A high-heat dissipation and high-power LED lamp bead and its manufacturing method

By using beryllium oxide ceramic substrate and eutectic layer in high-power LED lamp beads combined with silicone packaging glue and phosphor, the heat dissipation and light efficiency problems are solved, achieving high brightness and high heat dissipation effects while reducing costs.

CN110242877BActive Publication Date: 2024-11-08JIANGXI SUOPUXIN IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910402425.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-04-12
Filing Date
2019-05-15
Publication Date
2024-11-08
Estimated Expiration
2039-05-15

AI Technical Summary

Technical Problem

Existing high-power LED lamp beads are difficult to meet the needs in terms of heat dissipation, light efficiency, reliability and cost. Especially, small-volume, high-power LED lamp beads have increasingly high requirements for lighting power and brightness, but the cost and reliability are reduced. .

Method used

Using beryllium oxide ceramic substrate as the heat dissipation substrate, the flip LED chip and RGB light source are fixed on the substrate through the eutectic layer, and silicone packaging glue and phosphor are used to combine metal dams and coupling agents to achieve high heat dissipation and high brightness. LED light beads.

Benefits of technology

It improves the heat dissipation performance and brightness of LED lamp beads, reduces eutectic time, avoids leakage problems of gold wire connection, realizes full color luminescence and higher luminous flux, and controls the light color accuracy, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110242877B_ABST
    Figure CN110242877B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-heat dissipation high-power LED lamp bead and a manufacturing method thereof. The LED lamp bead comprises a heat dissipation substrate, a metal dam, an LED light source, a eutectic layer connecting the heat dissipation substrate and the LED light source, a packaging adhesive layer covering the LED light source, and a solder pad; the heat dissipation substrate is a beryllium oxide ceramic substrate or an aluminum nitride ceramic substrate; the LED light source comprises at least one flip-chip LED chip and at least one group of RGB light sources; the metal dam forms two cup-shaped structures, the flip-chip LED chip and the RGB light source are respectively arranged in different cup-shaped structures, one of the cup-shaped structures can emit white light, and the other cup-shaped structure can emit one or more of red, blue and green light; the material of the eutectic layer is a gold-tin alloy, wherein the mass percentage of tin is 20-30%. The high-heat dissipation high-power LED lamp bead of the present invention has high power and good heat dissipation effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of LED lamp beads, and in particular to a high-heat dissipation and high-power LED lamp bead and a manufacturing method thereof. Background Art

[0002] LED is mainly used in lighting systems, decoration, electronic equipment indicators, backlight, display and equipment. Among them, high-power LED lamp beads such as 5050 and 7070 lamp beads are mainly prepared by vertical or horizontal structure LED chips. Gold wire welding is required during the preparation process, which leads to reduced light efficiency and reduced reliability. Some high-power LED lamp beads use flip-chip LED chips and fluorescent glass or ceramics. Although they can improve heat dissipation performance and reliability, the cost of LED lamp beads remains high due to the high cost of fluorescent glass and ceramics and the complex processing technology. With the development of society, there is an increasing demand for small-volume, high-power LED lamp beads, and the requirements for lighting power and brightness are increasing, and the cost requirements are increasing. The current high-power LED lamp beads are increasingly difficult to meet the needs in terms of heat dissipation, light efficiency, reliability and cost. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a high-heat dissipation and high-power LED lamp bead and a manufacturing method thereof, so as to improve the power and heat dissipation performance of the LED lamp bead.

[0004] Another technical problem to be solved by the present invention is to provide a high-heat dissipation and high-power LED lamp bead and a manufacturing method thereof to improve the brightness of the LED lamp bead.

[0005] Another technical problem to be solved by the present invention is to provide a high-power LED lamp bead with high heat dissipation that can emit any color.

[0006] In order to solve the above technical problems, the present invention provides a high-heat dissipation and high-power LED lamp bead, comprising a heat dissipation substrate, a metal dam, an LED light source, a eutectic layer connecting the heat dissipation substrate and the LED light source, a packaging glue layer covering the LED light source, and a solder pad;

[0007] The heat dissipation substrate is a beryllium oxide ceramic substrate or an aluminum nitride ceramic substrate;

[0008] The LED light source includes at least one flip-chip LED chip and at least one group of RGB light sources;

[0009] The metal dam forms two cup-shaped structures, and the flip-chip LED chip and the RGB light source are respectively arranged in different cup-shaped structures, one of the cup-shaped structures can emit white light, and the other cup-shaped structure can emit one or more of red, blue and green light;

[0010] The material of the eutectic layer is a gold-tin alloy, wherein the mass percentage of tin is 20-30%.

[0011] As an improvement of the above solution, the material of the metal dam is gold-tin alloy, nickel-gold alloy, nickel-palladium-gold alloy, aluminum alloy, aluminum nitride ceramic, aluminum oxide ceramic or quartz glass;

[0012] The cup-shaped structure has a rectangular, polygonal, circular or triangular shape.

[0013] As an improvement of the above solution, the RGB light source includes a red LED chip, a green LED chip and a blue LED chip.

[0014] As an improvement of the above solution, the encapsulation adhesive layer includes an organic silicon encapsulation adhesive, wherein the encapsulation adhesive layer covering the flip-chip LED chip also includes fluorescent powder.

[0015] As an improvement of the above solution, the organic silicon encapsulation adhesive includes polydimethylsiloxane and silicone resin;

[0016] The fluorescent powder is an aluminate fluorescent powder or a silicate fluorescent powder.

[0017] As an improvement of the above scheme, the encapsulation glue layer covering the flip-chip LED chip also includes a coupling agent, which is one or more of γ-aminopropyl triethoxy silane (silane coupling agent KH550), γ-glycidyloxypropyl trimethoxy silane (silane coupling agent KH560), γ-methacryloxypropyl trimethoxy silane (silane coupling agent KH570), vinyl trimethoxy silane (silane coupling agent A-171), vinyl triethoxy silane (silane coupling agent A-151), isopropyl trioleate acyloxy titanate (titanate coupling agent TC-105), monoalkoxy tris (dioctylphosphoryloxy) titanate (titanate coupling agent CT-114), isopropyl tris (dioctyl pyrophosphate acyloxy) titanate (titanate coupling agent NDZ-201) or isopropoxy distearate acyloxy aluminate (aluminate coupling agent DL-411-A).

[0018] Accordingly, the present invention also provides a method for manufacturing a high-power LED lamp bead with high heat dissipation, comprising the following steps:

[0019] forming a metal dam on the heat dissipation substrate, wherein the metal dam forms two cup-shaped structures;

[0020] The eutectic material is coated on the heat dissipation substrate, and the flip-chip LED chip and the RGB light source are placed on the eutectic material, wherein the eutectic material is a gold-tin alloy, the mass percentage of tin is 20-30%, and the flip-chip LED chip and the RGB light source are respectively arranged in different cup-shaped structures;

[0021] The heat dissipation substrate and the flip-chip LED chip are eutectic, and the eutectic temperature is 290-330℃;

[0022] Apply fluorescent glue on the flip-chip LED chip and apply silicone encapsulation glue on the RGB light source, let it stand for 1.5-2.5 hours, and when the sedimentation rate of the fluorescent powder in the fluorescent glue reaches 85% or above, cure the fluorescent glue and silicone encapsulation glue at a curing temperature of 140-170°C and a curing time of 2.3-3.5 hours.

[0023] As an improvement of the above solution, the RGB light source includes a red LED chip, a green LED chip and a blue LED chip;

[0024] The fluorescent glue comprises fluorescent powder and organic silicon packaging glue.

[0025] As an improvement of the above scheme, the fluorescent glue also includes a coupling agent, which is one or more of γ-aminopropyl triethoxysilane (silane coupling agent KH550), γ-glycidyloxypropyl trimethoxysilane (silane coupling agent KH560), γ-methacryloxypropyl trimethoxysilane (silane coupling agent KH570), vinyl trimethoxysilane (silane coupling agent A-171), vinyl triethoxysilane (silane coupling agent A-151), isopropyl trioleate titanate (titanate coupling agent TC-105), monoalkoxy tris (dioctylphospho) titanate (titanate coupling agent CT-114), isopropyl tris (dioctyl pyrophosphate) titanate (titanate coupling agent NDZ-201) or isopropoxy distearate aluminate (aluminate coupling agent DL-411-A).

[0026] As an improvement to the above solution, preparing fluorescent glue includes the following steps:

[0027] The phosphor: silicone encapsulating adhesive: coupling agent are prepared and mixed in a ratio of 1:10-13:0.1-0.7 to obtain a mixture;

[0028] The mixture is stirred and heated at a temperature of 40-70°C.

[0029] The implementation of the present invention has the following beneficial effects:

[0030] The present invention directly eutectics the flip-chip LED chip on the heat dissipation substrate without the need for gold wire connection, which can not only improve the light extraction efficiency but also avoid leakage and improve the reliability of the LED lamp beads.

[0031] In addition, the present invention adopts a beryllium oxide ceramic substrate as a heat dissipation substrate, which effectively improves the heat dissipation effect of the LED lamp beads.

[0032] Secondly, the present invention effectively reduces the eutectic time and reduces the eutectic problem by adjusting the formula of the eutectic material, and improves the heat dissipation performance of the lamp bead.

[0033] Thirdly, the present invention adjusts the ratio of the organic silicon encapsulation glue and the ratio of the fluorescent glue, so that the viscosity of the organic silicon encapsulation glue is rapidly reduced at a specific temperature, thereby improving the precipitation uniformity of the fluorescent powder.

[0034] Furthermore, the LED light source of the present invention includes a flip-chip LED chip and an RGB light source, which can achieve full-color lighting.

[0035] Furthermore, the phosphor sedimentation process adopted by the present invention precipitates the phosphor to the bottom of the silicone encapsulation glue and covers the surface of the flip-chip LED chip, shortening the path of the flip-chip LED chip to excite the phosphor, reducing the loss of light energy, and stimulating a higher luminous flux; in addition, the light and heat resistance is reduced, the heat dissipation speed inside the lamp bead is improved, and the temperature of the colloid and chip on the surface of the lamp bead is better reduced, thereby improving the heat dissipation performance of the lamp bead.

[0036] Furthermore, the present invention limits the flow of the encapsulation adhesive layer by means of the metal dam, so that its shape after curing can be more accurately controlled, thereby achieving more precise light color control. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a schematic diagram of the structure of a high-heat dissipation and high-power LED lamp bead of the present invention;

[0038] Figure 2 It is a top view of the high-heat dissipation and high-power LED lamp bead of the present invention. DETAILED DESCRIPTION

[0039] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings.

[0040] See also Figure 1 and Figure 2 The present invention provides a high-heat dissipation and high-power LED lamp bead, comprising a heat dissipation substrate 10, a metal dam 30, an LED light source, a eutectic layer 20 connecting the heat dissipation substrate 10 and the LED light source, a packaging glue layer 40 covering the LED light source, and a solder pad 50.

[0041] In order to improve the heat dissipation performance of the lamp beads, the heat dissipation substrate 10 of the present invention is a beryllium oxide ceramic substrate or an aluminum nitride ceramic substrate.

[0042] The main component of beryllium oxide ceramic substrate is beryllium oxide ceramic, which has the characteristics of high thermal conductivity, high melting point, strength, high insulation, low dielectric constant, low dielectric loss and good packaging process adaptability. Among them, the thermal conductivity of beryllium oxide ceramic reaches 250W / (mK), which is 6-10 times that of ordinary alumina ceramics and 20%-30% higher than aluminum nitride ceramics. It is a dielectric material with unique electrical, thermal and mechanical properties.

[0043] The main component of aluminum nitride ceramic substrate is aluminum nitride ceramic, which has the characteristics of high thermal conductivity, high melting point, strength, high insulation, low dielectric constant, low dielectric loss and good packaging process adaptability. Among them, the thermal conductivity of aluminum nitride ceramic reaches 180W / (mK), which is 6-10 times that of ordinary alumina ceramic substrate.

[0044] Specifically, the present invention fixes the LED light source on the heat dissipation substrate 10 through the eutectic layer 20. Preferably, the material of the eutectic layer is a gold-tin alloy, wherein the mass percentage of tin is 20-30%. During the welding process, based on the mass percentage of tin in the gold-tin alloy being 20-30%, a relatively low temperature can melt the alloy and wet the device, effectively improving the solidification time and heat dissipation performance of the gold-tin alloy. More preferably, the material of the eutectic layer is a gold-tin alloy, wherein the mass percentage of tin is 23-27%.

[0045] In order to improve the power of the LED lamp bead so that the lamp bead can emit light of any color, the light source includes at least one flip-chip LED chip 60 and at least one group of RGB light sources 70. The RGB light source 70 includes a red LED chip 71, a green LED chip 72 and a blue LED chip 73.

[0046] Specifically, the number of flip-chip LED chips can be 3, 4, 5, 6, 8, or even more. The flip-chip LED chips can be connected in parallel or in series, or a mixture of parallel and series. The number of LED light sources of the three colors of red, green, and blue can be 2, 3, or even more. The number of LED light sources of each color of red, green, and blue can be equal or unequal. All red LED chips can be connected in parallel or in series, or a mixture of series and parallel. All blue LED chips can be connected in parallel or in series, or a mixture of series and parallel. All green LED chips can be connected in parallel or in series, or a mixture of series and parallel.

[0047] It should be noted that all the flip-chip LED chips, red LED chips, green LED chips, and blue LED chips are independent of each other and can be controlled separately. By controlling the red, green, and blue chips separately, a 160,000 true color display effect can be achieved based on the principle of three primary colors.

[0048] The LED lamp beads of the present invention can be used for stage lighting, emitting white light most of the time and emitting colored light according to stage effects.

[0049] Since the flip-chip LED chip of the present invention is directly eutectic on the heat dissipation substrate, no wire bonding is required, so space can be saved and more chips can be arranged on the chip of the same area. In addition, since there is a certain gap between each flip-chip LED chip, on the substrate of the same area, the use of a large area flip-chip LED chip can increase the light-emitting area and power, and improve the brightness of the lamp bead. Preferably, the size of the flip-chip LED chip is 40mil, 45mil, 55mil, 77mil or 80mil.

[0050] In addition, the red LED chip, green LED chip and blue LED chip are also flip-chip structures, wherein the size of the red LED chip is 40mil, 45mil, 55mil, 77mil or 80mil, the size of the blue LED chip is 40mil, 45mil, 55mil, 77mil or 80mil, and the size of the green LED chip is 40mil, 45mil, 55mil, 77mil or 80mil.

[0051] The encapsulation adhesive layer 40 of the present invention is divided into two types, one is to cover the flip-chip LED chip 60 , and the other is to cover the RGB light source 70 .

[0052] The encapsulation layer 40 covering the flip-chip LED chip 60 includes phosphor and silicone encapsulation, so that the flip-chip LED chip 60 emits white light. In addition, the encapsulation layer covering the RGB light source 70 includes silicone encapsulation, so that the red LED chip 71, the green LED chip 72 and the blue LED chip 73 emit light of their own colors.

[0053] It should be noted that the phosphor and the silicone encapsulation glue play an important role in the heat dissipation performance and brightness of the lamp beads. Preferably, the phosphor is an aluminate phosphor or a silicate phosphor. More preferably, the phosphor is Y3Al5O 12 :(Ce,Ca,Cd),Tb3Al5O 12 :(Ce,Ca,Cd) or (Sr,Ba,Ca)2SiO4:Eu.

[0054] Preferably, the organic silicon encapsulation glue includes polydimethylsiloxane and silicone resin. Since polydimethylsiloxane and silicone resin have high light refractive index, heat resistance and long-term stability, they can improve the heat dissipation effect and power of the lamp beads and ensure the long-term reliability of the lamp beads.

[0055] Due to the poor compatibility between phosphors and silicone encapsulants, it is difficult to evenly distribute the phosphors in the silicone encapsulant, and phosphors often agglomerate, resulting in a decrease in the mechanical and optical properties of the material. In addition, during the encapsulation and curing process, due to the large difference in density between the phosphors and the silicone encapsulant, phosphor sedimentation and stratification are likely to occur. These problems will also lead to a decrease in the optical consistency of the product, an increase in the defective rate, an increase in production costs, etc.

[0056] In order to solve the above problems, the encapsulation adhesive layer 40 covering the flip-chip LED chip 60 of the present invention further includes a coupling agent. Preferably, the coupling agent is one or more of γ-aminopropyl triethoxysilane (silane coupling agent KH550), γ-glycidyloxypropyl trimethoxysilane (silane coupling agent KH560), γ-methacryloxypropyl trimethoxysilane (silane coupling agent KH570), vinyl trimethoxysilane (silane coupling agent A-171), vinyl triethoxysilane (silane coupling agent A-151), isopropyl trioleate titanate (titanate coupling agent TC-105), monoalkoxy tris (dioctylphosphoryloxy) titanate (titanate coupling agent CT-114), isopropyl tris (dioctyl pyrophosphate) titanate (titanate coupling agent NDZ-201) or isopropoxy distearate aluminate (aluminate coupling agent DL-411-A).

[0057] A coupling agent is a compound that contains both organic and inorganic reactivity in one molecule. The coupling agent can effectively connect inorganic materials and organic materials through covalent bonds. The present invention increases the compatibility of the phosphor with the silicone encapsulation adhesive through the coupling agent, reduces the agglomeration effect, and improves the uniformity of the phosphor in the phosphor adhesive layer.

[0058] In order to accurately control the shape of the encapsulation glue layer 40 after curing, the present invention forms a metal dam 60 on the heat dissipation substrate 10, and the metal dam 60 forms two cup-shaped structures. The flip-chip LED chip 60 and the RGB light source 70 are respectively arranged in different cup-shaped structures, one of the cup-shaped structures can emit white light, and the other cup-shaped structure can emit one or more of red, blue and green light.

[0059] Specifically, the metal dam 60 is made of gold-tin alloy, nickel-gold alloy or nickel-palladium-gold alloy. The metal dam is soldered on the heat dissipation substrate using metal solder, or grown layer by layer on the heat dissipation substrate using magnetron sputtering.

[0060] Preferably, the metal dam 60 is higher than the packaging glue layer 40 .

[0061] The solder pad 50 is disposed on the substrate 10 , and the solder pad 50 is conductively connected to the flip-chip LED chip 30 .

[0062] The LED lamp bead of the present invention increases the power of the LED lamp bead by increasing the driving current and power density per unit area in a very small volume. Specifically, the power of the LED lamp bead of the present invention increases by more than 50%. Taking 5050 package as an example, the power of EMC5050 package is usually 5W to 10W, and the power of imported high-power LED 5050 package is 12W to 18W. The power of the 5050 package made by the manufacturing method of the present invention reaches 18 to 27W.

[0063] Accordingly, the present invention also provides a method for manufacturing a high-power LED lamp bead with high heat dissipation, comprising the following steps:

[0064] S1. forming a metal dam on a heat dissipation substrate, wherein the metal dam forms two cup-shaped structures;

[0065] The metal solder is welded on the heat dissipation substrate by welding, or the metal layer is grown layer by layer on the heat dissipation substrate by magnetron sputtering. Preferably, the material of the metal dam 60 is gold-tin alloy, nickel-gold alloy or nickel-palladium-gold alloy.

[0066] S2, coating the eutectic material on the heat dissipation substrate, and placing the flip-chip LED chip and the RGB light source on the eutectic material, wherein the flip-chip LED chip and the RGB light source are respectively arranged in different cup-shaped structures;

[0067] In order to improve the heat dissipation performance of the lamp beads, the heat dissipation substrate of the present invention is a beryllium oxide ceramic substrate or an aluminum nitride ceramic substrate.

[0068] The main component of beryllium oxide ceramic substrate is beryllium oxide ceramic, which has the characteristics of high thermal conductivity, high melting point, strength, high insulation, low dielectric constant, low dielectric loss and good packaging process adaptability. Among them, the thermal conductivity of beryllium oxide ceramic reaches 250W / (mK), which is 6-10 times that of ordinary alumina ceramics and 20%-30% higher than aluminum nitride ceramics. It is a dielectric material with unique electrical, thermal and mechanical properties.

[0069] The main component of aluminum nitride ceramic substrate is aluminum nitride ceramic, which has the characteristics of high thermal conductivity, high melting point, strength, high insulation, low dielectric constant, low dielectric loss and good packaging process adaptability. Among them, the thermal conductivity of aluminum nitride ceramic reaches 180W / (mK), which is 6-10 times that of ordinary alumina ceramic substrate.

[0070] In order to increase the power of the LED lamp bead so that the lamp bead can emit light of any color, the light source includes at least one flip-chip LED chip and at least one group of RGB light sources. The RGB light source includes a red LED chip, a green LED chip and a blue LED chip.

[0071] Specifically, the number of flip-chip LED chips can be 3, 4, 5, 6, 8, or even more. The flip-chip LED chips can be connected in parallel or in series, or a mixture of parallel and series. The number of LED light sources of the three colors of red, green, and blue can be 2, 3, or even more. The number of LED light sources of each color of red, green, and blue can be equal or unequal. All red LED chips can be connected in parallel or in series, or a mixture of series and parallel. All blue LED chips can be connected in parallel or in series, or a mixture of series and parallel. All green LED chips can be connected in parallel or in series, or a mixture of series and parallel.

[0072] It should be noted that all the flip-chip LED chips, red LED chips, green LED chips, and blue LED chips are independent of each other and can be controlled separately. By controlling the red, green, and blue chips separately, a 160,000 true color display effect can be achieved based on the principle of three primary colors.

[0073] Since the flip-chip LED chip of the present invention is directly eutectic on the heat dissipation substrate, no wire bonding is required, so space can be saved and more chips can be arranged on the chip of the same area. In addition, since there is a certain gap between each flip-chip LED chip, on the substrate of the same area, the use of a large area flip-chip LED chip can increase the light-emitting area and power, and improve the brightness of the lamp bead. Preferably, the size of the flip-chip LED chip is 40mil, 45mil, 55mil, 77mil or 80mil.

[0074] In addition, the red LED chip, green LED chip and blue LED chip are also flip-chip structures, wherein the size of the red LED chip is 40mil, 45mil, 55mil, 77mil or 80mil, the size of the blue LED chip is 40mil, 45mil, 55mil, 77mil or 80mil, and the size of the green LED chip is 40mil, 45mil, 55mil, 77mil or 80mil.

[0075] S3, eutecticizing the heat dissipation substrate and the flip-chip LED chip, with the eutectic temperature being 290-330°C;

[0076] Specifically, the eutectic material is a gold-tin alloy, wherein the mass percentage of tin is 20-30%. During the welding process, based on the mass percentage of tin in the gold-tin alloy being 20-30%, a lower temperature can melt the alloy and wet the device, effectively improving the solidification time and heat dissipation performance of the gold-tin alloy. More preferably, the mass percentage of tin in the eutectic material is 23-27%.

[0077] It should be noted that the eutectic temperature of the present invention only needs to be 290-330° C., and the eutectic time only needs to be 8-13 seconds.

[0078] S4, coating the fluorescent glue on the flip-chip LED chip, coating the silicone encapsulation glue on the RGB light source, and standing for 1.5-2.5 hours. When the sedimentation rate of the fluorescent powder in the fluorescent glue reaches 85% or more, curing the fluorescent glue and the silicone encapsulation glue, the curing temperature is 140-170° C., and the curing time is 2.3-3.5 hours;

[0079] The fluorescent glue includes fluorescent powder and organic silicon encapsulation glue. It should be noted that the fluorescent powder and organic silicon encapsulation glue play an important role in the heat dissipation performance and brightness of the lamp beads. Preferably, the fluorescent powder is an aluminate fluorescent powder and a silicate fluorescent powder. More preferably, the fluorescent powder is Y3Al5O 12 :(Ce,Ca,Cd),Tb3Al5O 12 :(Ce,Ca,Cd) or (Sr,Ba,Ca)2SiO4:Eu.

[0080] Preferably, the organic silicon encapsulation glue includes polydimethylsiloxane and silicone resin. Since polydimethylsiloxane and silicone resin have high light refractive index, heat resistance and long-term stability, they can improve the heat dissipation effect and power of the lamp beads and ensure the long-term reliability of the lamp beads.

[0081] Due to the poor compatibility between phosphors and silicone encapsulants, it is difficult to evenly distribute the phosphors in the silicone encapsulant, and phosphors often agglomerate, resulting in a decrease in the mechanical and optical properties of the material. In addition, during the encapsulation and curing process, due to the large difference in density between the phosphors and the silicone encapsulant, phosphor sedimentation and stratification are likely to occur. These problems will also lead to a decrease in the optical consistency of the product, an increase in the defective rate, an increase in production costs, etc.

[0082] In order to solve the above problems, the fluorescent glue of the present invention also includes a coupling agent. Preferably, the coupling agent is one or more of γ-aminopropyl triethoxysilane (silane coupling agent KH550), γ-glycidyloxypropyl trimethoxysilane (silane coupling agent KH560), γ-methacryloxypropyl trimethoxysilane (silane coupling agent KH570), vinyl trimethoxysilane (silane coupling agent A-171), vinyl triethoxysilane (silane coupling agent A-151), isopropyl trioleyl titanate (titanate coupling agent TC-105), monoalkoxy tris (dioctylphosphoryloxy) titanate (titanate coupling agent CT-114), isopropyl tris (dioctyl pyrophosphate) titanate (titanate coupling agent NDZ-201) or isopropoxy distearic acid acyloxy aluminate (aluminate coupling agent DL-411-A).

[0083] A coupling agent is a compound that contains both organic and inorganic reactivity in one molecule. The coupling agent can effectively connect inorganic materials and organic materials through covalent bonds. The present invention increases the compatibility of the phosphor with the silicone encapsulation adhesive through the coupling agent, reduces the agglomeration effect, and improves the uniformity of the phosphor in the phosphor adhesive layer.

[0084] Specifically, preparing fluorescent glue includes the following steps:

[0085] The phosphor: silicone encapsulating adhesive: coupling agent are prepared and mixed in a ratio of 1:10-13:0.1-0.7 to obtain a mixture;

[0086] The mixture is stirred and heated at a temperature of 40-70°C.

[0087] Preferably, the organic silicon encapsulation adhesive is prepared in a ratio of polydimethylsiloxane: silicone resin = 20-60: 40-80.

[0088] The present invention adjusts the ratio of the organic silicon encapsulation glue and the ratio of the fluorescent glue, so that the viscosity of the organic silicon encapsulation glue is rapidly reduced at a specific temperature, thereby improving the precipitation uniformity of the fluorescent powder.

[0089] The present invention adopts the above-mentioned phosphor sedimentation process to precipitate the phosphor to the bottom of the silicone encapsulation glue and cover the surface of the flip-chip LED chip, thereby shortening the path of the flip-chip LED chip to excite the phosphor, reducing light energy loss, and stimulating a higher luminous flux; in addition, the light and heat resistance is reduced, the heat dissipation speed inside the lamp bead is improved, and the temperature of the colloid and chip on the surface of the lamp bead is better reduced, thereby improving the heat dissipation performance of the lamp bead.

[0090] In addition, the present invention limits the flow of fluorescent glue by means of the metal dam, and can more accurately control its shape after curing, thereby achieving more precise light color control.

[0091] The above disclosure is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.

Claims

1. A high-heat dissipation and high-power LED lamp bead, characterized in that: It includes a heat dissipation substrate, a metal dam, an LED light source, a eutectic layer connecting the heat dissipation substrate and the LED light source, a packaging adhesive layer covering the LED light source, and a solder pad; The heat dissipation substrate is a beryllium oxide ceramic substrate or an aluminum nitride ceramic substrate; The LED light source includes at least one flip-chip LED chip and at least one group of RGB light sources; The metal dam forms two cup-shaped structures, and the flip-chip LED chip and the RGB light source are respectively arranged in different cup-shaped structures, one of the cup-shaped structures can emit white light, and the other cup-shaped structure can emit one or more of red, blue and green light; The material of the eutectic layer is a gold-tin alloy, wherein the mass percentage of tin is 20-30%; The encapsulation adhesive layer includes a fluorescent adhesive layer and an organic silicon encapsulation adhesive layer, wherein the organic silicon encapsulation adhesive is prepared and mixed in a ratio of polydimethylsiloxane: silicone resin = 20-60: 40-80, and the fluorescent adhesive is prepared and mixed in a ratio of fluorescent powder, organic silicon encapsulation adhesive and coupling agent in a ratio of 1:10-13:0.1-0.7; During the packaging process, the fluorescent glue is coated on the flip-chip LED chip, and the silicone encapsulation glue is coated on the RGB light source. The mixture is left to stand for 1.5-2.5 hours. When the phosphor sedimentation rate in the fluorescent glue reaches 85% or more, the fluorescent glue and the silicone encapsulation glue are cured at a curing temperature of 140-170°C and a curing time of 2.3-3.5 hours.

2. The high-heat dissipation and high-power LED lamp bead as claimed in claim 1, characterized in that: The material of the metal dam is gold-tin alloy, nickel-gold alloy, nickel-palladium-gold alloy, aluminum alloy, aluminum nitride ceramic, aluminum oxide ceramic or quartz glass; The cup-shaped structure is in the shape of a rectangle, a circle or a triangle.

3. The high-heat dissipation and high-power LED lamp bead as claimed in claim 1, characterized in that: The RGB light source includes a red LED chip, a green LED chip and a blue LED chip.

4. The high-heat dissipation and high-power LED lamp bead as claimed in claim 1, characterized in that: The organic silicon encapsulation adhesive comprises polydimethylsiloxane and silicone resin; The fluorescent powder is an aluminate fluorescent powder or a silicate fluorescent powder.

5. The high-heat dissipation and high-power LED lamp bead as claimed in claim 4, characterized in that: The encapsulation glue layer covering the flip-chip LED chip also includes a coupling agent, which is one or more of γ-aminopropyl triethoxysilane (silane coupling agent KH550), γ-glycidyloxypropyl trimethoxysilane (silane coupling agent KH560), γ-methacryloxypropyl trimethoxysilane (silane coupling agent KH570), vinyl trimethoxysilane (silane coupling agent A-171), vinyl triethoxysilane (silane coupling agent A-151), isopropyl trioleyl titanate (titanate coupling agent TC-105), monoalkoxy tris (dioctylphosphoryloxy) titanate (titanate coupling agent CT-114), isopropyl tris (dioctyl pyrophosphate) titanate (titanate coupling agent NDZ-201) or isopropoxy distearic acid acyloxy aluminate (aluminate coupling agent DL-411-A).

6. A method for manufacturing a high-heat dissipation high-power LED lamp bead as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: forming a metal dam on the heat dissipation substrate, wherein the metal dam forms two cup-shaped structures; The eutectic material is coated on the heat dissipation substrate, and the flip-chip LED chip and the RGB light source are placed on the eutectic material, wherein the eutectic material is a gold-tin alloy with a mass percentage of tin of 20-30%, and the flip-chip LED chip and the RGB light source are respectively arranged in different cup-shaped structures; The heat dissipation substrate and the flip-chip LED chip are eutectic, and the eutectic temperature is 290-330℃; Apply fluorescent glue on the flip-chip LED chip and apply silicone encapsulation glue on the RGB light source. Let it stand for 1.5-2.5 hours. When the sedimentation rate of the fluorescent powder in the fluorescent glue reaches 85% or above, cure the fluorescent glue and silicone encapsulation glue at a curing temperature of 140-170°C and a curing time of 2.3-3.5 hours.

7. The method for manufacturing a high-power LED lamp bead with high heat dissipation as claimed in claim 6, characterized in that: The RGB light source includes a red LED chip, a green LED chip and a blue LED chip; The fluorescent glue comprises fluorescent powder and organic silicon packaging glue.

8. The method for manufacturing a high-heat dissipation and high-power LED lamp bead as claimed in claim 7, characterized in that: The fluorescent glue also includes a coupling agent, which is one or more of γ-aminopropyl triethoxysilane (silane coupling agent KH550), γ-glycidyloxypropyl trimethoxysilane (silane coupling agent KH560), γ-methacryloxypropyl trimethoxysilane (silane coupling agent KH570), vinyl trimethoxysilane (silane coupling agent A-171), vinyl triethoxysilane (silane coupling agent A-151), isopropyl trioleyl titanate (titanate coupling agent TC-105), monoalkoxy tris (dioctylphospho) titanate (titanate coupling agent CT-114), isopropyl tris (dioctyl pyrophosphate) titanate (titanate coupling agent NDZ-201) or isopropoxy distearic acid acyloxy aluminate (aluminate coupling agent DL-411-A).

9. The method for manufacturing a high-heat dissipation and high-power LED lamp bead as claimed in claim 8, characterized in that: The preparation of fluorescent glue includes the following steps: The phosphor: silicone encapsulating adhesive: coupling agent are prepared and mixed in a ratio of 1:10-13:0.1-0.7 to obtain a mixture; The mixture is stirred and heated at a temperature of 40-70°C.