index of the ultra-high molecular weight polyethylene powder calculated from the following formula I is 57 ms or higher and 73 ms or lower. Mobility index = Tα × Rα / (Rα + Rβ) + Tβ × Rβ / (Rα + Rβ) (Equation I) (wherein Tα is the relaxation time (ms) of the low mobility component α, Rα is the abundance ratio of the low mobility component α, Tβ is the relaxation time (ms) of the intermediate component β, Rβ is the abundance ratio of the intermediate component β, and the Tα, Rα, Tβ, and Rβ are values obtained by approximating a free induction decay curve obtained by the Carr Purcell Meiboom Gill method using pulse NMR to three components, the low mobility component α, the intermediate component β, and the high mobility component γ). A method for producing high strength fibers.
13. The method for producing a high strength fiber according to claim 12, further comprising a kneading step of kneading the yarn gel prior to the extrusion step.
Citation Information
Patent Citations
PROCESS FOR THE PRODUCTION OF POLYOLEFINS AND THEIR COPOLYMERISATS
DE3127133A1
Ultrahigh molecular weight polyethylene powder
WO2019187727A1
Ultra high molecular weight polyethylene particle, method for producing the same and molded article by using the same
JP2012025817A
Method for producing ultra high molecular weight polyethylene particle and molded product using the ultra high molecular weight polyethylene particle
JP2012229417A
Non-entangled high or ultra-high molecular weight polyethylene produced using Ziegler-Natta catalysts
JP2017508837A
Cited By
Ethylene polymer particles, production method for same, and molded article of same
WO2026186622A1