Method for processing SOI substrate in single wafer cleaner
By using a rotary motion system and synchronous distribution technology in a single wafer cleaner, combined with nitrogen cushion protection, the problem of increased HF defects in SOI substrates in single wafer cleaners is solved, and efficient cleaning of FDSOI substrates is achieved, significantly reducing Number of HF defects and risk of damage to the silicon surface layer.
Patent Information
- Application Number
- CN201910851920.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-09-11
- Filing Date
- 2019-09-10
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2039-09-10
AI Technical Summary
When cleaning SOI substrates in a single wafer cleaner, the number of HF defects on FDSOI wafers increases significantly, requiring improved cleaning or etching methods to reduce these defects.
A system that uses rotational motion in a single wafer cleaner is used to hold the substrate and distribute a first solution by spraying on the front side of the substrate through a first nozzle, a second solution on the back side through a second nozzle, and a low or medium pressure spray on the front side via a third nozzle. Pressure liquid jet, dispense the second solution on the backside only when the first or third solution is dispensed, and form a nitrogen gas cushion between the front side of the substrate and the screen plate to protect the surface, the collector position changes only at low rotation speeds, To synchronize distribution and limit splashback.
Significantly reduces the number of HF defects on FDSOI substrates in single wafer cleaners, by 30% to 40% relative to standard processes, and reduces the risk of mechanical damage to the silicon surface layer through simultaneous distribution and nitrogen cushion protection mechanisms.
Smart Images

Figure CN110890270B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of microelectronics. In particular, the present invention relates to a method for cleaning a SOI (Silicon On Insulator) substrate using a single wafer cleaner. Background Art
[0002] Single wafer cleaners (SWC) are often used in microelectronics processes because of their high performance when cleaning large diameter wafers (especially 300 mm). In particular, single wafer cleaners can limit certain defects at the wafer edge as are usually associated with batch cleaners, which work via a series of immersions in a chemical bath. With single wafer cleaners, the risk of cross contamination between wafers of the same batch is also lower. Finally, these cleaners allow greater flexibility in the choice of cleaning processes, which can be adapted to individual wafers if necessary.
[0003] In a single wafer cleaner, the wafer is held by fingers around its periphery and moved by rotation during multiple cleaning or thinning (chemical etching) processes. An arm for dispensing chemical solutions and / or rinsing solutions is configured to move over the wafer; the dispensed solution is spread over the entire surface of the wafer by the centrifugal effect and thrown over the edge of the wafer. A plurality of conical collectors arranged in the space around the periphery of the wafer allow for the selective collection of chemical solutions dispensed continuously during the cleaning or thinning process. The collectors are able to change height relative to the wafer, so that each collector can be positioned to collect a specific solution when it is thrown over the edge of the wafer, thereby avoiding the mixing of incompatible chemical solutions.
[0004] The single wafer cleaner can be used, for example, for final cleaning and / or thinning of the silicon surface layer of SOI wafers, in particular final cleaning and / or thinning of FDSOI (fully depleted SOI) wafers having a very thin silicon layer (typically between a few nanometers and tens of nanometers).
[0005] Applicants have observed a 500% increase in the number of HF defects on FDSOI wafers with a surface silicon layer thickness of approximately 10 nm to 12 nm when final cleaning was performed in a single wafer cleaner compared to similar cleaning in a chemical bath multi-wafer cleaner (approximately two defects per wafer). Although these data are susceptible to variation with the nature of the surface layer, the increase in HF defects is still significant and there appears to be a need for improved methods of cleaning or etching SOI substrates in single wafer cleaners.
[0006] Recall that HF defects correspond to surface or bulk defects in the silicon surface layer that provide a path through the surface layer down to the underlying oxide layer of the SOI substrate. These defects are revealed by immersing the wafer in a hydrofluoric acid (HF) solution, which attacks the oxide layer by penetrating the surface layer and makes the defects apparent.
[0007] Purpose of the Invention
[0008] The present invention aims to overcome all or some of the above disadvantages. The present invention relates to a method of cleaning and / or thinning a SOI wafer in a single wafer cleaner. In particular, the present invention aims to provide a solution for reducing HF defects in FDSOI substrates after cleaning in a single wafer cleaner. Summary of the invention
[0009] The present invention relates to a method for processing an SOI substrate in a single wafer cleaner, the cleaner comprising:
[0010] A system for holding the substrate, which is capable of rotational movement;
[0011] a first nozzle for dispensing the first solution in the form of a spray over the front side of the substrate;
[0012] The method is noteworthy in that the kinetic energy per unit area of the droplet is less than or equal to 30 J / m2.
[0013] According to other advantageous and non-limiting features of the invention, which may be implemented individually or in any technically feasible combination:
[0014] The spray is formed by a mixture of a first liquid solution exhibiting a flow rate of 0.1 L / min to 0.2 L / min and nitrogen exhibiting a flow rate less than or equal to 70 L / min, preferably less than or equal to 60 L / min;
[0015] The single wafer cleaner includes a second nozzle for dispensing a second solution over the back side of the substrate, and the second solution is dispensed over the back side of the substrate only when the front side is protected by dispensing the first solution or by forming a nitrogen gas cushion;
[0016] The single wafer cleaner comprises a third nozzle for dispensing a third solution in the form of a low-pressure or medium-pressure liquid jet over the front side of the substrate and dispensing a second solution over the back side of the substrate only when the front side is protected by dispensing the third solution or the first solution or by forming a nitrogen gas cushion;
[0017] forming a nitrogen cushion between the front face of the substrate and a sieve plate which is positioned parallel to and a short distance from said front face and is capable of releasing nitrogen under pressure;
[0018] The dispensing of the solution over the back side of the substrate is synchronized with the dispensing of the solution over the front side of the substrate;
[0019] The single wafer cleaner comprises a plurality of conical collectors arranged in the space around the substrate to collect the solution after dispensing, and the positions of the respective collectors are changed only when the speed of the rotational movement of the system for holding the substrate is lower than or equal to 600 r / min. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Other features and advantages of the present invention will be readily understood through the following detailed description with reference to the accompanying drawings, in which:
[0021] - Figure 1a (i) and Figure 1a (ii) shows a schematic diagram of a single wafer cleaner;
[0022] - Figure 1b shows a stacked diagram of the front side of a plurality of FDSOI substrates processed according to standard processing in a single wafer cleaner;
[0023] - Figure 2 , Figure 3 and Figure 4 Each shows a stacked diagram of the front side of a plurality of FDSOI substrates processed according to the first embodiment, the second embodiment and the third embodiment of the method of the present invention, respectively. DETAILED DESCRIPTION
[0024] The present invention relates to a method of processing an SOI substrate in a single wafer cleaner (SWC).
[0025] Such a cleaner comprises a processing chamber in which is positioned a system (not shown) for clamping a substrate 1 to be processed. Typically, but not limitingly, said system comprises at least three fingers for mechanically holding the substrate 1 around its periphery. The clamping system is capable of a rotational movement which is transmitted to the substrate 1 during the treatment process.
[0026] The single wafer cleaner further comprises at least one nozzle 10, 30 for dispensing at least one solution over the front side 1a of the substrate 1. Recall that the front side 1a of the substrate 1 is the so-called active side. In particular for SOI substrates, the active side is the free side of the silicon surface layer. The nozzle 10, 30 is usually carried by a movable arm capable of positioning the nozzle 10, 30 substantially facing the center of the substrate 1 and / or capable of being moved over the substrate, for example by moving back and forth in an arc. The solution dispensed by the nozzle 10, 30 is spread over the entire surface of the substrate 1 by the centrifugal effect.
[0027] Various types of liquid solutions may be dispensed over the front side 1a of the substrate 1. For example, the following acidic or alkaline chemical solutions may be cited: hydrofluoric acid (HF), hydrochloric acid (HCl), sulfuric acid (H 2 SO 4 ), ozone (O 3 ), SC2-standard cleaning solution 2 (HCl / H 2 O 2 / H 2 O), SC1-standard cleaning solution 1 (NH 3 / H 2 O 2 / H 2 O), and variable concentrations of compounds or rinses (ultrapure water).
[0028] They can be distributed in the form of a low-pressure or medium-pressure liquid jet (usually 0.5 L / min to 2.5 L / min) or in the form of a spray. The spray is formed by mixing a high-pressure gas with a low-pressure liquid of the desired solution. The gas used is usually nitrogen.
[0029] The single wafer cleaner comprises in particular a first nozzle 10 which allows dispensing a first solution in the form of a spray in order to dispense over the front side 1a of the substrate 1. In the remainder of this specification, the term "first solution" will refer to any solution dispensed in the form of a spray over the front side 1a of the substrate 1. The first solution may be selected from the various liquid solutions mentioned above.
[0030] Spray dispensing is generally used to effectively remove specific contaminants from the surface of the substrate 1. In order to clean substrates made of silicon, whether exposed or with a uniform layer, whether structured or not, the spray is generally formed by a mixture of nitrogen with a flow rate between 0.5 L / min and 250 L / min and a liquid (the first solution, which may be, for example, an SC1 solution) with a flow rate between 50 mL / min and 300 mL / min.
[0031] The single wafer cleaner advantageously comprises at least one nozzle 20 for dispensing at least one solution over the back side 1b of the substrate 1 (opposite to its front side 1a). The nozzle 20 may be carried by a fixed arm capable of positioning the nozzle substantially facing the center of the substrate 1 on the back side 1b. Alternatively, the arm may be movable capable of positioning the nozzle 20 substantially facing the center of the substrate 1 and / or moving under the substrate (e.g. by moving back and forth in an arc). The solution dispensed by the nozzle 20 is spread over the entire back side 1b of the substrate 1 by the centrifugal effect.
[0032] Various types of liquid solutions, particularly those mentioned above for dispensing over the front side 1a, can be dispensed over the back side 1b of the substrate 1. Typically, the solution can be dispensed in the form of a low-pressure or medium-pressure liquid jet (typically 0.5L / min to 2.5L / min).
[0033] The single wafer cleaner comprises in particular a second nozzle 20 allowing the second solution to be dispensed, for dispensing over the back side 1 b of the substrate 1. In the remainder of this description, the term "second solution" will refer to any solution dispensed over the back side 1 b of the substrate 1.
[0034] Advantageously, the single-wafer cleaner comprises at least one other nozzle 30 (called "third nozzle") which allows dispensing a solution in the form of a low-pressure or medium-pressure liquid jet over the front side 1a of the substrate. In the remainder of this description, the term "third solution" will refer to any solution dispensed in the form of a low-pressure or medium-pressure liquid jet over the front side 1a of the substrate 1. The third solution may be selected from the plurality of liquid solutions mentioned above.
[0035] The single wafer cleaner advantageously comprises a plurality of collectors 40, which are arranged in a space ( Figure 1a (i)) and is intended to selectively collect the first solution, the second solution and / or the third solution used to process the substrate 1. Each collector 40 is conical in shape and can change height relative to the substrate 1; therefore, each collector 40 can be positioned to collect a specific solution when it is thrown over the edge of the wafer ( Figure 1a (ii)).
[0036] For example, the cleaning process is as follows:
[0037] Ozone (O 3 )
[0038] Rinse (DIW, deionized water)
[0039] SC1 or SC2
[0040] SC1 Spray (dispensed in spray form)
[0041] · Rinse (DIW)
[0042] SC2
[0043] · Rinse (DIW)
[0044] This cleaning process can be used to remove organic, particulate and metallic contaminants from SOI substrates. Table 1 shows a standard treatment applied to a substrate in a single wafer cleaner. Table 1 contains standard parameters for such a process according to the prior art (e.g., applied to an exposed silicon substrate or a silicon substrate with a uniform layer (e.g., oxide)). The various ingredients are given between brackets in Table 1 (NH in the case of SC1). 3 / H 2 O 2 / H 2 O, and in the case of SC2 it is HCl / H 2 O 2 / H 2 O) ratio, and the flow rates through the first nozzle 10, the second nozzle 20 and the third nozzle 30 are given.
[0045]
[0046] Table 1
[0047] In steps 1 , 2 , 3 , 5 , 6 and 7 , the third nozzle 30 dispenses in the form of a low-pressure or medium-pressure liquid jet (flow rate of about 2 L / min) over the front side 1 a of the substrate 1 .
[0048] In step 4, the SC1 solution is dispensed from the first nozzle 10 in the form of a spray; the spray is formed by a mixture of the first solution (SC1 in this embodiment) at a flow rate of 0.05 L / min and nitrogen at a flow rate of 100 L / min.
[0049] The applicant applied this standard process to an SOI substrate 1 in a single wafer cleaner. As is known, an SOI substrate comprises a silicon surface layer and a buried silicon oxide layer, which are located on a carrier substrate. SmartCut TM The SOI substrate is manufactured by a process based on the implantation of light hydrogen and / or helium ions into a donor substrate and, for example, bonding by molecular adhesion of the donor substrate to a carrier substrate, a silicon oxide layer is inserted between the two substrates. Then, a separation step allows a thin surface layer to be separated from the donor substrate, flush with a weakening plane defined by the implantation depth of the ions. A finishing step (which may include a high temperature heat treatment) finally provides the active layer with the required surface and crystal quality. The process is particularly suitable for the manufacture of very thin silicon surface layers. The step of finishing the SOI substrate also includes a process of cleaning and / or thinning the silicon surface layer.
[0050] Specifically, the standard process was applied to a FDSOI substrate comprising a silicon surface layer with a thickness of 10 nm and a buried silicon oxide with a thickness of 30 nm.
[0051] This cleaning process makes it possible to clean the front side 1a and the back side 1b of the SOI substrate 1 as for a silicon substrate; when the SC1 solution is dispensed over the front side 1a, it also allows the silicon surface layer to be thinned by a few nanometers in order to remove surface defects or to achieve a precise layer thickness.
[0052] Figure 1b A stack of the front side 1a of about 30 FDSOI substrates treated according to the standard process in a single wafer cleaner and after HF defects have been revealed is shown. The average number of HF defects on each wafer after treatment (represented by the points on the stack) is about five times greater than in the case of similar treatment in a chemical bath multi-wafer cleaner.
[0053] It should be noted that these graphs were obtained using an instrument for detecting defects (threshold value 0.1 μm) based on a dark field microscope (for example, KLA-TENCOR Surfscan SP (registered trademark)).
[0054] It is worth noting that according to the processing method of the present invention, the step of spraying and dispensing the first solution over the front surface of the FDSOI substrate is performed so that the kinetic energy per unit area of the droplets in the spray is less than or equal to 30 J / m 2 This kinetic energy per unit area corresponds to the energy transferred when the droplet hits the wafer 1. The value of the kinetic energy is calculated based on the following equation:
[0055]
[0056] Where m is the mass of the droplet, v is the velocity of the droplet, and r is the radius of the droplet.
[0057] Reference may be made to systems and techniques known in the art for characterizing the exit velocity of droplets in a spray.
[0058] For example, in the single wafer cleaner used here, for spray distribution, the nitrogen flow rate is 45 L / min, and the kinetic energy of the droplets is about 3.35E-9 J. The impact area of the droplets is about 3.14E-10 m 2 Therefore, the energy per unit area is about 10 J / m 2 .
[0059] In particular, the Applicant has observed that the spraying of these droplets on the front side 1a of the SOI substrate 1 tends to mechanically damage the silicon surface layer, and that the damage increases as the thickness of this layer decreases, especially for thicknesses less than 50 nm. The damage manifests itself as micropores or crystal defects that pass through the silicon surface layer, which is the cause of the increase in HF defects.
[0060] Table 2, Table 3 and Table 4 each show the processes applied to a substrate in a single wafer cleaner according to the first embodiment, the second embodiment and the third embodiment of the method of the present invention, respectively.
[0061] Table 2 gives the main parameters of a first embodiment of the method according to the invention. In step 4, a first solution (SC1) is dispensed in the form of a spray formed by a mixture of:
[0062] The first solution has a flow rate between 0.1 L / min and 0.2 L / min, preferably between 0.15 L / min and 0.2 L / min;
[0063] and nitrogen, with a flow rate of less than or equal to 70 L / min, preferably less than or equal to 60 L / min.
[0064] In this configuration, the kinetic energy per unit area of the droplet reaching the front side 1a of the SOI substrate 1 is less than or equal to 30 J / m 2 , which avoids or substantially reduces damage to the silicon surface layer.
[0065] The example used here is of spray dispensing a first (SC1 type) solution, but the nature of the solution is not critical and in particular it can be selected from the various types of solutions mentioned above. In any case, the method according to the invention provides that the energy per unit area of the droplets in the spray reaching the front side 1a of the SOI substrate 1 is lower than or equal to 30 J / m 2 , in order to limit mechanical damage to the silicon surface layer.
[0066] Preferably, the kinetic energy per unit area of the droplets in the spray will be chosen to be higher than 2 J / m 2 , in order to keep the efficiency of cleaning the substrate surface high.
[0067]
[0068] Table 2
[0069] Figure 2 A stack-up of the front side of about 30 FDSOI substrates after applying the method according to the first embodiment in a single wafer cleaner and after HF defects have been revealed. Figure 1b The average number of HF defects on each substrate was reduced by about 30% to 40%, which represents a significant improvement over the standard process.
[0070] Advantageously, during the method, the second solution is dispensed over the back side 1 b of the substrate 1 only when the front side 1 a of said substrate 1 is protected by dispensing the first solution or the third solution.
[0071] Table 3 gives the main parameters of the second embodiment of the method according to the present invention. In this second embodiment, if the first solution or the third solution is not dispensed (on the front side 1a), the second solution is not dispensed (on the back side 1b). The second embodiment also includes the optimization parameters of step 4 mentioned in the first embodiment.
[0072]
[0073] Table 3
[0074] The applicant has determined that liquid thrown from the back side 1b (second solution) over the edge of the substrate 1 can splash back onto the front side 1a of the substrate 1 (particularly through the conical wall of the splash collector 40). If the silicon surface layer is exposed, this splash back tends to mechanically damage it. This damage again manifests itself as micropores or crystal defects that pass through the silicon surface layer and tends to cause HF defects.
[0075] In contrast, if the silicon surface layer is covered by a liquid layer (when dispensing of the first solution or the third solution is performed), the back splashing has no detrimental effect on the surface layer.
[0076] According to this second embodiment, the distribution over the front side (from the first nozzle 10 or from the third nozzle 30) and the distribution over the back side (from the second nozzle 20) occur simultaneously. This is called synchronized distribution. This involves taking into account the time required to deliver the distributed solution to each of the faces 1a, 1b simultaneously, the time required mainly depending on the length of the tube used to supply the solution. This synchronization allows limiting or eliminating the time during which one of the faces 1a, 1b remains unprotected by one of the distributed solutions, thereby limiting the risk of damage to the unprotected face. By synchronizing the distribution over the front side with the distribution over the back side, the variability of the angle of exit of the first solution, the second solution and / or the third solution from the edge of the substrate 1 is also limited, thereby reducing the risk of splashing back out of the conical wall of the collector 40.
[0077] Figure 3 A stack-up of the front side of about 30 FDSOI substrates after applying the method according to the second embodiment in a single wafer cleaner and after HF defects have been revealed. Figure 2 (First embodiment), the average number of HF defects on each wafer was reduced by about 20%, which represents a significant improvement over the first embodiment of the method and a significant improvement over the standard process.
[0078] It should be noted that the simultaneous dispensing over the front side 1 a and over the back side 1 b can be achieved independently of the optimization of the dispensing of the first solution in the form of a spray over the front side 1 a .
[0079] According to a variation of the second embodiment, the front side 1a of the substrate 1 is protected by forming a nitrogen cushion while dispensing the second solution over the back side 1b of the substrate 1. Preferably, a nitrogen cushion is formed between the front side of the SOI substrate and a screen plate, which is positioned parallel to the front side and at a short distance (typically about 1 to 2 mm) therefrom; the screen plate is capable of releasing a nitrogen flow under pressure, which prevents projection from the edge of the substrate 1 back to the front side 1a.
[0080] In the same way that the liquid layer protects the silicon surface layer from splashback from dispensing over the back side, the gas layer also allows limiting this detrimental effect.
[0081] Advantageously, throughout the method, when the speed of the rotational movement of the system for holding the substrate 1 is lower than or equal to 600 r / min, the position of each of the plurality of collectors 40 of the single wafer cleaner is changed.
[0082] Table 4 gives the main parameters of this third embodiment of the method according to the invention. This third embodiment includes the optimizations mentioned in the first and second embodiments and includes an action to limit the rotation speed of the substrate 1 when the position of the collector 40 is changed. This limiting action makes it possible to limit the back splashing out of the conical wall of the collector 40 onto the front side 1a of the substrate 1.
[0083]
[0084] Table 4
[0085] Figure 4 A stack-up of the front side of about 30 FDSOI substrates after applying the method according to the third embodiment in a single wafer cleaner and after HF defects have been revealed. Figure 3 (Second embodiment), the average number of HF defects on each wafer was reduced by about 20%, which represents a substantial improvement over the first and second embodiments of the method and over the standard process.
[0086] It should be noted that when the position of the collector 40 is changed, limiting the rotation speed of the wafer can be achieved independently of the simultaneous distribution over the front side 1a and over the back side 1b and / or independently of optimizing the distribution of the first solution in the form of a spray over the front side 1a.
[0087] The method according to the invention is particularly suitable for processing SOI substrates featuring thin (silicon and oxide) layers with a thickness of less than 50 nm, and in particular substrates with a silicon surface layer thickness of less than 20 nm.
[0088] Of course, the invention is not limited to the embodiments and examples described and variant embodiments may be introduced therein without departing from the scope of the invention as defined in the claims.
Claims
1. A method for processing an SOI substrate (1) in a single wafer cleaner, the single wafer cleaner include: a system for holding the substrate (1), the system being capable of rotational movement; A first nozzle (10) for dispensing a first solution in the form of a spray over the front side (1a) of the substrate (1), wherein the kinetic energy per unit area of the droplets is less than or equal to 30 J / m 2 ;as well as A second nozzle (20) is used to dispense a second solution over the back side (1b) of the substrate (1), and wherein the second solution is dispensed over the back side (1b) of the substrate (1) only when the front side (1a) is protected by dispensing the first solution or by forming a nitrogen pad.
2. The method according to claim 1, in, The spray is formed from a mixture of a first liquid solution exhibiting a flow rate between 0.1 L / min and 0.2 L / min and nitrogen gas exhibiting a flow rate less than or equal to 70 L / min.
3. The method according to claim 2, in, The flow rate of the first liquid solution is between 0.15 L / min and 0.2 L / min.
4. The method according to claim 2, in, The flow rate of the nitrogen is less than or equal to 60 L / min.
5. The method according to claim 1, in, The single wafer cleaner comprises a third nozzle (30) for dispensing a third solution in the form of a low-pressure or medium-pressure liquid jet over the front side (1a) of the substrate (1), and wherein the second solution is dispensed over the back side (1b) of the substrate (1) only when the front side (1a) is protected by dispensing the third solution or the first solution or by forming a nitrogen pad.
6. The method according to claim 1, in, The nitrogen cushion is formed between the front side (1a) of the substrate and a sieve plate, which is positioned parallel to and a short distance from the front side (1a) and is capable of releasing nitrogen under pressure.
7. The method according to claim 1, in, The dispensing of the solution over the back side (1 b) of the substrate (1) is synchronized with the dispensing of the solution over the front side (1 a) of the substrate (1).
8. The method according to claim 1, in, The single wafer cleaner comprises a plurality of conical collectors (40) which are arranged in the space around the substrate (1) so as to collect the solution after distribution, and wherein the position of each collector (40) is changed only when the speed of the rotational movement of the system for clamping the substrate is less than or equal to 600 r / min.