RAMO4 substrate and method for manufacturing the same, and group III nitride semiconductor

By measuring the X-ray shaking curve on the RAMO4 substrate and controlling the radius of curvature and correlation coefficient, combined with a specific crystal lifting process, the cracking problem of the substrate when forming the Group III nitride crystal is solved, and high-quality Group III nitride is achieved Preparation of semiconductors.

CN111286781BActive Publication Date: 2024-11-12PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201911239070.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-12-10
Filing Date
2019-12-05
Publication Date
2024-11-12
Estimated Expiration
2039-12-05

AI Technical Summary

Technical Problem

When the Group III nitride crystal is formed or after it is produced, the base substrate is prone to warping and rupture due to lattice mismatch and difference in thermal expansion coefficient, resulting in a decrease in yield.

Method used

By measuring the X-ray sway curve on the crystalline surface of the RAMO4 substrate, determining the radius of curvature and correlation coefficient, controlling its radius of curvature is more than 52m and the square of the correlation coefficient is more than 0.81, and combining with resistance heating or high-frequency heating furnace crystal lifting The device was used to prepare a stable ScAlMgO4 single crystal substrate, and a buffer layer and Group III nitride crystal were formed on its surface to reduce the stress caused by lattice mismatch and thermal expansion.

Benefits of technology

Effectively prevent the substrate from rupturing when the Group III nitride crystal is formed or after it is formed, improving the yield and quality of the Group III nitride semiconductor, ensuring the stability and service life of the substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111286781B_ABST
    Figure CN111286781B_ABST
Patent Text Reader

Abstract

The present invention relates to a RAMO4 substrate and a method for manufacturing the same, as well as a group III nitride semiconductor. The present invention provides a RAMO4 substrate that is difficult to crack when forming a group III nitride crystal or after it is made. The following RAMO4 substrate is made, which includes a single crystal represented by the general formula RAMO4 (in the general formula, R represents one or more trivalent elements selected from Sc, In, Y and lanthanide elements, A represents one or more trivalent elements selected from Fe(III), Ga and Al, and M represents one or more divalent elements selected from Mg, Mn, Fe(II), Co, Cu, Zn and Cd), when the X-ray peak position ωi of multiple positions Xi is measured on a straight line passing through the center of the above RAMO4 substrate, the absolute value of the curvature radius r of the crystal surface calculated from the ωi and the measured position Xi is greater than 52m, and the square of the correlation coefficient ρ between the ω and the measured position Xi is greater than 0.81.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application involves RAMO 4 A substrate and a method for manufacturing the same, and a group III nitride semiconductor. Background Art

[0002] Contains general formula RAMO 4 The single crystal (in the general formula, R represents one or more trivalent elements selected from Sc, In, Y and lanthanide elements, A represents one or more trivalent elements selected from Fe(III), Ga and Al, and M represents one or more divalent elements selected from Mg, Mn, Fe(II), Co, Cu, Zn and Cd) of RAMO 4 The substrate has attracted attention as a base substrate for forming a Group III nitride crystal including gallium nitride (GaN).

[0003] Compared with sapphire, which is the existing base substrate, RAMO 4 ScAlMgO, one of the substrates 4 The lattice mismatch between the substrate and GaN is about 1 / 10 of that. 4 By forming GaN using a single crystal as a base substrate, a high-quality GaN crystal with a low dislocation defect density can be obtained.

[0004] Patent Document 1 shows that in ScAlMgO 4 A method in which an amorphous or polycrystalline buffer layer is formed on a substrate at a low temperature of about 600°C, and then a GaN single crystal thin film is formed at a high temperature of 1050°C using a Metal Organic Chemical Vapor Deposition (MOCVD) method.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2015-178448 Summary of the invention

[0008] Problems to be solved by the invention

[0009] However, the method described in Patent Document 1 also has the following problem: due to the lattice mismatch and linear expansion coefficient difference between the GaN present in the base substrate, the base substrate warps after the GaN single crystal thin film is formed, and the base substrate cracks at the stress concentrated portion. Therefore, a base substrate that is difficult to crack during or after the production of the III-nitride crystal is required.

[0010] The purpose of the present application is to provide a RAMO which is difficult to crack during or after the formation of a group III nitride crystal. 4 substrate.

[0011] Solutions to Solve Problems

[0012] The present application provides a RAMO 4 A substrate comprising a general formula RAMO 4 The single crystal RAMO shown in the general formula (in which R represents one or more trivalent elements selected from Sc, In, Y and lanthanide elements, A represents one or more trivalent elements selected from Fe(III), Ga and Al, and M represents one or more divalent elements selected from Mg, Mn, Fe(II), Co, Cu, Zn and Cd) 4 substrate, through the above RAMO 4 The X-ray rocking curve is measured at a plurality of positions Xi (i=1, 2, 3, ..., n) on a straight line at the center of the substrate, and the X-ray peak position ωi of the diffraction spectrum of the X-ray rocking curve at each position Xi is determined. Based on the regression line obtained from the relationship between the X-ray peak position ωi and the position Xi, the absolute value of the radius of curvature r of the crystal surface is calculated. Furthermore, based on the X-ray peak position ωi and the position Xi, the square of the correlation coefficient ρ calculated by the following formula is calculated:

[0013] [Mathematical formula 1]

[0014]

[0015] ( represents the average value of ωi, represents the average value of Xi)

[0016] The curvature radius r is greater than or equal to 52 m, and the square of the correlation coefficient ρ is greater than or equal to 0.81.

[0017] Effects of the Invention

[0018] According to the present application, it is possible to provide a RAMO which is difficult to crack during or after the formation of a group III nitride crystal. 4 substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 RAMO is a RAMO showing an embodiment of the present application. 4 Schematic diagram of a resistance heating furnace used in the method for manufacturing a substrate.

[0020] Figure 2 RAMO is a RAMO showing an embodiment of the present application. 4 Schematic diagram of a high-frequency heating furnace used in the method for manufacturing a substrate.

[0021] Figure 3 This is a schematic diagram showing a schematic cross section of a Group III nitride semiconductor in an embodiment of the present application.

[0022] Figure 4 It is a RAMO that represents an embodiment of the present application. 4 Schematic diagram of elements related to the crystal growth interface in a method for manufacturing a substrate.

[0023] Figure 5 ScAlMgO of Example 1 in the embodiment of the present application 4 A graph showing the correlation between the X-ray peak position ω of the substrate and the measurement position.

[0024] Figure 6 ScAlMgO of Comparative Example 1 in the embodiment of the present application 4 A graph showing the correlation between the X-ray peak position ω of the substrate and the measurement position.

[0025] Figure 7 ScAlMgO of Comparative Example 5 in the embodiment of the present application 4 A graph showing the correlation between the X-ray peak position ω of the substrate and the measurement position.

[0026] Figure 8 ScAlMgO of Comparative Example 9 in the embodiment of the present application 4 A graph showing the correlation between the X-ray peak position ω of the substrate and the measurement position.

[0027] Fig. 9 ScAlMgO of Examples 1 to 8 and Comparative Examples 1 to 9 in the embodiment of the present application 4 A graph showing the absolute value of the radius of curvature r of the crystal surface of the substrate and the square value of the correlation coefficient ρ. DETAILED DESCRIPTION

[0028] Hereinafter, embodiments of the present application will be described with reference to the accompanying drawings.

[0029] (Crystal Growth Process)

[0030] RAMO constituting one embodiment of the present application 4 RAMO of substrate 4 The single crystal can be produced using a crystal pulling device based on the Czochralski method (hereinafter also referred to as "CZ method"). The crystal pulling device used in the crystal growth step of this embodiment includes a resistance heating furnace or a high frequency heating furnace. Figure 1 1 is a schematic diagram showing the structure of a resistance heating furnace 100. Figure 22 is a schematic diagram showing the structure of a high-frequency heating furnace 200. 4 ScAlMgO, one of the single crystals 4 The case of a single crystal is used as an example to illustrate RAMO 4 Single crystal (RAMO 4 The present invention relates to a method for manufacturing a RAMO substrate. 4 Single crystal (RAMO 4 Substrate) is not limited to ScAlMgO 4 Single crystal (ScAlMgO 4 substrate).

[0031] Figure 1 The resistance heating furnace 100 shown in the figure has a raw material 110, a crucible 120, a crucible support shaft 121, a refractory material 122, an insulating material 130, a heater 140, a crystal pulling shaft 150, a seed crystal holder 151, a seed crystal 152, and a position detector 160 of the melt surface. Figure 1 However, the resistance heating furnace 100 may also have a chamber, a vacuum pump, a gas supply source, a gas exhaust port, a heater power supply, and a temperature or gas flow control device that are necessary for crystal pulling based on the CZ method.

[0032] The raw material 110 is scandium oxide (Sc 2 O 3 ) and aluminum oxide (Al 2 O 3 ) and magnesium oxide (MgO). After the mixture is sintered to increase the packing density, it is filled into the crucible 120 and heated to melt.

[0033] The crucible 120 is made of iridium and filled with the raw material 110. The material of the crucible 120 is not limited thereto, and various materials can be used as long as they have heat resistance at the melting temperature of the raw material 110 and resistance to reaction with the raw material 110. Examples of the material of the crucible 120 include platinum, tungsten, molybdenum, and tantalum.

[0034] The crucible support shaft 121 is made of tungsten and has the function of rotating and lifting at a set speed. The material of the crucible support shaft 121 is not limited thereto, and various materials having heat resistance at the heating temperature of this part and strength to support the raw material 110 and the crucible 120 can be used.

[0035] The refractory material 122 is made of zirconia and has a reactivity resistance to the materials of the crucible 120 and the crucible support shaft 121 .

[0036] The heat insulating material 130 is made of carbon, and through holes for inserting the crystal pulling shaft 150 and the crucible supporting shaft 121 are provided in the upper and lower parts of the heat insulating material 130 , respectively.

[0037] Heater 140 is made of carbon and generates heat when current flows. Heat from heater 140 heats the entire atmosphere inside insulating material 130, thereby heating raw material 110 in crucible 120. The material of heater 140 is not limited to carbon, and a heater made of metal such as tungsten may also be used.

[0038] The crystal pulling shaft 150 is made of alumina and has the function of rotating and lifting at a set speed. The material of the crystal pulling shaft 150 is not limited thereto, and various materials having heat resistance at the heating temperature of this part and resistance to reaction with the surrounding atmosphere can be used.

[0039] The seed crystal holder 151 is made of iridium and is connected to the crystal pulling shaft 150. The seed crystal 152 can be placed at the front end of the seed crystal holder 151. The material of the seed crystal holder 151 is not limited thereto, and various materials having heat resistance at the melting temperature of the raw material and resistance to reaction with the seed crystal 152 can be used.

[0040] Seed 152 is ScAlMgO 4 The seed crystal 152 is made into a square column, but the shape is not limited to this as long as it can be processed. The shape of the seed crystal 152 can be various shapes such as a cylinder, a prism with a cutout, etc.

[0041] The position detector 160 of the melt surface is an area sensor camera that captures the melt surface of the raw material 110 and the surroundings of the seed crystal 152, and detects the height position of the melt surface by image processing. The mechanism of the position detector 160 of the melt surface is not limited to this, and a laser displacement meter, an ultrasonic level meter, etc. may also be used.

[0042] When heating and melting the raw material 110 and growing the crystal, the internal atmosphere of the resistance heating furnace 100 is replaced with a desired gas atmosphere. Specifically, after the resistance heating furnace 100 is evacuated, a specified gas is introduced and set to normal pressure. The gas is supplied from a gas supply source (not shown) outside the resistance heating furnace 100 to the inside of the resistance heating furnace 100.

[0043] As the gas component, argon gas, which is an inert gas, is mainly used, but the gas component is not limited thereto. For example, in order to prevent oxygen deficiency in crystallization, a gas obtained by mixing 1% by volume or less of oxygen with respect to argon gas can be used as a gas component. In addition, in order to prevent reduction of the raw material 110, a gas obtained by mixing 1% by volume or less of carbon dioxide with respect to argon gas can also be used. In addition, as an inert gas, helium gas or the like can also be used instead of argon gas. Among them, from the perspective of cost, it is desirable to use argon gas, which can be obtained at a relatively low price, as an inert gas.

[0044] After replacing the above-mentioned gas atmosphere, the raw material 110 is heated and melted, and crystal growth is performed. First, current is passed through the heater 140 to heat the inside of the resistance heating furnace 100. Then, the power applied to the heater 140 is gradually increased over a period of time to heat the raw material 110 filled in the crucible 120 until it melts and does not cause a large load on the crucible 120. The time for heating and melting depends on the size of the crucible 120. When the outer diameter of the crucible 120 is 80 mm to 150 mm, it is preferably 15 hours to 60 hours.

[0045] After confirming that the raw material 110 is melted, the crystallization pulling shaft 150 is rotated at a constant speed while slowly descending until the seed crystal 152 is in contact with the raw material 110. After the temperature of the raw material 110 is stabilized at a temperature suitable for pulling the crystal, the crystallization pulling shaft 150 is raised at a specified speed to pull the crystal. A load sensor (not shown) is provided at the upper end of the crystallization pulling shaft 150, which can measure the weight of the crystal during pulling. After the pulling starts, the output of the heater is adjusted based on the crystal diameter calculated from the weight measurement value. In addition, the automatic diameter control (Automatic Diameter Control (ADC)) is used to control the desired crystal shape. In this embodiment, the pulling speed of the crystallization pulling shaft 150 is preferably greater than 0.1 mm / h and less than 1.0 mm / h, and more preferably greater than 0.3 mm / h and less than 0.7 mm / h. The rotation speed is preferably in the range of greater than 1 rpm and less than 10 rpm.

[0046] After the crystal is pulled to a desired length, the crystal is separated from the raw material 110, and the power applied to the heater 140 is slowly reduced for a period of time to cool the crucible 120 to a degree that does not impose a large load. The cooling time depends on the size of the crucible 120, and when the outer diameter of the crucible 120 is 80 mm or more and 150 mm or less, it is preferably 20 hours or more and 70 hours or less.

[0047] Next, for the use Figure 2The high frequency heating furnace 200 shown in FIG. 1 is described below. The high frequency heating furnace 200 may be configured as follows except that a heating coil 240 is disposed outside the heat insulating material 230 instead of the heater 140 being disposed inside the heat insulating material 130. Figure 1 The resistance heating furnace 100 has the same structure as Figure 1 The same components are denoted by the same reference numerals, and detailed description thereof will be omitted.

[0048] The heat insulating material 230 is made of zirconia and is arranged so as to surround the crucible 120 .

[0049] The heating coil 240 is made of copper and is arranged so as to surround the insulating material 230. Cooling water circulates inside the copper tube. When a high-frequency current flows through the heating coil 240, a high-frequency magnetic flux is generated. Due to the high-frequency magnetic flux, an eddy current is generated in the crucible 120, and the surface of the crucible 120 is heated. As a result, the raw material 110 in the crucible 120 is heated.

[0050] It should be noted that, although not shown in the figure, the high-frequency heating furnace 200 further includes a mechanism for raising and lowering the heating coil 240 .

[0051] When the high frequency heating furnace 200 is used for crystal growth, the internal atmosphere is also replaced with a desired gas atmosphere during heating. As a gas component, nitrogen is mainly used. Among them, the gas component is not limited to nitrogen. In order to prevent oxygen deficiency in crystallization, a gas obtained by mixing 1 volume % or less of oxygen with respect to nitrogen can be used. In addition, in order to prevent reduction of the raw material 110, a gas obtained by mixing 1 volume % or less of carbon dioxide with respect to nitrogen can be used. In addition, argon can also be used instead of nitrogen as an inert gas.

[0052] The heating, melting, and crystal growth of the raw material 110 after replacing the atmosphere in the high-frequency heating furnace 200 with the above-mentioned gas atmosphere are the same as those in the case of using the above-mentioned resistance heating furnace 100.

[0053] (Substrate Formation Process)

[0054] After the crystal growth step, the cooled ScAlMgO 4 Single crystal, ScAlMgO is made by cleaving and surface processing. 4 Substrate. At this time, ScAlMgO 4 One surface of the substrate is used as the epitaxial growth surface. 4The epitaxial growth surface of the substrate is aligned to arrange the new crystal (epitaxial growth), and high-quality group III nitride semiconductors can be obtained. In epitaxial growth, metal organic chemical vapor deposition (hereinafter referred to as MOCVD method), hydride vapor phase epitaxy (hereinafter referred to as HVPE method), gallium oxide method (hereinafter referred to as Oxide Vaper Phase Epitaxy: OVPE method) and the like are used to grow crystals of compound semiconductors such as group III nitrides.

[0055] Figure 3 This means that ScAlMgO in this embodiment is used. 4 A schematic cross-sectional view of a group III nitride semiconductor 300 of a substrate. The group III nitride semiconductor 300 includes: 4 Single crystal ScAlMgO 4 Substrate 301, ScAlMgO 4 A buffer layer 302 including In and a nitride of a group III element other than In is formed on a substrate 301 , and a group III nitride crystal 303 is formed on the buffer layer 302 .

[0056] The above ScAlMgO 4 Single crystal ScO with rock-salt structure 2 Layer and hexagonal structure of AlMgO 2 The structure of the alternately stacked layers has the same property as graphite and hexagonal BN, that the crystal is cleaved on the (0001) plane (cleavage plane). 4 The group III nitride semiconductor 300 can be obtained by heteroepitaxially growing a group III nitride crystal on the cleaved surface of the substrate 301 as an epitaxial growth surface.

[0057] Among them, if in ScAlMgO 4 If there are defects or foreign matter on the epitaxial growth surface of the substrate 301, which may become the seed of accidental crystal growth, the group III atoms will gather in this part, resulting in local uneven growth. 4 The surface of the substrate 301 is processed to form a plurality of cleavage planes separated from each other by height differences and regularly distributed, and these planes are used as epitaxial growth planes. 4When GaN, a group III nitride, is grown on the substrate 301 using, for example, the MOCVD method, trimethylgallium (TMG) or the like is used as a Ga raw material. Furthermore, when the MOCVD method is performed, Ga moves (migrates) on the cleavage plane, which is the epitaxial growth plane, while being partially bonded to the methyl group. Furthermore, if there is a stable position, it stops at the position and cuts off the bond with the methyl group, and then bonds with N to perform epitaxial growth. Therefore, by forming a plurality of cleavage planes separated from each other by height differences, and flexibly using the height difference portions of adjacent cleavage planes as the above-mentioned stable positions, epitaxial growth can be stabilized.

[0058] The ScAlMgO in the group III nitride semiconductor 300 of this embodiment 4 The thickness of the substrate 301 can be appropriately selected according to the application of the group III nitride semiconductor, and is preferably 100 μm or more and 1000 μm or less, and more preferably 300 μm or more and 600 μm or less. 4 The thickness of the substrate 301 is within this range. 4 When the substrate 301 is formed, the group III nitride crystal 303 is formed, and the ScAlMgO 4 The frequency of cracking of the substrate 301. In addition, ScAlMgO 4 The shape of the substrate 301 is appropriately selected depending on the application of the group III nitride semiconductor, but in consideration of industrial applicability, it is preferably a wafer having a diameter of 25 mm to 200 mm.

[0059] (Group III Nitride Semiconductor)

[0060] For the use of the above ScAlMgO 4 The group III nitride semiconductor of the substrate 301 will be described in more detail below.

[0061] The buffer layer 302 is a layer containing In and a nitride of a group III element other than In, and can be made into an amorphous, single crystal, or polycrystalline layer containing a compound of a composition represented by InGaN, for example. In addition, the buffer layer 302 preferably further contains Al, and is more preferably an amorphous, single crystal, or polycrystalline layer containing a compound represented by InAlGaN. By using InAlGaN for the buffer layer 302, the ScAlMgO 4 The lattice mismatch between the substrate 301 and the group III nitride crystal 303. As a result, a high-quality group III nitride crystal 303 with a low dislocation defect density can be easily obtained.

[0062] On the other hand, the III-nitride crystal 303 is formed by forming a ScAlMgO 4The layer formed by heteroepitaxial growth on the epitaxial growth surface of the substrate 301 via the buffer layer 302 may be a layer of crystals containing a nitride of a group III element (eg, Ga, Al, In, Tl, B, Sc, etc.), preferably GaN or AlN.

[0063] The manufacturing method of the III-nitride semiconductor 300 of the present application is not particularly limited. For example, the buffer layer 302 and the III-nitride crystal 303 can be formed by forming the III-nitride on ScAlMgO by MOCVD. 4 The substrate 301 is formed by epitaxial growth.

[0064] When the buffer layer 302 and the group III nitride crystal 303 are formed by MOCVD, trimethyl gallium (TMG), trimethyl indium (TMI), trimethyl aluminum (TMA), etc. can be used as a group III element source. In addition, ammonia (NH 3 Furthermore, hydrogen or nitrogen can be used as a carrier gas when performing the MOCVD method.

[0065] Before the implementation of MOCVD, ScAlMgO 4 The substrate 301 is preferably thermally cleaned at 1100° C. for 10 minutes in a hydrogen atmosphere. During thermal cleaning, ScAlMgO 4 Carbon-based dirt and the like on the surface of the substrate 301 are removed. After cleaning, ScAlMgO 4 The surface temperature of the substrate 301 is lowered to, for example, 425° C. Then, nitrides of In and group III elements other than In are deposited on the ScAlMgO substrate by MOCVD. 4 A buffer layer 302 is formed on the substrate 301. The buffer layer 302 can be formed at a relatively low temperature of 400°C or higher and less than 700°C. If the buffer layer 302 is formed at such a low temperature, the buffer layer 302 becomes an amorphous or polycrystalline layer, and the group III nitride crystal 303 formed on the buffer layer 302 is less likely to have lattice defects. The thickness and composition of the buffer layer 302 are adjusted by the film formation time and the ratio of the raw materials.

[0066] After the buffer layer 302 is formed, ScAlMgO 4The temperature of the substrate 301 is raised to, for example, 1125° C., and the III-nitride is epitaxially grown to obtain the III-nitride crystal 303. The thickness and composition of the III-nitride crystal 303 are also adjusted by the film formation time and the ratio of the raw materials. The formation temperature of the III-nitride crystal 303 can be set to be greater than 700° C. and less than 1300° C. If the III-nitride is epitaxially grown at such a temperature, it is easy to obtain the III-nitride crystal 303 with less lattice defects.

[0067] It should be noted that in the III-group nitride semiconductor 300 of the present application, a general formula RAMO can be used. 4 RAMO is shown as a substantially single crystalline material. 4 Substrate to replace the above ScAlMgO 4 Substrate 301. In the above general formula, R represents one or more trivalent elements selected from Sc, In, Y and lanthanide elements, A represents one or more trivalent elements selected from Fe(III), Ga and Al, and M represents one or more divalent elements selected from Mg, Mn, Fe(II), Co, Cu, Zn and Cd. It should be noted that a substantially single crystalline material refers to: RAMO constituting the epitaxial growth surface 4 The content of is 90 atomic % (atom %) or more and when paying attention to any crystal axis, the orientation is the same in any part of the epitaxial growth surface. Among them, the crystal in which the orientation of the local crystal axis changes and the crystal containing local lattice defects are also regarded as single crystals. It should be noted that O is oxygen. Among them, as mentioned above, it is preferred that R is set to Sc, A is set to Al, and M is set to Mg.

[0068] In addition, as described above, the group III element constituting the buffer layer 302 and the group III nitride crystal 303 is particularly preferably gallium (Ga), but for example, only one of aluminum (Al), indium (In), thallium (Tl), etc. may be used, or two or more of them may be used in combination. For example, as a material constituting the group III nitride crystal 303, at least one selected from aluminum (Al), gallium (Ga) and indium (In) may be used. In this case, the composition of the manufactured group III nitride crystal 303 is Al. s Ga t In (1-(s+t)) N (where 0≤s≤1, 0≤t≤1, s+t≤1). In addition, a dopant material may also coexist in the III-nitride crystal 303. The dopant is not particularly limited, and examples thereof include germanium oxide (e.g., Ge 2 O 3 ,Ge 2 O, etc.

[0069] As a method for forming the group III nitride crystal 303 , HVPE, OVPE, sputtering, MBE, or the like may be used instead of MOCVD.

[0070] (ScAlMgO 4 Evaluation of substrate)

[0071] As mentioned above, for general ScAlMgO 4 For the substrate, during the cooling process after the formation of the III-nitride crystal 303, the ScAlMgO 4 The lattice mismatch and thermal expansion coefficient difference between the substrate 301 and the group III nitride crystal 303 result in ScAlMgO 4 The substrate 301 is warped. And there are the following problems: ScAlMgO 4 The substrate 301 is prone to cracking at locations where stress is concentrated, which has a significant adverse effect on the yield of the product.

[0072] As a result of in-depth research, the inventors found that by properly controlling the ScAlMgO 4 The curvature radius of the crystal surface of the substrate 301 and the uniformity of the crystal orientation, so that after the formation of the group III nitride crystal 303, ScAlMgO 4 The substrate 301 is difficult to break.

[0073] ScAlMgO 4 The curvature radius of the crystal plane of the substrate 301 and the uniformity of the crystal orientation can be evaluated by X-ray diffraction before forming the buffer layer 302 and the group III nitride crystal 303 .

[0074] Specifically, in ScAlMgO 4 Multiple X-ray rocking curves are measured on a straight line passing through the center of the substrate within the surface of the substrate 301 to obtain the X-ray peak position (ω) of each diffraction spectrum. The curvature radius and the uniformity of the crystal orientation are evaluated from the measured position (X) and the X-ray peak position (ω).

[0075] Specifically, the X-ray rocking curve is measured at each measurement position Xi (i=1, 2, 3, ..., n (n is the number of measurement positions)) on a straight line passing through the center of the substrate. And, the regression line represented by the following formula 1 is determined from a graph where the X-ray peak position corresponding to each Xi is represented as ωi and the coordinates of the data are represented as (Xi, ωi).

[0076] ω=aX+b···(Formula 1)

[0077] The slope a and intercept b of the regression line obtained using the least squares method are expressed by equations 2 and 3, respectively.

[0078] [Mathematical formula 2]

[0079]

[0080] Here, is the average value of ωi, is the average value of Xi.

[0081] Then, ScAlMgO is calculated using the following formula 4: 4 The curvature radius r of the crystal surface of the substrate 301.

[0082] [Mathematical formula 3]

[0083]

[0084] When the sign of the curvature radius r is positive, it indicates that a crystal plane convexly projects downwards, and when the sign is negative, it indicates that a crystal plane convexly projects upwards. In addition, the larger the absolute value of the curvature radius r, the smaller the warping of the crystal plane of the substrate. It should be noted that the crystal plane mentioned here refers to the (0001) plane. 4 In addition, the curvature radius r (warp) mentioned here is not the curvature radius of the ScAlMgO 4 The warping of the surface of the substrate 301 is not the warping of the crystal plane, but the warping of the crystal.

[0085] On the other hand, the uniformity of the crystal orientation can be determined by the square of the correlation coefficient ρ between the measurement position Xi and the X-ray peak position ωi (ρ 2 The correlation coefficient ρ between the measurement position Xi and the X-ray peak position ωi is calculated using the following equation 5.

[0086] [Formula 4]

[0087]

[0088] Here, is the average value of ωi, is the average value of Xi.

[0089] ρ 2 The larger the value, the more uniform the orientation of the crystal axes at each point in the crystal plane of the substrate.

[0090] It should be noted that, with respect to the correlation coefficient ρ, the greater the number of measurement positions (n), the more significant the correlation coefficient ρ is, which is preferred for evaluating the uniformity of the crystal orientation. In the test of the correlation coefficient ρ, the limit value of the correlation coefficient at a 5% significance level, that is, the lowest value of the correlation coefficient ρ that becomes significant, is set to 0.88 when the number of points (n) is 5, 0.81 when the number of points (n) is 6, and 0.75 when the number of points (n) is 7. It is preferably set to 6 or more measurement positions where the correlation coefficient ρ of 0.81 or more becomes significant. In addition, the limit value of the correlation coefficient at a stricter 1% significance level, that is, the lowest value of the correlation coefficient ρ that becomes significant, is set to 0.83 when the number of points (n) is 8, 0.80 when the number of points (n) is 9, and 0.76 when the number of points (n) is 10. It is more preferably set to 9 or more where the correlation coefficient ρ of 0.80 or more becomes significant.

[0091] In addition, the inventors have conducted in-depth research and found that: by cultivating ScAlMgO 4 In the process of single crystal formation, the shape of the crystal growth interface is controlled to form ScAlMgO 4 The curvature radius r of the crystal surface of the substrate 301 and the uniformity of the crystal orientation (the above-mentioned ρ 2 ) is set to the desired range.

[0092] Figure 4 1 is a schematic diagram showing a crystal growth interface 420 and related elements in the crystal growth process using the above-mentioned resistance heating furnace 100. The boundary between the crystal 410 grown from the seed crystal 152 as the starting point and the melt of the raw material 110 is the crystal growth interface 420. The shape of the crystal growth interface 420 is mainly determined by the balance of the temperature gradient 440 near the melt surface 430 of the raw material 110 (hereinafter also referred to as the "melt surface"), the pulling speed 450 of the crystal pulling shaft, the rotation speed 460 of the crystal pulling shaft, and the convection 470 of the melt. The temperature gradient 440 refers to the temperature difference per unit length in the height direction near the melt surface 430. In the Czochralski method, the larger the temperature gradient 440 is, the more it can promote the solidification of the raw material 110 from the melt to the crystal, and the amount of crystal growth per unit time also increases. If the pulling speed 450 of the crystal pulling axis deviates from the appropriate range relative to the crystal growth amount per unit time, the flatness of the crystal growth interface 420 is destroyed due to the load caused by pulling. The flatness of the crystal growth interface 420 is directly related to the growth of ScAlMgO 4 The curvature radius r of the crystal surface of the single crystal and the uniformity of the crystal orientation (the above ρ 2), therefore, it is important to properly control the temperature gradient 440 and the pulling speed 450. In addition, if the rotation speed 460 of the crystal pulling shaft is increased, the convection 470 of the melt is promoted, and the frequency of the high-temperature melt near the heater 140 approaching the crystal growth interface 420 increases. As a result, the temperature state near the melt surface 430 changes, affecting the flatness of the crystal growth interface 420. Therefore, it is important to properly control the rotation speed 460.

[0093] Here, the temperature gradient 440 is mainly determined by the heat supplied from the heater 140 to the vicinity of the melt surface 430, the structure of the insulating material (not shown) around and above the crucible 120, and the flow rate of the atmosphere gas near the melt surface 430 (not shown). Among them, the temperature gradient 440 varies greatly due to the positional relationship between the height of the melt surface 430 and the height of the heater 140. In the embodiment of the present application, the position detector 160 of the melt surface 430 is used to measure the height position of the melt surface 430 of the raw material 110. In addition, the distance (hereinafter also referred to as "vertical distance") 480 between the melt surface 430 and the upper end of the heater 140 along the crystal pulling direction is kept constant by raising and lowering the crucible support shaft 121. As a result, the temperature gradient 440 near the melt surface 430 of the raw material 110 is easy to fall into the desired range. It should be noted that the smaller the vertical distance between the melt surface 430 and the upper end of the heater 140, that is, the closer the heater 140 is to the bottom, the more the heating of the bottom of the crucible 120 is promoted, and the less the heat radiated from the heater 140 to the top of the melt surface 430. Therefore, the temperature gradient 440 becomes larger. Among them, if the heating of the bottom of the crucible 120 is excessively promoted, the temperature distribution in the melt of the raw material 110 becomes larger, and the speed of the convection 470 of the melt becomes too fast. As a result, the flatness of the crystal growth interface 420 is adversely affected. Therefore, it is preferred to adjust the vertical distance 480 between the melt surface 430 and the upper end of the heater 140 while achieving a balance with the state of the convection 470 of the melt, so as to obtain an appropriate temperature gradient 440.

[0094] Specifically, when the above-mentioned crystal growth process is performed, the raw material 110 is consumed as the crystal 410 is pulled, and the position of the melt surface 430 in the crucible 120 begins to drop from the set initial value. Therefore, in this embodiment, in order to eliminate this drop, the crucible support shaft 121 is raised to raise the position of the crucible 120. In addition, the vertical distance 480 between the melt surface 430 and the upper end of the heater 140 is kept constant. The position of the melt surface 430 is measured by the position detector 160. In addition, the measured value is input into a computer (not shown), and the computer processes based on the input value, and controls the crucible support shaft 121 in a manner to raise the position of the crucible 120 based on the processing result.

[0095] At this time, the vertical distance 480 between the melt surface 430 and the upper end of the heater 140 is determined by the ScAlMgO 4 The diameter of the single crystal is appropriately selected, and in the present embodiment, is preferably 19 mm or more and 29 mm or less.

[0096] It should be noted that when the heating coil 240 is used instead of the heater 140, the heating coil 240 can be raised or lowered instead of the crucible support shaft 121, as long as the relative distance between the melt surface 430 and the upper end of the heating coil 240 is kept constant by raising or lowering both.

[0097] Here, the computer may include a system LSI (Large Scale Integration) or a plurality of dedicated electronic circuits. In addition, the height control of the crucible 120 may be implemented by executing instructions or software programs stored in a non-temporary memory using a processor. It should be noted that these processes may be implemented by a program execution unit such as a CPU or a processor reading a software program recorded in a recording medium such as a hard disk or a semiconductor memory and executing it.

[0098] By appropriately combining the temperature gradient 440 obtained by the above method with the pulling speed 450 and the rotation speed 460 of the crystal pulling shaft 150, the shape of the crystal growth interface 420 can be controlled, and the ScAlMgO 4 The curvature radius r of the crystal surface of the substrate 301 and the uniformity of the crystal orientation (the above ρ 2 ) is set to the desired range.

[0099] When the high frequency heating furnace 200 is used to perform the crystal growth step, the height position of the melt surface 430 of the raw material 110 is measured using the melt surface position detector 160. In addition, by adjusting the vertical distance 480 between the melt surface 430 of the raw material 110 and the upper end of the heating coil 240 by raising and lowering the heating coil 240, the temperature gradient 440 near the melt surface of the raw material 110 can be similarly adjusted.

[0100] As mentioned above, by making ScAlMgO 4 Single crystal (ScAlMgO 4 substrate), so that when or after the formation of the III-nitride crystal, ScAlMgO 4 The substrate is less likely to crack, and the yield of the group III nitride semiconductor is improved.

[0101] Example

[0102] Hereinafter, the present application will be described in more detail using examples, but the scope of the present application is not to be construed as being limitative of these examples.

[0103] (Example)

[0104] Using the embodiment shown Figure 1 Resistance heating furnace 100 or Figure 2 The high frequency heating furnace 200 is used to grow ScAlMgO 4 Single crystal. As the raw material for new crystal growth, use Sc 2 O 3 :Al 2 O 3 :MgO=27.5%:26.5%:46.0% (atomic %). After sintering, the mixture is filled into an iridium crucible 120 and heated to melt to obtain a molten raw material 110. After the seed crystal 152 is brought into contact with the molten raw material 110, the generated crystal is pulled while rotating the crystal pulling shaft 150 to grow an outer diameter ScAlMgO 4 The pulling speed 450 and the rotation speed 460 of the crystal pulling shaft 150, and the vertical distance 480 between the melt surface 430 and the upper end of the heat source (the upper end of the heater 140 or the heating coil 240) which is kept constant by the melt surface position detector 160 are set to the conditions of Examples 1 to 8 shown in Table 1.

[0105] [Table 1]

[0106]

[0107] After the crystal growth step, the cooled ScAlMgO 4 Single crystal, processed to outer diameter Thickness 400μm, making ScAlMgO 4 Substrate 301. ScAlMgO 4 The substrate 301 has one cleavage surface processed into an epitaxial growth surface.

[0108] ScAlMgO 4 The curvature radius of the crystal surface and the uniformity of the crystal orientation of the substrate 301 were evaluated using an X-ray diffraction device D8 DISCOVER manufactured by BrukerAXS. The measurement beam width was set to 1 mm × 7 mm, and the X-ray rocking curve was measured at 13 locations on a straight line passing through the center of the substrate at a spacing of 4.8 mm to obtain the X-ray peak position (ω) of each diffraction spectrum.

[0109] Figure 5This is a graph showing the correlation between the X-ray peak position ωi and the measurement position Xi in Example 1. The slope a of the regression line ω=aX+b in the graph is 0.0011, the absolute value of the curvature radius r calculated from the slope a is 52.1 m, and the square of the correlation coefficient ρ is 0.97. This indicates that the warping of the crystal surface of the substrate is small and the orientation of the crystal axis at each point in the crystal surface of the substrate is consistent.

[0110] Table 2 shows the absolute value of the curvature radius r and the square of the correlation coefficient ρ calculated from the X-ray peak position ωi and the measurement position Xi for each of Examples 1 to 8.

[0111] [Table 2]

[0112]

[0113] In Examples 1 to 8, ScAlMgO 4 A buffer layer 302 containing amorphous or polycrystalline InGaN with a film thickness of 20 nm and containing 3 atomic % of In is formed on a substrate 301, and a group III nitride crystal 303 containing a GaN single crystal with a film thickness of 2 μm is formed on the buffer layer 302, thereby manufacturing a group III nitride semiconductor 300. It should be noted that the above-mentioned MOCVD method is used as an epitaxial growth method when forming the group III nitride crystal 303, and the formation temperature is set to 1125°C.

[0114] In any of Examples 1 to 8, the substrate taken out after the device was cooled had no warping or cracking, and a good Group III nitride semiconductor 300 was obtained.

[0115] (Comparative Example)

[0116] In the conventional structure in which the position detector 160 of the melt surface is not used, the vertical distance 480 between the melt surface 430 of the raw material 110 and the upper end of the heat source (the upper end of the heater 140 or the heating coil 240) is not adjusted, and the pulling speed 450 and the rotation speed 460 of the crystal pulling shaft 150 are set. ScAlMgO is grown by the same method as in the embodiment. 4 Single crystal.

[0117] The pulling speed 450 and the rotation speed 460 of the crystal pulling shaft 150 were set to the conditions of Comparative Examples 1 to 7 shown in Table 3. It should be noted that in Comparative Examples 1 to 4, the vertical distance 480 between the melt surface 430 of the raw material 110 and the upper end of the heat source was not adjusted under the same setting of the pulling speed 450 and the rotation speed 460 as in Example 1, and four attempts were made to grow crystals. That is, the sample produced by the first pulling is Comparative Example 1, the sample produced by the second pulling is Comparative Example 2, the sample produced by the third pulling is Comparative Example 3, and the sample produced by the fourth pulling is Comparative Example 4. In addition, in Comparative Examples 5 to 7, the vertical distance 480 between the melt surface 430 of the raw material 110 and the upper end of the heat source was not adjusted under the same setting of the pulling speed 450 as in Example 2, and the rotation speed 460 was set to three modes to try to grow crystals.

[0118] [Table 3]

[0119]

[0120] After the crystal growth step, ScAlMgO was processed by the same processing method as in the example. 4 The substrate 301 was prepared, and the curvature radius r of the crystal plane and the uniformity of the crystal orientation (square of the correlation coefficient ρ) were evaluated based on X-ray diffraction.

[0121] Figure 6 This is a graph showing the correlation between the X-ray peak position ω and the measurement position in Comparative Example 1. The slope a of the regression line ω=aX+b is 0.0007, the absolute value of the radius of curvature r calculated from the slope a is 81.9 m, and the square of the correlation coefficient ρ is 0.62. This means that although the radius of curvature r indicating the warpage of the crystal surface of the substrate is small, the square of ρ indicating the orientation of the crystal axis at each point in the crystal surface of the substrate is small, and the orientation of the crystal axis is inconsistent.

[0122] Figure 7 This is a graph showing the correlation between the X-ray peak position ω and the measurement position in Comparative Example 5. The slope a of the regression line ω=aX+b is 0.0008, the absolute value of the radius of curvature r calculated from the slope a is 71.6 m, and the square of the correlation coefficient ρ is 0.71. This also shows that: although the radius of curvature r indicating the warpage of the crystal surface of the substrate is small, the square of ρ indicating the orientation of the crystal axis at each point in the crystal surface of the substrate is small, and the orientation of the crystal axis is inconsistent.

[0123] Table 4 shows the curvature radius r and the square of the correlation coefficient ρ calculated from the X-ray peak position ω and the measurement position of each of Comparative Examples 1 to 7.

[0124] [Table 4]

[0125]

[0126] In Comparative Examples 1 to 7, ScAlMgO 4 On the substrate 301, a buffer layer 302 and a group III nitride crystal 303 are formed by the same epitaxial growth method as in the embodiment.

[0127] In all of Comparative Examples 1 to 7, the substrates taken out after the device was cooled had ScAlMgO 4 The substrate 301 was cracked, and a good Group III nitride semiconductor 300 could not be obtained.

[0128] (Comparative example where the pulling speed is out of the appropriate range)

[0129] Next, similarly to the embodiment using the melt surface position detector 160, while the vertical distance 480 between the melt surface 430 of the raw material 110 and the upper end of the heat source (the upper end of the heater 140 or the heating coil 240) is kept constant, the pulling speed 450 of the crystal pulling shaft 150 is set higher than that of the embodiment. It should be noted that the other matters are the same as those of the embodiment, and the ScAlMgO is grown. 4 The pulling speed 450 and the rotation speed 460 of the crystal pulling shaft 150, and the vertical distance 480 between the melt surface 430 and the upper end of the heat source (the upper end of the heater 140 or the heating coil 240) measured by the melt surface position detector 160 were set to the conditions of Comparative Examples 8 to 9 shown in Table 5.

[0130] [Table 5]

[0131]

[0132] After the crystal growth step, ScAlMgO was processed by the same processing method as in the example. 4 The substrate 301 was prepared, and the curvature radius of the crystal plane and the uniformity of the crystal orientation were evaluated by X-ray diffraction.

[0133] Figure 8 This is a graph showing the correlation between the X-ray peak position ω and the measurement position in Comparative Example 9. The slope a of the regression line ω=aX+b is -0.0029, the absolute value of the radius of curvature r calculated from the slope a is 19.8 m, and the square of the correlation coefficient R is 0.81. This indicates that although the orientation of the crystal axis at each point in the crystal plane of the substrate is consistent, the warp (radius of curvature r) of the crystal plane of the substrate is large.

[0134] Table 6 shows the curvature radius r and the square of the correlation coefficient ρ calculated from the X-ray peak position ω and the measurement position of each of Comparative Examples 8 to 9.

[0135] [Table 6]

[0136]

[0137] In Comparative Examples 8 to 9, ScAlMgO 4 On the substrate 301, a buffer layer 302 and a group III nitride crystal 303 are formed by the same epitaxial growth method as in the embodiment.

[0138] In any of Comparative Examples 8 to 9, the substrates taken out after the device was cooled were cracked due to stress caused by the warping, and a good Group III nitride semiconductor 300 could not be obtained.

[0139] That is, by making ScAlMgO 4 The crystal pulling speed during the single crystal (crystal growth process) is controlled to be 0.7 mm / h or less, and the vertical distance 480 between the melt surface 430 and the upper end of the heater 140 is controlled to be 19 mm or more and 29 mm or less, and ScAlMgO having the above-mentioned preferred curvature radius r and the square of the correlation coefficient ρ can be produced. 4 Substrate 301. In addition, under the above conditions, it is more preferable to set the pulling speed to 0.3 mm / h or more.

[0140] Here, for ScAlMgO 4 The preferred ranges of the absolute value of the radius of curvature r of the crystal surface of the substrate 301 and the square of the correlation coefficient ρ are described below. Fig. 9 ScAlMgO of Examples 1 to 8 and Comparative Examples 1 to 9 4 The absolute value of the radius of curvature r of the crystal surface of the substrate 301 and the square value of the correlation coefficient ρ are plotted, and the III-nitride semiconductor 300 produced using each substrate is indicated by a circle when there is no crack, and by an x ​​when there is crack. Fig. 9 It is found that when the absolute value of the radius of curvature r is 52 m or more and the square of the correlation coefficient R is 0.81 or more, a good Group III nitride semiconductor 300 without cracks can be obtained.

[0141] It should be noted that in the production of ScAlMgO 4 When the substrate 301 is used, the following determination process can be implemented: check whether the radius of curvature r and the square of the correlation coefficient ρ fall within a specified range, and if they are within the range, it is determined to be a qualified product. 4 Substrate (RAMO 4) substrate, measuring the X-ray rocking curve at a plurality of positions Xi on a straight line passing through the center thereof, and determining the X-ray peak position ωi of the diffraction spectrum of the X-ray rocking curve at each position Xi. And, the ScAlMgO having a curvature radius r of 52 m or more and a correlation coefficient ρ square of 0.81 or more obtained from these values ​​can be obtained. 4 Substrate (RAMO 4 Substrates that are judged as qualified products can be used to manufacture electronic devices such as LEDs and power devices. Substrates that are not judged as qualified products can be discarded or melted and reused as raw materials.

[0142] Industrial Applicability

[0143] According to the present application, substrate cracking during formation of group III nitride crystals can be suppressed, and the high quality of group III nitride semiconductors can be improved. Therefore, the present invention is useful as a base substrate for light emitting diodes (LEDs), laser diodes (LDs), and the like.

[0144] Description of Reference Numerals

[0145] 100 Resistance Heating Furnace

[0146] 110 Raw Materials

[0147] 120 Crucible

[0148] 121 Crucible support shaft

[0149] 122 Refractory materials

[0150] 130 Insulation Materials

[0151] 140 Heater

[0152] 150 Crystallization pull shaft

[0153] 151 Seed Holder

[0154] 152 Seed

[0155] 160 Melt surface position detector

[0156] 200 High frequency heating furnace

[0157] 230 Insulation Materials

[0158] 240 Heating Coil

[0159] 300 Group III Nitride Semiconductors

[0160] 301 ScAlMgO 4 substrate

[0161] 302 Buffer layer

[0162] 303 III-nitride crystal

[0163] 410 Crystallization

[0164] 420 Crystal Growth Interface

[0165] 430 Melt surface

[0166] 440 Temperature Gradient

[0167] 450 Pulling speed

[0168] 460 rotation speed

[0169] 470 Convection of the melt

[0170] 480 Vertical distance between the melt surface and the upper end of the heat source

Claims

1. A RAMO4 substrate, comprising a single crystal represented by the general formula RAMO4, wherein R represents one or more trivalent elements selected from Sc, In, Y and lanthanide elements, A represents one or more trivalent elements selected from Fe(III), Ga and Al, and M represents one or more divalent elements selected from Mg, Mn, Fe(II), Co, Cu, Zn and Cd, The X-ray rocking curve is measured at a plurality of positions Xi on a straight line passing through the center of the RAMO4 substrate, and the X-ray peak position ωi of the diffraction spectrum of the X-ray rocking curve at each position Xi is determined, wherein, i=1,2,3,…,n, Based on the regression line obtained from the relationship between the X-ray peak position ωi and the position Xi, the absolute value of the radius of curvature r of the crystal surface is calculated. Furthermore, based on the X-ray peak position ωi and the position Xi, the square of the correlation coefficient ρ calculated by the following formula is calculated: represents the average value of ωi, represents the average value of Xi, n represents the number of measurement positions, The radius of curvature r is greater than 52 m, and the square of the correlation coefficient ρ is greater than 0.81, When the regression line is represented by ω=aX+b, a and b are represented by the following formula: represents the average value of ωi, represents the average value of Xi; The curvature radius r is expressed by the following formula:

2. The RAMO4 substrate according to claim 1, wherein: In the general formula RAMO4, R is Sc, A is Al, and M is Mg. 3 . The RAMO 4 substrate according to claim 1 , wherein the thickness thereof is in the range of 100 μm to 1000 μm.

4. The RAMO4 substrate according to claim 1 or 2, wherein the diameter thereof is in the range of 25 mm to 200 mm.

5. A Group III nitride semiconductor having: The RAMO4 substrate according to any one of claims 1 to 4; A buffer layer configured on an epitaxial growth surface formed on one surface of the RAMO4 substrate; and A group III nitride crystal is disposed on the buffer layer.

6. The Group III nitride semiconductor according to claim 5, wherein The buffer layer is an amorphous, single-crystal, or polycrystalline layer including a compound represented by InAlGaN.

7. The Group III nitride semiconductor according to claim 5 or 6, wherein: The group III nitride crystal is GaN or AlN.

8. A method for manufacturing the RAMO4 substrate according to claim 1, wherein: The RAMO4 substrate comprises a single crystal represented by the general formula RAMO4, wherein R represents one or more trivalent elements selected from Sc, In, Y and lanthanide elements, A represents one or more trivalent elements selected from Fe(III), Ga and Al, and M represents one or more divalent elements selected from Mg, Mn, Fe(II), Co, Cu, Zn and Cd. The manufacturing method includes a crystal growing step of bringing a seed crystal into contact with a melt of a raw material of the single crystal indicated by RAMO4 to generate a crystal, and pulling up the crystal to grow the single crystal. In the crystal growing step, the pulling speed of the crystal is 0.3 mm / h or more and 0.7 mm / h or less. The distance between the surface of the melt during the crystal pulling and the upper end of the heater for heating the melt is 19 mm or more and 29 mm or less.

9. The method for manufacturing a RAMO4 substrate according to claim 8, further comprising a determination step after the crystal growth step: X-ray rocking curves are measured at a plurality of positions Xi on a straight line passing through the center of the obtained single crystal, and the X-ray peak position ωi of the diffraction spectrum of the X-ray rocking curve at each position Xi is determined, where: i=1,2,3,…,n, Based on the regression line obtained from the relationship between the X-ray peak position ωi and the position Xi, the absolute value of the radius of curvature r of the crystal surface is calculated. Furthermore, based on the X-ray peak position ωi and the position Xi, the square of the correlation coefficient ρ calculated by the following formula is calculated: represents the average value of ωi, represents the average value of Xi, It is determined whether the curvature radius r is greater than or equal to 52 m and whether the square of the correlation coefficient ρ is greater than or equal to 0.81.