A sintering furnace and method for improving the sintering rate of a rotary ceramic component

By designing a rotatable load-bearing tube and inclined furnace structure in a sintering furnace, uniform rotation drying and sintering of ceramic blanks is solved, and the deformation and quality problems of rotary ceramic components during the sintering process is improved, and the firing rate and Productivity.

CN110186276BActive Publication Date: 2024-11-22JINGDUN NEW MATERIAL TECHNOLOGY (HENAN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910600871.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-07-04
Publication Date
2024-11-22
Estimated Expiration
2039-07-04

AI Technical Summary

Technical Problem

The extrusion deformation caused by its own gravity during the sintering process and the volume shrinkage unevenness of the rotary ceramic components during the drying process leads to a decrease in mass and sintering rate. The prior art cannot effectively solve these problems.

Method used

A sintering furnace is designed, including the furnace chamber in the furnace body and a rotatable bearing tube arranged parallel to the furnace. The bearing tube is rotated in the same direction through the driving mechanism, and combined with the inclined furnace body structure, the ceramic blank is realized during the drying and sintering process. even rotation and movement to reduce deformation risk.

Benefits of technology

Through uniform rotary drying and sintering, the drying uniformity and sintering rate of the rotary ceramic components are significantly improved, drying deformation is reduced, the damage of the blank during the handling process is avoided, the production cycle is shortened and the production efficiency is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110186276B_ABST
    Figure CN110186276B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of material processing technology, and more particularly, relates to a sintering furnace and method for improving the firing rate of rotary ceramic components. The present invention can realize the drying and sintering of the rotary ceramic body while rotating, improve the drying uniformity of the rotary ceramic body, reduce drying deformation, and thus greatly improve the quality and firing rate of the rotary ceramic component. The method of the present invention completes the drying and sintering processes of the rotary ceramic body in a sintering furnace, eliminating the transportation process of the ceramic body after drying, reducing the probability of damage to the ceramic body, and further improving the firing rate of the rotary ceramic component. In addition, by reasonably adjusting the rotation speed of the device and the inclination angle of the furnace body, the feeding, drying, sintering, and discharging of the rotary ceramic body can be continuously carried out in a high-temperature environment, eliminating the heating and cooling process of the sintering furnace, thereby greatly shortening the production cycle, reducing production costs, and improving production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material processing, and in particular relates to a sintering furnace and a method for improving the sintering rate of a rotary ceramic component. Background Art

[0002] Ceramics refer to a class of inorganic non-metallic materials made from natural or synthetic compounds through molding and sintering. They are widely used in aviation, aerospace, chemical industry, environmental protection and other fields. Molding and sintering are two important processes for preparing ceramic components. The rationality of the process directly determines the quality and firing rate of ceramic components. Deformation is a common problem during the sintering of ceramic components. Slowing down the heating rate is a common method to reduce the deformation of ceramic components, but it will reduce production efficiency. For spherical and some large aspect ratio tubular and rod-shaped rotational ceramic blanks, their own gravity during the sintering process will cause the part where the lower arc surface contacts the support surface to deform due to extrusion, seriously reducing the roundness of the rotational ceramic component. Therefore, even if a slower sintering rate is used, the deformation problem of the rotational ceramic component still exists.

[0003] In order to improve the quality and firing rate of ceramic components, the ceramic body needs to be dried before sintering to prevent the body from dehydrating too quickly during sintering and causing cracks. Since the drying of the body is accompanied by volume shrinkage, and the difference in the dehydration rate of different parts of the body is accompanied by different volume shrinkage rates, different volume shrinkage rates will cause the body to deform or even crack. The common measure to solve the cracking of the body during drying is to reduce the drying temperature and increase the ambient humidity to slow down the drying rate of the body, but too slow a drying rate will also reduce production efficiency. For spherical and some large aspect ratio tubular and rod-shaped rotating ceramic bodies, even if the drying temperature is reduced and the ambient humidity is increased, the problem of drying deformation is still difficult to solve. In addition, the strength of the dried ceramic body is very low, and it is very easy to be damaged during the process of transporting the body to the sintering furnace, which will further reduce the quality and firing rate of the ceramic component.

[0004] Up to now, there is no literature available on methods, technologies and devices for reducing the deformation of rotating ceramic components, and there are only some utility model reports for improving the uniformity of heat treatment of powdered materials. The utility model "A tiltable rotary furnace" (application number: 201120162234.8) discloses a tiltable rotary furnace, which replaces the round furnace tube with a special-shaped furnace tube on the basis of a conventional tube furnace. By rotating the special-shaped furnace tube in the furnace and tilting the furnace body as a whole, the powdered material to be heat-treated can be fully moved in the furnace tube, thereby improving the uniformity of heat treatment of the powdered material. The utility model "A tiltable rotary furnace" (application number: 201520679270.X) discloses a tiltable rotary furnace, which is used to improve the heat treatment effect of powdered materials by adding a set of ventilation devices and tilting devices to the conventional tube furnace. The utility model "A corundum tube high-temperature rotary furnace" (application number: 201320399376.5) discloses a tiltable rotary furnace, which has a double-layer furnace tube structure, with the outer layer being a circular corundum tube and the inner layer being a corundum furnace core, for improving the heat treatment effect of powdered materials.

[0005] The rotary kiln disclosed in the above patent can only be used to improve the uniformity of heat treatment of powdered materials, but cannot be used to improve the deformation problem of the rotary ceramic body during the drying and sintering process. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the present invention provides a sintering furnace and method for improving the sintering rate of a rotary ceramic component.

[0007] The technical solution of the present invention to solve the above-mentioned technical problems is as follows: a sintering furnace for improving the sintering rate of rotating ceramic components, which is special in that it includes a furnace body, a furnace chamber arranged in the furnace body and a pair of supporting tubes arranged parallel to the furnace chamber; the two ends of the supporting tubes respectively extend out of the two sides of the furnace chamber, and the two ends of the supporting tubes are respectively rotatably supported on the furnace body; and it also includes a driving mechanism that can make the pair of supporting tubes rotate in the same direction.

[0008] Based on the above technical solution, the present invention can also be improved as follows.

[0009] Further, the support tube includes a first support tube and a second support tube; the first support tube and the second support tube are respectively provided with a top cone I and a top cone II at the same end on one side, and a top cone III and a top cone IV at the same end on the other side; the top cone I and the top cone II are connected by a belt;

[0010] The driving mechanism includes a driving motor and a reducer. A keyway is provided at one end of the top cone I, and the first supporting tube is connected to the output shaft of the reducer through the keyway.

[0011] Furthermore, the top cone I, top cone II, top cone III and top cone IV all include a top cone head and a top cone shaft; the top cone shaft of the top cone I and the top cone shaft of the top cone II are connected by a belt;

[0012] A keyway is arranged at one end of the top cone shaft of the top cone I.

[0013] The beneficial effect of adopting the above further scheme is that, driven by the motor, the belt drives the first supporting tube and the second supporting tube to rotate in the same direction, so that the rotary ceramic body is dried while rotating, thereby improving the drying uniformity of the rotary ceramic body and reducing drying deformation.

[0014] Furthermore, the first supporting tube and the second supporting tube are spaced 2-4 mm apart.

[0015] The beneficial effect of adopting the above further solution is to ensure the same-direction rotation of the supporting tube and the firing rate of the ceramic body.

[0016] Furthermore, the supporting tube is a corundum tube.

[0017] Furthermore, the top cone I, top cone II, top cone III and top cone IV are made of polytetrafluoroethylene.

[0018] The beneficial effect of adopting the above further solution is that, due to the large thermal expansion coefficient of the corundum tube, it will stretch to both ends after high temperature expansion, and it is very easy to be damaged by the resistance of the bearing seats at both ends. Since polytetrafluoroethylene has good elasticity and plasticity, when the corundum tube stretches due to heat, the polytetrafluoroethylene top cone can prevent the two ends of the corundum tube from being damaged by rigid extrusion, thereby improving the reliability of the device.

[0019] Furthermore, the furnace body also includes an angle adjustment mechanism capable of causing the supporting tube to form an inclination angle.

[0020] Furthermore, the angle adjustment mechanism includes an adjustment bolt arranged on the furnace body foot.

[0021] The beneficial effect of adopting the above further solution is that the sintering furnace can be tilted at a certain angle from left to right, and the ceramic body can rotate and move slowly to the right during the sintering process.

[0022] The second object of the present invention is to provide a fixed drying and sintering method for ceramic components, using the above-mentioned sintering furnace, the steps are as follows:

[0023] (1) The first supporting tube and the second supporting tube are kept horizontal, and the silicon nitride ceramic body is placed on the first supporting tube and the second supporting tube;

[0024] (2) Adjust the speed of the drive motor so that the speed at the output end of the reducer is 1.0-2.5r / min;

[0025] (3) Raise the furnace temperature to 80-90°C at a rate of 5-10°C / min and keep it at that temperature for 100-200min to complete the green body drying;

[0026] (4) Continue to raise the furnace temperature to 1200-1300°C at a rate of 5-10°C / min and keep it at that temperature for 60-120min to complete the sintering of the green body;

[0027] (5) Lower the furnace temperature to 600-700°C at a rate of 10-20°C / min, and then cool naturally; take out the fired ceramic component.

[0028] The third object of the present invention is to provide a continuous drying and sintering method for ceramic components, using the above-mentioned sintering furnace, the steps are as follows:

[0029] (1) The left side of the sintering furnace is made higher than the right side by adjusting the bolts, so that the angle between the first supporting tube and the second supporting tube and the horizontal plane is 3-5 degrees;

[0030] (2) Raise the furnace temperature to 1200-1300°C at a rate of 5-10°C / min and maintain;

[0031] (3) Adjust the speed of the drive motor so that the speed of the reducer output end is 4-8r / min;

[0032] (4) The silicon nitride ceramic body is sent into the sintering furnace from the left end and placed on the first supporting tube and the second supporting tube. During the sintering process, the silicon nitride ceramic body rotates and moves rightward, and the sintered ceramic component is taken out from the right end of the sintering furnace.

[0033] The beneficial effects of the present invention are:

[0034] The present invention can realize drying and sintering of a rotary ceramic body while rotating, improve the drying uniformity of the rotary ceramic body, reduce drying deformation, and thus greatly improve the quality and firing rate of the rotary ceramic component. The method of the present invention completes the drying and sintering processes of the rotary ceramic body in a sintering furnace, eliminating the transportation process of the ceramic body after drying, reducing the probability of damage to the ceramic body, and further improving the firing rate of the rotary ceramic component. In addition, by reasonably adjusting the rotation speed of the device and the inclination angle of the furnace body, the rotary ceramic body can be continuously fed, dried, sintered, and discharged in a high-temperature environment, eliminating the heating and cooling processes of the sintering furnace, thereby greatly shortening the production cycle, reducing production costs, and improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a structural schematic diagram of the present invention;

[0036] Figure 2 for Figure 1 A top view of

[0037] Figure 3 It is the structural schematic diagram of top cone I;

[0038] Figure 4 It is a schematic diagram of the structures of top cone II, top cone III and top cone IV;

[0039] Figure 5 The whole and partial photos of three silicon nitride ceramic tubes fired in Example 1;

[0040] Figure 6 This is a photo of the sintered product in Example 2;

[0041] In the figure, 1, furnace body; 2, furnace chamber; 3, first bearing tube; 4, second bearing tube; 5, top cone I; 6, top cone II; 7, top cone III; 8, top cone IV; 9, top cone head; 10, top cone shaft; 11, belt; 12, drive motor; 13, reducer; 14, keyway; 15, adjusting bolt. DETAILED DESCRIPTION

[0042] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0043] A sintering furnace for improving the firing rate of a rotary ceramic component, comprising a furnace body 1, a furnace chamber 2 arranged in the furnace body, and a first supporting tube 3 and a second supporting tube 4 arranged in parallel in the furnace chamber (the first supporting tube and the second supporting tube are spaced 2 mm apart); the two ends of the supporting tube extend out of the two sides of the furnace chamber respectively, and the two ends of the supporting tube are rotatably supported on the furnace body respectively; and also comprising a driving mechanism capable of rotating the first supporting tube and the second supporting tube in the same direction;

[0044] The first supporting tube and the second supporting tube are provided with a top cone Ⅰ5 and a top cone Ⅱ6 at the same end on one side, and a top cone Ⅲ7 and a top cone Ⅳ8 at the same end on the other side; the top cone Ⅰ, the top cone Ⅱ, the top cone Ⅲ and the top cone Ⅳ all include a top cone head 9 and a top cone shaft 10; the top cone shaft of the top cone Ⅰ and the top cone shaft of the top cone Ⅱ are connected by a belt 11;

[0045] The driving mechanism includes a driving motor 12 and a reducer 13. A keyway 14 is provided at one end of the top cone shaft of the top cone I. The first supporting tube is connected to the output shaft of the reducer through the keyway.

[0046] The furnace body foot is provided with an adjusting bolt 15 .

[0047] The supporting tube (corundum tube) used in the embodiment of the present invention has an outer diameter of 25 mm and an inner diameter of 19 mm.

[0048] Example 1

[0049] A drying and sintering method for a ceramic pipe fitting comprises the following steps:

[0050] (1) The first supporting tube and the second supporting tube are kept horizontal, and a silicon nitride ceramic tube blank with a length of 400 mm, an outer diameter of 45 mm, and an inner diameter of 25 mm is placed on the first supporting tube and the second supporting tube;

[0051] (2) Adjust the speed of the drive motor so that the speed at the output end of the reducer is 2.5r / min;

[0052] (3) Raise the furnace temperature to 90°C at a rate of 5°C / min and keep it at this temperature for 120 min to complete the green body drying;

[0053] (4) Continue to raise the furnace temperature to 1300°C at a rate of 5°C / min and keep it at this temperature for 120 min to complete the sintering of the green body;

[0054] (5) The furnace temperature is lowered to 600°C at a rate of 10°C / min, and then cooled naturally; the fired ceramic pipe fittings are taken out.

[0055] Depend on Figure 5 It can be seen that the three silicon nitride ceramic tubes can be closely placed together, and almost no gaps can be seen between them, which shows that the silicon nitride ceramic tube fired in this embodiment has a very high cylindricity; and the inner and outer circles of the three silicon nitride ceramic tubes have a very high roundness.

[0056] Comparative Example

[0057] Refer to the raw material preparation, sintering temperature and sintering time of the silicon nitride ceramic tube disclosed in the document “XMLi, PTWu, DLZhu, The effect of the crystallization of oxidation-derived SiO2 on the properties of porous Si3N4-SiO2 ceramics synthesized by oxidation. Ceramics International. 40 (2014) 4897-4902.” published by the inventors as a comparative example.

[0058] Table 1 shows the changes in the bending strength and porosity of the silicon nitride ceramic tubes obtained in Example 1 and the comparative example as a function of sintering temperature and time.

[0059] Table 1

[0060]

[0061] It can be seen from Table 1 that, under the same raw material formulation, sintering temperature and sintering time, the bending strength value of the silicon nitride ceramic tube fired in Example 1 is slightly higher and the porosity value is slightly lower. This is because the green body of Example 1 is always in a rotating state during the firing process, and the place where the outer circle of the green body contacts the two corundum tubes is subjected to an external force similar to inward extrusion due to the deadweight of the green body, which leads to an increase in the density of the silicon nitride ceramic tube, a decrease in porosity, and then an increase in strength.

[0062] Example 2

[0063] A method for drying and sintering a ceramic cylinder, comprising the following steps:

[0064] (1) The left side of the sintering furnace is made higher than the right side by adjusting the bolts, so that the angle between the first supporting tube and the second supporting tube and the horizontal plane is 3-5 degrees;

[0065] (2) Raise the furnace temperature to 1250°C at a rate of 10°C / min and maintain it;

[0066] (3) Adjust the speed of the drive motor so that the speed of the reducer output end is 4-8r / min;

[0067] (4) A silicon nitride cylindrical blank with a height of 20 mm and a diameter of 15 mm is fed into the sintering furnace from the left end and placed on the first supporting tube and the second supporting tube. The silicon nitride cylindrical blank is rotated and moved to the right. When the first blank moves 30 mm to the right, the second silicon nitride cylindrical blank is placed from the leftmost end of the sintering furnace, and so on.

[0068] (5) As the silicon nitride cylindrical body moves to the right, it first passes through the low-temperature zone on the left to complete drying and heating, then completes sintering in the high-temperature zone in the middle, and finally completes cooling in the low-temperature zone on the right. When the silicon nitride ceramic cylinder moves right to the rightmost end of the sintering furnace, it is removed to complete sintering.

[0069] Figure 6 (a) is a photo of the silicon nitride cylindrical body used in this embodiment. Figure 6 (b) is a photo of the silicon nitride ceramic cylinder fired in this embodiment. Figure 6 (c) is a photo of a silicon nitride ceramic cylinder fired in a box furnace. Figure 6 It can be seen that the silicon nitride cylindrical blank is a regular cylindrical shape, and the silicon nitride ceramic cylinder fired in a box furnace has obvious deformation, while the silicon nitride ceramic cylinder fired in Example 2 is still a regular cylindrical shape with a high cylindricity.

[0070] Table 2 shows the bending strength and porosity of the silicon nitride ceramic cylinder fired in Example 2 when the inclination angle of the sintering furnace is 3, 4, and 5 degrees, and the speed of the output end of the reducer is 4, 6, and 8 r / min, respectively. Combined with the change law of the values ​​in Table 2, as the inclination angle of the sintering furnace and the speed of the reducer increase, the speed at which the silicon nitride cylindrical blank moves to the right in the furnace tube increases, which means that the sintering time is shortened, which will lead to a decrease in the bending strength of the silicon nitride ceramic cylinder.

[0071] In Table 2, when the sintering furnace inclination angle is 4 degrees and the corundum tube rotation speed is 6r / min, the bending strength of the silicon nitride ceramic cylinder is 23MPa and the porosity is 42%, which is completely consistent with the performance of the silicon nitride ceramic tube obtained by firing at 1250°C for 60min in Example 1. When the sintering furnace inclination angle is 3 degrees and the corundum tube rotation speed is 4r / min, the bending strength of the silicon nitride ceramic cylinder is 34MPa and the porosity is 40%, which is completely consistent with the performance of the silicon nitride ceramic tube obtained by firing at 1250°C for 120min in Example 1.

[0072] Table 2

[0073]

[0074]

[0075] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A sintering furnace for improving the sintering rate of a rotary ceramic component, characterized in that: The invention comprises a furnace body, a furnace chamber arranged in the furnace body, and a pair of supporting tubes arranged in parallel in the furnace chamber; two ends of the supporting tubes extend out of two sides of the furnace chamber respectively, and the two ends of the supporting tubes are rotatably supported on the furnace body respectively; and a driving mechanism capable of rotating the pair of supporting tubes in the same direction is also included; The support tube comprises a first support tube and a second support tube; the first support tube and the second support tube are respectively provided with a top cone I and a top cone II at the same end on one side, and a top cone III and a top cone IV at the same end on the other side; the top cone I and the top cone II are connected by a belt; The driving mechanism includes a driving motor and a reducer, a keyway is provided at one end of the top cone I, and the first bearing tube is connected to the output shaft of the reducer through the keyway; The top cone I, top cone II, top cone III and top cone IV all include a top cone head and a top cone shaft; the top cone shaft of the top cone I and the top cone shaft of the top cone II are connected by a belt; a keyway is provided at one end of the top cone shaft of the top cone I; The first supporting tube and the second supporting tube are spaced 2-4 mm apart; The supporting tube is a corundum tube; The top cone I, top cone II, top cone III and top cone IV are made of polytetrafluoroethylene; The furnace body further comprises an angle adjustment mechanism capable of causing the supporting tube to form an inclination angle, and the angle adjustment mechanism comprises an adjustment bolt arranged on the furnace body foot.

2. A fixed drying and sintering method for a ceramic component, comprising the sintering furnace as claimed in claim 1, and the steps are as follows: (1) The first supporting tube and the second supporting tube are kept horizontal, and the silicon nitride ceramic body is placed on the first supporting tube and the second supporting tube; (2) Adjust the speed of the drive motor so that the speed at the output end of the reducer is 1.0-2.5r / min; (3) Raise the furnace temperature to 80-90°C at a rate of 5-10°C / min and keep it at that temperature for 100-200min to complete the green body drying; (4) Continue to raise the furnace temperature to 1200-1300°C at a rate of 5-10°C / min and keep it at that temperature for 60-120min to complete the sintering of the green body; (5) Lower the furnace temperature to 600-700°C at a rate of 10-20°C / min, and then cool naturally; take out the fired ceramic component.

3. A continuous drying and sintering method for a ceramic component, comprising the sintering furnace as claimed in claim 1, and the steps are as follows: (1) The left side of the sintering furnace is made higher than the right side by adjusting the bolts, so that the angle between the first supporting tube and the second supporting tube and the horizontal plane is 3-5 degrees; (2) Raise the furnace temperature to 1200-1300°C at a rate of 5-10°C / min and maintain; (3) Adjust the speed of the drive motor so that the speed of the reducer output end is 4-8r / min; (4) The silicon nitride ceramic body is sent into the sintering furnace from the left end and placed on the first supporting tube and the second supporting tube. During the sintering process, the silicon nitride ceramic body rotates and moves rightward, and the sintered ceramic component is taken out from the right end of the sintering furnace.