Plastic matrix abrasive tool, method for manufacturing abrasive tool matrix and materials used therefor

By using materials such as phenolic resin and hot-pressing sintering technology, the plastic matrix grinding tools produced solve the problem of high rotational load caused by the heavy weight of existing grinding tools, achieving high-precision and efficient high-speed cutting processing, and are suitable for high-end grinding tools of production.

CN109159034BActive Publication Date: 2024-10-15QINHUANGDAO DAOTIAN PRECISION GRINDING TOOL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201810855402.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-07-31
Publication Date
2024-10-15
Estimated Expiration
2038-07-31

AI Technical Summary

Technical Problem

The base body of existing abrasive tools is made of steel or aluminum, which results in a heavy weight of the abrasive tool and a large rotation load during rotation, which affects the machining accuracy.

Method used

Plastic matrix grinding tools made of phenolic resin, composite curing agent, reinforcing agent, hardener and other materials are used. The metal matrix core is fixed in the plastic matrix through a hot pressing mold. Combined with the sintering method, the strength and hardness of the grinding tool are improved. At the same time, the overall weight is reduced.

Benefits of technology

It can reduce the weight of the abrasive tools, reduce the rotation load, and improve the processing accuracy while ensuring the strength and hardness. It is suitable for the production of high-end abrasive tools and has good impact resistance, tensile resistance, bending resistance and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109159034B_ABST
    Figure CN109159034B_ABST
Patent Text Reader

Abstract

The invention aims at the disadvantage that the rotation load of the mold base in the prior art greatly affects the processing precision, and provides a plastic matrix mold, a manufacturing method of the mold base and the materials used. The materials used for the mold base include phenolic resin, composite curing agent, reinforcing agent, hardener and additives, and the mass percentage of each component is: 30-45% of phenolic resin, 2-8% of composite curing agent, 35-50% of reinforcing agent, 2-15% of hardener, and 2-5% of additives; the additive is a mixture of zinc stearate and silane coupling agent, and the mass percentages of the two components in the total components are: 1-4.5% of zinc stearate and 0-1.5% of silane coupling agent; the composite curing agent includes hexamethylenetetramine and magnesium oxide, and the mass percentages of the composite curing agent and magnesium oxide in the total components are: 1-7% of hexamethylenetetramine and 1-5% of magnesium oxide. By using the materials provided by the invention, the overall weight of the mold base is reduced while the strength and hardness of the mold base are guaranteed, the rotation load of the mold during rotation is reduced, and the influence on the processing precision is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a plastic matrix grinding tool, a method for manufacturing the grinding tool matrix and materials used for the grinding tool matrix. Background Art

[0002] At present, in the field of abrasive tools, which is known as the "teeth of industry", with the development of high-precision, high-accuracy, high-efficiency and other technical requirements, more and more high-precision abrasive tools are able to exert their superior performance in various fields. The finished abrasive tools are generally composed of two parts: an abrasive layer and a base layer that supports the abrasive layer. The abrasive tool bases circulating on the market are made of steel, aluminum, and other metal agents considering the strength requirements. The abrasive tool bases made of the above materials are heavy, so when the abrasive tool rotates at high speed, the rotating load is large, which can easily cause the spindle to deform and affect the processing accuracy. Summary of the invention

[0003] The purpose of the present invention is to provide a plastic-based mold, a method for manufacturing the mold base and the materials used therein, in view of the fact that the mold bases in the prior art are all made of steel, aluminum and other metal agents. Due to the heavy weight of the mold, when the mold rotates, the rotational load is large, which affects the processing accuracy.

[0004] The objective of the present invention is achieved through the following technical solutions:

[0005] A material for a grinding tool matrix, comprising phenolic resin, composite curing agent, reinforcing agent, hardener and additives, wherein the mass percentage of each component is: 30-45% of phenolic resin, 2-8% of composite curing agent, 35-50% of reinforcing agent, 2-15% of hardener, and 2-5% of additives; the additive is a mixture of zinc stearate and silane coupling agent, and the mass percentages of the two in the total components are: 1-4.5% of zinc stearate and 0-1.5% of silane coupling agent; the composite curing agent comprises hexamethylenetetramine and magnesium oxide, and the mass percentages of the two in the total components are: 1-7% of hexamethylenetetramine and 1-5% of magnesium oxide;

[0006] Further, the reinforcing agent is glass fiber or aramid fiber;

[0007] Furthermore, the hardener is a mixture of asbestos and one of wood powder / quartz powder / mica powder, and the mass percentages of the two in the total components are: asbestos 0-11%, wood powder / quartz powder / mica powder 2-13%.

[0008] A plastic matrix abrasive tool, comprising an abrasive layer and a matrix, wherein the abrasive layer is supported and fixed by the matrix, the matrix comprises a plastic matrix and a metal matrix core, the metal matrix core is provided with an axial through hole, the metal matrix core is fixed in the plastic matrix, and the plastic matrix is ​​made of the material used for the abrasive tool matrix;

[0009] Further, the metal matrix core is fixed on one end surface of the plastic matrix;

[0010] Furthermore, the plastic matrix is ​​sleeved outside the metal matrix core;

[0011] Furthermore, the metal matrix core is fixed in the plastic matrix by sintering, and a positioning hole is arranged on the metal matrix core.

[0012] A method for manufacturing a mold base comprises the following steps: firstly loading a plastic base material containing phenolic resin and a metal base core provided with an axial through hole into a hot pressing mold, so that the plastic base material at least surrounds the circumference or one end face of the metal base core, and then heating and pressing the mold base material and the metal base core by hot pressing to form the mold base.

[0013] Furthermore, the heating temperature is 140-190°C, the pressurizing pressure is 50Mpa±10Mpa, and the holding time is 10min-60min;

[0014] Furthermore, the mold base adopts the material used for the aforementioned mold base, and the material used for the mold base is first made into particles, and then added into the hot pressing mold.

[0015] The abrasive tool matrix provided by the present invention is made of a composite material, which includes 30-45% of phenolic resin, 2-5% of a composite curing agent, 35-50% of a reinforcing agent, 5-10% of a hardener and 2-5% of an additive. When the composite material is used to make the abrasive tool matrix, the phenolic resin is the main body combined with a supporting agent, and the composite curing agent cooperates with the phenolic resin to play a curing role. The reinforcing agent improves the strength of the abrasive tool matrix, and the hardener improves the hardness of the abrasive tool matrix. The additives promote the combination and dispersion of various substances. Since the supporting agent of the abrasive tool matrix made of the composite material is phenolic resin, the weight of the phenolic resin is lighter than that of steel, aluminum and other metals in the prior art, and the strength and hardness of the plastic matrix abrasive tool are improved by the reinforcing agent and the hardener, thereby reducing the overall weight of the abrasive tool matrix while ensuring the strength and hardness of the abrasive tool matrix, reducing the rotational load of the abrasive tool during rotation, and reducing the influence on the precision of the spindle, so that the application range of the abrasive tool is expanded, and it can be used for the production of high-end abrasive tools.

[0016] The method of the present invention is used to make a mold substrate, and the mold substrate can be made by combining a plastic substrate and a metal substrate core together by hot pressing and sintering to obtain a well-bonded composite substrate with high bonding strength and easy ring release. In addition, the composite matrix material of the present invention can be used to obtain a composite matrix abrasive tool with strong bonding force, good hardness, and high-speed operation support, and the density can reach 1.4-2.0g / cm3, the linear expansion coefficient can reach (11.2-13)x10-6, the tensile strength is ≥55Mpa and can reach 85Mpa, the bending strength is ≥80Mpa and can reach 110Mpa, and the impact strength is ≥18KJ / m2 and can reach 31KJ / m2. Since its manufacturing density (that is, the density of the plastic matrix) reaches 1.4-2.0g / cm3, the overall weight of the grinding wheel is light; through compression molding and the ratio of various reinforcing agents and hardeners, the abrasive tool itself has good density, and the linear expansion coefficient can reach (11.2-13) x10-6. By adding reinforcing materials and heat-resistant materials, the abrasive tool has good heat resistance. When the cutting heat is generated during high-speed operation, the abrasive tool is not easy to deform, so the processing accuracy can be maintained. It is more suitable for high-speed and large-volume processing and production, and can be used for high-end abrasive tools. The impact strength of the abrasive tool matrix is ​​≥18 KJ / m2, which makes the abrasive tool matrix impact-resistant, which is conducive to cutting, and the abrasive tool is not easily deformed due to impact force.

[0017] The plastic-based mold using the structure and material of the present invention not only has the good impact resistance, tensile strength, bending resistance and heat resistance of metal molds, but also has a light weight, which is only 22% of the weight of ordinary metal molds and 63% of the weight of aluminum alloy molds, but the cost is 57% of that of aluminum alloy molds. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a bottom view structural schematic diagram of an embodiment of the abrasive tool base in the invention;

[0019] Figure 2 yes Figure 1 Sectional view of AA in the middle;

[0020] Figure 3 and Figure 4 They are respectively schematic structural diagrams of another embodiment of the abrasive tool base of the present invention.

[0021] Description of Reference Numerals

[0022] In the figure: 1- mold base; 2- metal structure; 3- positioning hole; 4- positioning platform; 5- axis center hole. DETAILED DESCRIPTION

[0023] The present invention will be further described below in conjunction with specific embodiments:

[0024] A grinding tool substrate, the substrate is made of a composite material, the composite material includes a phenolic resin, a composite curing agent, a reinforcing agent, a hardener and an additive, the mass percentages of the above components are as follows: 30-45% of phenolic resin, 2-8% of composite curing agent, 35-50% of reinforcing agent, 2-13% of hardener, 2-5% of additive, preferably, the reinforcing agent is glass fiber or aramid fiber, preferably, the hardener is mineral powder, the mineral powder includes asbestos and wood powder, the mass percentages of the two in the total components are as follows: 0-11% of asbestos, 2-15% of wood powder, preferably the two are mixed and added as a hardener, the addition of asbestos improves the temperature resistance of the substrate, enhances the adaptability to the working environment, and has a better ability to adapt to grinding heat The effect of adding wood powder is to improve the hardness, which mainly plays a role of hardening. Quartz powder and mica powder can also be used as hardeners. Preferably, the additives include zinc stearate and silane coupling agent, and the mass percentages of the two components are as follows: zinc stearate 1-4.5%, silane coupling agent 0-1.5%. By adding silane coupling agent, the binding force of the matrix material can be improved, and it is easier to shape when making the mold matrix; preferably, the composite curing agent includes hexamethylenetetramine and magnesium oxide, and the mass percentages of the two components are as follows: hexamethylenetetramine 1-7%, magnesium oxide 1-5%, wherein hexamethylenetetramine plays a role of curing, and magnesium oxide is a accelerator to improve the efficiency of curing and reduce the time required for curing.

[0025] When the above-mentioned composite material is used to make the abrasive tool substrate 1, an axial through hole is firstly provided on the metal structural part, and the plastic matrix material and the metal structural part 2 are firstly loaded into the hot pressing mold, and the metal structural part 2 is pre-embedded in the plastic matrix material as the metal matrix core, so that at least the circumference or at least one end face of the metal structural part 2 is buried by the plastic matrix material. It is preferable that the plastic matrix material is buried on the circumference and one end face of the metal structural part 2 to facilitate the combination of the plastic matrix material and the metal matrix core. Generally, if the abrasive layer is provided at the circumference of the substrate, it is necessary that the plastic matrix material is provided on at least the circumferential surface of the metal matrix core, and it is preferable that the plastic matrix material is provided on the circumference and the other end face of the substrate core. The plastic matrix material is placed on the metal matrix core, so that the plastic matrix material will be surrounded by the metal matrix core, so that the circumference and at least one end face of the metal matrix core are both provided with the plastic matrix material. If the abrasive is located on one end face of the matrix, the plastic matrix material must be placed on at least one end face of the matrix. Of course, it is best to place the plastic matrix material on the circumference and one end face. In this way, the overall weight of the mold is light. The plastic matrix material and the metal matrix core are heated and pressed by a hot pressing mold to form a mold matrix 1, and then a positioning hole 3 is manufactured on the mold matrix 1 by mechanical processing. Preferably, when hot pressing is performed, the heating temperature is 140-190°C, the pressing pressure is 50Mpa±10 Mpa, and the insulation time is 10min-60min. Depending on the purpose of the mold, the shaft center hole 5 can also be set on the metal matrix core, and the positioning hole 3 can also be set on the metal matrix as a mounting hole, and the shaft center hole 5 and the positioning hole 3 can also be set on the matrix at the same time.

[0026] The mold base 1 is manufactured by using the above-mentioned materials and methods. The supporting agent is a thermal phenolic resin. The thermal phenolic resin is lighter than the steel, aluminum and other metals in the prior art. The strength and hardness of the manufactured plastic mold base are improved by the effect of the reinforcing agent and the hardener. The overall mass of the mold base 1 is reduced while the strength and hardness of the mold base 1 are guaranteed, the rotational load of the mold during rotation is reduced, and the influence on the precision of the spindle is reduced.

[0027] like Figure 1 and Figure 2As shown, when the mold base 1 is manufactured, the metal structural part 2 is placed together in the hot pressing mold, so that the metal base core can be directly fixed in the mold base 1 without the need for secondary installation of the metal structural part. Preferably, an axial through hole is provided at the center of the metal structural part 2, which runs from top to bottom. When the hot pressing mold is pressed, the plastic matrix material of the mold base 1 enters the through hole, which increases the fluidity of the plastic matrix material, makes the pressed matrix material uniform and not easy to crack, and makes the lower side of the mold base 1 constitute a positioning platform 4 for positioning. Preferably, the positioning holes 3 are provided on the lower surface of the metal structural part 2 and distributed along the lower surface of the metal structural part 2. Preferably, the positioning holes 3 are threaded holes, and the mold base 1 can be fixed to the machine through the positioning holes 3. The manufacturing method of the abrasive tool and abrasive tool substrate using the structure of the present invention has a metal structural part 2 as a metal substrate core, and a composite resin material with phenolic resin as the main material is arranged on the outside of the metal substrate core, so the weight of the entire abrasive tool is greatly reduced. However, since the shaft center hole and the positioning hole are both arranged on the metal substrate core, the low hardness of the phenolic resin cannot achieve benchmark processing, which provides good conditions for making threads on the abrasive tool, can meet the requirements of the substrate rotation strength, and reduce the overall weight of the abrasive tool. The positioning hole can also be used as a mounting hole. The metal substrate core and the plastic substrate can also be fixedly connected together by bonding.

[0028] When manufacturing the mold matrix, the phenolic resin and the reinforcing agent, hardener, additives, etc. are uniformly mixed in advance, and the required material is made through roller pressing or screw extrusion, granulation and other processes. It is easy to disperse evenly during the molding process, the pressing state is complete, the molding yield is high, and it is also conducive to the combination with the embedded metal structural parts.

[0029] When the above-mentioned composite material is used to make a mold matrix, the ratio of each component in the composite material is different, and the properties of the matrix made are different.

[0030] Embodiment 1,

[0031] The proportion of the composite material is: 38% phenolic resin, 3% hexamethylenetetramine, 2% magnesium oxide, 44% glass fiber / aramid fiber, 8% asbestos, 2% wood powder, 2% zinc stearate, and 1% silane coupling agent. The abrasive tool matrix made of the composite material with the above proportion has the following characteristics: the finished density is 1.68g / cm3, the linear expansion coefficient is 11.3x10-6, the tensile strength is ≥70Mpa, the bending strength is ≥100 Mpa, and the impact strength is 25KJ / m2.

[0032] Other embodiments and their performance are listed in the table

[0033]

[0034] The tensile strength, bending strength and impact strength of the mold base provided by the above embodiment all meet the requirements of the mold base, and the weight is about 50% lighter than that of the mold base made of aluminum, which reduces the overall weight of the mold, reduces the rotation load, causes less damage to the machine tool spindle, and the expansion coefficient can reach the level of steel, and the ambient temperature has little effect on the mold base.

Claims

1. A plastic matrix abrasive tool, comprising an abrasive layer and a composite matrix, wherein the abrasive layer is supported and fixed by the composite matrix, characterized in that: The composite matrix comprises a plastic matrix and a metal matrix core, the metal matrix core is provided with an axial through hole, the metal matrix core is fixed on the plastic matrix, the plastic matrix material at least surrounds the circumference or one end face of the metal matrix core, and the plastic matrix material and the metal matrix core are heated and pressed by hot pressing to form a composite matrix combining plastic and metal; the composition of the plastic matrix material is as follows: comprising a phenolic resin, a composite curing agent, a reinforcing agent, a hardener and an additive, the mass percentage of each component is: phenolic resin 30-45%, composite curing agent 2-8%, reinforcing agent 35-50%, hardener 2-15%, additive 2-5%; the additive is a mixture of zinc stearate and silane coupling agent, the mass percentages of the two in the total components are: zinc stearate 1-4.5%, silane coupling agent 0-1.5%; the composite curing agent comprises hexamethylenetetramine and magnesium oxide, the mass percentages of which in the total components are: hexamethylenetetramine 1-7%, magnesium oxide 1-5%, and the reinforcing agent is glass fiber or aramid fiber; The plastic matrix material has the following characteristics: the linear expansion coefficient of the plastic matrix material is (11.2-13) x10 -6 The density of the plastic matrix material is 1.4-2.0 g / cm 3 , tensile strength ≥55Mpa, bending strength ≥80Mpa, impact strength ≥18 KJ / m 2 .

2. The plastic-based abrasive tool according to claim 1, characterized in that: The metal base core is fixed on one end surface of the plastic base.

3. The plastic-based abrasive tool according to claim 1, characterized in that: The plastic matrix is ​​sleeved outside the metal matrix core.

4. The plastic-based abrasive tool according to claim 2 or 3, characterized in that: The metal matrix core is fixed in the plastic matrix by sintering, and a positioning hole is arranged on the metal matrix core.

5. The plastic-based abrasive tool according to claim 1, wherein: The hardener is a mixture of asbestos and one of wood powder / quartz powder / mica powder, and the mass percentages of the two in the total components are: asbestos 0-11%, wood powder / quartz powder / mica powder 2-13%.

6. A method for manufacturing a composite matrix, characterized in that: The composite matrix comprises a metal matrix core and a plastic matrix made of a plastic matrix material, wherein the plastic matrix material comprises a phenolic resin, a composite curing agent, a reinforcing agent, a hardener and an additive, wherein the mass percentage of each component is: 30-45% of phenolic resin, 2-8% of composite curing agent, 35-50% of reinforcing agent, 2-15% of hardener and 2-5% of additive; the additive is a mixture of zinc stearate and a silane coupling agent, wherein the mass percentages of the two components in the total components are: 1-4.5% of zinc stearate and 0-1.5% of silane coupling agent; the composite curing agent comprises hexamethylenetetramine and magnesium oxide, wherein the mass percentages of the two components in the total components are: 1-7% of hexamethylenetetramine and 1-5% of magnesium oxide; the reinforcing agent is glass fiber or aramid fiber, and the plastic matrix material has the following characteristics: the linear expansion coefficient of the plastic matrix material is (11.2-13) x10 -6 ; The density of the plastic matrix material is 1.4-2.0g / cm 3 , tensile strength ≥55Mpa, bending strength ≥80 Mpa, impact strength ≥18 KJ / m 2 First, a plastic matrix material containing phenolic resin and a metal matrix core provided with an axial through hole are loaded into a hot pressing mold, so that the plastic matrix material at least surrounds the circumference or one end face of the metal matrix core, and the plastic matrix material and the metal matrix core are heated and pressed by hot pressing to form a composite matrix combining plastic and metal.

7. The method for manufacturing a composite matrix according to claim 6, wherein: The heating temperature is 140-190°C, the pressurization pressure is 50Mpa±10 Mpa, and the insulation time is 10min-60min.

8. The method for manufacturing a composite matrix according to claim 6, wherein: The plastic matrix material for the composite matrix is ​​first made into particles, and then added into a hot pressing mold to form a positioning platform on one end surface of the composite matrix.

9. The method for manufacturing a composite matrix according to claim 6, wherein: The hardener is a mixture of asbestos and one of wood powder / quartz powder / mica powder, and the mass percentages of the two in the total components are: asbestos 0-11%, wood powder / quartz powder / mica powder 2-13%.