Resin biocide composition comprising one or more resins selected from MF, UF, PF, MUF and phenolic resins and one or more soluble copper salts

By adding soluble copper salts to melamine-formaldehyde, urea-formaldehyde, and phenolic resins, a biocidal material is formed, which solves the problem of easy infection on the resin surface and achieves effective removal and prevention of bacteria, fungi, and viruses.

CN105579048BActive Publication Date: 2024-11-26L·A·艾姆斯蒂卡萨拉查
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201380079819.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2013-10-03
Publication Date
2024-11-26
Estimated Expiration
2033-10-03

AI Technical Summary

Technical Problem

Existing melamine-formaldehyde, urea-formaldehyde, and phenolic resin surfaces are prone to becoming habitats for microorganisms, leading to infection risks and making it difficult to effectively remove bacteria, fungi, and viruses from the surfaces.

Method used

By adding soluble copper salts to the resin, a biocidal material is formed. The copper ions bind to the resin network to kill microorganisms and form an antibacterial, antifungal, and antiviral coating on the resin surface.

Benefits of technology

It effectively removes bacteria, fungi, and viruses that come into contact with resin surfaces, preventing their reproduction and infection, maintaining surface hygiene, and is suitable for a variety of materials and products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_5
    Figure SMS_5
Patent Text Reader

Abstract

The present invention relates to a resin biocide composition, comprising one or more resins selected from melamine formaldehyde, urea formaldehyde, phenol formaldehyde, melamine urea formaldehyde and phenolic resins, and one or more copper salts soluble in an aqueous system and the resin solution, wherein the copper salt is generally selected from organic copper salts, R-Cu, R1-Cu-R2, wherein R, R1 and R2 can be (C3-C4) having one or more acids, aldehydes, esters, ethers, hydroxyls or amino groups in their structures. 18 ) alkyl chain. The invention also relates to a method for the manufacture of said resin biocide composition and to the use of said resin biocide composition to obtain, for example, flooring, impregnated paper, adhesive mixtures and molded products. The invention also relates to wood covered with paper impregnated with the resin biocide composition and to a method for obtaining it; and to a method for the manufacture of molded products having a biocide effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to obtaining a biocide material comprising a thermostable plastic such as melamine formaldehyde (MF), urea formaldehyde (UF), phenol formaldehyde (PF), melamine urea formaldehyde (MUF) and phenolic resins and a copper salt. The present invention relates to obtaining a biocide composition (antibacterial, antifungal and antiviral) from a resin by adding a copper salt soluble in the resin in a solution of the resin. The present invention relates to obtaining a biocide composition (antibacterial, antifungal and antiviral) by adding the resin in powder form and including a copper salt in the form of copper in the resin.

[0002] The present invention contemplates the inclusion of copper salts in melamine formaldehyde (MF), urea formaldehyde (UF), phenol formaldehyde (PF), melamine urea formaldehyde (MUF) and phenolic resins, as it has been determined that leaving free copper ions can provide biocide properties.

[0003] To achieve its purpose, the present invention contemplates that a synergistic effect is achieved by mixing soluble salts of different types of molecular weight and chemical structure to achieve release of the biocide when the salts are dispersed as ions on its surface.

[0004] Soluble copper salts with organic chains allowing interconnection with the melamine formaldehyde network, with the urea formaldehyde network, with the phenolic resin network and / or with mixtures of these resins maintaining a united structure.

[0005] In addition, the present invention includes a process for obtaining a biocide material containing melamine formaldehyde, urea formaldehyde, phenol formaldehyde, melamine urea formaldehyde and phenolic resins, and copper salts soluble in the resins. The resins with copper salts can be applied to the surface of carriers such as paper, wood, cotton, clay and other materials. In addition, they can be used without a carrier, as in the case of products obtained by molding. Background of the Invention

[0007] The advantages of copper salts are well documented in the literature. These salts, when in contact with water, release cuprous and / or cupric ions, depending on the type of salt. It is scientifically accepted that the mechanism by which fungi, bacteria and viruses are inactivated and / or eliminated by copper ions is their penetration through the membranes of the microorganisms. The ions that penetrate the membranes of these microorganisms alter the life systems (cell membrane permeability, protein degradation, inhibition of enzymatic reactions, and many other destructive effects).

[0008] Document US4181786 describes a process for obtaining melamine with antibacterial and antifungal properties by reacting with silver ions to form a carboxyl-containing organic compound with said properties. The silver organic compound is mixed with melamine. In addition to silver ions, the patent also indicates that it is possible to use copper and zinc ions. The process for obtaining the organic compound with copper can be through the reaction of copper with monomers and oligomers. In addition, it is also indicated that porous polymers and the inclusion of silver ions in the polymer pores are possible. The silver concentration in the polymer is in the range of 0.0009 millimoles per gram of polymer.

[0009] Document US20060166024A1 describes the use of antimicrobial agents in melamine resins to utilize the antimicrobial properties of their surfaces for decorative and molded products. The antimicrobial agents are triclosan, o-phenylphenol, zinc pyrithione, sodium pyrithione, biguanide, titanium dioxide, silver compounds, copper compounds and zinc compounds. For the latter, there is no specification. The antimicrobial agent is used in the range of 0.1 to 5% by weight of the melamine resin.

[0010] Document US2011000016A1 presents an invention involving the inclusion of an antimicrobial agent in a melamine resin capable of providing permanent antimicrobial properties. The antimicrobial agent is a finely divided powder dispersed in a fluid. The antimicrobial agent is of organic type: triclosan and metal pyrithione, preferably zinc pyrithione. The antimicrobial agent concentration is in the range of 0.3% to 1% by weight of the melamine resin.

[0011] Document US20060068662, by the same author as invention patent application US20110000616, presents an invention involving the inclusion of an antimicrobial agent in a melamine resin. The antimicrobial agent is a fine powder dispersed in a fluid. The powdered antimicrobial agent dispersed in the fluid is triclosan, o-phenylphenol, zinc pyrithione, sodium pyrithione, barium hydrate, zinc-containing zeolite and amorphous glass powder containing zinc. In the melamine resin, the weight of the antimicrobial powder dispersed in the fluid is between 0.1 and 5%.

[0012] Typically, surfaces obtained from melamine formaldehyde, urea formaldehyde and phenolic resins are hard, transparent, resistant to water and oil, have low flammability, are resistant to weak acids and other chemical products (acetone, ethanol, oil, etc.), are difficult to scratch, are resistant to heat and electricity, and are easy to clean.

[0013] Melamine formaldehyde, urea formaldehyde and phenolic resins are widely used in paper coverings for laminated wood applications and other decorative forms.

[0014] Paper impregnated with one of these resins, melamine formaldehyde, urea formaldehyde and phenolic resins, is passed through an oven at a speed of 20 to 60 m / min, wherein the resin is partially gelled. The paper surface impregnated with the partially gelled resin is pressed against a wood surface at high temperature to obtain decorative wood. This wood is used to make furniture, furniture coverings, flooring wood, floating floors, laminate floors, doors and all types of coverings. Other substrates that are not natural wood can also be used.

[0015] The decorative color on the wood surface is provided by the color and design of the impregnated paper; this is why it is so important that the surface left by the resin is transparent. A wide variety of colors exist, ranging from white to black, with a range of colors and designs that imitate various types of wood (cedar, pine, cherry, etc.) and other patterns.

[0016] Heat-stable plastics such as melamine formaldehyde (MF), urea formaldehyde (UF), phenol formaldehyde (PF), melamine urea formaldehyde (MUF) and phenolic resins can also be used for other purposes such as household items (plates, cutlery, cups), electrical items (plates, plugs, switches), bathroom items (toilet seats), door handles, containers, and decorative items using molding techniques and adhesives.

[0017] The amount of melamine formaldehyde, urea formaldehyde and phenolic resins applied to the surface depends on each application. In the case of paper, it varies between 10 and 200 grams per square meter of surface; the most commonly used amount in the industry is 30 to 120 grams per square meter.

[0018] In resin applications, catalysts are used to promote polymerization. Typically, polymerization is carried out at temperatures between 100°C and 250°C. The time for polymerization at a temperature of 100°C is called the gelation (curing) time. This can vary from a few seconds to a few minutes. For example, melamine formaldehyde resin does not polymerize when heated at 100°C without a catalyst; it can be heated for a long time (20 to 30 minutes) without reaction. In addition, melamine and urea resins have not polymerized for up to 30 to 45 days under ambient conditions.

[0019] The gel time of the mix is ​​very important for its final application. In the case of decorative molding, a short gel time is required. In the case of application on paper for pressing to wood or other materials, the gel time should be more than 3 minutes, ideally between 5 and 7 minutes.

[0020] Another important variable in resin polymerization is pH. In the case of melamine formaldehyde resin polymerization, the environment should be alkaline, ideally with a pH above 8.9, so any additives added to the resin, such as dust suppressants, defoamers, and additives to improve flexibility, should not lower the pH from 8.9.

[0021] Typically, microorganisms, such as bacteria, fungi, etc., tend to nest on surfaces that provide a habitat for feeding and reproduction. Microorganisms can survive on surfaces for a long time and spread infection by contact. Melamine-formaldehyde, urea-formaldehyde and phenolic surfaces are not exempt from this and they become carriers of infection, such as in the case of furniture with such resin surfaces, which are installed in hospitals, kitchens, wardrobes, floors, offices and other locations. Microorganisms living on these surfaces can be transferred to humans through contact and / or food placed on these surfaces and cause infection. This also occurs with decorative surfaces made of these materials.

[0022] The goal is therefore to convert these resin surfaces into biocidal surfaces, ie to eliminate microorganisms that come into contact with them and to keep the surfaces free of microorganisms that can cause infection by contact.

[0023] It would therefore be desirable to have biocide compounds based on melamine formaldehyde, urea formaldehyde and phenolic resins and soluble copper salts that are suitable for use with different materials as well as in a stand-alone manner.

[0024] One of the objects of the present invention is to obtain a biocide material comprising at least one layer formed by melamine formaldehyde, urea formaldehyde, phenol formaldehyde, melamine urea formaldehyde and phenolic resin, with the addition of a soluble copper salt, and a second layer formed by paper or other support.

[0025] Another object of the present invention is to obtain a molded biocide product comprising at least one resin in powder form selected from melamine formaldehyde, urea formaldehyde, phenol formaldehyde, melamine urea formaldehyde and phenolic resins, and one or more powdered copper salts.

[0026] Furthermore, it is sought that the gelling time for melamine formaldehyde resins is in the range of 5 to 10 minutes; for urea formaldehyde resins, 0.5 to 2 minutes; and for phenolic resins, 3 to 10 minutes. Summary of the invention

[0027] The present invention corresponds to a resin biocide composition, comprising one or more solutions selected from melamine formaldehyde, urea formaldehyde, phenol formaldehyde, melamine urea formaldehyde and phenolic resins, and one or more copper salts soluble in aqueous systems and melamine formaldehyde, urea formaldehyde, and phenolic solutions. The copper salt is copper citrate, copper lysine, copper gluconate, copper salicylate (salicinato de cobre), copper phthalocyanine, copper chelate, copper oxalate, copper acetate, copper methionine, copper tartrate, copper glycinate, copper picolinate, copper aspartate, ammonia copper complex, EDTA (ethylenediaminetetraacetic acid)-copper complex, glycolate copper (glicinato de cobre), glycerol copper, ascorbate copper type, and is generally an organic copper salt, R-Cu, R1-Cu-R2, wherein R, R1 and R2 can be an alkyl chain (C3-C4) having one or more acid, aldehyde, ester, ether, hydroxyl, amino or other groups in its structure. 18 ).

[0028] In addition, the present invention corresponds to a molded biocide product, which includes one or more powdered resins for molding, selected from melamine formaldehyde, urea formaldehyde, phenol formaldehyde, melamine urea formaldehyde and phenolic resins, and one or more powdered copper salts soluble in aqueous systems and melamine formaldehyde, urea formaldehyde and phenolic solutions. The copper salt is copper citrate, copper lysine, copper gluconate, copper salicylate, copper phthalocyanine, copper chelate, copper oxalate, copper acetate, copper methionine, copper tartrate, copper glycinate, copper picolinate, copper aspartate, ammonia copper complex, EDTA (ethylenediaminetetraacetic acid)-copper complex, glycolate copper, glycerol copper, ascorbate copper type, and is generally organic copper salt, R-Cu, R1-Cu-R2, wherein R, R1 and R2 can be alkyl chains (C3-C4) having one or more acid, aldehyde, ester, ether, hydroxyl, amino or other groups in its structure. 18 ).

[0029] Furthermore, the present invention describes a process for obtaining the resin biocide composition. DETAILED DESCRIPTION

[0030] The present invention corresponds to a resin biocide composition, comprising one or more resins selected from melamine formaldehyde (MF), urea formaldehyde (UF), phenol formaldehyde (PF), melamine urea formaldehyde (MUF) and phenolic resins, and one or more copper salts soluble in aqueous systems and melamine formaldehyde, urea formaldehyde, and phenolic solutions. The copper salt is copper citrate, copper lysine, copper gluconate, copper salicylate, copper phthalocyanine, copper chelate, copper oxalate, copper acetate, copper methionine, copper tartrate, copper glycinate, copper picolinate, copper aspartate, ammonia copper complex, EDTA (ethylenediaminetetraacetic acid)-copper complex, glycolate copper (copperglycolate), glycerol copper, ascorbate copper type, and generally, organic copper salts, R-Cu, R1-Cu-R2, wherein R, R1 and R2 can be alkyl chains (C3-C4) having one or more acid, aldehyde, ester, ether, hydroxyl, amino or other groups in its structure. 18 ).

[0031] The present invention corresponds to a resin biocide composition comprising adding a resin as a resin solution, and a copper salt as an aqueous solution containing the copper salt.

[0032] The present invention corresponds to a resin biocide composition, comprising an added resin as a resin in powder form, and a copper salt in powder form.

[0033] The copper salts are in combinations of two or more, preferably two or three. The copper salts are added to the resin in an amount such that the copper ion concentration in the finished resin biocide composition is between 20 and 2500 ppm (parts per million), and preferably between 100 and 1000 ppm. The finished resin biocide composition refers to the powder composition obtained once the copper salt is mixed with the resin or to the dry composition, which corresponds to the biocide composition in the resin solution once water has evaporated from the resin solution mixture and from the copper salt solution.

[0034] In the case of resin biocide compositions in solution, the copper salt dissolves to form an aqueous solution having a pH in the range of 3.8 to 5.5, so that when mixed with melamine formaldehyde, urea formaldehyde, phenol formaldehyde, melamine urea formaldehyde and phenolic solutions, the pH in the resin solution is not significantly changed. If applicable, a base or a weak acid is used to adjust the pH. Preferred acids are citric acid, tartaric acid, acetic acid, preferably of organic origin; preferred bases are ammonium hydroxide, methylamine, ethylamine, propylamine, preferably of organic origin.

[0035] The process of obtaining a resin biocide composition in solution comprises mixing one or more copper salts, in which the copper salt is soluble, with a resin solution, which contains one or more resin solutions before the gelation process ("polymerization"). The copper salts contained in the resin solution are added as an aqueous solution and they remain evenly distributed in the resin and are captured (interlocked) by the resin polymer network during the polymerization process. In the copper salts, the free radicals R of the carbon chains with carboxyl, acid, amine and hydroxyl groups are interwoven with the polymer to form a single structure, preventing them from falling off. In addition, catalysts suitable for each resin can also be used, such as p-toluenesulfonic acid solutions for melamine formaldehyde resins and salts from strong acids for urea-formaldehyde resins, preferably aluminum chloride or ammonium sulfate. Catalysts are usually necessary during the resin polymerization or gelation stage.

[0036] The copper salt used does not change the resin polymerization (gelation) rate, which means that there is no need to change the process. Optionally, it would be recommended to use a chelating agent in a molar ratio from 1 / 2 to 1 / 50 to keep the copper ions in solution and prevent their precipitation. Preferably, the chelating agents are EDTA and DTPA (diethylenetriaminepentaacetic acid).

[0037] Generally, the surface formed by the polymerization of these resins is solid, transparent, anti-fouling, easy to clean, high in hardness, resistant to alkali and acid, and resistant to high temperatures.

[0038] The process of obtaining the powder resin composition includes mixing the powder resin and the powder copper salt into a uniform mixture, and then molding at a temperature of 100° C. to 250° C. and a pressure of 50 to 400 atm. Then, the molding mixture is pressurized for 1 to 10 minutes to obtain a molded final product.

[0039] One application of these highly important resin biocide compositions is to obtain boards with decorative surfaces made of resin impregnated paper. The boards can be medium density fiberboard, medium density plywood, etc. These are used in the manufacture of furniture, cabinets, kitchen surfaces and other applications. In case the boards are made by laminating urea and then melamine resin, the copper salt can be applied to both resins or only to the resin on the outer surface.

[0040] Other applications of the resin biocide composition of the invention correspond to floating floors, decorative floors, and paper with decorative patterns (impregnated in resin), usually the aqueous resin solution contains a catalyst that promotes polymerization (commonly known as resin gelation). These articles are then placed at a temperature between 80°C and 250°C to allow polymerization to occur on the surface and for water to evaporate from the resin biocide composition solution.

[0041] In addition, another application of the resin biocide composition of the present invention corresponds to obtaining a board based on paper impregnated with the resin composition of the present invention. Obtaining the board includes pressing a paper with a polymeric resin on both sides of a wood substrate under high pressure and temperature. This can be a fiberboard or a plywood. In the case of melamine resin, the resulting board surface has the characteristics of high hardness, waterproof, easy to clean, high temperature resistant, and alkali and acid resistant. In addition, these boards have the characteristics of removing bacteria, fungi and viruses contacted with these surfaces in a very short time, preventing their growth and removing the biocide characteristics of the infection carrier. This is a very desirable characteristic in areas where there may be microorganisms that can infect people, such as other surfaces of furniture, desks, school furniture and hospital areas.

[0042] The paper used for impregnation is porous, ranging from 10g / m 2 Up to 200g / m 2 Usually, the paper is 30 to 120 g / m 2 The resin biocide solution of the present invention, i.e., melamine formaldehyde, urea formaldehyde, phenol formaldehyde, melamine urea formaldehyde resin and phenolic resin, is forced to penetrate the paper pores by rollers. These rollers can control the amount of resin remaining on the paper. The amount of resin on the paper can be from 20 to 120 g / m 2 Changes, distributed on both sides of the paper.

[0043] Coated wood is produced from impregnated paper, which comprises a surface layer and a substrate. The surface layer is formed by impregnating paper in a resin biocide solution and the substrate is wood.

[0044] Another application of the resin composition in solution of the present invention includes applying the composition to another type of substrate, such as ceramics, polymer sheets, and paperboard.

[0045] Furthermore, another application of the resin composition is toilet seats, door handles, containers, furniture parts, kitchen utensils, and bathroom accessories obtained by a powder resin molding process.

[0046] Additionally, the resin biocide composition can be used to protect adhesive mixtures, melamine urea formaldehyde mixtures, phenol-melamine formaldehyde and phenol-urea-formaldehyde mixtures by itself or with additives such as starch, cellulose, or other substances from microbial action but excluding catalysts.

[0047] Furthermore, the resin biocide composition, both in solution and in powder form, includes added additives which may be dust suppressants, humectants and defoamers, agents promoting flexibility, mold release agents, agents preventing (sheet-to-sheet) surface adhesion, fillers, adsorbents, agents increasing hardness, bleaching agents, colorants, pigments and other agents.

[0048] Alternatively, the addition of the antimicrobial agent can be carried out by adding the copper salt directly to the resin solution.

[0049] The addition of copper salts does not change the gel time (polymerization) of the resin at normal operating temperatures.

[0050] Embodiment 1:

[0051] Paper surfaces were prepared with melamine resin and copper and then subjected to a challenge test to measure the antimicrobial activity. The test used was the International Standard ISO 22196 (ISO 22196-2007) (E). First edition 2007-10-15. "Plastics - Measurement of antimicrobial activity on plastic surfaces".

[0052] Antimicrobial activity measurements were performed using a prototype strain of methicillin-resistant Staphylococcus aureus (MRSA) ATCC-43300.

[0053] Use standard 80 g / m 2 The porous paper produces a melamine surface.

[0054] A solution based on 50% melamine formaldehyde was prepared. Several biocide solutions for testing were prepared with copper salts at different copper concentrations. Then, several mixtures were prepared based on the melamine formaldehyde solution and the copper salt solution, and 0.797 parts of the copper salt solution were added to every 100 parts of each of the mixtures. In addition, the melamine formaldehyde resin biocide composition included a melamine catalyst (CYTEC's CYCAT 400, equivalent to p-toluenesulfonic acid solution) and some additives, such as a humectant (Alton 833), a mold release agent (Alton R1000), an anti-adhesion agent (Alton AT837), and a dust suppressant (Alton AP100). Table 1 lists each component or ingredient that forms the resin biocide composition and indicates its content in the total mixture.

[0055] Table 1: Resin biocide compositions for paper impregnation

[0056] Element Number of copies Resin: Melamine formaldehyde (50%) 93.81 Additive water 4.065 Moisturizer 0.125 catalyst 0.344 Release agent 0.281 Anti-adhesion agent 0.281 Dust Repellent 0.297 Disinfectant solution 0.797

[0057] Aqueous fungicidal solutions containing copper salts were prepared by mixing two and three different types of copper salts. The copper salts were mixed in different molar ratios to obtain fungicidal solutions of different concentrations. Table 2 shows each salt mixture prepared, represented by the letters B, C, D, E, F, G, H, Y and J. The letter A represents a control solution without copper salt.

[0058] Table 2: Prepared copper salt solutions and their different concentrations in ppm

[0059] test Copper salts in fungicide solutions Salt molar ratio in fungicide solution (Cu) Copper ions ppm present in finished resin biocide composition (solid resin) A None (control) 0 B Copper Gluconate Copper Glycinate 3 / 1 100 C Same as B 3 / 1 200 D Same as B 3 / 1 500 E Same as B 1 / 1 150 F Same as B 1 / 3 150 G Copper Gluconate Copper Citrate 1 / 1 500 H Copper Glycinate Copper Citrate 1 / 1 1000 I Copper salicylate Copper lysinate 4 / 1 1000 J Copper Gluconate Copper Glycinate Copper Lysinate 3 / 1 / 1 500

[0060] As shown in Table 2, nine copper salt solutions were prepared, varying the type of copper salt added, the total amount of copper salt added, the molar ratio between the copper salts, and the copper ppm to obtain solid resin. The B, C, and D fungicide solutions included the same copper salts and the same molar ratio between them, but the copper ppm obtained in the solid resin was different, i.e., the actual amount of each copper salt added to the fungicide solution by weight was different to obtain different copper ppm in the solid resin. Table 2 does not show the actual amount of copper salt parts by weight added to obtain the corresponding copper ppm in the solid resin; however, the following is a method for calculating the actual amount of copper salt parts by weight in each case.

[0061] The following example is a calculation showing the amount of copper salt by weight that should be added to a copper salt fungicide solution prepared to obtain 100 ppm copper in solid resin (Test B). For clarity, X is defined as the amount of copper gluconate by weight, and Y is defined as the amount of copper glycinate by weight that should be added to the copper salt solution to obtain 100 ppm copper in solid resin.

[0062] According to the biocide composition formula of the resin in Table 1, 93.81 parts of 50% (in solution) melamine formaldehyde were added to the total mixture. This means that 46.905 parts of solid resin (93.81 x 0.5) were actually added.

[0063] Considering that the amount of solid resin is equal to 46.905 parts, this means that if one wants to prepare a solution of 100 ppm copper in solid resin, one should add 0.0046905 parts of copper to every 46.905 parts of solid resin:

[0064]

[0065]

[0066] Copper parts = 0.0046905

[0067] In Test B (Table 2), the copper salts used were copper gluconate and copper glycinate, and their molecular weights were 453.8 Kg / Kgmole and 211.66 Kg / Kgmole, respectively. On the other hand, the atomic weight of copper is 63.546. The atomic weight of copper, together with the salt molecular weight, calculates the amount of copper per mole of copper salt molecules.

[0068] Copper gluconate 63.546 / 453.8 = 0.14

[0069] Copper glycinate 63.546 / 211.66 = 0.3

[0070] Thus, one mole of copper gluconate contains 0.14 parts of copper, and one mole of copper glycinate contains 0.3 parts of copper.

[0071] Considering that the total copper parts added to obtain 100 ppm copper in the solid resin is 0.0046905, i.e., 0.14 parts of copper per mole of copper gluconate molecules and 0.3 parts of copper per mole of copper glycinate molecules, and the molar ratio of copper gluconate / copper glycinate is 3 / 1 (see Table 2), the values ​​of X and Y can be calculated with certainty:

[0072] 0.14X + 0.3Y = 0.0046905

[0073] (X / 453.8) / (Y / 211.66) = 3 / 1

[0074] Solution: We get: X = 0.02515

[0075] Y = 0.00391 parts

[0076] Therefore, to obtain 0.707 parts of the fungicide solution (Table 1), 0.02515 parts of copper gluconate, 0.00391 parts of copper glycinate and 0.76794 parts of water need to be added.

[0077] Additionally, in the case of Test J (500 ppm copper in solid resin when copper gluconate / copper glycinate / copper lysinate were mixed in a 3 / 1 / 1 molar ratio), the amounts of copper gluconate (X), copper glycinate (Y) and copper lysinate (Z) by weight were:

[0078]

[0079]

[0080] Copper parts = 0.0234525

[0081] Copper gluconate 63.546 / 453.8 = 0.14

[0082] Copper glycinate 63.546 / 211.66 = 0.3

[0083] Copper lysinate 63.546 / 355.5 = 0.179

[0084] 0.14X + 0.3Y + 0.179Z = 0.0234525

[0085] (X / 453.8) / (Y / 211.66) = 3 / 1

[0086] (X / 453.8) / (Z / 355.5) = 3 / 1

[0087] Solving, we get: X = 0.10049 parts

[0088] Y = 0.01562 parts

[0089] Z = 0.02624 copies

[0090] Thus, to obtain 0.797 parts of the fungicide solution (Test J, Table 1), 0.10049 parts of copper gluconate, 0.01562 parts of copper glycinate, 0.02624 parts of copper lysinate, and 0.65465 parts of water should be added.

[0091] Thereafter, each of the prepared resin biocide compositions was impregnated on paper. Each paper was impregnated with 40 g / m2 of the prepared resin biocide composition.

[0092] The impregnated paper was dried at 100°C and then pressed onto wood to form the melamine surface. The wood melamine surface was subjected to the above microbiological challenge to measure its antimicrobial activity.

[0093] Table 3 below shows the surface antimicrobial results measured as percent MRSA elimination.

[0094] Table 3: MRSA removal on paper surface (melamine surface)

[0095] test Cu ppm in finished resin biocide composition (melamine formaldehyde resin) MRSA removal % on paper surface (melamine surface) A 0 -65% B 100 85% C 200 98% D 500 100% E 150 94% F 150 92% G 500 88% H 1,000 99% I 1,000 100% J 500 100%

[0096] The control sample has a negative percentage, i.e., MRSA bacteria multiply on the melamine surface formed by the biocide composition of melamine formaldehyde resin without copper salt solution. On the other hand, all melamine surfaces formed with the biocide composition of melamine formaldehyde resin with copper salt solution showed the elimination of MRSA bacteria; even D, I and J solutions showed 100% elimination of MRSA bacteria.

[0097] Embodiment 2:

[0098] Paper surfaces treated with urea-formaldehyde resin compositions and copper solutions were prepared and tested to measure antimicrobial activity. The test used was International Standard ISO 22196 (ISO 22196-2007) (E). First edition 2007-10-15. "Plastics - Measurement of antimicrobial activity on plastic surfaces".

[0099] The antibacterial activity was measured using the prototype strain of Escherichia coli, ATCC-25922.

[0100] Use 80 g / m 2 of porous paper.

[0101] The resin biocide composition is prepared based on 50% urea-formaldehyde resin and copper salt. In addition, the resin biocide composition includes a urea catalyst corresponding to a salt of a strong acid, preferably aluminum chloride or ammonium sulfate. The components of the resin biocide composition are listed in Table 4, expressed in terms of their content in the total mixture.

[0102] Table 4: Resin biocide compositions for paper impregnation

[0103] Element Number of copies Urea-formaldehyde solution (50%) 85.370 water 13.390 catalyst 0.385 Disinfectant solution 0.855

[0104] Urea-formaldehyde resin solutions were prepared and aqueous solutions containing copper salts were added. Solutions were prepared to add 0.855 parts of the tested fungicide solutions (copper salt solutions) to the urea-formaldehyde solution. Several biocide resin compositions were prepared, each with a different copper ion concentration. Table 5 lists the different fungicide solutions (copper salt solutions) prepared and is represented by the letters B2, C2, D2, E2 and F2. The letter A2 represents a control solution without copper salts.

[0105] Table 5: Prepared copper salt solutions and their different concentrations in ppm

[0106] test Copper salts in fungicide solutions Salt molar ratio in fungicide solution (Cu) Copper ions ppm present in finished resin biocide composition (solid resin) A2 None (control) 0 B2 Copper Gluconate Copper Glycinate 3 / 1 100 C2 Copper Gluconate Copper Citrate 1 / 1 500 D2 Copper Glycinate Copper Citrate 1 / 1 1000 E2 Copper salicylate Copper lysinate 4 / 1 1000 F2 Copper Gluconate Copper Glycinate Copper Lysinate 3 / 1 / 1 500

[0107] Thereafter, the paper was impregnated with 50 grams per square meter of the urea-formaldehyde resin biocide composition.

[0108] The impregnated paper was dried at 100°C and then pressed onto wood to form the urea surface. The wood urea surface was subjected to the above microbial challenge to measure its antimicrobial activity.

[0109] Table 6 shows the antimicrobial effect of wood urea surfaces treated with the resin biocide compositions, measured as percentage of E. coli elimination (ATCC-25922).

[0110] Table 6: Removal percentage of Escherichia coli (ATCC-25922) on paper surface (urea surface)

[0111] test Cu ppm in finished biocide composition (urea-formaldehyde resin) % Removal of Escherichia coli (ATCC-25922) on paper surface (urea surface) A2 0 -15% B2 100 80% C2 500 95% D2 1000 100% E2 1000 100% F2 500 100%

[0112] The control sample had a negative percentage, i.e., bacteria colonized the urea surfaces formed by the urea-formaldehyde resin biocide composition without the copper salt solution. On the other hand, all urea surfaces formed with the copper salt solution urea-formaldehyde resin composition were cleared of bacteria of Escherichia coli (ATCC-25922). Even the copper salt solutions D2, E2, and F2 showed 100% bacterial clearance.

[0113] Embodiment 3:

[0114] Paper surfaces treated with melamine formaldehyde resin biocide composition and copper solution were prepared and challenge tested to measure antimicrobial activity. The test used was International Standard ISO 22196 (ISO 22196-2007) (E). First edition 2007-10-15. "Plastics - Measurement of antimicrobial activity on plastic surfaces".

[0115] The antibacterial activity was measured using Escherichia coli, ATCC-25922 prototype strain.

[0116] Use 80 g / m 2 of porous paper.

[0117] A solution was prepared based on melamine formaldehyde, which included 50% melamine formaldehyde. Several biocide solutions were tested with copper salts at different copper concentrations. Then, several mixtures were prepared based on melamine formaldehyde solutions and copper salt solutions, and 0.81 parts of copper salt solution were added to every 100 parts of each of the mixtures. In addition, the resin biocide composition included a melamine catalyst (CYTEC's CYCAT 400, equivalent to p-toluenesulfonic acid solution). Table 7 shows each component or ingredient that forms the resin biocide composition and indicates its content in the total mixture.

[0118] Table 7: Resin biocide compositions for paper impregnation

[0119] Element Number of copies Melamine formaldehyde solution (50%) 94.83 water 4.11 catalyst 0.25 Disinfectant solution 0.81

[0120] Aqueous fungicides containing copper salts were prepared by mixing two different types of copper salts. The copper salts were mixed in different molar ratios to obtain fungicides solutions of different concentrations. Table 8 shows each of the salt mixtures prepared, represented by the letters B3, C3 and D3. The letter A3 represents a control solution without copper salt.

[0121] Table 8: Prepared copper salt solutions and their different concentrations in ppm

[0122] test Copper salts in fungicide solutions Salt molar ratio in fungicide solution (Cu) Copper ions ppm present in finished resin biocide composition (solid resin) A3 None (control) 0 B3 Copper Gluconate Copper Glycinate 3 / 1 100 C3 Copper Gluconate Copper Citrate 1 / 1 500 D3 Copper Glycinate Copper Citrate 1 / 1 1000

[0123] Thereafter, the paper was impregnated with 40 g / m2 of melamine formaldehyde resin.

[0124] The impregnated paper was dried at 100°C and then pressed onto wood to form the melamine surface. The wood melamine surface was subjected to the above microbiological challenge to measure its antimicrobial activity.

[0125] Table 9 below shows the surface antimicrobial results, measured as percent elimination of E. coli (ATCC-25922).

[0126] Table 9: Removal percentage of Escherichia coli (ATCC-25922) on paper surface

[0127] test Finished resin biocide composition (melamine formaldehyde resin) Elimination % of Escherichia coli (ATCC-25922) on paper surface (melamine surface) A3 0 -65% B3 100 85% C3 500 98% D3 1000 100%

[0128] The control sample had a negative percentage of growth of the bacteria Escherichia coli (ATCC-25922) on the melamine surface formed by the melamine formaldehyde resin biocide composition without the copper salt solution.

[0129] Examples 1 and 3 demonstrate that the biocide effect is due to the copper salt and not to the process additive since no additional process additive was included in Example 3 and the results were equivalent to Example 1 which included the use of the process additive.

[0130] Embodiment 4:

[0131] A molded product, also called a plate, of 10×10 cm square and 0.5 cm high was prepared. For this, the already prepared molding mixture, 30% of melamine formaldehyde and 70% of urea formaldehyde (MF-UF), in powder form was used. Powdered copper salt was added and mixed to obtain a uniform mixture. Table 10 shows the components in the resin composition and indicates their content in the total mixture. The mixture was molded at about 170°C and a pressure of about 30 MPa (296 atmospheres). Then, it was pressurized for about 2 minutes to obtain a molded plate.

[0132] Table 10: Powder resin biocide composition

[0133]

[0134] The copper salts were mixed in different molar ratios to obtain powdered resin biocide compositions with different copper salt contents. Table 11 shows each of the prepared salt mixtures, represented by letters B4, C4, D4 and E4. Letter A4 represents a control sample without copper salt.

[0135] Table 11: Prepared copper salt solutions and their different concentrations in ppm

[0136] test Copper salts in fungicide mixtures Salt molar ratio in fungicide mixture (Cu) Copper ions ppm present in finished resin biocide composition (solid resin) A4 Control, no copper 0 B4 Copper Gluconate Copper Glycinate 3 / 1 2000 C4 Copper Gluconate Copper Glycinate 1 / 1 500 D4 Copper tartrate Copper salicylate 1 / 1 1200 E4 Copper Gluconate Copper Lysinate 1 / 1 1500

[0137] The obtained plates were subjected to the microbiological challenge as described in Example 1; MRSA was used to evaluate its effectiveness. The results are shown in Table 12.

[0138] Table 12: MRSA removal percentage on panel surfaces

[0139] test Cu ppm in finished resin biocide composition (solid resin) MRSA removal percentage on the board surface A4 0 -10% B4 2000 99% C4 500 84% D4 1200 100% E4 1500 100%

[0140] The control samples had negative percentages, i.e. MRSA bacteria multiplied on the surface of the plates without copper salts. On the other hand, all plates with copper salts showed MRSA bacteria elimination; even D4 and E4 samples with copper showed 100% MRSA bacteria elimination.

[0141] Embodiment 5:

[0142] As in Example 4, a molded product of 0×10 cm square and 0.5 cm high, also referred to as a plate, was prepared. The molded plate was made of powdered urea-formaldehyde and powdered copper salt. In addition, some additives were included in the mixture, such as a lubricant to help demoulding (zinc stearate), a filler material (cellulose, calcium carbonate, flour, or some mineral compound) and a pigment (titanium dioxide). Table 13 shows the components of the powdered resin composition used for molding and indicates its content in the total mixture. The molding conditions were the same as in Example 4.

[0143] The copper salt corresponds to a mixture of copper gluconate and copper glycinate in a molar ratio of 1:1, tested at two copper ion concentrations, indicated by the letters B5 and C5. The indicated copper ppm corresponds to the copper ppm in the finished resin biocide composition (solid resin, board). In addition, the letter A5 represents the copper salt control sample.

[0144] Table 13: Powder resin biocide composition

[0145] 695 ppm 1,946 ppm Number of copies Copper Free Cu Cu A5 B5 C5 Urea-formaldehyde 67.50 67.50 67.50 Cellulose 30.00 29.50 28.60 Zinc stearate 0.5 0.5 0.5 Titanium Dioxide 2.00 2.00 2.00 Copper salt 0.00 0.50 1.40 total 100.00 100.00 100.00

[0146] The obtained plates were subjected to the microbiological challenge as described in Example 1; MRSA was used to evaluate the effectiveness. Table 14 shows the results.

[0147] Table 14: MRSA removal percentage on panel surfaces

[0148] test Cu ppm in finished resin biocide composition (board) MRSA removal % on board surface A5 0 0% B5 695 90% C5 1946 100%

[0149] The control sample did not eliminate MRSA bacterial growth, as the elimination percentage was equal to zero. On the other hand, the plates with copper salts showed MRSA bacterial elimination; even sample C5 showed 100% MRSA bacterial elimination.

[0150] The obtained sheet can be used to make toilet seats.

[0151] Embodiment 6:

[0152] Melamine formaldehyde and copper salt molding plates were prepared. The plate molding conditions and dimensions were the same as in Examples 4 and 5. The additives in the mixture were the same as in Example 5. Table 15 lists the components forming the molding powder resin composition and indicates their contents in the total mixture.

[0153] The copper salt corresponds to a mixture of copper gluconate and copper glycinate in a molar ratio of 1:1. Two copper ion concentrations corresponding to the letters B6 and C6 were tested. The copper ppm indicated corresponds to the copper ppm in the finished resin biocide composition (solid resin, board). The letter A6 represents a control sample without copper salt.

[0154] Table 15: Powdered resin biocide composition

[0155] Element Copper Free Cu 695 ppm Cu 1,946 ppm A6 B6 C6 Melamine formaldehyde 67.50 67.50 67.50 Cellulose 30.00 29.50 28.60 Zinc stearate 0.50 0.50 0.50 Titanium Dioxide 2.00 2.00 2.00 Copper salt 0.00 0.50 1.40 total 100.00 100.00 100.00

[0156] The obtained plates were subjected to the microbiological challenge as described in Example 1; MRSA was used to evaluate the effectiveness. Table 16 shows the results.

[0157] Table 16: MRSA removal percentage on panel surface

[0158] test Cu ppm in finished resin biocide composition (sheet) MRSA removal % on board surface A6 0 0% B6 695 90% C6 1946 100%

[0159] As in Example 5, the control sample did not eliminate MRSA bacterial growth, as the elimination percentage was equal to zero. On the other hand, the panels with copper salts showed MRSA bacterial elimination; even sample C6 showed 100% MRSA bacterial elimination.

[0160] The results of Examples 5 and 6 allow to conclude that the copper salts have the same independent effect on the resins used, since the percentage of MRSA bacterial elimination is the same in both experiments at the same concentration per plate.

[0161] Embodiment 7:

[0162] Phenolic molding plates were prepared with copper salts. Some additives were added to the mixture, such as lubricants to help demoulding (zinc stearate); filler materials (cellulose, calcium carbonate, flour, or some other mineral compounds); and additives to increase the hardness and water resistance of the resin (hexamine). Table 17 shows the powder resin composition used for molding and indicates its content in the total mixture.

[0163] The copper salt corresponds to a composition of copper gluconate and copper glycinate in a molar ratio of 1:1, which was tested with two copper ion concentrations represented by the letters B7 and C7. The copper ppm shown corresponds to the ppm in the finished resin biocide composition (solid resin, board). The letter A7 represents a control sample without any copper salt.

[0164] The plate molding conditions and dimensions were the same as in Examples 4 and 5.

[0165] Table 17: Powder resin biocide composition

[0166] 695 ppm 1,946 ppm Number of copies Copper Free Cu Cu A7 B7 C7 Phenolic 50.00 50.00 50.00 Cellulose 43.00 42.50 41.60 Hexamine 1.50 1.50 1.50 Zinc stearate 0.50 0.50 0.50 Calcium carbonate 5.00 5.00 5.00 Copper salt 0.00 0.50 1.40 total 100.00 100.00 100.00

[0167] The obtained plates were subjected to the microbiological challenge as described in Example 1; MRSA was used to evaluate the effectiveness. Table 18 shows the results.

[0168] Table 18: MRSA removal percentage on panel surfaces

[0169] test Cu ppm in finished resin biocide composition (sheet) MRSA removal % on board surface A7 0 0% B7 695 91% C7 1946 100%

[0170] As with the results of Examples 5 and 6, the results of Example 7 allow the conclusion to be drawn that the copper salts have the same independent effect on the resins used, since the percentage of MRSA elimination is the same in all examples at the same copper concentration per sheet.

[0171] Embodiment 8:

[0172] The adhesive was prepared based on melamine urea formaldehyde and copper salts.

[0173] A commercially available resin compound was used which was equivalent to applying the IM-300 mixture directly on the wood board without applying the copper salt. Once the IM-300 mixture was applied to the wood, it was left to harden. On the other hand, two IM-300 and copper salt mixtures were prepared (a 1:1 mixture of copper gluconate and copper lysinate in a molar ratio). The copper salt was added to the IM-300 mixture so that there were 750 and 1500 Cu ppm in the adhesive (finished resin biocide composition), i.e., 0.54 parts (B8) and 1.08 parts (C8), respectively. Each of the mixtures was applied to the wood board and left to harden. Table 19 lists each component that forms the resin composition for the adhesive and indicates its content in the total mixture.

[0174] Table 19: Resin biocide composition in mixture for adhesive

[0175] The number of parts in the formula A8 B8 C8 IM-300 100 99.46 98.92 Copper salt 0 0.54 1.08

[0176] The wood panels with dry adhesive on their surface were subjected to the microbiological challenge as described in Example 1; MRSA was used to assess effectiveness. Table 20 shows the results.

[0177] Table 20: Percentage of MRSA removal on wooden surfaces

[0178] test Cu ppm in adhesive (finished resin biocide composition) MRSA removal % on wooden surfaces A8 0 -10% B8 750 93% C8 1500 100%

[0179] Embodiment 9:

[0180] A resin biocide composition was prepared based on a resin solution mixture of about 25% of 50% melamine formaldehyde resin and about 75% of 50% urea formaldehyde, and a copper salt. In addition, the resin biocide composition included a CYTEC CYCAT 400 melamine catalyst, corresponding to p-toluenesulfonic acid, and a urea catalyst corresponding to a strong acid salt, preferably aluminum chloride or ammonium sulfate. The copper salt corresponded to a 1:1 molar mixture of copper gluconate and copper glycinate, tested with two copper ion concentrations represented by the letters B9 and C9. The letter A9 represents the neutralized solution without any copper salt. The components forming the resin biocide composition, indicating their content in the total mixture, are all found in Table 21.

[0181] Table 21: Resin biocide compositions for paper impregnation

[0182] Element Copper Free 953 Cu ppm 1974 Cu ppm Number of copies Number of copies Number of copies A9 B9 C9 Melamine formaldehyde (55%) 24.92 24.86 24.80 Melamine catalyst 0.08 0.08 0.08 Urea formaldehyde (55%) 74.58 74.40 74.20 Urea Catalyst 0.42 0.42 0.42 Copper Gluconate 0.00 0.12 0.25 Copper Glycinate 0.00 0.12 0.25 total 100.00 100.00 100.00

[0183] Thereafter, the paper was impregnated with 40 g / m2 of the prepared resin biocide composition.

[0184] The impregnated paper was dried at 100°C and then pressed onto wood to form the melamine urea surface. The wood melamine urea surface was subjected to microbiological tests according to Example 1 to measure its antimicrobial activity.

[0185] Table 22 shows the surface antimicrobial efficacy, measured as percent MRSA elimination.

[0186] Table 22: Percentage of MRSA removal on paper surfaces

[0187] test Cu ppm in finished resin biocide composition (MF-UF resin) MRSA removal % on paper surface (melamine urea surface) A9 0 -15% B9 952 96% C9 1974 100%

[0188] Embodiment 10:

[0189] Preparation of melamine formaldehyde and copper salt molding plates. The plate molding conditions and dimensions were the same as in Examples 4 and 5. Table 23 lists the components that formed the molding mixture. In this experiment, only the homogeneously mixed resin and copper salt were molded.

[0190] The copper salt corresponds to a 1:1 mixture of copper gluconate and copper glycinate in a molar ratio, and is tested with two copper ion concentrations, denoted by the letters B10 and C10. The letter A10 represents a control sample without any copper salt.

[0191] Table 23: Powder resin biocide components

[0192] Element Copper Free 956 Cu ppm 2493 Cu ppm A10 B10 C10 Melamine formaldehyde 100 99.5 98.7 Copper salt fungicide mixture 0 0.5 1.3 total 100 100 100

[0193] The copper ppm was calculated based on the copper contribution from each salt and referenced to the solid resin.

[0194] The obtained plates were subjected to the microbiological challenge as described in Example 1; MRSA was used to evaluate the effectiveness. Table 24 shows the results.

[0195] Table 24: MRSA removal percentage on panel surfaces

[0196] test Cu ppm in finished resin biocide composition (board) MRSA removal % on plate surface A10 0 0% B10 959 91% C10 2493 100%

[0197] The control sample did not eliminate MRSA bacterial growth, as its elimination percentage was equal to zero. On the other hand, the plates with copper salts showed MRSA bacterial elimination; even sample C10 showed 100% MRSA bacterial elimination.

Claims

1. A resin biocide composition, It is characterized in that include: A resin selected from melamine formaldehyde resin or urea formaldehyde resin; A combination of two or three different organic copper salts selected from the following: Copper gluconate-copper glycinate at a molar ratio of 3:1, copper gluconate-copper glycinate at a molar ratio of 1:1, copper gluconate-copper glycinate at a molar ratio of 1:3, copper gluconate-copper citrate at a molar ratio of 1:1, copper glycinate-copper citrate at a molar ratio of 1:1, copper salicylate-copper lysinate at a molar ratio of 4:1, copper tartrate-copper salicylate at a molar ratio of 1:1, copper gluconate-copper lysinate at a molar ratio of 1:1, and copper gluconate-copper glycinate-copper lysinate at a molar ratio of 3:1:1, wherein each of the two or three different organic copper salts in the combination is soluble in an aqueous system as well as a melamine formaldehyde resin solution and a urea formaldehyde resin solution; a catalyst for the resin solution; Defoaming agents; as well as Optionally one or more additives selected from the group consisting of dust suppressants, moisturizers, agents that promote flexibility, mold release agents, agents that prevent surface adhesion, fillers, adsorbents, and bleaching agents; wherein the resin is in the form of a resin solution, and the organic copper salt is in the form of an aqueous solution containing the organic copper salt; wherein when the solution of the combination of two or three different organic copper salts and the resin solution are mixed, a homogeneous mixture is obtained, and When the resin biocide composition is a dry composition, the concentration of copper ions in the resin biocide composition is between 20 and 2500 ppm.

2. The resin biocide composition according to claim 1, It is characterized in that The organic copper salt is dissolved prior to incorporation to form an aqueous solution and then brought to a pH between 3.8 and 5.

5.

3. The resin biocide composition according to claim 1, It is characterized in that The concentration of organic copper ions in the finished resin biocide composition is between 100 and 1000 ppm.

4. The resin biocide composition according to claim 1, It is characterized in that The catalyst is selected from p-toluenesulfonic acid solution for melamine formaldehyde resin and aluminum chloride or ammonium sulfate for urea formaldehyde resin.

5. A process for producing a resin biocide composition, It is characterized in that include: a) having a resin solution selected from melamine formaldehyde resin or urea formaldehyde resin; b) a solution having a combination of two or three different organic copper salts selected from copper gluconate-glycinate at a molar ratio of 3:1, copper gluconate-glycinate at a molar ratio of 1:1, copper gluconate-glycinate at a molar ratio of 1:3, copper gluconate-citrate at a molar ratio of 1:1, copper glycinate-citrate at a molar ratio of 1:1, copper salicylate-lysinate at a molar ratio of 4:1, copper tartrate-salicylate at a molar ratio of 1:1, copper gluconate-lysinate at a molar ratio of 1:1, and copper gluconate-glycinate-lysinate at a molar ratio of 3:1:1, wherein each of the two or three different organic copper salts in the combination is soluble in an aqueous system as well as a melamine formaldehyde solution and a urea-formaldehyde solution; c) mixing the organic copper salt; d) bringing together the organic copper salt and a resin; and e) adding a defoaming agent; and optionally one or more additives selected from the group consisting of dust suppressants, moisturizers, agents promoting flexibility, mold release agents, agents preventing surface adhesion, fillers, adsorbents, and bleaching agents.

6. A process for producing a resin biocide composition according to claim 5, It is characterized in that The two or three different organic copper salts are dissolved to form an aqueous solution and a pH between 3.8 and 5.5 is produced before being incorporated into the resin solution.

7. A process for producing a resin biocide composition according to claim 6, It is characterized in that Acids and bases are used to adjust pH.

8. A process for producing a resin biocide composition according to claim 7, It is characterized in that The acid is of organic origin.

9. A process for producing a resin biocide composition according to claim 7, It is characterized in that The acid is selected from citric acid, tartaric acid and acetic acid.

10. A process for producing a resin biocide composition according to claim 7, It is characterized in that The base is of organic origin.

11. A process for producing a resin biocide composition according to claim 7, It is characterized in that The base is selected from ammonium hydroxide, methylamine, ethylamine, and propylamine.

12. A process for producing a resin biocide composition according to any one of claims 5 to 11, It is characterized in that During polymerization or gelation, the organic copper salt contained in the solution is uniformly distributed in the resin and captured by the polymer network.

13. A process for producing a resin biocide composition according to any one of claims 5 to 11, It is characterized in that A catalyst selected from p-toluenesulfonic acid solution for melamine formaldehyde resins and aluminum chloride or ammonium sulfate for urea formaldehyde resins is additionally used.

14. A process for producing a resin biocide composition according to claim 13, It is characterized in that Catalysts are necessary during the polymerization or gelation stage of the resin.

15. A process for producing a resin biocide composition according to any one of claims 5 to 11, It is characterized in that A chelating agent is optionally used in a molar ratio of from 1 / 2 to 1 / 50 to keep the organic copper ions in solution and prevent their precipitation.

16. A process for producing a resin biocide composition according to claim 15, It is characterized in that The chelating agent is selected from EDTA (ethylenediaminetetraacetic acid) and DTPA (diethylenetriaminepentaacetic acid).

17. Use of the resin biocide composition according to any one of claims 1 to 4, It is characterized in that It is used to obtain resin-impregnated paper, boards covered with said paper, polymer sheets, resin-covered paperboards and resin-covered ceramics.

18. Use of the resin biocide composition according to any one of claims 1 to 4, It is characterized in that It is used to obtain floating floors, decorative floors and paper with decorative patterns impregnated with the resin composition.

19. Use of the resin biocide composition according to any one of claims 1 to 4, It is characterized in that It is used in adhesive mixtures.

20. Use of the resin biocide composition according to any one of claims 1 to 4, It is characterized in that It is used to make toilet seats, door handles, containers, furniture components, kitchen utensils and bathroom accessories.

21. A process for obtaining a paper covered board impregnated with a resin biocide composition, It is characterized in that It comprises impregnating paper with the resin biocide composition of any one of claims 1 to 4, drying the paper at a temperature of 100° C. to 250° C., and pressing the impregnated paper onto the board.

22. Process for obtaining a paper covered board impregnated in a resin biocide composition according to claim 21, It is characterized in that The paper used for impregnation is porous and has a thickness between 10 g / m 2 Up to 200g / m 2 .

23. Process for obtaining a paper covered board impregnated in a resin biocide composition according to claim 22, It is characterized in that Paper used for impregnation ranges from 30 to 120 g / m 2 .

24. A process for obtaining a paper covered board impregnated in a resin biocide composition according to claim 22, It is characterized in that A roller was used to force the resin biocide composition to penetrate the paper pores.

25. Process for obtaining a paper covered board impregnated in a resin biocide composition according to claim 24, It is characterized in that The amount of the resin biocide composition on the paper is from 20 to 120 g / m 2 Changes, distributed on both sides of the paper.

26. A board covered with paper impregnated with a resin biocide composition, It is characterized in that Comprising a surface layer and a substrate, wherein the surface layer is formed by impregnating paper in the resin biocide composition of any one of claims 1 to 4 and the substrate is a board.

27. A process for producing a product having biocide properties, It is characterized in that The homogeneous mixture obtained by the resin biocide composition according to any one of claims 1 to 4 is molded at a molding temperature of 100 to 250° C. and at a pressure of 50 to 400 atm.

28. Process for producing a product having biocide properties according to claim 27, It is characterized in that The molded mixture is pressed for 1 to 10 minutes to obtain a molded product.