A method for metallizing the surface of activated carbon fiber felt for hydrogen storage, and its product and application

By metallizing the activated carbon fiber felt, the problems of high cost and short life of carbon nanofiber hydrogen storage materials are solved, and efficient hydrogen storage and desorption performance are improved.

CN110424154BActive Publication Date: 2024-10-11SHANDONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910707255.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-08-01
Publication Date
2024-10-11
Estimated Expiration
2039-08-01

AI Technical Summary

Technical Problem

Existing carbon nanofiber hydrogen storage materials have problems such as high hydrogen storage medium cost, slow desorption speed, and short cycle life, making them difficult to be suitable for large-scale storage and transportation.

Method used

By metallizing the activated carbon fiber felt, ultrasonic technology is used to conduct current treatment in the preheated metal treatment liquid to form a metal deposition layer and improve its hydrogen storage capacity.

Benefits of technology

It achieves the effects of high hydrogen storage capacity, fast desorption, recycling and long life, and improves the hydrogen storage performance of the carbon fiber felt.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110424154B_ABST
    Figure CN110424154B_ABST
Patent Text Reader

Abstract

The present invention provides a method for metallizing the surface of activated carbon fiber felt for hydrogen storage, a product and an application thereof, the method comprising carbonizing and activating the carbon fiber felt to obtain the activated carbon fiber felt, and metallizing the activated carbon fiber felt, including placing the activated carbon fiber felt in a metal treatment liquid into which an electric current is passed for ultrasonic treatment. The present invention has a simple process, convenient operation and low cost, and the surface of the monofilament fiber has a good degree of uniformity of treatment. The method can effectively control the type and thickness of the metal layer on the fiber surface, and the treated activated carbon fiber felt with a metal layer can be used in the field of hydrogen storage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of carbonaceous materials for hydrogen storage, and in particular to a method for metallizing the surface of activated carbon fiber felt for hydrogen storage, a product and an application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] The application of hydrogen energy has become the main development direction of the current new energy revolution, and the storage of hydrogen energy has become a scientific problem that needs to be solved urgently. Among them, solid hydrogen storage materials have attracted the attention of researchers due to their high safety and low energy consumption. The solid hydrogen storage materials currently under research and development mainly include alloy metal materials, carbon materials, composite chemical hydrogen compound materials, and metal organic framework compound materials. Among them, carbonaceous materials have excellent characteristics such as large hydrogen absorption capacity, light weight, and strong anti-poisoning performance. Their physical adsorption hydrogen storage capacity is also considered to be the most promising in the current new energy storage field. Among them, the more developed ones include hydrogen storage adsorption carbonaceous materials, such as activated carbon fibers, carbon nanotubes, graphene, etc. However, the inventors found that these materials still have defects. For example, although carbon nanofiber hydrogen storage has a large hydrogen storage capacity, the cost of the hydrogen storage medium is very high, and the desorption rate is slow and the cycle life is short, which is not suitable for large-scale storage and transportation. Summary of the invention

[0004] Activated carbon fiber, with its excellent porous surface characteristics, exhibits strong adsorption characteristics, and has become an economical, applicable, high hydrogen storage, fast desorption, recyclable and long life hydrogen storage adsorption material. The present invention has found in research that metallization treatment of the surface of activated carbon fiber felt can simultaneously bring into play the adsorption characteristics of the microporous structure on the surface of the single fiber of the activated carbon felt and the inherent hydrogen storage characteristics of the hydrogen storage metal, thereby more effectively improving the hydrogen storage capacity. Therefore, the present invention provides a method for metallization of the surface of activated carbon fiber felt for hydrogen storage, which performs metallization treatment on the surface of the single fiber of the carbon fiber activated felt, is simple to operate, has strong feasibility, and is suitable for production applications.

[0005] Specifically, the present invention has the following technical solutions:

[0006] In the first aspect of the present invention, a method for metallizing the surface of activated carbon fiber felt for hydrogen storage is provided, which comprises carbonizing and activating the carbon fiber felt to obtain activated carbon fiber felt, and metallizing the activated carbon fiber felt, including placing it in a metal treatment solution through which electric current is passed for ultrasonic treatment.

[0007] In the embodiment of the present invention, the metal treatment liquid needs to be preheated, which can be achieved by heating in a water bath to a temperature of 50-60° C. This treatment can improve the treatment activity and optimize the treatment effect.

[0008] In an embodiment of the present invention, after the metal treatment liquid is preheated to a certain temperature, activated carbon fiber felt is added to perform metallization treatment.

[0009] In the embodiment of the present invention, the current density during the metallization process is 0.1-10A / dm 2 , the processing time is 5-150 minutes.

[0010] In an embodiment of the present invention, the ultrasonic frequency is 16.5-40KHz, the ultrasonic power is 1000-4000W, and the voltage of the ultrasonic generator is 220V.

[0011] In certain embodiments of the present invention, the carbon fiber felt of the present invention is a high-performance pre-oxidized fiber felt, which is made of polyacrylonitrile pre-oxidized fiber felt and / or viscose-based pre-oxidized fiber felt as raw materials, and the tensile strength of the monofilament fiber in the pre-oxidized fiber felt is not less than 200MPa, such as 260-300MPa, the tensile modulus is not less than 1.0GPa, such as 1.4-1.6GPa, and the fiber body density is not less than 1.3g / cm 3 , the density of carbon felt is not less than 0.07g / m 3 , such as 0.07-0.085g / cm 3 , the carbon content of the fiber is not less than 65wt%, for example, 55-75wt%.

[0012] In certain embodiments of the present invention, the carbonization process in the activation process uses high-purity nitrogen with a purity of more than 99.99999% and an introduction pressure of not less than 0.2MPa; the heating carbonization temperature rise rate is controlled within the range of 5-15°C / min, the final carbonization temperature is controlled within the range of 1000-1500°C, the rate of introducing water vapor at the carbonization temperature is controlled within the range of 3-15g / min, the final activation time is controlled within the range of 20-50min, and after the activation treatment is completed, the cooling temperature under nitrogen protection is controlled within the range of 150-200°C. The surface pore size of the carbon felt fiber finally obtained is controlled within the range of 0.6-0.7nm.

[0013] In certain embodiments of the present invention, the carbon fiber felt comprises at least two layers of alternately stacked webs, and needle-punched fibers that are needle-punched between the alternately stacked webs to connect and fix adjacent stacked layers; in some embodiments, the density of the carbon fiber felt is 0.05-0.09 g / m 3 .

[0014] In some embodiments of the present invention, the surface pore size of the activated carbon fiber felt is not higher than 0.7 nm, or not higher than 0.65 nm, or not higher than 0.6 nm, or 0.6-0.7 nm.

[0015] In some embodiments of the present invention, the web is made of pre-oxidized fiber; wherein the pre-oxidized fiber has a tensile strength of not less than 200 MPa, a tensile modulus of not less than 1.0 GPa, and a fiber body density of not less than 1.3 g / cm 3 , the carbon content of the fiber is not less than 65wt%.

[0016] In some embodiments of the present invention, the pre-oxidized fiber is a polyacrylonitrile pre-oxidized fiber and / or a viscose-based pre-oxidized fiber.

[0017] In some embodiments of the present invention, the single-layer web has a gram weight of 10-50 g / m 2 .

[0018] In some embodiments of the present invention, the needle-punched fibers are needle-punched through the laminated web in a direction perpendicular to the laminated surface.

[0019] In certain embodiments of the present invention, the method for preparing the activated carbon fiber felt described in the present invention includes using pre-oxidized fiber as raw material, combing it into a web by a combing process; the web is stacked by a lamination process, the stacked layers are needle-punched with needle-punched fibers to obtain a fiber felt, and the fiber felt is carbonized and activated and then cooled to obtain an activated carbon fiber felt.

[0020] In an embodiment of the present invention, the present invention first uses high-performance pre-oxidized fibers as raw materials, and uses a combing process to comb them into a web; then the web is laminated using a mixed lamination process and needle-punched into a felt, and the needle-punching process controls the needle-punching density and the mixing ratio of the needle-punched fibers in the thickness direction; finally, an activation process is used to control the flow rate and temperature of the activation medium during the activation process, so as to achieve the purpose of controlling the surface pore size of the single fiber of the activated carbon fiber felt (the pore size is not greater than 0.7nm), and to prepare an activated carbon fiber felt material with controllable surface pore structure characteristics.

[0021] The pre-oxidized fiber raw material of the present invention can be selected from polyacrylonitrile pre-oxidized fiber and / or viscose-based pre-oxidized fiber. The tensile strength of the pre-oxidized fiber is not less than 200 MPa, such as 250-300 MPa, the tensile modulus is not less than 1.0 GPa, such as 1.2-2.0 GPa, and the fiber body density is not less than 1.3 g / cm 3 , for example 1.3-1.5g / cm 3 The density of carbon felt is not less than 0.07g / m 3 , such as 0.07-0.085g / cm 3, the carbon content of the fiber is not less than 65wt%, for example, 55-75wt%.

[0022] The web combing process of the present invention uses the high-performance pre-oxidized fiber as raw material for web combing, and the web combing ensures that the weight of the single-layer web is 10-50g / m 2 range, further 10-45g / m 2 , for example 10g / m 2 , 40g / m 2 or 45g / m 2 When using mixed combs of different types of fibers, the mixing ratio of the combs can be flexibly adjusted according to requirements. For example, when using mixed combs of different pre-oxidized fibers, such as mixing polyacrylonitrile pre-oxidized fibers and viscose-based pre-oxidized fibers, the mixing ratio (mass ratio) can be flexibly adjusted, such as 1:1-99 or 1-99:1, such as 1:1, 1:5 or 4:1.

[0023] The web mixed layer of the present invention can be mixed with webs of different weights to adjust the density gradient of fibers in different layers. The needling of the layer is carried out in a direction perpendicular to the layer surface (i.e., along the Z axis direction), and the needling density is controlled at 10-40 needles / cm 2 Within the range, the needle-punched fiber is selected from pre-oxidized fiber, and the needle-punched fiber can be a mixture of different pre-oxidized fibers, and the mixing ratio can be flexibly adjusted. For example, the needle-punched fiber can be a mixture of polyacrylonitrile pre-oxidized fiber and viscose-based pre-oxidized fiber, and the mixing ratio (mass ratio) of the two, that is, polyacrylonitrile pre-oxidized fiber and viscose-based pre-oxidized fiber, can be 1-99:1 or 1:1-99. In the technical solution of the present invention, the ratio is 1-10:1, especially 3-8:1, which is easier to achieve the technical purpose of the present invention, such as 3:1, 4:1 or 8:1.

[0024] The carbonization activation processing technology described in the present invention adopts a process of simultaneous carbonization and activation. The prepared carbon fiber felt is fed into the furnace of an activation furnace at room temperature, and then nitrogen is introduced into the furnace. Carbonization and heating are carried out at different heating rates. After reaching a certain temperature, water vapor is introduced. After reaching a predetermined temperature, constant temperature activation is performed for a certain time. Finally, the felt is cooled to a certain temperature under nitrogen protection, and then naturally cooled to room temperature to complete the activation and carbonization treatment of the carbon felt.

[0025] In certain embodiments of the present invention, the needle punching is performed in a direction perpendicular to the laminated surface (ie, along the Z-axis direction).

[0026] In certain embodiments of the present invention, the acupuncture density is 10-50 needles / cm 2 .

[0027] In certain embodiments of the present invention, the carbonization treatment comprises raising the temperature to 1000-1500° C. and introducing water vapor to carbonize the carbon fiber felt.

[0028] In an embodiment of the present invention, the carbonization is performed in a nitrogen atmosphere.

[0029] In certain embodiments of the present invention, the carbonization is carried out at a heating rate of 5-15°C / min to a temperature of 1000-1500°C.

[0030] In certain embodiments of the present invention, water vapor is introduced after the temperature is raised to a carbonization temperature of 1000-1500° C., and the rate of introduction of water vapor is 3-15 g / min.

[0031] In certain embodiments of the present invention, the carbonization time is 20-50 min.

[0032] In certain embodiments of the present invention, after carbonization is completed, the mixture is cooled to 150-200° C. in a nitrogen atmosphere, and then naturally cooled to room temperature.

[0033] The nitrogen described in the present invention is high-purity nitrogen with a purity of more than 99.99999% and an input pressure of not less than 0.2 MPa.

[0034] The preparation method of the invention can control the surface pore size of the prepared activated carbon fiber felt to be within the range of 0.6-0.7nm.

[0035] In an embodiment of the present invention, the activated carbonization of the present invention can be carried out by a carbonization activation heating device (such as Figure 1 The device shown in the figure is realized, and the device includes a heat preservation furnace, a heater and a temperature control device. High-purity nitrogen is introduced into the entire heat preservation furnace through a flow inlet, and the gas flow is controlled by a flow controller; at the same time, activated water vapor is introduced through the flow inlet, and the water vapor activation flow is controlled by a flow controller. Therefore, the process for preparing the activated carbon fiber felt of the present invention based on the device is particularly easy to realize technological process.

[0036] Therefore, in the preparation method of the present invention, the carbonization activation treatment can be based on the above-mentioned carbonization activation heating device or a similar device with the above-mentioned structure, which includes: feeding the above-prepared carbon fiber felt into the insulation furnace 1 at room temperature, and then introducing nitrogen into the furnace through the flow inlet 4, and controlling the nitrogen introduction pressure to be not less than 0.2MPa through the flow controller 5, controlling the heater 2 to heat up to 1000-1500℃ at a heating rate of 5-15℃ / min through the temperature control device 3, and then introducing activating water vapor through the flow inlet 6, and controlling the water vapor flow rate to 3-15g / min with the flow controller 7, carbonizing at a temperature of 1000-1500℃ for 20-50min, and then continuing to cool to 150-200℃ in a nitrogen atmosphere; and then naturally cooling to room temperature to complete the activation and carbonization treatment of the carbon fiber felt to obtain activated carbon fiber felt.

[0037] In an embodiment of the present invention, the metal treatment liquid is uniformly deposited on the surface of the single fiber of the activated carbon fiber felt during the ultrasonic vibration process to form a metal deposition treatment layer; the formed metal deposition treatment layer is washed with water and dried to obtain a metal layer, which is attached to the surface of the activated carbon fiber felt; in some embodiments of the present invention, the thickness of the metal layer is controllable in the range of 1μm-100μm.

[0038] In an embodiment of the present invention, the metal treatment liquid used in the metallization treatment of the present invention can be a conventional single metal or alloy metal treatment liquid, and the metal is, for example, nickel, copper, cobalt, magnesium or a combination thereof.

[0039] In an embodiment of the present invention, the surface metallization treatment process is carried out in a metallization surface treatment device, which is equipped with a metal treatment device, an ultrasonic generating device and electrodes.

[0040] In some embodiments of the present invention, the ultrasonic generating device adopts a parallel arrangement of multiple ultrasonic probes, and the ultrasonic probe controls the frequency and ultrasonic power of the ultrasonic probe through an ultrasonic generating source, wherein the ultrasonic frequency and power can be flexibly adjusted, wherein the ultrasonic frequency of the ultrasonic probe is selectable in the range of 16.5 to 40KHz, and the ultrasonic power is selectable in the range of 1000-4000W, and the voltage of the ultrasonic generator is 220V.

[0041] In the embodiments of the present invention, the metallization process needs to strictly control and select the current density and processing time during the process. In some embodiments of the present invention, the current density is controlled at 0.1-10A / dm 2 After the treatment power is turned on, the metal treatment liquid forms a uniformly coated surface deposit of the activated carbon fiber felt monofilament fiber through the ultrasonic vibration process in the current in the metal treatment device, that is, a carbon fiber felt with a metal layer attached to the surface is obtained.

[0042] The current density is unstable and the treatment uniformity is poor. If the treatment time is too short, such as less than 5 minutes, the treatment effect will be poor. If it is too long, such as more than 150 minutes, it will cause the fiber mechanical properties to lose. If the current density is too high, such as higher than 10A / dm 2 The fibers will be damaged.

[0043] After the deposition treatment layer is formed, it can be optionally washed with water and dried in an oven to obtain a carbon fiber felt with a metal layer attached to the surface.

[0044] The thickness of the metal layer can be controlled by adjusting factors such as current and processing time. The thickness of the metal layer after processing can be controlled between 1μm-100μm.

[0045] In an embodiment of the present invention, the present invention can obtain treatment layers of different compositions by selecting different types of treatment liquids and processes. The method described in the present invention can be used for processing treatment layers of various metals currently available. The metal layer can be a single metal layer such as nickel, magnesium, copper, cobalt, etc., or it can be various binary and ternary alloys, such as nickel-cobalt alloy.

[0046] In one embodiment of the present invention, a three-dimensional activated carbon fiber felt structure with a suitable pore structure is first prepared, and then a suitable treatment current density and surface metallization treatment time are selected on the surface of the activated carbon fiber felt according to the requirements of the metallization treatment thickness. During the treatment, the carbon fiber felt is simultaneously subjected to ultrasonic vibration operation to ensure the uniformity and stability of the treatment process, and finally a three-dimensional chopped felt-like carbon fiber structure with a uniform metallized surface layer is formed, i.e., activated carbon fiber felt for hydrogen storage.

[0047] In the second aspect of the present invention, the present invention also provides a surface metallized activated carbon fiber felt prepared by the method as described above, wherein the surface of the activated carbon fiber felt contains a metal layer, and the thickness of the metal layer is controllable between 1 μm and 100 μm.

[0048] In the third aspect of the present invention, the present invention also provides the use of the above-mentioned surface metallized activated carbon fiber felt in the field of hydrogen energy storage and / or adsorption. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] The drawings constituting part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. The embodiments of the present invention are described in detail below in conjunction with the drawings, wherein:

[0050] Figure 1The figure is a schematic diagram of a carbonization activation heating device for activated carbon fiber felt, which includes a heat-insulating furnace 1, a heater 2 and a temperature control device 3. High-purity nitrogen is introduced into the entire heat-insulating furnace 1 through a flow inlet 4, and the nitrogen flow is controlled by a flow controller 5. At the same time, water vapor for activation is introduced through a flow inlet 6, and the water vapor flow is controlled by a flow controller 7.

[0051] Figure 2 It is a schematic diagram of a metallization surface treatment device, which includes a metal treatment device 1 (treatment liquid is placed in the metal treatment device 1), an ultrasonic generating device 2 and an electrode 3, wherein 4 is a treatment sample. DETAILED DESCRIPTION

[0052] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0053] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar to or equivalent to the described content can be applied to the method of the present invention. The preferred implementation methods and materials described in the text are for demonstration purposes only.

[0054] In an embodiment of the present invention, the activation treatment may be based on Figure 1 The carbonization activation heating device shown, the activation process includes: feeding the carbon fiber felt into the heat preservation furnace 1 at room temperature, then passing nitrogen into the furnace through the flow inlet 4, and controlling the nitrogen pressure to be not less than 0.2MPa through the flow controller 5, controlling the heater 2 to heat up to 1000-1500℃ at a heating rate of 5-15℃ / min through the temperature control device 3, and then passing the activation water vapor through the flow inlet 6, and controlling the water vapor flow rate to 3-15g / min by the flow controller 7, carbonizing at 1000-1500℃ for 20-50min, and then continuing to cool to 150-200℃ in a nitrogen atmosphere; and then naturally cooling to room temperature to obtain activated carbon fiber felt. Its surface pore size is controlled to be not higher than 0.7nm, or not higher than 0.65nm, or not higher than 0.6nm, or within the range of 0.6-0.7nm.

[0055] In the embodiment of the present invention, the metallization process needs to strictly control and select the current density and processing time during the process. Figure 2The metallization surface treatment device shown in the figure is used to carry out the metallization surface treatment. The metal treatment liquid is placed in the metal treatment device 1, and the activated carbon fiber felt to be treated is also placed therein. The power is turned on to control the current density to be controlled at 0.1-10A / dm 2 , and turn on the ultrasonic generator for ultrasonic oscillation. The metallization treatment process time is controlled to be about 5-150 minutes. The metal treatment liquid forms a uniformly plated surface deposit of the activated carbon fiber felt monofilament through the ultrasonic vibration process in the metal treatment device in the electric current, that is, a carbon fiber felt with a metal layer attached to the surface is obtained. After the deposition treatment layer is formed, it can be optionally washed with water and dried in an oven. The thickness of the metal layer can be controlled by adjusting factors such as current and treatment time. The thickness of the treated metal layer can be controlled between 1μm-100μm.

[0056] In an embodiment of the present invention, the carbon fiber felt body can directly adopt a carbon fiber felt that meets the requirements of the present invention, that is, the carbon fiber felt of the present invention is a high-performance pre-oxidized fiber felt, which uses polyacrylonitrile pre-oxidized fiber and / or viscose-based pre-oxidized fiber felt as raw materials, and the tensile strength of the monofilament fiber in the pre-oxidized fiber felt is not less than 200MPa, such as 260-300MPa, the tensile modulus is not less than 1.0GPa, such as 1.4-1.6GPa, and the fiber body density is not less than 1.3g / cm 3 .

[0057] Alternatively, the carbon fiber felt that meets the requirements of the present invention is prepared by the following method:

[0058] Firstly, high-performance pre-oxidized fiber is used as raw material, and a web is formed by a combing process; then, the web is laminated by a mixed lamination process and needle-punched into a felt, and the needle-punching density in the thickness direction and the mixing ratio of the needle-punched fibers are controlled during the needle-punching process.

[0059] In the above preparation process, the pre-oxidized fiber raw material of the present invention can be selected from polyacrylonitrile pre-oxidized fiber and / or viscose-based pre-oxidized fiber, the tensile strength of the pre-oxidized fiber is not less than 200MPa, such as 250-300MPa, the tensile modulus is not less than 1.0GPa, such as 1.2-2.0GPa, and the fiber body density is not less than 1.3g / cm 3 , for example 1.3-1.5g / cm 3 , the carbon content of the fiber is not less than 65wt%, for example, 55-75wt%.

[0060] The web combing step described in the above preparation process uses the above high-performance pre-oxidized fiber (which can be a single fiber or a mixed fiber) as a raw material for web combing, and the web combing ensures that the weight of the single-layer web is 10-50g / m 2 range, further 10-45g / m 2 , for example 10g / m2 , 40g / m 2 or 45g / m 2 . When using a mixed comb web with different types of fibers, the mixing ratio of the comb web can be flexibly adjusted according to the requirements. For example, when using a mixed comb web with different pre-oxidized fibers, such as mixing polyacrylonitrile pre-oxidized fibers and viscose-based pre-oxidized fibers, the mixing ratio (mass ratio) can be flexibly adjusted, such as 1:1-99 or 1-99:1, for example 1:1, 1:5 or 4:1. The mixed stack of meshes described in the present invention can be mixed with meshes of different gram weights to adjust the density gradient of fibers in different layers. The stacking needling is carried out in a direction perpendicular to the stacking surface (i.e., along the Z-axis direction), and the density of the needling is controlled at 10-40 needles / cm 2 Within the range, the needle-punched fiber is selected from pre-oxidized fiber, and the needle-punched fiber can be a mixture of different pre-oxidized fibers, and the mixing ratio can be flexibly adjusted. For example, the needle-punched fiber can be a mixture of polyacrylonitrile pre-oxidized fiber and viscose-based pre-oxidized fiber, and the mixing ratio (mass ratio) of the two, that is, polyacrylonitrile pre-oxidized fiber and viscose-based pre-oxidized fiber, can be 1-99:1 or 1:1-99. In the technical solution of the present invention, the ratio is 1-10:1, especially 3-8:1, which is easier to achieve the technical purpose of the present invention, such as 3:1, 4:1 or 8:1.

[0061] The activated carbon fiber felt containing a metal layer on the surface prepared by the above embodiment of the present invention has a metal layer thickness controllable in the range of 1μm-100μm. Compared with the carbon fiber felt or activated carbon fiber felt that has not been metallized, the hydrogen adsorption and hydrogen storage properties are greatly improved, with the improvement range reaching 5-20%.

[0062] Specifically, according to the above preparation method, the present invention provides the following preparation examples:

[0063] Example 1

[0064] The process of activation treatment of carbon fiber felt is as follows:

[0065] The tensile strength is 285MPa, the tensile modulus is 1.6GPa, and the carbon felt density is 0.08g / cm 3 , polyacrylonitrile pre-oxidized fiber felt with a carbon content of 65% was placed in an insulating furnace, and high-purity nitrogen with a purity of more than 99.99999% at a pressure of not less than 0.2MPa was introduced, and carbonization and activation treatment were carried out simultaneously. First, the carbonization temperature was set at 1000℃, and the heating rate was 5℃ / min. Then, when the carbonization temperature was reached, water vapor was introduced at a rate of 3g / min. After 20 minutes of activation treatment, the temperature was reduced to 150℃ under nitrogen protection, and then naturally cooled to room temperature. The surface pore size of the carbon felt fiber finally obtained was controlled within the range of 0.6nm.

[0066] Metallization treatment: Use sulfamate metal treatment liquid, sulfamate nickel 420g / L, nickel chloride 5g / L, boric acid 40g / L, put the treatment liquid into the metal treatment device after preparation, heat it to 60℃ in a water bath, then put the activated carbon fiber felt into the metal treatment device, use ultrasonic generator to treat it, turn on the power during the treatment process to adjust the current density to 0.6A / dm 2 The treatment time is 120 minutes. A metal nickel layer activated carbon fiber felt with a thickness of about 1.2 μm is prepared.

[0067] Example 2

[0068] The process of activation treatment of carbon fiber felt is as follows:

[0069] The tensile strength is 260MPa, the tensile modulus is 1.5GPa, and the carbon felt density is 0.07g / m 3 , a viscose-based pre-oxidized fiber felt with a carbon content of 75% is placed in an insulating furnace, and high-purity nitrogen with a purity of more than 99.9999% at a pressure of not less than 0.3MPa is introduced, and carbonization and activation treatments are carried out simultaneously. First, the carbonization temperature is set at 1500℃, and the heating rate is 15℃ / min. Then, when the carbonization temperature is reached, water vapor is introduced at a rate of 15g / min. After 26 minutes of activation treatment, the temperature is reduced to 150℃ under nitrogen protection, and then naturally cooled to room temperature. Finally, the surface pore size of the carbon felt fiber is controlled within the range of 0.6nm.

[0070] Metallization treatment: Use sulfamate metal treatment liquid, sulfamate nickel 420g / L, nickel chloride 5g / L, boric acid 40g / L, put the treatment liquid into the metal treatment device after preparation, heat it to 50℃ in a water bath, then put the activated carbon fiber felt into the metal treatment device, use ultrasonic generator to treat it, and adjust the current density to 2A / dm 2 The treatment time is 80 minutes. A metal nickel layer activated carbon fiber felt with a thickness of about 20 μm is prepared.

[0071] Example 3

[0072] The process of activation treatment of carbon fiber felt is as follows:

[0073] The tensile strength is 260MPa, the tensile modulus is 1.5GPa, and the carbon felt density is 0.07g / m 3, a viscose-based pre-oxidized fiber felt with a carbon content of 75% is placed in an insulating furnace, and high-purity nitrogen with a purity of more than 99.99999% at a pressure of not less than 0.4MPa is introduced, and carbonization and activation treatments are carried out simultaneously. First, the carbonization temperature is set at 1400°C, and the heating rate is 12°C / min. Then, when the carbonization temperature is reached, water vapor is introduced at a rate of 12g / min. After 30 minutes of activation treatment, the temperature is reduced to 110°C under nitrogen protection, and then naturally cooled to room temperature. Finally, the surface pore size of the carbon felt fiber is controlled within the range of 0.65nm.

[0074] Metallization treatment: Use metal sulfate treatment solution, copper sulfate 200g / L, sulfuric acid 70g / L, put the treatment solution into the metal treatment device after preparation, heat it to 60℃ in a water bath, then put the activated carbon fiber felt into the metal treatment device, use ultrasonic generator to treat it, and adjust the current density to 5A / dm 2 The treatment time is 40 minutes, and a metal copper layer activated carbon fiber felt with a thickness of about 100 μm is obtained.

[0075] Example 4

[0076] The process of activation treatment of carbon fiber felt is as follows:

[0077] The tensile strength is 264MPa, the tensile modulus is 1.45GPa, and the carbon felt density is 0.085g / m 3 , the viscose-based pre-oxidized fiber felt with a carbon content of 67% is placed in an insulating furnace, and high-purity nitrogen with a purity of more than 99.99999% at a pressure of not less than 0.5MPa is introduced, and carbonization and activation treatments are carried out simultaneously. First, the carbonization temperature is set at 1500℃, and the heating rate is 8℃ / min. Then, when the carbonization temperature is reached, water vapor is introduced at a rate of 10g / min. After 33 minutes of activation treatment, the temperature is reduced to 190℃ under nitrogen protection, and then naturally cooled to room temperature. Finally, the surface pore size of the carbon felt fiber is controlled within the range of 0.7nm.

[0078] Metallization treatment: Use sulfamate metal treatment liquid, 600g / L nickel sulfamate, 1.25g / L cobalt sulfamate, 10g / L nickel chloride and 35g / L boric acid. After the treatment liquid is prepared, put it into the metal treatment device and heat it to 60°C in a water bath. Then put the activated carbon fiber felt into the metal treatment device and treat it with an ultrasonic generator. Adjust the current density to 3A / dm 2 , the treatment time is 25 minutes. The thickness of the metal nickel layer activated carbon fiber felt is about 2μm.

[0079] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for metallizing the surface of activated carbon fiber felt for hydrogen storage, comprising carbonizing and activating the carbon fiber felt to obtain the activated carbon fiber felt, and metallizing the activated carbon fiber felt, including placing the activated carbon fiber felt in a metal treatment solution in which an electric current is passed for ultrasonic treatment; The preparation method of the activated carbon fiber felt comprises: using pre-oxidized fiber as raw material, combing it into a web by a web combing process; laminating the web by a lamination process, needle-punching the laminated fiber to obtain the carbon fiber felt, and cooling the carbon fiber felt after carbonization treatment to obtain the activated carbon fiber felt; The metal treatment liquid is uniformly deposited on the surface of the single fiber of the activated carbon fiber felt during the ultrasonic vibration process to form a metal deposition treatment layer; the formed metal deposition treatment layer is washed with water and dried to obtain a metal layer, and the metal layer is attached to the surface of the activated carbon fiber felt; The thickness of the metal layer is controllable between 1 μm and 100 μm; During the metallization process, the current density is 0.1-10A / dm 2 , the processing time is 5-150 minutes; The ultrasonic frequency is 16.5-40KHz, the ultrasonic power is 1000-4000W, and the voltage of the ultrasonic generator is 220V; The carbon fiber felt carbonization activation device comprises a heat preservation furnace, a heater and a temperature control device, high-purity nitrogen is introduced into the entire heat preservation furnace through a flow inlet, and the gas flow is controlled by a flow controller; at the same time, activated water vapor is introduced through the flow inlet, and the water vapor activation flow is controlled by a flow controller; The method for carbonizing and activating the fiber felt comprises: raising the temperature to 1000-1500° C. and introducing water vapor; The heating rate is 5-15°C / min; The rate of introducing water vapor is 3-15 g / min.

2. The method according to claim 1, It is characterized in that The carbonization time is maintained at 1000-1500° C. for 20-50 minutes.

3. The method according to claim 1, It is characterized in that The carbonization is performed under a nitrogen atmosphere.

4. The method according to claim 1, It is characterized in that After carbonization and activation are completed, the mixture is cooled to 150-200° C. in a nitrogen atmosphere; and then naturally cooled to room temperature to obtain activated carbon fiber felt.

5. The method according to claim 1, It is characterized in that The carbon fiber felt comprises at least two layers of alternately stacked webs, and needle-punched fibers that are needle-punched and penetrate between the alternately stacked webs to connect and fix adjacent stacked layers.

6. The method according to claim 1, It is characterized in that The density of the carbon fiber felt is 0.05-0.09 g / m 3 .

7. The method according to claim 1, It is characterized in that The surface pore size of the activated carbon fiber felt is no greater than 0.7 nm.

8. The method according to claim 1, It is characterized in that The surface pore size of the activated carbon fiber felt is no greater than 0.65 nm.

9. The method according to claim 1, It is characterized in that The surface pore size of the activated carbon fiber felt is no greater than 0.6 nm.

10. The method according to claim 1, It is characterized in that The surface pore size of the activated carbon fiber felt is 0.6-0.7 nm.

11. The method according to claim 5, It is characterized in that The web tire is made of pre-oxidized fiber as raw material.

12. The method according to claim 11, It is characterized in that The tensile strength of the pre-oxidized fiber is not less than 200 MPa, the tensile modulus is not less than 1.0 GPa, and the fiber body density is not less than 1.3 g / cm 3 , the carbon content of the fiber is not less than 65wt%.

13. The method according to claim 12, It is characterized in that The pre-oxidized fibers are polyacrylonitrile pre-oxidized fibers and / or viscose-based pre-oxidized fibers.

14. The method according to claim 5, It is characterized in that The single-layer web has a gram weight of 10-50 g / m 2 .

15. The method according to claim 5, It is characterized in that The needle-punched fibers are needle-punched through the laminated webs in a direction perpendicular to the laminated surface.

16. The method according to claim 5, It is characterized in that The needling is performed in a direction perpendicular to the laminated surface.

17. The method according to claim 5, It is characterized in that The acupuncture density is 10-40 needles / cm 2 .

18. The method according to claim 5, It is characterized in that The carbonization treatment includes heating the carbon fiber felt to 1000-1500° C. at a rate of 5-15° C. / min in a nitrogen atmosphere and introducing water vapor at a rate of 3-15 g / min to carbonize and activate the carbon fiber felt for 20-50 minutes.

19. The method according to claim 5, It is characterized in that The method for preparing the activated carbon fiber felt further comprises cooling to 150-200° C. in a nitrogen atmosphere after the carbonization is completed; and then naturally cooling to room temperature.

20. The surface metallized activated carbon fiber felt prepared by the method according to any one of claims 1 to 19.

21. Use of the surface metallized activated carbon fiber felt according to claim 20 in the field of hydrogen energy storage and / or adsorption.