Cutting Tools

By designing an exposed part that is not covered by the coating on the cutting tool edge and adopting a gradient thickness coating structure, the problems of coating surface defects and sticking chips in the existing technology are solved, and high-precision and high-smooth cutting effects are achieved.

CN110976992BActive Publication Date: 2024-10-29SHENZHENSHI YUZHAN PRECISION TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN201911300046.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-13
Publication Date
2024-10-29
Estimated Expiration
2039-12-13

AI Technical Summary

Technical Problem

In high-precision machining of existing cutting tools, the coating surface finish is low, inconsistency, and defects such as droplets and pits lead to film chipping and chip sticking on the cutting edge, resulting in a dull machined surface and low machine yield, which is difficult to satisfy. Super finishing requirements.

Method used

A cutting tool is designed. Its cutting edge includes an exposed part that is not covered by the coating. The gradient part of the coating thickness is thinner closer to the exposed part and thicker away from the exposed part. It satisfies Tmin/Tmax≤0.58. Combined with the uniform thickness part, The formed thickness gradient coating structure avoids droplets and stress concentration and ensures edge consistency.

Benefits of technology

Through the combination of the exposed edge structure and the thickness gradient coating, the cutting performance is significantly improved, the friction and adhesion are reduced, the tool life is extended, and high-finish and high-precision processing effects are achieved. It is suitable for metals, alloys, plastics and Superfinishing of composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110976992B_ABST
    Figure CN110976992B_ABST
Patent Text Reader

Abstract

The present invention provides a cutting tool. The cutting tool includes a cutting edge and a coating formed on the cutting edge. The cutting edge includes a front cutting face, a back cutting face and a cutting edge connected between the front cutting face and the back cutting face. The cutting edge includes an exposed portion that is not covered by the above-mentioned coating. The coating includes a thickness gradient portion. The thickness of the thickness gradient portion is thinner as it is closer to the exposed portion, and thicker as it is farther away from the exposed portion. The thickness gradient portion satisfies Tmin / Tmax≤0.58, wherein Tmin is the thickness of the thinnest part of the coating thickness gradient portion at the end where the coating thickness is thinner, and Tmax is the thickness of the thickest part of the coating thickness gradient portion at the end where the coating thickness is thicker. The width W of the exposed portion is k*Tmax, 0.2≤k≤20.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of mechanical finishing, and in particular to a cutting tool capable of realizing super finishing. Background Art

[0002] With the continuous development of science and technology, the demand for precision processing of various workpieces is getting higher and higher. For example, metal cutting processing has gradually developed from ordinary rough and fine processing to super-fine processing and nano-level processing. The cutting processing of the surface of metal workpieces is even expected to achieve the requirements of mirror effect directly without subsequent polishing.

[0003] In the past, uncoated bare tools could be used to cut metal workpieces with relatively low requirements for machining accuracy and surface roughness. However, for high finish, high brightness of the cutting surface, or super-finishing requirements, tools protected by hard coatings must be used for processing. Because when uncoated bare tools are used to process metal materials, the tool edges are prone to sticking chips, and the cutting edges will wear quickly during rapid milling, making the cut metal surface foggy and dull, and even producing horizontal lines, so uncoated bare tools cannot be used in high-precision metal cutting.

[0004] Hard coatings have the characteristics of high hardness, oxidation resistance, and wear resistance. They are widely used in cutting tools, molds, and mechanical wear-resistant parts, and can effectively meet the performance and life requirements of cutting tools. However, cutting tools protected by coatings in the prior art often have the following defects: the surface finish and consistency of the tool edge coating are low, and there are defects such as droplets, pits, and sawtooth on the cutting edge; during the cutting process, the cutting edge coating often has broken films of microns or more in size, which can easily lead to sticky chips. In actual trials of various coated tools, it was found that the existing various coated tools have a low yield, large performance randomness, and low machine yield, and cannot be used on a large scale.

[0005] In response to this problem, many domestic and foreign companies and research institutions have been optimizing and improving the coating process, with the main directions being the following two aspects:

[0006] 1. Regarding the sputtering deposition process, its main drawback is that the low energy of the deposited particles leads to low bonding strength between the coating and the substrate, and between the coating grains, making it difficult to avoid the phenomenon of film breakage at the cutting edge and chip sticking during cutting. Therefore, the direction of improvement is to use high-energy pulse sputtering. High-energy pulse sputtering improves the particle bonding strength, but it will bring new problems. The furnace cavity has serious ash falling and point-like particles appear on the coating surface, resulting in poor surface finish. At the same time, the internal stress of the coating also increases, and the coating breaks at the cutting edge. At present, there is no suitable coating process in application to solve the above problems.

[0007] Second, for the cathodic arc deposition process, the main problem is the poor surface finish caused by droplets, and the large stress in the film layer will cause local film breakage during cutting. Therefore, the direction of improvement is to reduce droplets and stress. The methods include adjusting the arc flow and arc spot speed, magnetic filtration, coating time, etc. in the process to reduce droplets and reduce stress, and increase post-coating polishing to reduce droplets on the cutting edge. This solution has improved the broken film caused by droplets and stress, but there are still large problems with machine yield and life, and there is no significant effect, so the problem of broken film caused by droplets and stress still has great room for improvement.

[0008] In addition, in order to solve the impact of droplets in the above-mentioned coating on the surface of the processed product and improve the processing effect of coated tools, the industry has also explored various methods for post-processing of tool coatings in the past decade.

[0009] For example, Japanese patents, patent numbers 2105396 and 2825693, disclose methods for mechanically polishing coatings at cutting edges.

[0010] For example, Chinese invention patent 200210082479.9 discloses a method for passivating a coating by shot peening the front face of a blade having a coating formed thereon.

[0011] For example, China Invention Patent Application Publication No. 201910133238.4 discloses another method for tool coating passivation, which uses 160-1000# walnut sand and a rotation speed of 10-80r / min for 10-15min of coating passivation.

[0012] For example: China Invention Patent Application Publication No. 201711443229.2 also discloses a method of removing coating particles by using a drag-type polishing and passivation machine to polish the coating area by rotating forward for 30 minutes and reverse for 30 minutes.

[0013] For example, US Pat. No. 7,090,914 B2 also discloses that the surface roughness of the coating is preferably limited to 0.2 microns or less.

[0014] Although the above-mentioned coating post-treatment processes can reduce or remove the droplets on the coating, or optimize the surface roughness of the coating to a predetermined range, no matter which coating passivation process is used, the coating at the cutting edge of the tool after the coating passivation treatment is still very easy to peel off locally after the tool has been used for a period of time, resulting in scratches or cutting lines on the processed surface, and easily causing chips to stick to the tool tip. In short, the above-mentioned various coating process optimization methods and coating post-treatment coated tools are still difficult to meet the actual requirements in terms of performance, and the yield rate is very low, and it is impossible to carry out mass production applications. Summary of the invention

[0015] In view of this, it is necessary to provide a cutting tool with lower coating internal stress, good edge consistency, low chip sticking, and capable of achieving super finishing.

[0016] The present invention provides a cutting tool. The cutting tool includes a cutting edge and a coating formed on the cutting edge. The cutting edge includes a front cutting face, a back cutting face and a cutting edge connected between the front cutting face and the back cutting face. The cutting edge includes an exposed portion that is not covered by the above-mentioned coating. The coating includes a thickness gradient portion. The thickness of the thickness gradient portion is thinner as it is closer to the exposed portion, and thicker as it is farther away from the exposed portion. The thickness gradient portion satisfies Tmin / Tmax≤0.58, wherein Tmin is the thickness of the thinnest part of the coating thickness gradient portion at the end where the coating thickness is thinner, and Tmax is the thickness of the thickest part of the coating thickness gradient portion at the end where the coating thickness is thicker. The width W of the exposed portion is k*Tmax, 0.2≤k≤20.

[0017] Preferably, the length L of the coating thickness gradual change portion is m*Tmax, wherein cot60°≤m≤cot3°.

[0018] Preferably, the coating includes a uniform thickness portion connected to an end of the coating with a thicker thickness in the thickness gradient portion, and the thickness of the uniform thickness portion is equal to the thickness of the thickest part of the coating with a thicker thickness.

[0019] Preferably, the thickness of the coating at the thinner end of the coating thickness gradient portion is 0.

[0020] Preferably, the thickness gradient portion includes a thickness gradient portion located on the front cutting edge side and a thickness gradient portion located on the back cutting edge side, and a length Lrear of the thickness gradient portion coating on the back cutting edge side is greater than a length Lfront of the thickness gradient portion coating on the front cutting edge side.

[0021] Preferably, the thickness gradient portion includes a thickness gradient portion located on the front cutting edge side and a thickness gradient portion located on the back cutting edge side, and the thickness Tmax_rear of the thickest end of the coating of the thickness gradient portion located on the back cutting edge side and the thickness Tmax_front of the thickest end of the coating of the thickness gradient portion located on the front cutting edge side satisfy |Tmax_rear / Tmax_front-1|≤0.15.

[0022] Preferably, Lrear / Tmax_rear of the gradual thickness coating portion located on the back face side is greater than Lfront / Tmax_front of the gradual thickness coating portion located on the front face side.

[0023] Preferably, the cutting edge includes a middle area. The middle area of ​​the cutting edge includes an outward convex curved surface. The curvature of the outward convex curved surface is greater than the curvatures of the front blade face and the rear blade face. The middle area of ​​the cutting edge includes the above-mentioned exposed portion.

[0024] Conventional technology generally believes that the closer the cutting edge is to the cutting edge, the smaller the angle and the thinner the structure, which is more susceptible to wear during high-speed cutting. Therefore, a hard coating must be used to cover the cutting edge, and the cutting edge coating must meet a certain thickness after subsequent passivation treatment to provide adequate protection for the "fragile" cutting edge.

[0025] However, the applicant has found that if the cutting edge is covered with a coating, a two-phase structure of the cutting edge substrate and the coating material is formed at the cutting edge of the cutting edge. This fundamentally determines that no matter what coating deposition process is used or what coating material is selected, it is difficult to ensure the consistency of the microstructure of the tool cutting edge. Therefore, the tool yield is very low and the performance is very random.

[0026] The present invention overcomes the inherent technical prejudice in the field for a long time, exposes part of the middle area of ​​the cutting edge, and sets a thickness gradient coating. Since the exposed cutting edge is completely made of a single material of the cutting edge substrate, the consistency of the cutting edge is naturally ensured, and the problems of uneven thickness, droplets, stress concentration, etc. of the cutting edge coating in the prior art are completely avoided. During cutting, the exposed cutting edge substrate is mainly used to cut the workpiece. Since the exposed cutting edge is completely made of a single material and has better consistency, the cutting performance is significantly improved. At the same time, the present invention does not mainly utilize the hard coating to increase wear resistance and assist cutting, but mainly utilizes the lubrication, chip guiding, and chip removal functions of the thickness gradient coating, reduces friction during the cutting process, reduces the adhesion of chips to the tool, and thus suppresses the generation of chip accumulation, thereby reducing tool wear, improving the quality of the processed surface, and increasing the life of the tool. Through the combination of the exposed cutting edge structure and the thickness gradient coating, a technical effect unexpected by a technician in this field is obtained.

[0027] At the same time, the present invention makes the coating near the edge be designed with a gradual thickness change and ensures that the gradual thickness change portion satisfies Tmin / Tmax≤0.58 (where Tmin is the thickness of the thinnest part of the coating in the gradual thickness change portion, and Tmax is the thickness of the thickest part of the coating in the gradual thickness change portion). The closer the thickness gradual thickness change portion is to the exposed portion, the thinner it is, and the farther it is from the exposed portion, the thicker it is, and the width of the exposed portion is W=k*Tmax, 0.2≤k≤20. Such a design can greatly avoid or reduce the retention of droplets in the coating near the edge, and at the same time solve the problem of broken film caused by excessive stress at the edge.

[0028] In addition, the coating structure of the cutting tool in the present invention is designed to have a partially exposed cutting edge and a gradually distributed coating thickness at the cutting edge. This greatly expands the application scenarios compared to conventional coated tools, and can not only achieve high-gloss and high-mirror cutting of metals, but also achieve ultra-precision machining and nano-machining of other metal alloys, plastics and their composite materials.

[0029] For example, the cutting tool designed with the coating structure of the present invention can be directly used for processing molds, and can directly cut the mold steel into a mirror-like mold cavity surface with high finish without subsequent polishing treatment.

[0030] In addition, the cutting tool with the coating structure of the present invention also has an unexpected processing effect on the processing of plastic materials. For example, in the processing of holes and grooves of PCB boards, high dimensional accuracy processing can also be achieved. What is more important is that the directly processed grooves are clean and are not prone to burrs and burrs. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a three-dimensional schematic diagram of a chamfering milling cutter for machining the chamfer structure of an earphone in an embodiment of the present invention.

[0032] Figure 2 for Figure 1 The chamfer milling cutter is shown as a schematic diagram of the processing state of the above-mentioned earphone chamfer.

[0033] Figure 3 for Figure 1 The chamfer milling cutter's cutting edge is shown as a partially enlarged schematic diagram at the edge of circle III.

[0034] Figure 4 It is a three-dimensional schematic diagram of a contour milling cutter for processing a mobile phone frame in an embodiment of the present invention.

[0035] Figure 5 for Figure 4 The schematic diagram of the processing state of the contour milling cutter processing the above-mentioned mobile phone frame is shown.

[0036] Figure 6 for Figure 4 Cross-sectional view of the contour milling cutter along the VI-VI direction.

[0037] Figure 7 for Figure 6 The cutting edge of the contour milling cutter shown is a partially enlarged schematic diagram of the cutting edge at circle VII.

[0038] Figure 8 This is a microscopic morphology of the cutting edge of the magnetron sputtering coating tool A before coating treatment in the comparative test of the present invention.

[0039] Fig. 9This is a microscopic morphology of the cutting edge of the cathode arc evaporation coating tool B before coating treatment in the comparative test of the present invention.

[0040] Fig.10 This is the microscopic morphology of the cutting edge of magnetron sputtering coated tool A after coating treatment to make the coating thickness uniformly distributed (that is, A1 group tool).

[0041] Fig.11 This is the microscopic morphology of the cutting edge of the cathodic arc evaporation coated tool A after coating treatment to make the coating thickness uniformly distributed (that is, the tool of group B1).

[0042] Fig.12 yes Fig.10 The microscopic morphology of the cutting edge section of the A1 group tool is shown.

[0043] Fig.13 yes Fig.11 The microscopic morphology of the cutting edge section of the B1 group tool is shown.

[0044] Fig.14 This is a microscopic morphology of the cutting edge of the magnetron sputtering coated tool A that has been coated to make the coating thickness gradually distributed (that is, the A2 group tool) and is partially exposed.

[0045] Fig.15 This is a microscopic morphology of the partially exposed cutting edge of the cathodic arc evaporation coated tool B after coating treatment to make the coating thickness gradually distributed (that is, the B2 group tool).

[0046] Fig.16 yes Fig.14 The microscopic morphology of the cutting edge cross section of the A2 group of tools is shown.

[0047] Fig.17 yes Fig.15 The microscopic morphology of the cutting edge cross section of the B2 group of tools is shown.

[0048] Main component symbols

[0049] Handle 10

[0050] Cutting part 20, 50

[0051] Headphones 30

[0052] Mobile phone frame 60

[0053] Cutting edge 21, 51

[0054] Chip groove 23

[0055] Rake face 211, 511

[0056] Flank 212, 512

[0057] Cutting edge 213, 513

[0058] Near rake face area 216,516

[0059] Near the back face area 218,518

[0060] Middle area 219,519

[0061] Near rake edge coating 252, 552

[0062] Edge coating near the back face 254, 554

[0063] Uniform coating 257, 259, 557, 559

[0064] The following specific implementation manner will further illustrate the present invention in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION

[0065] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0066] It should be noted that when an element is considered to be "connected" to another element, it may be directly connected to the other element or there may be a centrally disposed element at the same time. When an element is considered to be "disposed on" another element, it may be directly disposed on the other element or there may be a centrally disposed element at the same time.

[0067] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0068] Please refer to Figure 1 , which is an implementation of the present invention concept applied to a chamfering milling cutter. However, it should be pointed out that the application of the invention concept of the gradient thickness coating structure of the present invention is not limited to milling cutters, but can also be applied to other cutting tools, such as taps, drills, reamers, boring tools, etc. These cutting tools that apply the present invention concept should all be considered within the protection scope of the present invention.

[0069] The chamfering milling cutter includes a tool handle 10 and a cutting portion 20 disposed at one end of the tool handle 10. The tool handle and the cutting portion 20 are integrally formed. In other applications, the milling cutter may also be a combined tool combining a cutter head and a blade, in which case the cutting edge 20 is disposed on the blade. Both the integrated tool and the combined tool should be considered within the protection scope of the present invention.

[0070] In this embodiment, the chamfering milling cutter is used to process a chamfer structure of the earphone 30 (see Figure 2 The base of the earphone chamfering structure is made of stainless steel (SUS316-Li), the handle 10 and the cutting part 20 are made of cemented carbide, and according to the different cutting materials, the material of the cutting part 20 can also be replaced by other suitable materials, such as carbon tool steel, alloy tool steel, high-speed steel, ceramics, etc., which should be regarded as within the protection scope of the present invention.

[0071] The cutting portion 20 includes a plurality of cutting edges 21, a plurality of chip grooves 23 corresponding to the cutting edges, and a coating formed on the cutting edges 21. In this embodiment, the material of the coating is an AlCrN coating, but the concept of the present invention is not limited to a specific material, and the material of the coating can also be replaced by other materials, such as a DLC coating, a cubic boron nitride coating, a TiN coating, a TiC coating, a TiCN coating, a TiAlN coating, a CrN coating, a TiSiN coating, an A12O3 coating, etc. or various composite coatings, such as a nitride / nitride coating, a nitride / carbide coating, a nitride or carbide / metal coating, a nitride / oxide coating, etc., which should be considered within the scope of protection of the present invention. The chip groove 23 guides the metal chips, so that the metal chips generated during cutting can be smoothly discharged from the chip groove 23.

[0072] Each cutting edge 21 includes a rake face 211, a flank face 212, and a cutting edge 213 at the intersection of the rake face and the flank face (see Figure 3 ). Please refer to Figure 3 , Figure 3 2 is an enlarged schematic diagram of the cutting edge 213 of the cutting edge 21. The cutting edge 213 includes a near rake face region 216 connected to the rake face 211, a near flank face region 218 connected to the flank face 212, and a middle region 219 connected between the near rake face region 216 and the near flank face region 218. The middle region 219 has an exposed region, which is not covered by the coating.

[0073] In this embodiment, the middle area 219 of the cutting edge includes an outer convex curved surface (also called R angle), and the curvature of the outer convex curved surface is greater than the curvatures of the rake face 211 and the flank face 212. The helix angle of the chamfering cutter in this embodiment is 0, and the rake face 211 and the flank face 212 are basically planes near the cutting edge 213, and the curvature of each point is 0, that is, less than the curvature of the outer convex curved surface.

[0074] Microscopically, it can be observed through a scanning electron microscope that the front cutting surface 211 and the back cutting surface 212 extend toward the cutting edge 213, and finally extend to the cutting edge 213 region used for contact and friction with the workpiece and cutting. In the cutting edge 213 region, the cutting edge near the front cutting surface region 216 and the cutting edge near the back cutting surface region 218 continue to extend and finally connect to a convex surface with a large curvature, i.e., the R angle. From a macroscopic perspective, this convex surface is the sharpest tip of the cutting edge, and is also the main area of ​​contact and friction with the processed product for cutting. The present invention defines the area at the cutting edge containing the convex surface as the cutting edge middle region 219.

[0075] It should be noted that the definition of the cutting edge near rake face region 216 and the cutting edge near flank face region 218 is only for the convenience of the reader to understand the relative position of the thickness gradient coating deposited thereon, and there is no objective physical boundary between the cutting edge near rake face region 216 and the rake face 211, and between the cutting edge near flank face region 218 and the flank face 212. The thickness gradient coating may extend from the exposed area of ​​the cutting edge to the rake face 211 or the flank face 212, or may only exist in the cutting edge 213 region.

[0076] The coating includes a near rake edge coating 252 formed in the near rake area 216 of the cutting edge 213, and a near flank edge coating 254 formed in the near flank area 228 of the cutting edge. The thickness of the near rake edge coating 252 and the near flank edge coating 254 gradually decreases along the direction of the exposed area close to the cutting edge.

[0077] In order to reduce the stress at the cutting edge and improve the consistency at the cutting edge, the thickness of the thickness gradient portion, that is, the coating 252 near the front cutting edge and the coating 254 near the back cutting edge, both satisfy Tmin / Tmax≤0.58, wherein Tmin is the thickness of the thinnest coating at the thinner end of the coating thickness gradient portion, and Tmax is the thickness of the thickest coating at the thicker end of the coating thickness gradient portion.

[0078] In this embodiment, the thickness of the coating 252 near the rake face gradually decreases along the direction close to the exposed edge area, and finally decreases to 0 at the middle edge area 219. The thickness of the coating 254 near the flank face gradually decreases along the direction close to the exposed edge area, and finally decreases to 0 at the exposed edge area.

[0079] However, it should be noted that the tooth profile design of the cutting edge may change accordingly according to the cutting requirements of different workpieces. Therefore, in the case of certain cutting edge tooth profile structures, the thickness of only one of the coating 252 near the front cutting edge or the coating 254 near the back cutting edge may be designed to gradually decrease in the direction close to the exposed area of ​​the cutting edge, while the thickness of the coating on the other side of the cutting edge remains uniform. These cutting tools with different designs should all be considered within the protection scope of the present invention.

[0080] The applicant has found that if the coating thickness is processed into a gradual distribution, and the thickness gradual change part satisfies Tmin / Tmax≤0.58, and a part of the cutting edge 213 is completely exposed and not covered by the coating, the cutting effect and machine yield will be better than the tool whose cutting edge is completely covered by the coating. However, the exposed in the present invention means not being covered by a hard coating, and being covered by other soft materials, such as a polymer coating or an organic material coating is still considered exposed and should be considered to fall within the protection scope of the present invention.

[0081] In order to further obtain better edge consistency, the width W of the exposed part can preferably meet the following conditions: W = k*Tmax, where 0.2≤k≤20. The reason for optimizing the width W of the exposed part to this range is that, on the one hand, the width W of the exposed part cannot be too small. If the width of the exposed part is too small, the structure is similar to a fully coated tool, and the consistency of the tool edge is difficult to ensure. On the other hand, the width W of the exposed part cannot be too large. If the width W of the exposed part is too large, it is similar to a bare blade, and the bare blade is prone to sticky chips, and the cutting effect will be foggy and produce horizontal stripes. It should be pointed out that the thickness Tmax of the thickest coating at the end of the coating thickness gradient part of the present invention is not limited to a specific range, and a specific Tmax and the width W of the exposed part can be designed according to the cutting needs of the specific product.

[0082] In order to further obtain better cutting performance, the length L of the gradual thickness change portion of the coating may preferably satisfy the following condition: L=m*Tmax, wherein cot60°≤m≤cot3°.

[0083] It should be pointed out that the cutting tool of the present invention is not limited to a specific size. No matter how large its blade diameter is, the length L of the coating thickness gradient portion, the thickness Tmax of the thickest coating at the thicker end of the coating thickness gradient portion, and the width W of the exposed portion of the blade edge can be determined according to actual cutting needs and the above-mentioned relationship.

[0084] The chamfering milling cutter in this embodiment has a blade diameter of 6 mm, a coating thickness Tmax of about 0.6-0.8 μm at the thicker end of the coating thickness gradient portion, a length L of about 2.6-3.1 μm, and a width W of the exposed portion of about 1.2 μm.

[0085] In this embodiment, the length Lrear of the coating layer 254 near the flank face located on the flank face side is greater than the length Lfront of the coating layer 252 near the rake face located on the rake face side.

[0086] In this embodiment, the coating includes a uniform coating 257 formed on the front cutting edge 211, and a uniform coating 259 formed on the back cutting edge 212. However, it should be noted that the connection position of the uniform coating 257 and the coating 252 near the front cutting edge is not limited to a fixed position, and can be set at the front cutting edge 211 or the front cutting edge near the front cutting edge region 216. Similarly, the connection position of the uniform coating 259 and the coating 254 near the back cutting edge is not limited to a fixed position, and can be set at the back cutting edge 212 or the back cutting edge near the back cutting edge region 218. These cutting tools with different designs should all be considered to be within the protection scope of the present invention.

[0087] Preferably, the thickness Tmax_rear of the thickest coating at the thicker end of the coating layer 254 near the flank face on the flank face side and the thickness Tmax_front of the thickest coating at the thicker end of the coating layer 252 near the rake face on the rake face side satisfy |Tmax_rear / Tmax_front-1|≤0.15. In this embodiment, the thickness Tmax_rear of the thickest coating at the thicker end of the coating layer 254 near the flank face on the flank face side is substantially equal to the thickness Tmax_front of the thickest coating at the thicker end of the coating layer 252 near the rake face on the rake face side.

[0088] In this embodiment, Lrear / Tmax_rear of the coating layer 254 near the flank face on the flank face side is greater than Lfront / Tmax_front of the coating layer 252 near the rake face on the rake face side.

[0089] See also Figure 4 , Figure 4 The present invention is conceived to be applied to an embodiment of a profile milling cutter. In this embodiment, the profile milling cutter is used to process the profile of the mobile phone frame 60 (see Figure 5). In order to make the cutting process conform to the appearance contour of the product, the rotational projection of the cutting edge of the contour milling cutter is a semi-closed concave surface. In this embodiment, the outer frame of the mobile phone is made of stainless steel (SUS316-Li) and aluminum alloy (AL7K03), and some areas contain super-hard engineering plastics and fiber composite materials. The contour milling cutter conceived by the coating structure of the present invention can not only realize the cutting process of semi-closed concave surfaces with greater processing difficulty, but also can directly cut the metal outer frame into a high-gloss mirror effect without subsequent polishing.

[0090] See also Figure 6 The profile milling cutter of this embodiment includes a plurality of spirally extending cutting edges 51 and a coating formed on the cutting edges 51. In this embodiment, the profile milling cutter has four cutting edges 51. However, it should be noted that the cutting edges of the present invention are not limited to a specific number, and a cutting tool having at least one cutting edge, as long as the coating structure of the present invention is adopted, should be considered within the protection scope of the present invention.

[0091] Figure 7 The figure shows a microscopic enlarged view of one of the cutting edges. Although the rake face and the flank face are both spirally extended curved surfaces in macroscopic terms, in microscopic terms, the rake face and the flank face are also approximately plane in cross section, and their curvature is also significantly smaller than the convex curved surface at the cutting edge 513 .

[0092] The cutting edge 51 includes a rake face 511, a flank face 512, and a cutting edge 513 connected between the rake face and the flank face. Figure 8 The cutting edge 513 includes a near rake face region 516 connected to the rake face 511, a near flank face region 518 connected to the flank face 512, and a middle region 519 connected between the near rake face region and the near flank face region. The middle region 519 includes an exposed region that is not covered by the coating.

[0093] The coating includes a near rake face edge coating 552 formed in a near rake face region 516 of the edge 513, and a near flank face edge coating 554 formed in a near flank face region 518 of the edge. The thickness of the near rake face edge coating 552 and the near flank face edge coating 554 gradually decreases along the direction close to the exposed edge region. In this embodiment, the thickness of the thinner end of the near rake face edge coating 552 and the near flank face edge coating 554 is reduced to 0 near the exposed edge region. It should be noted that the thickness of the thinner end of the coating thickness gradient portion may not be zero, but when it is not zero, it should satisfy Tmin / Tmax≤0.58.

[0094] In this embodiment, the length Lrear of the coating layer 554 near the flank face side is greater than the length Lfront of the coating layer 552 near the rake face side. The thickness Tmax_rear of the thicker end of the coating layer 554 near the flank face side at the thickest part of the coating is equal to the thickness Tmax_front of the thicker end of the coating layer 552 near the rake face side at the thickest part of the coating.

[0095] The contour milling cutter blade diameter in this embodiment is 16 mm, the coating thickness Tmax at the thicker end of the coating thickness gradient portion is about 1.2 μm, the length L of the coating thickness gradient portion is about 4.0-4.6 μm, and the width W of the exposed portion is about 2.2 μm.

[0096] Even for concave semi-enclosed contours, the exposed area of ​​the cutting edge without coating in this embodiment can achieve light cutting, and the chips can slide out smoothly from the smooth and defect-free coating surface, thereby ensuring that the cutting edge is not easy to stick to chips. At the same time, because the area of ​​the exposed area of ​​the cutting edge without coating is within a specific range, the front and rear blades of the tool are still coated, and the cutting heat is not easily transferred to the inside of the tool, which greatly reduces the degree of tool wear and can greatly increase the service life of the tool. Because the exposed area of ​​the cutting edge without coating has no unevenness and good consistency, it is easy to obtain a high-smooth surface during cutting, thereby meeting the required product processing requirements.

[0097] To further illustrate the unexpected technical effects achieved by the exposed cutting edge and gradient thickness coating structure of the present invention, the following is a comparative experiment between gradient thickness coating tools and existing uniform thickness coating tools.

[0098] Table 1 Coating scheme

[0099]

[0100] Please refer to Table 1, first use magnetron sputtering equipment and cathode arc equipment to prepare coating tool A (such as Figure 8 ) and coated tool B (such as Fig. 9 ). As can be seen from the figure, no matter the coating is directly produced by magnetron sputtering process or arc evaporation process, there are droplets.

[0101] The prepared tools A and B are divided into two groups, that is, the magnetron sputtering coated tools A are divided into groups A1 and A2, and the cathode arc evaporation coated tools B are divided into groups B1 and B2. Then, the two groups A1 and B1 are subjected to conventional post-coating processes, such as polishing, to reduce or remove defects such as droplets on the coating surface. Fig.10 This is the microscopic morphology of the cutting edge of magnetron sputtering coated tool A after the conventional post-processing to remove the droplets (that is, A1 group tool). Fig.11This is the microscopic morphology of the cutting edge of cathodic arc evaporation coated tool B after the conventional post-processing to remove the droplets (that is, B1 group tool). Fig.12 yes Fig.10 The microscopic morphology of the cutting edge section of the A1 group tool is shown. Fig.13 yes Fig.11 The microscopic morphology of the cutting edge section of the B1 group tool is shown in the figure. Fig.12 and Fig.13 It can be seen that the thickness of the cutting edge coating of both the magnetron sputtering coated tool group A1 and the cathode arc evaporation coated tool group B1 is roughly uniform after conventional coating post-treatment.

[0102] The tools in group A2 and group B2 are coated with a coating post-treatment process so that the thickness of the coating gradually decreases as it approaches the middle area of ​​the cutting edge. Fig.14 This is the microscopic morphology of the cutting edge of magnetron sputtering coated tool A after coating post-treatment to make the coating thickness gradually distributed (that is, A2 group tools). Fig.15 This is the microscopic morphology of the cutting edge of the cathodic arc evaporation coated tool B after coating post-treatment to make the coating thickness gradually distributed (that is, the B2 group tool). Fig.16 yes Fig.14 The microscopic morphology of the cutting edge cross section of the A2 group of tools is shown. Fig.17 yes Fig.15 The microscopic morphology of the cutting edge section of the B2 group tool is shown in the figure. It can be seen from the figure that after the coating post-treatment, the middle area of ​​the cutting edge of the A2 and B2 group tools has been partially exposed and not covered by the coating, and the thickness of the coating gradually decreases as it approaches the exposed area of ​​the cutting edge (see Fig.16 ,and Fig.17 ).

[0103] Then, the high-gloss cutting effects of the tool groups A1, A2, B1 and B2 were compared. The cutting parameters are shown in Table 2.

[0104] Table 2 Cutting plan parameters

[0105]

[0106] The specific program data and result data are as follows:

[0107] Table 3 Comparison results

[0108]

[0109]

[0110] It should be pointed out that although the coating deposition processes selected for comparison in this comparative test are magnetron sputtering and cathode arc evaporation, various experiments have verified that the concept of the present invention is not limited to the type of coating deposition process, nor is it limited to the type of coating material. After actual application comparison, the cutting edge is partially exposed, and the coating thickness at the cutting edge is processed into a gradual distribution. Compared with the coated tool with uniform thickness distribution, no matter which coating deposition process is used or different coating materials are changed, the cutting performance and machine yield of the coated tool of the present invention are greatly improved.

[0111] In summary, the cutting tool of the present invention is used to perform the cutting action with the exposed substrate at the cutting edge, rather than the coating at the cutting edge. The main function of the coating structure of the present invention is to increase lubrication for chip guiding and chip removal, rather than the coating used to cover and protect the cutting edge and perform the cutting of the workpiece as in the conventional technology. The present invention overcomes the technical prejudice in the prior art that high-precision machining cutting tools must be covered with a coating at the cutting edge. By exposing the substrate at the cutting edge and designing a coating structure with a gradual thickness, high-precision and high-finish cutting processing is achieved.

[0112] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A cutting tool, comprising a cutting edge and a coating formed on the cutting edge, the cutting edge comprising a rake face, a flank face and a cutting edge connected between the rake face and the flank face, the cutting edge comprising an exposed portion not covered by the coating, the exposed portion being formed between two planes of the rake face and the flank face, the coating comprising a thickness gradient portion, the thickness of the thickness gradient portion being thinner as it approaches the exposed portion and thicker as it moves away from the exposed portion, the thickness gradient portion satisfying Tmin / Tmax≤0.58, wherein, Tmin is the thickness of the thinnest part of the coating thickness gradient part, Tmax is the thickness of the thickest part of the coating thickness gradient part, the width of the exposed part W = k*Tmax, 0.2≤k≤20, the thickness gradient part includes the thickness gradient part located on the front blade side and the thickness gradient part located on the back blade side, the length Lrear of the coating of the thickness gradient part located on the back blade side is greater than the length Lfront of the coating of the thickness gradient part located on the front blade side, the length L of the coating thickness gradient part = m*Tmax, wherein cot60°≤m≤cot3°.

2. The cutting tool according to claim 1, characterized in that: The coating includes a uniform thickness portion connected to an end of the coating with a thicker thickness in a thickness gradient portion, and the thickness of the uniform thickness portion is equal to the thickness of the thickest part of the end of the coating with a thicker thickness.

3. The cutting tool according to claim 1, characterized in that: The thickness of the coating at the thinner end of the coating thickness gradient portion gradually decreases to 0.

4. The cutting tool according to claim 1, characterized in that: The thickness gradient portion includes a thickness gradient portion located on the front cutting edge side and a thickness gradient portion located on the back cutting edge side. The thickness Tmax_rear of the thickest end of the coating of the thickness gradient portion located on the back cutting edge side and the thickness Tmax_front of the thickest end of the coating of the thickness gradient portion located on the front cutting edge side satisfy |Tmax_rear / Tmax_front-1|≤0.

15.

5. The cutting tool according to claim 1, characterized in that: The thickness gradient portion includes a thickness gradient portion located on the front cutting edge side and a thickness gradient portion located on the back cutting edge side. Lrear / Tmax_rear of the thickness gradient portion coating on the back cutting edge side is greater than Lfront / Tmax_front of the thickness gradient portion coating on the front cutting edge side.

6. The cutting tool according to claim 1, characterized in that: The cutting edge includes a middle area, the middle area of ​​the cutting edge includes an outward convex curved surface, the curvature of the outward convex curved surface is greater than the curvatures of the front cutting surface and the rear cutting surface, and the middle area of ​​the cutting edge includes the above-mentioned exposed portion.

Citation Information

Patent Citations

  • Pre-treatment technology for coating of welding reamer

    CN108118288A

  • Post-processing method of coating cutting tool and method of minimal lubrication processing after post-processing method

    CN109877713A

  • Coated cutting tool

    US7090914B2

  • Coated cutting tool and method for manufacturing the same

    CN104870686A

  • Cutting tool

    CN106457411A