Electrophotographic photosensitive member, process cartridge, and electrophotographic apparatus

By using a copolymer of a specific triarylamine compound and a polycarbonate resin in the surface layer of the electrophotographic photosensitive member, the film density and functional group uniformity are improved, and the problems of insufficient abrasion resistance and deep scratches in low-temperature and low-humidity environments are solved. , achieving higher wear resistance and image stability.

CN110554585BActive Publication Date: 2024-10-18CANON KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN201910467065.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-05-31
Publication Date
2024-10-18
Estimated Expiration
2040-10-18

AI Technical Summary

Technical Problem

Existing electrophotographic photosensitive members have insufficient abrasion resistance when used repeatedly in low-temperature and low-humidity environments, and are prone to deep scratches, especially wear caused by hardening of foreign matter such as paper powder and cleaning blades.

Method used

A copolymer composed of a specific triarylamine compound and polycarbonate resin is used as the surface layer to enhance wear resistance and inhibit the occurrence of deep scratches by increasing the density and functional group uniformity of the film. The specific method includes using a combination of a triarylamine compound with a small molecular weight and a polycarbonate resin in the surface layer to form a high-density film, and improving the density of the film through a specific coating and drying process.

Benefits of technology

In low temperature and low humidity environments, the wear resistance of electrophotographic photosensitive components is significantly improved, the occurrence of deep scratches is reduced, and the long-term use stability and image quality of the components are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110554585B_ABST
    Figure CN110554585B_ABST
Patent Text Reader

Abstract

The present invention relates to an electrophotographic photosensitive member, a process cartridge and an electrophotographic apparatus. The electrophotographic photosensitive member includes a support and a surface layer, wherein the surface layer contains a copolymer of a composition, the composition containing at least a compound represented by the following general formula (1) and a compound represented by the following general formula (2), the content of the compound represented by the general formula (1) in the composition is 25% by mass or more and 70% by mass or less relative to the total content of the compound represented by the general formula (1) and the compound represented by the general formula (2), and the total content of the compound represented by the general formula (1) and the compound represented by the general formula (2) is 55% by mass or more relative to the total mass of the composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrophotographic photosensitive member, a process cartridge having the electrophotographic photosensitive member, and an electrophotographic apparatus having the electrophotographic photosensitive member. Background Art

[0002] In order to improve image quality and durability, various studies have been conducted on electrophotographic photosensitive members mounted to electrophotographic equipment. As an example, there is a study on improving wear resistance (mechanical durability) by using a free radical polymerizable resin for the surface layer of an electrophotographic photosensitive member (hereinafter, also referred to as a photosensitive member). Although such a surface layer has high wear resistance, deep scratches and image defects may be caused by foreign matter such as external additives and paper powder. In order to suppress the occurrence of deep scratches, Japanese Patent Application Laid-Open No. 2015-225132 discloses the use of a triarylamine compound having one methacryloyloxy group. Japanese Patent Application Laid-Open No. 2010-170077 also discloses the use of a triarylamine compound having four or more methacryloyloxy groups. Summary of the invention

[0003] The above object is achieved by the present invention described below. That is, the electrophotographic photosensitive member according to the present invention is an electrophotographic photosensitive member comprising a support and a surface layer, wherein the surface layer comprises a copolymer of a composition containing at least a compound represented by the following general formula (1) and a compound represented by the following general formula (2), wherein the content of the compound represented by the general formula (1) in the composition is 25% by mass or more and 70% by mass or less relative to the total content of the compound represented by the general formula (1) and the compound represented by the general formula (2), and the total content of the compound represented by the general formula (1) and the compound represented by the general formula (2) is 55% by mass or more relative to the total mass of the composition:

[0004]

[0005]

[0006] In the general formula (1), a and b are 0 or 1, p is an integer of 2 to 5,

[0007] In the general formula (2), e is 0 or 1, q is an integer of 2 to 5,

[0008] However, at least one of a, b and e is 1.

[0009] Furthermore, a process cartridge according to the present invention integrally supports the above-mentioned electrophotographic photosensitive member and at least one unit selected from the group consisting of a charging unit, a developing unit, a transfer unit and a cleaning unit, and is detachably mountable to a main body of an electrophotographic apparatus.

[0010] In addition, an electrophotographic apparatus according to the present invention includes the above-mentioned electrophotographic photosensitive member, a charging unit, an exposure unit, a developing unit, and a transfer unit.

[0011] Further features of the present invention will become apparent from the following description of exemplary embodiments with reference to the attached drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is a diagram showing an example of a schematic configuration of an electrophotographic apparatus having a process cartridge provided with an electrophotographic photosensitive member. DETAILED DESCRIPTION

[0013] According to the research of the present inventors, it has been found that the configuration disclosed in Japanese Patent Application Laid-Open No. 2015-225132 causes deep scratches due to repeated use under a low temperature and low humidity environment. The reason is considered to be that the paper, paper powder, and in some cases, the cleaning blade and the charging roller, etc. surrounding the photosensitive member become hard due to a drop in temperature and are easily pushed into the photosensitive member, thereby easily causing deep scratches.

[0014] In addition, the configuration disclosed in Japanese Patent Application Laid-Open No. 2010-170077 does not have sufficient wear resistance when repeatedly used under a low temperature and low humidity environment. This is considered to be because under a low temperature and low humidity environment, the vibration of the triarylamine compound having four or more methacryloyloxy groups is suppressed, and external stress cannot be dissipated as heat and reach phenomena such as scratching.

[0015] Therefore, an object of the present invention is to provide an electrophotographic photosensitive member which has high wear resistance and suppresses the occurrence of deep scratches when repeatedly used under a low-temperature and low-humidity environment.

[0016] Hereinafter, the present invention will be described in detail with reference to preferred embodiments.

[0017] The present inventors considered whether there is a method of imparting high wear resistance to the surface layer and further suppressing the occurrence of deep scratches by paying attention to the combination of materials constituting the surface layer of the electrophotographic photosensitive member to select an appropriate material.

[0018] The present inventors have focused on the density of the film constituting the surface layer as a factor controlling the suppression of the occurrence of deep scratches and the improvement of wear resistance. The present inventors believe that because the network of the polymer is made dense by increasing the density of the film, the possibility of dissipating the external friction stress as heat rather than dissipating the external friction stress as destructive energy such as wear increases. In addition, the present inventors believe that because the functional groups are uniformly present and the heterogeneity of the surface free energy can be reduced by making the network dense, the adhesion of foreign matter can be suppressed and the occurrence of deep scratches can be suppressed.

[0019] An electrophotographic photosensitive member according to one aspect of the present invention is constructed as follows. The electrophotographic photosensitive member has a support and a surface layer, wherein the surface layer comprises a copolymer of a composition containing at least a compound represented by the following general formula (1) and a compound represented by the following general formula (2),

[0020] The content of the compound represented by the general formula (1) in the composition is 25% by mass or more and 70% by mass or less relative to the total content of the compound represented by the general formula (1) and the compound represented by the general formula (2), and

[0021] The total content of the compound represented by the general formula (1) and the compound represented by the general formula (2) is 55% by mass or more relative to the total mass of the composition.

[0022]

[0023]

[0024] In the general formula (1), a and b are 0 or 1, and p is an integer of 2 or more and 5 or less.

[0025] In the general formula (2), e is 0 or 1, and q is an integer of 2 to 5.

[0026] However, at least one of a, b and e is 1.

[0027] Combining the compounds represented by the general formula (1) and the general formula (2) is effective for suppressing the occurrence of deep scratches and improving wear resistance.

[0028] It is further preferred that a, b and e are a=b=1, therefore, e=0; or a=b=0, therefore, e=1. The reason is that it is believed that the density of the film will be improved.

[0029] With regard to the compounds represented by the general formula (1) and the general formula (2), specific exemplary compounds are shown below.

[0030] Exemplary compounds of formula (1)

[0031]

[0032] Exemplary compounds of formula (2)

[0033]

[0034] More preferably, the content of the compound represented by the general formula (1) in the composition is 30% by mass or more and 60% by mass or less relative to the total content of the compound represented by the general formula (1) and the compound represented by the general formula (2).

[0035] Furthermore, it is more preferred that the total content of the compound represented by the general formula (1) and the compound represented by the general formula (2) is 70% by mass or more based on the total mass of the composition.

[0036] The present inventors speculate that the mechanism by which the above-mentioned technical problems can be solved by such a composition is as follows.

[0037] The density of the film can be increased by using a triarylamine compound having a small molecular weight as a basic skeleton of the film. Therefore, a film having a high density was produced using a triarylamine compound having a small molecular weight, and the wear resistance was evaluated.

[0038] The triarylamine compound and the polycarbonate resin shown in Table 1 were dissolved in chlorobenzene in a mass ratio of triarylamine compound / polycarbonate resin = 7 / 10. Then, a film was formed by coating an aluminum plate with the aid of a rod coater so that the film thickness was set to 20 μm and the aluminum plate was dried at 120° C. for 60 minutes. Thereafter, the amount of wear was measured using a rotary Taber's abrasion resistance tester (manufactured by Yasuda Seiki Seisakusho, Ltd.). When measuring, as wear rings, two wear rings (trade name: CS-0, manufactured by Taber Instruments Corporation) with a wrap film (trade name: C2000, manufactured by Fuji Film Corporation) were used, and a load of 4.9 N (500 g) was applied to each of the two wear rings. The weight loss before and after the rotational wear of each sample was measured, which was taken as the Taber wear amount.

[0039] This means that when the value of the wear amount shown in Table 1 is small, it is difficult to wear, and the film using the triarylamine compound shown by No.1 does not have sufficient wear resistance. In addition, it is known that the film using the triarylamine compound shown by No.2 is difficult to wear. However, due to the high oxidation potential, the charge exchange with the adjacent layer is insufficient; and due to the problem of charge accumulation, the film is not optimal as a structure constituting the surface layer. Next, the triarylamine compounds shown by No.3 and No.4 are mentioned as structures for forming films that are difficult to wear, and it is known that there is no problem with the value of the oxidation potential.

[0040] Although the compounds in Table 1 are not polymerized, as shown by No. 3 and No. 4, it is preferred for the compound to have at least one 3,4-dimethylbenzene group in terms of improving wear resistance. It is presumed that the number of portions that can dissipate heat increases as the compound has two methyl groups.

[0041] In addition, it is believed that by mixing a compound having one polymerizable functional group represented by the general formula (1) with a compound having two polymerizable functional groups represented by the general formula (2) within a specific range, a compound having a polymerizable functional group with a high degree of freedom enters the gap. Therefore, it is inferred that the film is highly dense. In addition, since the network becomes dense, it is believed that the possibility of external friction stress being dissipated as heat rather than external friction stress being dissipated as destructive energy such as wear is increased. In addition, it is inferred that the number of parts that can be heat dissipated is increased by having two methyl groups as one of the reasons for improving wear resistance.

[0042] In addition, as the density of the film increases, the functional groups tend to exist uniformly. Therefore, it is presumed that the occurrence of deep scratches is suppressed by reducing the difference in surface free energy and reducing the portion to which foreign matter is specifically attached.

[0043] The effects of the present invention can be obtained even when used repeatedly under a low-temperature and low-humidity environment.

[0044] In addition, when a methacryloxy group is used as a polymerizable functional group, the methacryloxy groups preferably react with each other, and therefore, it is known that abrasion resistance and suppression of deep scratches in a low temperature and low humidity environment are insufficient. The reason is presumed to be that the network is not dense by allowing the methacryloxy groups to preferably react with each other, and thus the density of the film is reduced. In addition, it is presumed that a portion with high surface free energy is generated, and foreign matter is easily attached. Since the attached foreign matter is difficult to roll or slide, it is thought that the foreign matter is pushed in by external impact and deep scratches occur.

[0045] In addition, when the surface layer contains a silicon-based or fluorine-based compound having high water repellency, these compounds easily move to the surface and the initial surface free energy decreases, but when the number of highly water repellent compounds present on the surface decreases, the effect decreases.

[0046] In addition, compounds having a molecular weight larger than that of the triarylamine compound used in the present invention tend to reduce wear resistance. The reason is presumably that the density is reduced.

[0047] As in the above-presumed mechanism, the compounds and composition ratios constituting the copolymer of the surface layer produce a synergistic effect, thereby obtaining the effects of the present invention.

[0048] [Table 1]

[0049]

[0050] [Electrophotographic photosensitive member]

[0051] An electrophotographic photosensitive member according to one aspect of the present invention has a support and a surface layer.

[0052] As a method for producing an electrophotographic photosensitive member, a method of preparing a coating liquid for each layer described later, applying the coating liquid in a desired layer order, and drying each layer can be mentioned. At this time, examples of the coating method of the coating liquid include dip coating, spray coating, inkjet coating, roll coating, die coating, blade coating, curtain coating, wire bar coating, ring coating, and the like. Among them, dip coating is preferred from the viewpoint of efficiency and productivity.

[0053] Hereinafter, each layer will be described.

[0054] <Support>

[0055] In the present invention, the electrophotographic photosensitive member has a support. In the present invention, the support is preferably a conductive support having conductivity. In addition, examples of the shape of the support include cylindrical, belt-shaped and sheet-shaped. Among them, a cylindrical support is preferred. In addition, the surface of the support may be subjected to electrochemical treatment such as anodizing, sandblasting, and cutting treatment, etc.

[0056] Examples of the material of the support preferably include metal, resin, glass, and the like.

[0057] Examples of the metal include aluminum, iron, nickel, copper, gold, stainless steel, or alloys thereof, etc. Among them, an aluminum support is preferred.

[0058] In addition, the resin or glass may be made conductive by treating it such as mixing it with a conductive material or coating it with a conductive material.

[0059] <Conductive layer>

[0060] In the present invention, a conductive layer may be provided on the support. By providing the conductive layer, scratches or irregularities on the surface of the support may be shielded to control light reflection on the surface of the support.

[0061] The conductive layer preferably contains conductive particles and a resin.

[0062] Examples of materials of the conductive particles include metal oxides, metals, and carbon black, etc. Examples of metal oxides include zinc oxide, aluminum oxide, indium oxide, silicon oxide, zirconium oxide, tin oxide, titanium oxide, magnesium oxide, antimony oxide, and bismuth oxide, etc. Examples of metals include aluminum, nickel, iron, nickel-chromium alloy, copper, zinc, and silver, etc.

[0063] Among them, it is preferable to use a metal oxide as the conductive particles, and in particular, it is more preferable to use titanium oxide, tin oxide, or zinc oxide as the conductive particles.

[0064] When a metal oxide is used as the conductive particles, the surface of the metal oxide may be treated with a silane coupling agent or the like, or the metal oxide may be doped with an element such as phosphorus or aluminum, or oxides of these elements.

[0065] In addition, the conductive particles may have a laminated structure having a core particle and a coating layer covering the particle. Examples of the core particle include titanium oxide, barium sulfate, zinc oxide, etc. The coating layer may be, for example, a metal oxide such as tin oxide.

[0066] In addition, when a metal oxide is used as the conductive particles, the volume average particle diameter is preferably 1 nm or more and 500 nm or less, and more preferably 3 nm or more and 400 nm or less.

[0067] Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenolic resin, alkyd resin, and the like.

[0068] In addition, the conductive layer may further contain a masking agent such as silicone oil, resin particles, and titanium oxide.

[0069] The average film thickness of the conductive layer is preferably 1 μm or more and 50 μm or less, and particularly preferably 3 μm or more and 40 μm or less.

[0070] The conductive layer can be formed by: preparing a conductive layer coating liquid containing the above-mentioned materials and a solvent; forming a coating film thereof; and drying the coating film. Examples of solvents used in the coating liquid include alcohol solvents, sulfoxide solvents, ketone solvents, ether solvents, ester solvents, and aromatic hydrocarbon solvents. Examples of a dispersion method for dispersing conductive particles in the conductive layer coating liquid include a method using a paint stirrer, a sand mill, a ball mill, or a liquid collision type high-speed disperser.

[0071] <Base Coating>

[0072] In the present invention, a primer layer may be provided on the support or the conductive layer. The primer layer can improve the adhesion function between the layers and provide a charge injection blocking function.

[0073] The primer layer preferably contains a resin. Alternatively, the primer layer can be formed as a cured film by polymerizing a composition containing a monomer having a polymerizable functional group.

[0074] Examples of the resin include polyester resins, polycarbonate resins, polyvinyl acetal resins, acrylic resins, epoxy resins, melamine resins, polyurethane resins, phenolic resins, polyvinylphenolic resins, alkyd resins, polyvinyl alcohol resins, polyethylene oxide resins, polypropylene oxide resins, polyamide resins, polyamic acid resins, polyimide resins, polyamideimide resins, cellulose resins, and the like.

[0075] Examples of the polymerizable functional group of the monomer having a polymerizable functional group include an isocyanate group, a blocked isocyanate group, a methylol group, an alkylated methylol group, an epoxy group, a metal alkoxide group, a hydroxyl group, an amino group, a carboxyl group, a thiol group, a carboxylic anhydride group, and a carbon-carbon double bond group.

[0076] In order to improve the electrical characteristics, the undercoat layer may further contain an electron transporting substance, a metal oxide, a metal, a conductive polymer, etc. Among them, the electron transporting substance and the metal oxide are preferably used.

[0077] Examples of the electron transport substance include quinone compounds, imide compounds, benzimidazole compounds, cyclopentadienylidene compounds, fluorenone compounds, xanthone compounds, benzophenone compounds, cyanovinyl compounds, halogenated aryl compounds, silole compounds, boron compounds and the like.

[0078] The undercoat layer can be formed as a cured film by using an electron transporting substance having a polymerizable functional group as the electron transporting substance and copolymerizing with a monomer having the above-mentioned polymerizable functional group.

[0079] Examples of metal oxides include indium tin oxide, tin oxide, indium oxide, titanium oxide, zinc oxide, aluminum oxide, silicon dioxide, etc. Examples of metals include gold, silver, aluminum, and the like.

[0080] In addition, the undercoat layer may further contain additives.

[0081] The average thickness of the primer layer is preferably 0.1 μm or more and 50 μm or less, more preferably 0.2 μm or more and 40 μm or less, particularly preferably 0.3 μm or more and 30 μm or less.

[0082] The undercoat layer can be formed by: preparing an undercoat layer coating solution containing the above-mentioned materials and a solvent; forming a coating film thereof; and drying and / or curing the coating film. Examples of solvents used in the coating solution include alcohol solvents, ketone solvents, ether solvents, ester solvents, and aromatic hydrocarbon solvents.

[0083] <Photosensitive layer>

[0084] The photosensitive layer of the electrophotographic photosensitive member is mainly classified into (1) a laminated photosensitive layer and (2) a single-layer photosensitive layer. (1) The laminated photosensitive layer has a charge generating layer containing a charge generating substance and a charge transporting layer containing a charge transporting substance. (2) The single-layer photosensitive layer has a photosensitive layer containing both a charge generating substance and a charge transporting substance.

[0085] (1) Laminated photosensitive layer

[0086] The laminated photosensitive layer has a charge generating layer and a charge transporting layer.

[0087] (1-1) Charge Generation Layer

[0088] The charge generating layer preferably contains a charge generating substance and a resin.

[0089] Examples of the charge generating material include azo pigments, perylene pigments, polycyclic quinone pigments, indigo pigments, and phthalocyanine pigments. Among them, azo pigments and phthalocyanine pigments are preferred. Among phthalocyanine pigments, oxytitanium phthalocyanine pigments, chlorogallium phthalocyanine pigments, and hydroxygallium phthalocyanine pigments are preferred.

[0090] The content of the charge generating substance in the charge generating layer is preferably 40% by mass or more and 85% by mass or less, and more preferably 60% by mass or more and 80% by mass or less, based on the total mass of the charge generating layer.

[0091] Examples of the resin include polyester resins, polycarbonate resins, polyvinyl acetal resins, polyvinyl butyral resins, acrylic resins, silicone resins, epoxy resins, melamine resins, polyurethane resins, phenolic resins, polyvinyl alcohol resins, cellulose resins, polystyrene resins, polyvinyl acetate resins, polyvinyl chloride resins, etc. Among them, polyvinyl butyral resins are more preferred.

[0092] In addition, the charge generation layer may further contain additives such as an antioxidant and an ultraviolet absorber. Specifically, hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds and the like may be mentioned.

[0093] The average film thickness of the charge generating layer is preferably 0.1 μm or more and 1 μm or less, and more preferably 0.15 μm or more and 0.4 μm or less.

[0094] The charge generation layer can be formed by preparing a charge generation layer coating solution containing the above-mentioned materials and a solvent; forming a coating film thereof; and drying each coating film. Examples of the solvent used for the coating solution include alcohol solvents, sulfoxide solvents, ketone solvents, ether solvents, ester solvents, and aromatic hydrocarbon solvents.

[0095] (1-2) Charge transport layer

[0096] When the electrophotographic photosensitive member has no protective layer, the charge transport layer is a surface layer in the present invention. That is, the charge transport layer contains a copolymer of a composition containing a compound represented by the general formula (1) and a compound represented by the general formula (2).

[0097] The charge transporting layer preferably contains a charge transporting substance and a resin.

[0098] Examples of the charge transporting substance include polycyclic aromatic compounds, heterocyclic compounds, hydrazone compounds, styryl compounds, enamine compounds, benzidine compounds, triarylamine compounds, and resins having groups derived from these substances. Among them, triarylamine compounds and benzidine compounds are preferred.

[0099] In addition, when the electrophotographic photosensitive member has a protective layer, the surface layer of the present invention is not a charge transport layer but a protective layer. At this time, the glass transition temperature of at least one type of charge transport substance in the charge transport layer is 70° C. or higher and the content of the charge transport substance having a glass transition temperature of 70° C. or higher is 20% by mass or more relative to the content of all charge transport substances in the charge transport layer. More preferably, the content of the charge transport substance is 40% by mass or more.

[0100] The reason is considered to be that the charge transport layer can maintain a relatively hard state under a low-temperature and low-humidity environment, and the protective layer can be a surface layer that is hardly affected by the charge transport layer, and the effect of the present invention can be more obtained.

[0101] In addition, in the case where the electrophotographic photosensitive member has a protective layer, the charge transporting substance in the charge transporting layer has no substituent of an aromatic ring, or preferably has a methyl group, an ethyl group, a phenyl group, etc. as a substituent. It is believed that the reason is that the protective layer is a surface layer that is hardly affected by the charge transporting layer, and the effect of the present invention can be obtained more.

[0102] Hereinafter, the following Table 2 shows exemplary compounds of the charge transporting substance.

[0103] [Table 2]

[0104]

[0105] The content of the charge transporting substance in the charge transporting layer is preferably 35% by mass or more and 70% by mass or less, and more preferably 40% by mass or more and 55% by mass or less, relative to the total mass of the charge transporting layer.

[0106] Examples of the resin include polyester resins, polycarbonate resins, acrylic resins, polystyrene resins, etc. Among them, polycarbonate resins and polyester resins are preferred. As the polyester resin, polyarylate resins are particularly preferred.

[0107] The content ratio (mass ratio) of the charge transporting substance and the resin is preferably from 6:10 to 20:10, more preferably from 7:10 to 12:10.

[0108] In addition, the charge transport layer may further contain additives such as an antioxidant, an ultraviolet absorber, a plasticizer, a leveling agent, a slip property imparting agent, and an abrasion resistance improving agent.

[0109] Specifically, hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, boron nitride particles and the like may be present.

[0110] The average film thickness of the charge transport layer is preferably 5 μm or more and 30 μm or less, more preferably 8 μm or more and 20 μm or less, particularly preferably 10 μm or more and 16 μm or less.

[0111] When the average film thickness of the charge transport layer is 10 μm or more and 16 μm or less and the electrophotographic photosensitive member has a protective layer as a surface layer, the film thickness of the surface layer is more preferably 17.0% or more and 21.5% or less relative to the sum of the film thickness of the surface layer and the film thickness of the charge transport layer.

[0112] This means that it is preferred that the film thickness of the charge transport layer is the film thickness of a specific surface layer (protective layer). The reason is considered to be that, since the hardness varies according to the film thickness of the charge transport layer under a low temperature and low humidity environment, by appropriately combining the film thickness of the charge transport layer and the film thickness of the surface layer, the surface layer is hardly affected by the charge transport layer, and the effect of the present invention can be obtained more.

[0113] The charge transport layer can be formed by: preparing a charge transport layer coating solution containing the above-mentioned materials and a solvent; forming a coating film thereof; and drying the coating film. Examples of the solvent used for the coating solution include alcohol solvents, ketone solvents, ether solvents, ester solvents, and aromatic hydrocarbon solvents. Among these solvents, ether solvents or aromatic hydrocarbon solvents are preferred.

[0114] (2) Single-layer photosensitive layer

[0115] The single-layer photosensitive layer can be formed by preparing a photosensitive layer coating solution containing a charge generating substance, a charge transporting substance, a resin and a solvent; forming a coating film thereof; and drying the coating film. The charge generating substance, the charge transporting substance and the resin are the same as the examples of the materials in the above-mentioned "(1) laminated photosensitive layer".

[0116] When the electrophotographic photosensitive member has no protective layer, the photosensitive layer is a surface layer of the present invention. That is, the photosensitive layer contains a copolymer of a composition containing a compound represented by the general formula (1) and a compound represented by the general formula (2).

[0117] <Protective layer>

[0118] The electrophotographic photosensitive member according to one aspect of the present invention may have a protective layer on the photosensitive layer. When the electrophotographic photosensitive member has a protective layer, the protective layer is a surface layer in the present invention.

[0119] As described above, the protective layer as the surface layer contains a copolymer of a composition containing a compound represented by the general formula (1) and a compound represented by the general formula (2).

[0120] The composition for forming the protective layer may further contain a compound having a polymerizable functional group in addition to the compound represented by the general formula (1) and the compound represented by the general formula (2). Examples of the polymerizable functional group of the compound having a polymerizable functional group include an acryloyloxy group. As the compound having a polymerizable functional group, a material having no charge transporting ability may be used. Examples of the reaction method for forming the protective layer include thermal polymerization, photopolymerization, and radiation polymerization.

[0121] The protective layer may further contain additives such as an antioxidant, an ultraviolet absorber, a plasticizer, a leveling agent, a sliding property improver, and an abrasion resistance improver.

[0122] Specifically, hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, boron nitride particles and the like may be present.

[0123] The protective layer may contain conductive particles and / or a charge transporting substance, and a resin as long as the effects of the present invention are not impaired.

[0124] Examples of the conductive particles include particles of metal oxides such as titanium oxide, zinc oxide, tin oxide, and indium oxide.

[0125] Examples of the charge transporting substance include benzidine compounds, triarylamine compounds, and the like.

[0126] Examples of the resin include polyester resins, acrylic resins, phenoxy resins, polycarbonate resins, polystyrene resins, phenol resins, melamine resins, epoxy resins, etc. Among them, polycarbonate resins, polyester resins, and acrylic resins are preferred.

[0127] The average film thickness of the protective layer is preferably 0.5 μm or more and 10 μm or less, and more preferably 1 μm or more and 7 μm or less.

[0128] The protective layer can be formed by: preparing a protective layer coating solution containing the above-mentioned materials and a solvent; forming a coating film thereof; and drying and / or curing the coating film. Examples of the solvent used in the coating solution include alcohol solvents, ketone solvents, ether solvents, sulfoxide solvents, ester solvents, and aromatic hydrocarbon solvents.

[0129] [Process cartridge and electrophotographic apparatus]

[0130] In addition, a process cartridge according to one aspect of the present invention integrally supports the above-mentioned electrophotographic photosensitive member and at least one unit selected from the group consisting of a charging unit, a developing unit, a transfer unit and a cleaning unit, and is detachably mountable to a main body of an electrophotographic apparatus.

[0131] In addition, an electrophotographic apparatus according to an aspect of the present invention includes the above-mentioned electrophotographic photosensitive member, a charging unit, an exposure unit, a developing unit, and a transfer unit.

[0132] Figure 1 An example of a schematic configuration of an electrophotographic apparatus having a process cartridge provided with an electrophotographic photosensitive member is shown.

[0133] First, reference numerals will be described.

[0134] Reference numeral 1 is an electrophotographic photosensitive member, reference numeral 2 is an axis, reference numeral 3 is a charging unit, reference numeral 4 is exposure light, reference numeral 5 is a developing unit, reference numeral 6 is a transfer unit, reference numeral 7 is a transfer material, reference numeral 8 is a fixing unit, reference numeral 9 is a cleaning unit, and reference numeral 10 is pre-exposure light.

[0135] Reference numeral 11 is a process cartridge and reference numeral 12 is a guide unit.

[0136] Reference numeral 1 is a cylindrical electrophotographic photosensitive member and is rotationally driven around an axis 2 in the direction of an arrow at a predetermined circumferential speed. The surface of the electrophotographic photosensitive member 1 is charged to a predetermined positive or negative potential by a charging unit 3. In addition, although a roller charging system using a roller-type charging member is shown in the drawings, charging systems such as a corona charging system, a proximity charging system, and an injection charging system may be adopted. Exposure light 4 is emitted from an exposure unit (not shown) to the charged surface of the electrophotographic photosensitive member 1, and an electrostatic latent image corresponding to target image information is formed on the charged surface of the electrophotographic photosensitive member 1. The electrostatic latent image formed on the surface of the electrophotographic photosensitive member 1 is developed by a toner contained in a developing unit 5, and a toner image is formed on the surface of the electrophotographic photosensitive member 1. The toner image formed on the surface of the electrophotographic photosensitive member 1 is transferred to a transfer material 7 by a transfer unit 6. The transfer material 7 on which the toner image is transferred is conveyed to the fixing unit 8, subjected to a fixing process of the toner image, and printed out to the outside of the electrophotographic apparatus. The electrophotographic apparatus may have a cleaning unit 9 for removing attachments such as toner remaining on the surface of the electrophotographic photosensitive member 1 after transfer. In addition, a so-called cleaner-less system may be used in which attachments are removed using a developing unit or the like without a separate cleaning unit. The electrophotographic apparatus may have an antistatic mechanism for removing electricity from the surface of the electrophotographic photosensitive member 1 using pre-exposure light 10 from a pre-exposure unit (not shown). In addition, in order to disassemble the processing box 11 according to an aspect of the present invention from the main body of the electrophotographic apparatus, a guide unit 12 such as a guide rail may be provided.

[0137] The electrophotographic photosensitive member according to one aspect of the present invention can be used in, for example, a laser beam printer, an LED printer, a copying machine, a facsimile machine, or a multifunctional composite machine thereof.

[0138] [Example]

[0139] The present invention will be described in more detail below with reference to Examples and Comparative Examples. The present invention is not limited to the following Examples, as long as it does not deviate from the gist of the present invention. In the description of the following Examples, "parts" are based on mass, unless otherwise indicated.

[0140] <Production of Electrophotographic Photosensitive Member>

[0141] [Example 1]

[0142] An aluminum cylinder (JIS-A3003, aluminum alloy) having a diameter of 24 mm and a length of 257.5 mm was used as a support (conductive support).

[0143] Next, prepare the following materials.

[0144] 214 parts of titanium oxide (TiO2) particles coated with oxygen-deficient tin oxide (SnO2) as metal oxide particles (average primary particle size: 230 nm)

[0145] 132 parts of phenolic resin (monomer / oligomer of phenolic resin) as a binder (trade name: Plyofen J-325, Dainippon Ink and Chemicals, Inc., resin solid content: 60% by mass)

[0146] 98 parts of 1-methoxy-2-propanol as solvent

[0147] These materials were put into a sand mill using 450 parts of glass beads having a diameter of 0.8 mm, and subjected to dispersion treatment under the conditions of a rotation number of 2,000 rpm, a dispersion treatment time of 4.5 hours, and a preset temperature of cooling water of 18° C., thereby obtaining a dispersion liquid. The glass beads were removed from the dispersion liquid by a mesh screen (mesh screen opening: 150 μm).

[0148] The surface roughening agent was added to the obtained dispersion so as to be 10% by mass relative to the total mass of the metal oxide particles and the binding material in the dispersion after removing the glass beads. Silicone resin particles (trade name: Tospearl 120, manufactured by Momentive Performance Materials Co., Ltd., average particle size: 2 μm) were used as the surface roughening agent.

[0149] In addition, silicone oil (trade name: SH28PA, manufactured by Dow Corning Toray Co., Ltd.) as a leveling agent was added to the dispersion liquid so as to be 0.01% by mass with respect to the total mass of the metal oxide particles and the binding material in the dispersion liquid.

[0150] Next, a mixed solvent of methanol and 1-methoxy-2-propanol (mass ratio: 1:1) was added to the dispersion so that the total mass of the metal oxide particles, the binder and the surface roughening agent in the dispersion (i.e., the mass of the solid content) was 67% by mass relative to the mass of the dispersion. The mixture was stirred to prepare a conductive layer coating solution.

[0151] The support was dip-coated with the conductive layer coating liquid, and heated at 140° C. for 1 hour to form a conductive layer having a film thickness of 30 μm.

[0152] Next, prepare the following materials.

[0153] 4 parts of an electron transporting substance represented by the following formula E-1

[0154] 5.5 parts of blocked isocyanate (trade name: Duranate SBN-70D, manufactured by Asahi Kasei Chemicals Corporation)

[0155] 0.3 parts of polyvinyl butyral resin (S-LEC KS-5Z, manufactured by Sekisui Chemical Co., Ltd.)

[0156] 0.05 parts of zinc (II) hexanoate as a catalyst (Mitsuwa Chemicals Co., Ltd.)

[0157] These materials were dissolved in a mixed solvent of 50 parts of tetrahydrofuran and 50 parts of 1-methoxy-2-propanol to prepare a coating liquid for an undercoat layer.

[0158] The conductive layer undercoat layer coating liquid was dip-coated and heated at 170° C. for 30 minutes to form an undercoat layer having a film thickness of 0.7 μm.

[0159]

[0160] Next, prepare the following materials.

[0161] 10 parts of hydroxygallium phthalocyanine in a crystalline form having peaks at positions of 7.5° and 28.4° in a spectrum obtained from CuKα characteristic X-ray diffraction

[0162] 5 parts of polyvinyl butyral resin (trade name: S-LEC BX-1, manufactured by Sekisui Chemical Co., Ltd.)

[0163] These materials were added to 200 parts of cyclohexanone and dispersed in a sand mill using glass beads having a diameter of 0.9 mm for 6 hours.

[0164] 150 parts of cyclohexanone and 350 parts of ethyl acetate were further added to the mixture and diluted to obtain a charge generating layer coating solution. The undercoat layer was dip-coated with the obtained coating solution and dried at 95° C. for 10 minutes to form a charge generating layer having a thickness of 0.20 μm.

[0165] In addition, the measurement of X-ray diffraction was performed under the following conditions.

[0166] [Powder X-ray diffraction measurement]

[0167] Measuring instrument used: X-ray diffractometer RINT-TTRII, manufactured by Rigaku Denki Co., Ltd.

[0168] X-ray tube: Cu

[0169] Tube voltage: 50KV

[0170] Tube current: 300mA

[0171] Scanning method: 2θ / θ scanning

[0172] Scanning speed: 4.0° / min

[0173] Sampling interval: 0.02°

[0174] Starting angle (2θ): 5.0°

[0175] Stop angle (2θ): 40.0°

[0176] Accessories: Standard sample holder

[0177] Filter: Not used

[0178] Incident Monochromator: Use

[0179] Counter Monochromator: Not used

[0180] Diverging Slits: Open

[0181] Divergence longitudinal limiting slit: 10.00mm

[0182] Scattering slits: Open

[0183] Light receiving slit: Open

[0184] Flat-plate monochromator: Use

[0185] Counter: Scintillation counter

[0186] Next, prepare the following materials.

[0187] 6 parts of a charge transporting material represented by the following formula C-1

[0188] · 3 parts of a charge transporting material represented by the following formula C-2

[0189] 1 part of a charge transporting material represented by the following formula C-3

[0190] 10 parts of polycarbonate (trade name: Iupilon Z400, manufactured by Mitsubishi Engineering-Plastics Corporation)

[0191] 0.02 parts of a polycarbonate resin having copolymerized units of D-1 and D-2 (x / y=0.95 / 0.05, viscosity average molecular weight=20,000)

[0192] These materials were dissolved in a mixed solvent of 25 parts of o-xylene / 25 parts of methyl benzoate / 25 parts of dimethoxymethane to prepare a charge transport layer coating liquid. The charge generation layer was dip-coated with the charge transport layer coating liquid to form a coating film, and the coating film was dried at 120° C. for 30 minutes to form a charge transport layer with a film thickness of 9 μm.

[0193] In addition, the measurement of the glass transition temperature of the charge transport material is carried out under the following conditions. As the glass transition temperature described in this application, the temperature at the intersection between the tangent line of the temperature range before the change point and the tangent line of the temperature range after the change point in the endothermic peak appearing at the second 170°C temperature increase under the following temperature conditions is adopted.

[0194] [Measurement of glass transition point]

[0195] Measuring instrument used: X-DSC7000, manufactured by Hitachi High-Tech Science Corporation

[0196] Temperature conditions:

[0197] Cool down from 25℃ to 0℃ at 10℃ / min

[0198] Keep at 0℃ for 5 minutes

[0199] Heating from 0℃ to 170℃ at 10℃ / min

[0200] Keep at 170℃ for 5 minutes

[0201] Cool down from 170℃ to 0℃ at 50℃ / min

[0202] Keep at 0℃ for 5 minutes

[0203] Heating from 0℃ to 170℃ at 10℃ / min

[0204] Keep at 170℃ for 5 minutes

[0205] Cool down from 170℃ to 25℃ at 50℃ / min

[0206] Keep at 25℃ for 5 minutes

[0207] Sample volume: 3mg

[0208] Measurement environment: Under N2 gas flow

[0209]

[0210] Next, prepare the following materials.

[0211] 21.7 parts of compound 1-5 represented by general formula (1)

[0212] 9.3 parts of compound 2-1 represented by general formula (2)

[0213] 0.2 parts of a siloxane-modified acrylic compound (BYK-3550, manufactured by BYK Japan KK)

[0214] These materials were mixed with a solvent of 20.7 parts of 1-propanol and 48.3 parts of cyclohexane and the mixture was stirred. By doing so, a surface layer coating liquid was prepared and a composition containing the compound represented by the general formula (1) and the compound represented by the general formula (2) was obtained.

[0215] The charge transport layer was dip-coated with a surface layer coating liquid to form a coating film, and the obtained coating film was dried at 50°C for 5 minutes. Thereafter, the coating film was irradiated with an electron beam for 1.6 seconds while the support (irradiated body) was rotated at a speed of 300Rpm under a nitrogen atmosphere at an accelerating voltage of 70kV and a beam current of 5.0mA. The dose at the surface position was 15kGy. Then, under a nitrogen atmosphere, the temperature of the coating film was raised to 117°C. The oxygen concentration from electron beam irradiation to subsequent heating treatment was 10ppm. Next, after the coating film was naturally cooled in an atmospheric atmosphere until the temperature of the coating film was 25°C, the coating film was subjected to a heat treatment for 1 hour at a temperature of 120°C to obtain a protective layer as a surface layer having a film thickness of 5μm. By doing so, a cylindrical (drum-shaped) electrophotographic photosensitive member having a surface layer of Example 1 was produced.

[0216] [Examples 2 to 10 and 12 to 16]

[0217] In Example 1, the compound represented by the general formula (1) and the compound represented by the general formula (2) were each changed as shown in Table 3. Here, the content ratio of the compound represented by the general formula (1) to the total content of the compound represented by the general formula (1) and the compound represented by the general formula (2) in the composition (hereinafter referred to as the ratio of the general formula (1)) was changed as shown in Table 3. In addition, the total content ratio of the compound represented by the general formula (1) and the compound represented by the general formula (2) to the total mass of the composition (hereinafter referred to as the total ratio of the general formulas (1) and (2)) was changed as shown in Table 3.

[0218] In addition, the kind and mass ratio of the charge transporting substance used to form the charge transporting layer were changed as shown in Table 4.

[0219] In addition, the film thicknesses of the surface layer and the charge transport layer and the ratio of the film thickness of the surface layer to the sum of the film thickness of the surface layer and the film thickness of the charge transport layer (hereinafter referred to as S / (S+CT) ratio) were each changed as shown in Table 5.

[0220] Except for the above, an electrophotographic photosensitive member was produced in the same manner as in Example 1. In addition, the compound represented by the general formula (1) in Example 16 was a mixture of Compound 1-3 and Compound 1-9, and the mass ratio thereof was Compound 1-3 / Compound 1-9=7 / 3.

[0221] [Example 11]

[0222] In Example 1, the compound represented by the general formula (1) and the compound represented by the general formula (2) used to form the surface layer were 10.3 parts of the compound 1-1 represented by the general formula (1) and 6.8 parts of the compound 2-2 represented by the general formula (2), respectively. In addition, 14.0 parts of the compound represented by the following formula F-1 were used for the preparation of the composition. In addition, the film thickness of the surface layer and the charge transport layer and the S / (S+CT) ratio were each changed as shown in Table 5. Except for the above, an electrophotographic photosensitive member was produced in the same manner as in Example 1.

[0223]

[0224] [Example 17]

[0225] In Example 1, the compound represented by the general formula (1) and the compound represented by the general formula (2) used to form the surface layer were 7.4 parts of the compound 1-3 represented by the general formula (1) and 17.3 parts of the compound 2-1 represented by the general formula (2), respectively. In addition, 6.2 parts of the compound represented by the following formula F-2 were used for the preparation of the composition. In addition, the film thickness of the surface layer and the charge transport layer and the S / (S+CT) ratio were each changed as shown in Table 5. Except for the above, an electrophotographic photosensitive member was produced in the same manner as in Example 1.

[0226]

[0227] [Comparative Example 1]

[0228] In Example 1, the compound represented by the general formula (1) and the compound represented by the general formula (2) used to form the surface layer were 0.03 parts of the compound 1-3 represented by the general formula (1) and 30.9 parts of the compound 2-2 represented by the general formula (2), respectively. In addition, the film thickness of the surface layer and the charge transport layer and the S / (S+CT) ratio were each changed as shown in Table 5. Except for the above, an electrophotographic photosensitive member was produced in the same manner as in Example 1.

[0229] [Comparative Example 2]

[0230] In Example 1, the compound represented by the general formula (1) and the compound represented by the general formula (2) used to form the surface layer were 10.2 parts of the compound 1-3 represented by the general formula (1) and 20.7 parts of the compound 2-2 represented by the general formula (2), respectively. In addition, the film thickness of the surface layer and the charge transport layer and the S / (S+CT) ratio were each changed as shown in Table 5. Except for the above, an electrophotographic photosensitive member was produced in the same manner as in Example 1.

[0231] [Comparative Example 3]

[0232] In Example 1, the compound represented by the general formula (1) and the compound represented by the general formula (2) used to form the surface layer were 6.2 parts of the compound 1-3 represented by the general formula (1) and 24.8 parts of the compound 2-1 represented by the general formula (2), respectively. In addition, the film thickness of the surface layer and the charge transport layer and the S / (S+CT) ratio were each changed as shown in Table 5. Except for the above, an electrophotographic photosensitive member was produced in the same manner as in Example 1.

[0233] [Comparative Example 4]

[0234] In Example 1, the compound represented by the general formula (1) and the compound represented by the general formula (2) used to form the surface layer were 24.8 parts of the compound 1-3 represented by the general formula (1) and 6.2 parts of the compound 2-1 represented by the general formula (2), respectively. In addition, the film thickness of the surface layer and the charge transport layer and the S / (S+CT) ratio were each changed as shown in Table 5. Except for the above, an electrophotographic photosensitive member was produced in the same manner as in Example 1.

[0235] [Comparative Example 5]

[0236] In Example 1, 20.7 parts of the compound 2-2 represented by the general formula (2) was used instead of the compound represented by the general formula (1). In addition, instead of the compound represented by the general formula (1), 10.2 parts of the compound represented by the following formula F-3 were used for the preparation of the composition. In addition, the film thickness of the surface layer and the charge transport layer and the S / (S+CT) ratio were each changed as shown in Table 5. Except for the above, an electrophotographic photosensitive member was produced in the same manner as in Example 1.

[0237]

[0238] [Table 3]

[0239]

[0240] [Table 4]

[0241]

[0242] [Table 5]

[0243]

[0244] <Evaluation>

[0245] Abrasion resistance, scratch resistance, and occurrence of deep scratches were evaluated under the following conditions by using the produced electrophotographic photosensitive members of Examples 1 to 17 and the electrophotographic photosensitive members of Comparative Examples 1 to 5.

[0246] As an evaluation device, by using a laser beam printer manufactured by Hewlett-Packard Company (trade name: HP Color LaserJet Enterprise M652), the drive system was modified so that the rotation speed of the electrophotographic photosensitive member was 350 mm / sec. The evaluation device was placed under a low temperature and low humidity environment with a temperature of 15°C and a relative humidity of 10% for more than 7 days. The produced electrophotographic photosensitive member was mounted to a box and placed under a low temperature and low humidity environment for more than 7 days, then mounted to the evaluation device, and 10,000 sheets of continuous paper were passed using an A4 test pattern with a printing rate of 1%. Then, one sheet was printed with a single-point knight of Japanese chess pattern.

[0247] The wear resistance was evaluated based on the degree of film loss by measuring the film thickness. The film thickness was measured under the following conditions.

[0248] Measuring instrument used: Spectral interference displacement type multilayer film thickness measuring instrument, manufactured by Keyence Corporation (spectral unit: SI-T80)

[0249] Measuring method: The generatrix direction and the circumferential direction of the cylindrical electrophotographic photosensitive member were measured at intervals of 1 mm and averaged. The measured value was the film thickness obtained by combining the charge transport layer and the outermost surface layer, and the difference in film thickness before and after continuous paper passing was calculated as the grinding amount (μm).

[0250] As for the presence or absence of occurrence of deep scratches, the image of a single-dot knight (horse of Japanese chess) pattern was visually observed, and judged based on the presence or absence of image defects.

[0251] In addition, the scratch resistance was evaluated by measuring the surface roughness. The surface roughness was measured under the following conditions.

[0252] Measuring instrument used: Stylus type surface roughness tester (trade name: SE3500), manufactured by Kosaka Laboratory Ltd.

[0253] Measuring method: The measurement is performed by moving the stylus in parallel with the length direction of the support (the axial direction of the cylinder). The measurement is performed in accordance with JIS B0601 1994, and the conditions are as follows.

[0254] Measuring length: 6.0mm

[0255] Cutoff: 0.8mm

[0256] Stylus tip shape: conical

[0257] Stylus tip angle: 60°

[0258] Stylus tip radius: 5μm

[0259] Measuring speed: 0.1mm / sec

[0260] Measurement position: The electrophotographic photosensitive member is visually observed, and the Rmax value is adopted by measuring at a portion where a scratch seems to be deep or a portion corresponding to a portion where there is an image defect on an image that seems to be caused by the scratch.

[0261] The evaluation results are shown in Table 6.

[0262] [Table 6]

[0263]

[0264] According to the present invention, there is provided an electrophotographic photosensitive member having high wear resistance and suppressing the occurrence of deep scratches when repeatedly used under a low temperature and low humidity environment.

[0265] While the present invention has been described with reference to exemplary embodiments, it is to be understood that the invention is not limited to the disclosed exemplary embodiments. The scope of the claims is to be accorded the broadest interpretation so as to encompass all such modifications and equivalent structures and functions.

Claims

1. An electrophotographic photosensitive member comprising a support and a surface layer, characterized in that The surface layer comprises a copolymer of a composition containing at least a compound represented by the following general formula (1) and a compound represented by the following general formula (2), The content of the compound represented by the general formula (1) in the composition is 25% by mass or more and 70% by mass or less relative to the total content of the compound represented by the general formula (1) and the compound represented by the general formula (2), and The total content of the compound represented by the general formula (1) and the compound represented by the general formula (2) is 55% by mass or more relative to the total mass of the composition: In the general formula (1), a and b are 0 or 1, and p is an integer of 2 to 5: In the general formula (2), e is 1, and q is an integer of 2 to 5.

2. An electrophotographic photosensitive member according to claim 1, wherein a charge generating layer, a charge transporting layer and a surface layer are sequentially provided on the support, the film thickness of the charge transporting layer is 10 μm or more and 16 μm or less, and the film thickness of the surface layer is 17.0% or more and 21.5% or less relative to the sum of the film thickness of the surface layer and the film thickness of the charge transporting layer.

3. The electrophotographic photosensitive member according to claim 2, wherein the glass transition temperature of at least one charge transporting substance in the charge transporting layer is 70° C. or higher, and the content of the charge transporting substance having a glass transition temperature of 70° C. or higher is 20% by mass or more relative to the content of all charge transporting substances in the charge transporting layer.

4. A processing box, characterized in that: Its integrated support The electrophotographic photosensitive member according to claim 1, and at least one unit selected from the group consisting of a charging unit, a developing unit, a transfer unit and a cleaning unit, the process cartridge being detachably mountable to a main body of an electrophotographic apparatus.

5. An electronic photographic device, characterized in that: It includes the electrophotographic photosensitive member according to claim 1, a charging unit, an exposure unit, a developing unit, and a transfer unit.

Citation Information

Patent Citations

  • Electrophotographic photoreceptor, manufacturing method of electrophotographic photoreceptor, processing cartridge, and image forming apparatus

    JP2010170077A

  • Electrophotographic photosensitive member, method of producing the same, process cartridge, and electrophotographic apparatus