Transparent conductive film and preparation method thereof, and light transmission control device and preparation method thereof
Through the combination of copper-reduced graphene oxide-core-shell nanowire film with a transparent substrate and a polymer matrix layer, the problem that the existing transparent conductive film cannot simultaneously meet the requirements of light transmittance, conductivity, flexibility and cost is solved, achieving Efficient light control device applications.
Patent Information
- Application Number
- CN201710898772.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2017-09-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2037-09-28
AI Technical Summary
Existing transparent conductive films cannot meet the requirements of good light transmittance, conductivity, flexibility and cost at the same time, which limits their wide application in optoelectronic devices and light control devices.
A copper-reduced graphene oxide-core-shell nanowire film is used as a transparent conductive film, combined with a transparent substrate and a polymer matrix layer, and a flexible film with high light transmittance and low resistance is prepared through a specific deposition and reduction process. Application in optical transmission control devices.
It achieves high transmittance and conductivity of the transparent conductive film while ensuring flexibility and low cost, and improves the switching stability and reversibility of the light control device.
Smart Images

Figure CN107765451B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of thin film technology, and in particular to a transparent conductive film and a preparation method thereof, and a light transmission control device and a preparation method thereof. Background Art
[0002] Transparent conductive film (TCF) is a thin film that allows photons to pass or transmit optically (i.e. transparent) and allows electrons to pass or transmit electrically (i.e. conductive). Therefore, transmittance and conductivity are two technical characteristics of transparent conductive films, and the conduction of photons and electrons is very important for many optoelectronic devices, such as displays (liquid crystal displays (LCDs), inorganic light-emitting diodes (LEDs) and organic light-emitting diodes (OLEDs)), photovoltaic devices, touch screens and electrochromic glass. In these devices, TCF acts as an electrode, and when the optoelectronic element is excited by electrons or photons, the excited photons are injected and exported through the electrodes.
[0003] In some applications, electrons are injected into the active components of the device, and the active components convert the electron energy into photons, which then emit light through transparent electrodes, such as LED and OLED devices. In some other applications, photons are injected into the active components of the device through transparent electrodes, and the active components are excited to convert the photons into charges, which are collected by electrodes in the device (such as photovoltaic devices and photoelectric sensors). In addition, there are some applications in which a chemical reaction occurs in the active components of the sandwich by applying a voltage between two electrodes and generating an electromagnetic field. In view of the wide application of transparent conductive films, the requirements for them are not only good transmittance and conductivity, but also flexibility, stability and cost. However, the transparent conductive films in the prior art cannot meet the above requirements at the same time. Summary of the invention
[0004] In view of the above problems, a transparent conductive film and a method for preparing the same, and a light transmission control device and a method for preparing the same are proposed in the present invention so as to simultaneously meet the above requirements.
[0005] According to one aspect of the present invention, there is provided a transparent conductive film, the transparent conductive film comprising: a transparent substrate and a copper-reduced graphene oxide-core-shell nanowire film;
[0006] The copper-reduced graphene oxide-core-shell nanowire film is deposited on the transparent substrate.
[0007] Optionally, the transparent substrate is glass or polymer.
[0008] Optionally, the copper-reduced graphene oxide-core-shell nanowire film has a thickness of 50 nanometers to 250 nanometers.
[0009] Optionally, the copper-reduced graphene oxide-core-shell nanowire film has a light transmittance of 75%-95%.
[0010] Optionally, the sheet resistance of the copper-reduced graphene oxide-core-shell nanowire film is 10 ohms to 100 ohms.
[0011] Optionally, a light transmission control device comprises: a first transparent conductive film, a second transparent conductive film, and a polymer matrix layer filled between the first transparent conductive film and the second transparent conductive film;
[0012] The first transparent conductive film and / or the second transparent conductive film is the transparent conductive film as described above, and the polymer matrix layer is filled between the copper-reduced graphene oxide-core-shell nanowire film of the first transparent conductive film and the copper-reduced graphene oxide-core-shell nanowire film of the second transparent conductive film.
[0013] Optionally, the polymer matrix layer comprises a polymer base material and a plurality of suspended particles, each of the suspended particles comprises a suspension medium and a plurality of light polarizing particles;
[0014] The suspension medium material of the suspended particles is different from the polymer matrix material, and the suspended particles are suspended in the polymer matrix material in a liquid or gel form.
[0015] Optionally, the polymer matrix material is cross-linked polysiloxane or acrylate; if the polymer matrix material is acrylate, the suspension medium material of the suspended particles is silicone oil or isotridecyl trimellitate;
[0016] The light polarizing particles of the suspended particles are polyhalides, titanium dioxide, or quinine iodide sulfate.
[0017] Optionally, each of the light polarizing particles has a length of 100 nanometers to 500 nanometers and a diameter of 20 nanometers to 100 nanometers.
[0018] Optionally, the polymer matrix layer has a thickness of 20 micrometers to 250 micrometers.
[0019] According to another aspect of the present invention, a method for preparing a transparent conductive film is provided, the method comprising:
[0020] preparing the copper-graphene oxide-core-shell nanowire film;
[0021] The copper-graphene oxide-core-shell nanowire film is transferred to a transparent substrate, and the copper-graphene oxide-core-shell nanowire film on the transparent substrate is reduced to a copper-reduced graphene oxide-core-shell nanowire film, and the transparent substrate and the copper-reduced graphene oxide-core-shell nanowire film constitute a transparent conductive film.
[0022] Optionally, the preparation of the copper-graphene oxide-core-shell nanowire film comprises:
[0023] stirring a mixture of the graphene oxide and the isopropanol suspension of the copper nanowires to obtain a dispersion of copper-graphene oxide-core-shell nanowires;
[0024] The copper-graphene oxide-core-shell nanowire dispersion is vacuum filtered to obtain the copper / graphene oxide core-shell nanofilm.
[0025] Optionally, the step of transferring the copper-graphene oxide-core-shell nanowire film to a transparent substrate further comprises:
[0026] A preset pressure value is applied to the copper-graphene oxide-core-shell nanowire film on the transparent substrate for a first preset time.
[0027] Optionally, reducing the copper-graphene oxide-core-shell nanowire film on the transparent substrate to a copper-reduced graphene oxide-core-shell nanowire film comprises:
[0028] Placing the transparent substrate and the copper-graphene oxide-core-shell nanowire film on the transparent substrate in a reducing atmosphere and performing thermal annealing at a preset temperature;
[0029] or,
[0030] The transparent substrate and the copper-graphene oxide-core-shell nanowire film on the transparent substrate are exposed to a reducing environment; after a second preset time, the copper-graphene oxide-core-shell nanowire film is placed in a reducing atmosphere and thermally annealed at a preset temperature.
[0031] According to another aspect of the present invention, there is provided a method for preparing an optical transmission control device, the method comprising:
[0032] The first transparent conductive film and the second transparent conductive film are prepared by the method as described above;
[0033] Filling a polymer matrix between the copper-reduced graphene oxide-core-shell nanowire film of the first transparent conductive film and the copper-reduced graphene oxide-core-shell nanowire film of the second transparent conductive film to form a polymer matrix layer;
[0034] The first transparent conductive film, the second transparent conductive film and the polymer matrix constitute the light transmission control device.
[0035] Optionally, the transparent substrate is glass;
[0036] The step of filling a polymer matrix between the copper-reduced graphene oxide-core-shell nanowire film of the first transparent conductive film and the copper-reduced graphene oxide-core-shell nanowire film of the second transparent conductive film to form a polymer matrix layer comprises:
[0037] On the copper-reduced graphene oxide-core-shell nanowire film of the first transparent conductive film, a preset filling space is enclosed by a spacer gasket;
[0038] Filling the polymer matrix into a preset filling space surrounded by a spacer;
[0039] Using the second transparent conductive film to cover the filled polymer matrix;
[0040] The first transparent conductive film, the second transparent conductive film and the filled polymer matrix are cured by ultraviolet light to form the polymer matrix layer.
[0041] Optionally, the transparent substrate is a polymer;
[0042] The step of filling a polymer matrix between the copper-reduced graphene oxide-core-shell nanowire film of the first transparent conductive film and the copper-reduced graphene oxide-core-shell nanowire film of the second transparent conductive film to form a polymer matrix layer comprises:
[0043] scraping the polymer matrix onto the first transparent conductive film;
[0044] curing the polymer matrix on the first transparent conductive film with ultraviolet light to form the polymer matrix layer;
[0045] The second transparent conductive film is used to cover the polymer matrix layer.
[0046] In summary, the beneficial effects of the technical solution of the present invention are: providing a transparent conductive film, which has good light transmittance and conductivity, and at the same time the transparent substrate and the copper-reduced graphene oxide-core-shell nanowire film are both flexible materials, which ensures the flexibility of the transparent conductive film and has low cost. After the transparent conductive film is applied to a light control device, the switch switching of the device has good stability and reversibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 A schematic diagram of the structure of an optical transmission control device provided by one embodiment of the present invention;
[0048] Figure 2 A schematic flow chart of a method for preparing a transparent conductive film provided by one embodiment of the present invention;
[0049] Figure 3A schematic flow chart of a method for preparing an optical transmission control device provided by one embodiment of the present invention;
[0050] Figure 4 A transmission electron microscope image of a copper-graphene oxide-core-shell nanowire film provided by one embodiment of the present invention;
[0051] Figure 5 A schematic diagram of the transmittance and square resistance of a copper-reduced graphene oxide-core-shell nanowire film prepared at different thermal annealing temperatures provided in one embodiment of the present invention;
[0052] Figure 6 A schematic diagram of the light transmittance of a copper-reduced graphene oxide-core-shell nanowire film at different thicknesses provided by one embodiment of the present invention;
[0053] Figure 7 A transmission spectrum diagram of a light control device provided by an embodiment of the present invention before and after applying a voltage of 110V;
[0054] Figure 8 The light transmittance of a light control device provided by an embodiment of the present invention under a switching voltage cycle. DETAILED DESCRIPTION
[0055] Transparent conductive films are usually used as transparent electrodes. Although indium tin oxide (ITO) has long been the industry standard for transparent conductive films, there are still some problems: ITO is relatively expensive and its brittleness does not match the flexible substrate. In addition, the shortage of indium resources limits its practical application.
[0056] In addition, the market increasingly demands light transmission control devices with transparent electrodes, also known as light valves (LVs), such as smart windows, to replace traditional curtains or blinds to achieve comfortable living and energy saving. Therefore, in order to enable large-scale application of light transmission control devices, the cost of transparent electrodes needs to be taken into account, and the high cost of transparent electrodes cannot become an economic barrier to their large-scale application.
[0057] Considering that an electric field is generated between the two electrodes of the device, the current does not need to flow from one electrode to another electrode, which makes the transparent conductive film (TCF) have a higher light transmittance and does not require high conductivity. Therefore, TCF with relatively low conductivity has better economic potential, so copper-reduced graphene oxide-core-shell nanowires become the object of choice of the present invention. In order to make the purpose, technical solution and advantages of the present invention clearer, the embodiments of the present invention will be further described in detail below in conjunction with the accompanying drawings.
[0058] The invention provides a transparent conductive film, which comprises: a transparent substrate and a copper-reduced graphene oxide-core-shell nanowire film; the copper-reduced graphene oxide-core-shell nanowire (Cu-rGO-csNW) film is deposited on the transparent substrate.
[0059] In one embodiment of the present invention, the transparent substrate is glass or polymer, including but not limited to: polyethylene terephthalate (PET), polyethylene (PE), polyethylene naphthalate (PEN), polymethyl methacrylate (PMMA) and polycarbonate (PC).
[0060] In one embodiment of the present invention, the light transmittance of the transparent substrate should be equal to or greater than 80%; more preferably, the light transmittance should be greater than or equal to 90%.
[0061] To ensure that the transparent conductive film has good light transmittance and conductivity, in one embodiment of the present invention, the thickness of the Cu-rGO-csNW film is 50 nanometers to 250 nanometers.
[0062] In one embodiment of the present invention, the light transmittance of the Cu-rGO-csNW film is 75%-95%.
[0063] In one embodiment of the present invention, the sheet resistance of the Cu-rGO-csNW film is 10 ohms to 100 ohms.
[0064] The present invention also provides an optical transmission control device, and the above-mentioned transparent conductive film can be applied to the optical transmission control device. The optical transmission control device comprises: a first transparent conductive film, a second transparent conductive film, and a polymer matrix layer filled between the first transparent conductive film and the second transparent conductive film; the first transparent conductive film and / or the second transparent conductive film is a transparent conductive film in any of the above-mentioned embodiments, and the polymer matrix layer is filled between the copper-reduced graphene oxide-core-shell nanowire film of the first transparent conductive film and the copper-reduced graphene oxide-core-shell nanowire film of the second transparent conductive film.
[0065] In one embodiment of the present invention, the polymer matrix layer comprises a polymer base material and a plurality of suspended particles, each of which comprises a suspension medium and a plurality of light polarizing particles.
[0066] The suspension medium material of the suspended particles is different from the polymer matrix material, and the suspended particles are suspended in the polymer matrix material in a liquid or gel form.
[0067] Figure 1 FIG. 1 is a schematic diagram of the structure of an optical transmission control device provided by an embodiment of the present invention. Figure 1As shown, the optical transmission control device includes: a first transparent substrate 100, a first copper-reduced graphene oxide-core-shell nanowire film 200, a polymer matrix layer 300, a second copper-reduced graphene oxide-core-shell nanowire film 400, and a second transparent substrate 500. An alternating current AC is connected between the first copper-reduced graphene oxide-core-shell nanowire film 200 and the second copper-reduced graphene oxide-core-shell nanowire film 400.
[0068] The polymer matrix layer 300 includes a polymer base material 310 and a plurality of suspended particles 320 , each of which includes a suspension medium 321 and a plurality of light polarizing particles 322 , and the plurality of light polarizing particles can be reoriented under the action of an electric field.
[0069] The first transparent substrate 100 and the second transparent substrate 500 can be made of the same material or different materials. However, in order to simplify the processing and match the final device, they are preferably made of the same material.
[0070] In this embodiment, the first Cu-rGO-csNW film 200 and the second Cu-rGO-csNW film 400 are both Cu-rGO-csNW films, so that they can have similar optical properties on both sides of the polymer matrix layer 300, can control light in a symmetrical manner, and ultimately help reduce the haze of the optical transmission control device.
[0071] In this embodiment, the polymer matrix layer should be a plastic material with good light transmittance. Preferably, the polymer matrix can be formed by photocuring, so the shrinkage of the layer can be strictly controlled. In one embodiment of the present invention, the polymer matrix material is a cross-linked polysiloxane or acrylate formed by an ethylenically unsaturated substance and a liquid siloxane copolymer.
[0072] Furthermore, because the suspension medium material of the suspended particles is different from the polymer matrix material, if the polymer matrix material is acrylate, the suspension medium material of the suspended particles can be selected from silicone oil or isotridecyl trimellitate.
[0073] In one embodiment of the present invention, the light polarizing particle of the suspended particles is one of polyhalide, titanium dioxide and quinine iodosulfate.
[0074] Furthermore, as described above, each polarized light particle can be reoriented under the action of the power plant, so the collective size of the polarized light particles should be reasonably selected. In one embodiment of the present invention, the length of each polarized light particle is 100 nanometers to 500 nanometers, and the diameter is 20 nanometers to 100 nanometers.
[0075] Preferably, the length of each light polarizing particle is between 150nm and 300nm, and the diameter should be between 30nm and 60nm.
[0076] Because the light transmittance of the optical transmission control device is related to the thickness of the polymer matrix layer, in one embodiment of the present invention, the thickness of the polymer matrix layer is 20 microns to 250 microns to meet the light transmittance requirement of the optical transmission control device.
[0077] In one embodiment of the present invention, other additives may be added to the polymer matrix layer, for example, a stabilizer and / or an emulsifier.
[0078] The light transmittance of the transparent conductive film provided by the present invention can be as high as 95%, and the square resistance is about 1000Ω / sq. Therefore, the present invention also provides a method for preparing the transparent conductive film, and the transparent conductive film prepared by the method can achieve the above-mentioned effect. Figure 2 A schematic diagram of a process for preparing a transparent conductive film according to an embodiment of the present invention is shown below. Figure 2 As shown, the method includes:
[0079] Step S210, preparing a copper-graphene oxide-core-shell nanowire (Cu-GO-csNW) film.
[0080] Step S210, transferring the copper-graphene oxide-core-shell nanowire film to a transparent substrate, reducing the copper-graphene oxide-core-shell nanowire film on the transparent substrate to a copper-reduced graphene oxide-core-shell nanowire film, and the transparent substrate and the copper-reduced graphene oxide-core-shell nanowire film form a transparent conductive film.
[0081] In this embodiment, the copper-graphene oxide-core-shell nanowire film can be transferred to the transparent substrate by printing, spraying, scraping, dripping and other coating methods. The concentration and volume of Cu-GO-csNW can also be changed to obtain films with different thicknesses and transmittances.
[0082] In one embodiment of the present invention, the preparation of the copper-graphene oxide-core-shell nanowire film in the above step S210 includes:
[0083] Step S211, stirring the mixture of graphene oxide and the isopropanol suspension of copper nanowires to obtain a dispersion of copper-graphene oxide-core-shell nanowires.
[0084] In this embodiment, the surface ratio and chemical composition of copper nanowires and graphene oxide can be adjusted to change their concentrations, thereby optimizing the ratio of copper nanowire and graphene thickness, and ultimately obtaining composite nanowires and films with good electrical and optical properties.
[0085] Step S212, vacuum filtering the dispersion of copper-graphene oxide-core-shell nanowires to obtain a copper / graphene oxide core-shell nanofilm.
[0086] In one embodiment of the present invention, transferring the copper-graphene oxide-core-shell nanowire film to the transparent substrate in step S220 further includes: applying a preset pressure value to the copper-graphene oxide-core-shell nanowire film on the transparent substrate for a first preset time.
[0087] For example, the preset pressure value is a weight of 3 kg, and the first preset time is 6 hours. However, this is only a specific example, and the preset pressure value and the first preset time in this embodiment can be set according to needs, and are not specifically limited here.
[0088] In one embodiment of the present invention, reducing the copper-graphene oxide-core-shell nanowire film on the transparent substrate into the copper-reduced graphene oxide-core-shell nanowire film in step S220 includes: a one-step reduction method or a two-step reduction method.
[0089] (1) One-step reduction method: The transparent substrate and the copper-graphene oxide-core-shell nanowire film on the transparent substrate are placed in a reducing atmosphere and thermally annealed at a preset temperature.
[0090] Here, the reducing atmosphere may be argon:hydrogen (Ar:H2) or nitrogen:hydrogen (N2:H2). The preset temperature is 200°C to 400°C.
[0091] (2) Two-step reduction method: the transparent substrate and the copper-graphene oxide-core-shell nanowire film on the transparent substrate are exposed to a reducing environment; after a second preset time, the copper-graphene oxide-core-shell nanowire film is placed in a reducing atmosphere and thermally annealed at a preset temperature.
[0092] Here, the reducing environment is different from the reducing atmosphere. The reducing environment can be a liquid environment or a gas environment, for example, hydrazine vapor or soaking in sodium borohydride and ascorbic acid solution; while the reducing atmosphere is hydrogen (Ar:H2) or nitrogen:hydrogen (N2:H2). Similarly, the preset temperature here is 200°C to 400°C.
[0093] In the above-mentioned one-step reduction method or two-step reduction method, the thermal annealing step improves the reduction degree of the film, and more importantly, sintering the nanowire (NWs) nodes together to make the network structure more tightly connected. Considering that the melting point of the material at the nanoscale will be greatly reduced, too high an annealing temperature will destroy the nanowires. However, too low a temperature will not easily form NWs nodes and reduce graphene. Therefore, the annealing temperature needs to be carefully selected, with a preferred range of 200 to 400°C, and an optimal temperature of 240 to 300°C.
[0094] Figure 3 A schematic diagram of a process for preparing an optical transmission control device according to an embodiment of the present invention. Figure 3As shown, the method includes:
[0095] Step S310, using Figure 2 The method of any one of the embodiments is used to prepare a first transparent conductive film and a second transparent conductive film;
[0096] Step S320, filling a polymer matrix between the copper-reduced graphene oxide-core-shell nanowire film of the prepared first transparent conductive film and the copper-reduced graphene oxide-core-shell nanowire film of the second transparent conductive film to form a polymer matrix layer;
[0097] In step S330 , the first transparent conductive film, the second transparent conductive film and the polymer matrix form a light transmission control device.
[0098] During the preparation process, the preparation process may vary according to the difference of transparent substrates in the first transparent conductive film and the second transparent conductive film.
[0099] In one embodiment of the present invention, if the transparent substrate in the first transparent conductive film and the second transparent conductive film is glass.
[0100] Then, in step S320, a polymer matrix is filled between the copper-reduced graphene oxide-core-shell nanowire film of the prepared first transparent conductive film and the copper-reduced graphene oxide-core-shell nanowire film of the second transparent conductive film to form a polymer matrix layer, including: on the copper-reduced graphene oxide-core-shell nanowire film of the first transparent conductive film, a preset filling space is enclosed by a spacer gasket; the polymer matrix is filled into the preset filling space enclosed by the spacer gasket; the second transparent conductive film is used to cover the filled polymer matrix; and the first transparent conductive film, the second transparent conductive film and the filled polymer matrix are subjected to ultraviolet light curing to form a polymer matrix layer.
[0101] In one embodiment of the present invention, if the transparent substrate in the first transparent conductive film and the second transparent conductive film is a polymer.
[0102] Then, in step S320, a polymer matrix is filled between the copper-reduced graphene oxide-core-shell nanowire film of the prepared first transparent conductive film and the copper-reduced graphene oxide-core-shell nanowire film of the second transparent conductive film to form a polymer matrix layer, including: scraping the polymer matrix on the first transparent conductive film; subjecting the polymer matrix on the first transparent conductive film to ultraviolet light curing to form a polymer matrix layer; and covering the polymer matrix layer with a second transparent conductive film.
[0103] The above-mentioned ultraviolet light curing is to place the polymer matrix on the first transparent conductive film under ultraviolet light for radiation.
[0104] The technical method of the present invention is further illustrated by means of several specific examples below.
[0105] Example 1:
[0106] Cu-GO-csNW nanomaterials were prepared by mixing a graphene (GO) aqueous solution (concentration of 0.5 mg / ml, volume of 2 ml) and an isopropyl alcohol (IPA) suspension of copper nanowires (Cu-NW) by stirring. The mixture was then washed N times by centrifugation (8000RMP, 5min) to remove residual GO. Here, the optical and electrical properties of the core-shell composite NW and film can be balanced by adjusting and optimizing the ratio of Cu-NW diameter to GO thickness. The morphology of the synthesized Cu-GO-csNW was characterized using transmission electron microscopy (TEM). Figure 4 A transmission electron microscope image of a copper-graphene oxide-core-shell nanowire film provided in one embodiment of the present invention. Figure 4 As shown, the average length of the synthesized Cu-GO-csNW is 40 ± 10 μm, the diameter is 20 ± 5 nm, and the thickness of the GO shell is about 5 nm.
[0107] Then, the dispersion containing the Cu-GO-csNW structure was vacuum filtered through a polytetrafluoroethylene porous filter membrane to obtain a Cu-GO-csNW membrane. The obtained Cu-GO-csNW membrane was transferred to a glass substrate, and uniform pressure (3 kg weight) was applied to the Cu-GO-csNW membrane for 6 hours. The prepared Cu-GO-csNW membrane was exposed to a mixed atmosphere containing 95% volume of argon (Ar) and 5% volume of hydrogen (H2), and annealed at 240°C for 2 hours (for comparison, a part of the Cu-GO-csNW membrane was annealed at 260°C for 2 hours). Thermal annealing can not only improve the degree of reduction of the film, but more importantly, it can sinter the NW together to form a close contact point. After reduction, the Cu-GO-csNW membrane is transformed into a Cu-rGO-csNW membrane. The transmittance and conductivity of the Cu-rGO-csNW film were characterized by UV-Vis-NIR spectrophotometer and four-probe, respectively. Figure 5 A schematic diagram of the transmittance and square resistance of a copper-reduced graphene oxide-core-shell nanowire film prepared at different thermal annealing temperatures provided in one embodiment of the present invention. Figure 5 As shown, when the annealing temperature is 240°C, the transmittance of the Cu-rGO-csNW film is 92.7% and the surface resistance is 86.5Ω / sq; at 260°C, the transmittance of the Cu-rGO-csNW film is about 91.5% and the surface resistance is 101Ω / sq.
[0108] Example 2:
[0109] Because the concentration and volume of Cu-GO-csNW can be changed, films with different thicknesses and transmittances can be obtained.
[0110] According to the method described in Example 1 above, the volume of the suspension in the vacuum filtration was changed to obtain Cu-rGO-csNW films with different thicknesses. Figure 6 A schematic diagram of the light transmittance of a copper-reduced graphene oxide-core-shell nanowire film at different thicknesses provided by one embodiment of the present invention. Figure 6 As shown, 1-5 represent different thicknesses, and the thickness relationship is 1<2<3<4<5. It can be found from the figure that with the increase of thickness, the transmittance of the film at a wavelength of 550nm gradually decreases from 92.7% to 72.5%.
[0111] Example three:
[0112] In this embodiment, a 2 cm×2 cm optical transmission control device is assembled using the Cu-rGO-csNW film prepared in Example 1 or Example 2 using an adhesive spacing method, wherein the transparent substrate, the Cu-rGO-csNW film, the polymer matrix layer, the Cu-rGO-csNW film and the transparent substrate are glass, the Cu-rGO-csNW film (90% transmittance and 70 Ω / sq prepared in Example 2), a transparent matrix layer containing suspended polyhalides, the Cu-rGO-csNW film (90% transmittance and 70 Ω / sq prepared in Example 2) and glass.
[0113] The transmission spectra of the prepared optical transmission control device were measured before (off state) and after (on state) a voltage of 110 V was applied. Figure 7 The transmission spectrum of the light control device provided by one embodiment of the present invention before and after applying a voltage of 110V. Figure 7 As shown, the optical transmission control device obtains a maximum optical modulation of 49.6% near a wavelength of 756 nm, which can be applied in real life. Figure 8 The light transmittance of the light control device provided by one embodiment of the present invention under the switching voltage cycle. Figure 8 As shown, the device can be reversibly switched between high and low transmittance, with the switching time of on and off being 20s and 40s respectively, and the results of reversible switching over 100 times show no significant change. This indicates that the on / off switching process of the optical transmission control device prepared by the technical solution of the present invention has good reversibility.
[0114] Example 4:
[0115] Using the same conditions as in Example 3, but with the transmittance of the Cu-rGO-csNW film reduced to 80%, the maximum optical modulation of the fabricated optical transmission control device was reduced to 39.1%.
[0116] In summary, the beneficial effects of the technical solution of the present invention are: providing a transparent conductive film, which has good light transmittance and conductivity, and at the same time the transparent substrate and the copper-reduced graphene oxide-core-shell nanowire film are both flexible materials, which ensures the flexibility of the transparent conductive film and has low cost. After the transparent conductive film is applied to a light control device, the switch switching of the device has good stability and reversibility.
[0117] The above is only a specific embodiment of the present invention. Under the above teachings of the present invention, those skilled in the art can make other improvements or modifications on the basis of the above embodiments. Those skilled in the art should understand that the above specific description is only to better explain the purpose of the present invention, and the protection scope of the present invention shall be based on the protection scope of the claims.
Claims
1. An optical transmission control device, It is characterized in that The device comprises: a first transparent conductive film, a second transparent conductive film, and a polymer matrix layer filled between the first transparent conductive film and the second transparent conductive film; The first transparent conductive film and / or the second transparent conductive film comprises: A transparent substrate and a copper-reduced graphene oxide-core-shell nanowire film; the copper-reduced graphene oxide-core-shell nanowire film is deposited on the transparent substrate; the transparent substrate is glass or polymer; the thickness of the copper-reduced graphene oxide-core-shell nanowire film is 50 nanometers to 250 nanometers; the transmittance of the copper-reduced graphene oxide-core-shell nanowire film is 75%-95%; the square resistance of the copper-reduced graphene oxide-core-shell nanowire film is 10 ohms to 100 ohms; the copper-reduced graphene oxide-core-shell nanowire film is transferred to a transparent substrate, the copper-reduced graphene oxide-core-shell nanowire film on the transparent substrate is reduced to a copper-reduced graphene oxide-core-shell nanowire film, the transparent substrate and the copper-reduced graphene oxide-core-shell nanowire film form a transparent conductive film, and the polymer matrix layer is filled between the copper-reduced graphene oxide-core-shell nanowire film of the first transparent conductive film and the copper-reduced graphene oxide-core-shell nanowire film of the second transparent conductive film; An alternating current is connected between the first transparent conductive film, the second transparent conductive film and the polymer matrix layer; The polymer matrix layer includes a polymer matrix material and a plurality of suspended particles, each of the suspended particles includes a suspension medium and a plurality of light polarizing particles, and the plurality of light polarizing particles are reoriented under the action of an alternating current electric field; The suspension medium material of the suspended particles is different from the polymer matrix material, and the suspended particles are suspended in the polymer matrix material in a liquid or gel form; Each of the light polarizing particles has a length of 100 nanometers to 500 nanometers and a diameter of 20 nanometers to 100 nanometers, and the thickness of the polymer matrix layer is 20 micrometers to 250 micrometers.
2. The device according to claim 1, It is characterized in that The polymer matrix material is cross-linked polysiloxane or acrylate; if the polymer matrix material is acrylate, the suspension medium material of the suspended particles is silicone oil or isotridecyl trimellitate; The light polarizing particles of the suspended particles are polyhalides, titanium dioxide, or quinine iodide sulfate.
3. A method for preparing an optical transmission control device, It is characterized in that The method comprises: The first transparent conductive film and the second transparent conductive film are prepared, specifically comprising: Preparation of copper-graphene oxide-core-shell nanowire films; Transferring the copper-graphene oxide-core-shell nanowire film to a transparent substrate, reducing the copper-graphene oxide-core-shell nanowire film on the transparent substrate to a copper-reduced graphene oxide-core-shell nanowire film, wherein the transparent substrate and the copper-reduced graphene oxide-core-shell nanowire film form a transparent conductive film; The method for preparing the copper-graphene oxide-core-shell nanowire film comprises: stirring a mixture of the graphene oxide and the isopropanol suspension of the copper nanowires to obtain a dispersion of copper-graphene oxide-core-shell nanowires; Vacuum filtering the copper-graphene oxide-core-shell nanowire dispersion to obtain the copper / graphene oxide core-shell nanofilm; The step of transferring the copper-graphene oxide-core-shell nanowire film to a transparent substrate further comprises: Applying a preset pressure value to the copper-graphene oxide-core-shell nanowire film on the transparent substrate for a first preset time; The reducing the copper-graphene oxide-core-shell nanowire film on the transparent substrate into a copper-reduced graphene oxide-core-shell nanowire film comprises: Placing the transparent substrate and the copper-graphene oxide-core-shell nanowire film on the transparent substrate in a reducing atmosphere and performing thermal annealing at a preset temperature; or, Exposing the transparent substrate and the copper-graphene oxide-core-shell nanowire film on the transparent substrate to a reducing environment; after a second preset time, placing the copper-graphene oxide-core-shell nanowire film in a reducing atmosphere and performing thermal annealing at a preset temperature; Filling a polymer matrix between the copper-reduced graphene oxide-core-shell nanowire film of the first transparent conductive film and the copper-reduced graphene oxide-core-shell nanowire film of the second transparent conductive film to form a polymer matrix layer; The first transparent conductive film, the second transparent conductive film and the polymer matrix constitute the light transmission control device, and alternating current is connected between the first transparent conductive film, the second transparent conductive film and the polymer matrix layer.
4. The method according to claim 3, It is characterized in that The transparent substrate is glass; The step of filling a polymer matrix between the copper-reduced graphene oxide-core-shell nanowire film of the first transparent conductive film and the copper-reduced graphene oxide-core-shell nanowire film of the second transparent conductive film to form a polymer matrix layer comprises: On the copper-reduced graphene oxide-core-shell nanowire film of the first transparent conductive film, a preset filling space is enclosed by a spacer gasket; Filling the polymer matrix into a preset filling space surrounded by a spacer; Using the second transparent conductive film to cover the filled polymer matrix; The first transparent conductive film, the second transparent conductive film and the filled polymer matrix are cured by ultraviolet light to form the polymer matrix layer.
5. The method according to claim 4, It is characterized in that The transparent substrate is a polymer; The step of filling a polymer matrix between the copper-reduced graphene oxide-core-shell nanowire film of the first transparent conductive film and the copper-reduced graphene oxide-core-shell nanowire film of the second transparent conductive film to form a polymer matrix layer comprises: scraping the polymer matrix onto the first transparent conductive film; curing the polymer matrix on the first transparent conductive film with ultraviolet light to form the polymer matrix layer; The second transparent conductive film is used to cover the polymer matrix layer.