An oilfield wellbore under-scale corrosion experimental device and method

By designing an experimental device for under-scale corrosion of wellbore in oil fields, setting up multiple blind holes and wires at different depths to simulate corrosion and scale under-scale wellbore environments, the problem that the existing technology cannot truly reflect the on-site situation is solved, and corrosion of under-scale wellbore is achieved and accurate analysis and protective measures for scaling environments.

CN111305793BActive Publication Date: 2024-11-26PETROCHINA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010128948.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-02-28
Publication Date
2024-11-26
Estimated Expiration
2040-02-28

AI Technical Summary

Technical Problem

The existing technology is difficult to truly reflect the actual situation of under-scale corrosion in the wellbore of the oil field. There is a big difference between the indoor experimental results and the on-site conditions, and it is impossible to accurately simulate and evaluate the formation and development mechanism of under-scale corrosion.

Method used

Design an experimental device for corrosion under scale of wellbore in oil field, including hollow columnar body, plug seal and wire, and set up multiple blind holes and screw holes of different depths. The wire extends into the inner cavity of the body through the through holes, which is used to simulate the wellbore Corrosion and scaling in the environment, suspended underground and recovered after more than three months.

Benefits of technology

This device can truly reflect the corrosion and scale environment under the wellbore of the oil field, clarify the scaling and perforation mechanism of the column corrosion, scale and perforation, and provide targeted anti-corrosion and scale measures to slow down the occurrence of corrosion under the scale.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111305793B_ABST
    Figure CN111305793B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of oil and gas field wellbore pipe anti-corrosion research, and specifically relates to an oilfield wellbore under-scale corrosion experimental device and method. The present invention is composed of a main body, a plugging plug and a conducting wire; the main body is a hollow cylindrical body composed of a pentagonal prism and a cylinder, and the inner wall of the cylinder is provided with a thread; two blind holes are provided on each edge surface of the outer wall of the pentagonal prism, and a screw hole and a through hole connected to the inner cavity of the main body are provided in the first blind hole away from one end of the cylinder, and the conducting wire fixed by a nylon screw in the first blind hole extends into the cavity of the column through the through hole. The present invention completes an experiment that truly reflects the corrosion and scaling environment of the oilfield bottom well pipe through four steps: connecting the oilfield wellbore under-scale corrosion experimental device, lowering the oilfield wellbore under-scale corrosion experimental device into the well, recovering the oilfield wellbore under-scale corrosion experimental device and collecting and analyzing solid sediments, so as to take targeted anti-corrosion and anti-scaling measures to slow down the occurrence of under-scale corrosion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oil and gas field wellbore pipe anti-corrosion research, and in particular relates to an oil field wellbore under-scale corrosion experimental device and method. Background Art

[0002] Oilfield development faces the threat of corrosion and scaling. The oil and gas production wellbore pipe string has high mineralization of formation fluid and contains Ca 2+ Mg 2+ , Ba 2+ , Sr 2+ Scaling cations, SO contained in other mining layers 4 2- , HCO 3 - , CO 3 2- The scaling anions are not compatible. The scaling ion content of different fluids is different. Mixing in the wellbore will cause scaling problems. The carbonate in the formation will also produce natural scaling due to the change of temperature and pressure in the wellbore. At the same time, the medium in the oil field pipeline is rich in CO 2 , H 2 S, highly mineralized salt and other corrosive substances are highly corrosive, and the wellbore pipe string is seriously corroded and damaged. The on-site investigation found that the main feature of the oil pipe corrosion failure is local perforation damage. There are often several deeper corrosion pits under the scaling products, and even perforation damage. Corrosion and scaling are highly correlated.

[0003] Technicians have paid more and more attention to the corrosion under oilfield pipelines and have increased their research efforts. The research methods are concentrated on electrochemical testing in indoor simulated field environments, and the research directions are concentrated on (1) evaluating the various parameters of the medium inside and outside the scale layer formed by under-scale corrosion; (2) using the composition and characteristics of the scale layer involved in the diffusion channel; (3) accurately simulating the formation and development mechanism of under-scale corrosion. The research methods are diverse: for example, artificial cores of different thicknesses, grains and porosities are processed and covered on the surface of carbon steel test pieces to test the corrosion rate and electrochemical performance under different corrosive media; after the positive and negative electrodes in the homemade closed battery simulating under-scale corrosion are short-circuited for different times, the electrode in the closed anode area is scanned and tested using the dynamic potential polarization technology with a polarization scanning interval of -150-150mV. Xin and Li (Corrosion Science, 2014, 81(2):96-101) conducted long-term EIS monitoring of the corrosion behavior of 316L stainless steel at 72°C under the conditions of a simulated low-temperature multi-effect evaporator. The effects of the passive film and deposition layer on the corrosion of 316L stainless steel were obtained through the analysis of the impedance spectrum. ZL201420538170.0 Electrochemical equipment for testing under-scale corrosion of elemental sulfur. ZL201820650332.8 An experimental device for dynamically simulating under-scale corrosion, etc. The scaling layers used in these studies were generated in the laboratory and are very different from the scaling materials on site. The laboratory mainly uses chemical reagents to prepare pure scaling materials, such as calcium sulfate, calcium carbonate, barium sulfate, etc. The sediments in the on-site pipelines mainly include sand, silt, paraffin, corrosion products, scaling products, and bacterial corpses. The results of indoor studies cannot fully reflect the actual situation on site. Summary of the invention

[0004] The invention provides an oilfield wellbore under-scale corrosion experimental device and method, aiming to provide a research device and method which can truly reflect the actual on-site situation of oilfield wellbore under-scale corrosion.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] An oilfield wellbore under-scale corrosion experimental device comprises a body, a plug and a conductor; the body is a hollow column; a connecting hole is opened at one end of the body, and the connecting hole is matched and connected with the plug; a plurality of blind holes of different depths are opened on the outer wall of the body, wherein a part of the blind holes has a screw hole and a through hole connected with the inner cavity of the body, a fixing piece is connected in the screw hole, the fixing piece fixes one end of the conductor, and the other end of the conductor extends into the cavity of the body through the through hole.

[0007] The connecting hole is a threaded hole, and the plug has a thread matching the threaded hole; the screw hole is an M5 threaded hole, and the diameter of the through hole is 2mm; the fixing piece is a nylon bolt, and the connection between the nylon bolt and the wire is sealed with sealant.

[0008] The main body is a columnar body consisting of a hollow pentagonal prism and a hollow cylinder. The inner wall of the cylinder is threaded. The blind hole with the screw hole is the first blind hole, and the rest are the second blind holes. The first blind hole and the second blind hole are both located on each edge surface of the outer wall of the pentagonal prism.

[0009] The first blind holes and the second blind holes are grouped into five and are evenly arranged along the radial direction of the pentagonal prism.

[0010] The five first blind holes have the same diameter and different depths; the five second blind holes have the same diameter and different depths; and the first blind hole has the same diameter as the second blind hole.

[0011] The centers of the five blind holes in each group are cocircular; the diameters of the first blind hole and the second blind hole are both 30 mm, and the depths of the blind holes on the five facets are 2 mm, 4 mm, 6 mm, 8 mm and 10 mm respectively.

[0012] The conductor is a thin copper wire with an insulating skin, and the length of the conductor is 18 to 22 cm.

[0013] The plugging head is made of polytetrafluoroethylene, and the main body is made of carbon steel.

[0014] A method for using an oilfield wellbore under-scale corrosion test device comprises the following steps

[0015] Step 1: Connect the oilfield wellbore under-scale corrosion test device

[0016] Screw nylon bolts into a group of five blind holes on the body away from the cylinder and connect one end of the wire respectively. After one end of the wire is firmly connected, tighten the nylon bolts, and then pass the other end of the wire through the through hole into the inner cavity of the pentagonal prism. After all five wires are passed through, bind them together and tighten the plug to seal them; apply sealant to the connection between the nylon bolt and the wire, as well as the outer surface of the through hole;

[0017] Step 2: Lowering the oilfield wellbore corrosion test device into the well

[0018] The cylindrical internal thread part of the oilfield wellbore corrosion test device body connected in step 1 is connected to the screen pipe at the bottom of the oil well pump and tightened, and the oilfield wellbore corrosion test device is lowered into the bottom of the wellbore with the oil pipe along with the oil well pump;

[0019] Step 3: Recover the oilfield wellbore under-scale corrosion experimental device

[0020] After the completion of step 2, the oilfield wellbore under-scale corrosion experimental device is retrieved from the well after a predetermined suspension period;

[0021] Step 4: Collect and analyze solid sediment

[0022] Analyze the solid sediments of different thicknesses deposited in the first blind holes of different depths on the oilfield wellbore under-scale corrosion experimental device recovered in step 3;

[0023] Step 5: Analyze the recovered oilfield wellbore under-scale corrosion test device

[0024] The sediment in the second blind hole without a wire was cleaned up, and the second blind hole was cut open along the center line to observe the morphology and depth of the corrosion pit. The first blind hole with a wire was tested with an electrochemical system to analyze the impact on the under-scale corrosion of carbon steel. The experimental data were summarized and analyzed to obtain the extent and cause of under-scale corrosion in the wellbore of this block.

[0025] The predetermined suspension period in step three is greater than 3 months.

[0026] Beneficial effects: The present invention processes two rows of blind holes of different depths on the surface of the main body of the oilfield wellbore under-scale corrosion experimental device suspended at the lower end of the downhole tubing. One row is used to test the influence of scale layers of different thicknesses on the depth of corrosion pits, and the back of one row of blind holes is connected to a copper wire conductor for corrosion electrochemical performance research. The main body naturally scales under the high temperature and high pressure environment of the wellbore to form a scale layer of corresponding thickness. After more than three months, it is taken out for indoor analysis to obtain the corresponding relationship between scaling and corrosion. The present invention is easy to implement, can truly reflect the corrosion and scaling environment of the oilfield bottom well tubing, clarify the corrosion scaling and perforation mechanism of the tubing, can provide targeted anti-corrosion and anti-scaling measures, and slow down the occurrence of under-scale corrosion.

[0027] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 It is a schematic diagram of the structure of the present invention;

[0030] Figure 2 It is a cross-sectional view of the first blind hole with a wire of the present invention.

[0031] In the figure: 1-nylon bolt; 2-through hole; 3-wire; 4-body; 5-plugging; 6-connecting hole; 7-first blind hole; 8-screw hole; 9-pentagonal prism; 10-cylinder; 11-second blind hole. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] Embodiment 1:

[0034] according to Figure 1 The oilfield wellbore under-scale corrosion experimental device shown in the figure includes a body 4, a plug 5 and a conductor 3; the body 4 is a hollow cylindrical body; a connecting hole 6 is opened at one end of the body 4, and the connecting hole 6 is matched and connected with the plug 5; a plurality of blind holes of different depths are opened on the outer wall of the body 4, wherein a part of the blind holes is opened with a screw hole 8 and a through hole 2 connected with the inner cavity of the body 4, and a fixing piece is connected in the screw hole 8, and the fixing piece fixes one end of the conductor 3, and the other end of the conductor 3 extends into the cavity of the body 4 through the through hole 2.

[0035] In actual use, the blind holes connected to the wires 3 in the body 4 of the present invention are connected to one end of the wires 3 respectively. After the wires 3 are firmly connected, the other end of the wires 3 is inserted into the inner cavity of the body 4 through the through hole 2. After all the wires 3 are fully inserted, the plug is tightened to seal; the sealant is applied to the connection between the blind holes connected to the wires 3 and the wires 3, as well as the outer surface of the through hole 2; then the cylindrical 10 part of the connected oilfield wellbore corrosion test device body is connected to the screen pipe at the bottom of the oil pump and tightened, and the oilfield wellbore corrosion test device is lowered into the bottom of the wellbore with the oil pipe along with the oil pump. After the oilfield wellbore corrosion test device is suspended at the bottom of the wellbore for more than three months, the oilfield wellbore corrosion test device is retrieved from the well, and the solid sediments of different thicknesses deposited in the first blind holes of different depths on the oilfield wellbore corrosion test device are recovered, and the sediments are analyzed. The analysis of the sediments generally adopts the X-ray diffraction component analysis of the prior art, and the microscopic analysis of the typical sediments includes at least grain size, porosity, organizational structure, etc. Then, the recovered oilfield wellbore under-scale corrosion experimental device is analyzed, that is, the sediments in the blind holes without wires are cleaned, and the blind holes with wires are cut open along the center line to observe the morphology and depth of the corrosion pits; the blind holes with wires are tested with the electrochemical system of the existing technology, and the influence of under-scale corrosion in the blind holes with wires is analyzed. The experimental data are summarized and analyzed to obtain the degree and main causes of under-scale corrosion of the wellbore in this block.

[0036] The conductor 3 is provided in the technical solution of the present invention to facilitate the electrochemical law test, and can test the change of the corrosion current caused by the scale layers of different thicknesses in the blind hole, as well as the influence of the change of other corrosion factors on the corrosion current.

[0037] The invention is easy to implement, truly reflects the corrosion and scaling environment of the bottom pipe column in the oil field, clarifies the corrosion, scaling and perforation mechanism of the pipe column, and can thus provide targeted anti-corrosion and anti-scaling measures, slowing down the occurrence of under-scale corrosion.

[0038] Embodiment 2:

[0039] according to Figure 1 The oilfield wellbore under-scale corrosion experimental device shown in the figure is different from the embodiment 1 in that: the connecting hole 6 is a threaded hole, the plug 5 has a thread matching the threaded hole; the screw hole 8 is an M5 threaded hole, and the diameter of the through hole 2 is 2 mm; the fixing piece is a nylon bolt 1, and the connection between the nylon bolt 1 and the conductor 3 is sealed with sealant.

[0040] In actual use, the connection hole 6 and the plug seal 5 adopt this technical solution, making the connection of the plug seal 5 more convenient.

[0041] The screw hole 8 is an M5 threaded hole, which can conveniently tighten the nylon bolt 1, is easy to operate, and avoids the wire 3 from falling off during the experiment to affect the experimental effect. The connection between the nylon bolt 1 and the wire 3 is sealed with a sealant to avoid corrosion damage caused by the connection between the nylon bolt 1 and the wire 3, thereby affecting the accuracy of the experimental results.

[0042] The sealant in this embodiment is sealed with epoxy resin in the prior art.

[0043] Embodiment three:

[0044] according to Figure 1 and Figure 2 The oilfield wellbore under-scale corrosion experimental device shown in the figure is different from the embodiment 1 in that: the main body 4 is a columnar body consisting of a hollow pentagonal prism 9 and a hollow cylinder 10, and the inner wall of the cylinder 10 is threaded; the blind hole with the screw hole 8 is the first blind hole 7, and the rest are the second blind holes 11; the first blind hole 7 and the second blind hole 11 are both located on each edge surface of the outer wall of the pentagonal prism 9.

[0045] In actual use, the main body 4 adopts this technical solution because each facet of the pentagonal prism is a plane, which is convenient for processing blind holes of different depths and makes the distribution of blind holes more reasonable, making the subsequent data more comprehensive, and thus the analyzed data more scientific.

[0046] The pentagonal prism 9 is set as a hollow structure to facilitate the placement of the other end of the wire 3 and avoid the influence of the other end of the wire 3 on the test results. The hollow cylinder 10 is set as a hollow structure to facilitate the connection of the experimental device with the screen pipe at the bottom of the oil pump.

[0047] Embodiment 4:

[0048] according to Figure 1 The oilfield wellbore under-scale corrosion experimental device shown is different from the third embodiment in that: the first blind holes 7 and the second blind holes 11 are each grouped in five and are evenly arranged along the radial direction of the pentagonal prism 9 .

[0049] Preferably, the five first blind holes 7 have the same diameter and different depths; the five second blind holes 9 have the same diameter and different depths; and the first blind holes 7 and the second blind holes 9 have the same diameter.

[0050] Preferably, the centers of the five blind holes in each group are cocircular; the diameters of the first blind hole 7 and the second blind hole 9 are both 30 mm, and the depths of the blind holes of the five facets are 2 mm, 4 mm, 6 mm, 8 mm and 10 mm respectively.

[0051] In actual use, the 30mm diameter of the blind hole 7 is mainly convenient for screwing in the screw 1, and the 30mm diameter of the blind hole 11 is convenient for accumulating sufficient scale for microscopic analysis. The function of the center common circle is that the five blind holes 11 can be cut open along the center line at the same time in one machining process, which is convenient for experimental research and data analysis.

[0052] Embodiment five:

[0053] according to Figure 1 The oilfield wellbore under-scale corrosion experimental device shown is different from the third embodiment in that the conductor 3 is a thin copper wire with an insulating skin, and the length of the conductor 3 is 18 to 22 cm.

[0054] In actual use, the conductor 3 adopts the technical solution, which not only fully reflects the role of the conductor 3 in the present invention, but also saves experimental costs and can fully reflect the actual status of the scaling material in the well to be tested.

[0055] Embodiment six:

[0056] according to Figure 1 The oilfield wellbore under-scale corrosion experimental device shown is different from the first embodiment in that the plugging head 5 is made of polytetrafluoroethylene, and the body 4 is made of carbon steel.

[0057] In actual use, the plug seal 5 and the body 4 are threadedly connected to prevent highly mineralized water and dirt in the oil well from entering the cavity of the body 4, so that the wire 3 is not corroded and aged.

[0058] The plug seal 5 is made of polytetrafluoroethylene and is not easy to corrode; the body 4 is made of carbon steel, which makes the experiment closer to the actual site and makes the obtained experimental data more real.

[0059] Embodiment seven:

[0060] A method for using an oilfield wellbore under-scale corrosion test device comprises the following steps

[0061] Step 1: Connect the oilfield wellbore under-scale corrosion test device

[0062] Screw nylon bolts 1 into a group of five blind holes 7 on the body 4 away from the cylinder 10 and connect one end of the wire 3 respectively. After one end of the wire 3 is firmly connected, tighten the nylon bolt 1, and then pass the other end of the wire 3 through the through hole 2 into the inner cavity of the pentagonal prism 9. After all five wires are passed through, bind them together and tighten the plug 5 to seal them; apply sealant to the connection between the nylon bolt 1 and the wire 3, as well as the outer surface of the through hole 2;

[0063] Step 2: Lowering the oilfield wellbore corrosion test device into the well

[0064] The cylindrical internal thread part of the oilfield wellbore corrosion test device body 4 connected in step 1 is connected to the screen pipe at the bottom of the oil well pump and tightened, and the oilfield wellbore corrosion test device is lowered into the bottom of the wellbore with the oil pipe along with the oil well pump;

[0065] Step 3: Recover the oilfield wellbore under-scale corrosion experimental device

[0066] After the completion of step 2, the oilfield wellbore under-scale corrosion experimental device is retrieved from the well after a predetermined suspension period;

[0067] Step 4: Collect and analyze solid sediment

[0068] Analyze the solid sediments of different thicknesses deposited in the first blind holes 7 of different depths on the oilfield wellbore under-scale corrosion experimental device recovered in step 3;

[0069] Step 5: Analyze the recovered oilfield wellbore under-scale corrosion test device

[0070] The sediment in the second blind hole 11 without a conductor was cleaned up, and the second blind hole 11 was cut open along the center line to observe the morphology and depth of the corrosion pit. The first blind hole 7 with a conductor was tested with an electrochemical system to analyze the impact on the under-scale corrosion of carbon steel. The experimental data were summarized and analyzed to obtain the extent and cause of under-scale corrosion in the wellbore of this block.

[0071] The predetermined suspension period in step three is greater than 3 months.

[0072] The invention completes the oilfield wellbore under-scale corrosion experiment by connecting the oilfield wellbore under-scale corrosion experiment device, lowering the oilfield wellbore under-scale corrosion experiment device into the well, recovering the oilfield wellbore under-scale corrosion experiment device, and collecting and analyzing solid sediments. The invention is easy to implement, can truly reflect the corrosion and scaling environment of the oilfield bottom well column, clarify the corrosion and scaling perforation mechanism of the column, take targeted anti-corrosion and anti-scaling measures, and slow down the occurrence of under-scale corrosion.

[0073] The sealant in this embodiment adopts the epoxy resin of the prior art.

[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

[0075] In the absence of conflicts, technicians in this field can combine the relevant technical features in the above examples according to actual conditions to achieve corresponding technical effects. The specific combinations are not described here one by one.

[0076] It should be noted that all directional indications in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between various components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.

[0077] In addition, the descriptions of "first", "second", etc. in the present invention are only for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.

[0078] The above are only preferred embodiments of the present invention. The present invention will not be limited to the embodiments shown herein, but should conform to the widest scope consistent with the principles and novel features disclosed herein. Any simple modification, equivalent changes and modifications made to the above embodiments according to the technical essence of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. An oilfield wellbore under-scale corrosion test device, characterized in that: The invention comprises a body (4), a plug (5) and a conductor (3); the body (4) is a hollow column; a connecting hole (6) is formed at one end of the body (4), and the connecting hole (6) is connected to the plug (5); a plurality of blind holes of different depths are formed on the outer wall of the body (4), a portion of the blind holes having screw holes (8) and through holes (2) connected to the inner cavity of the body (4); a fixing piece is connected to the screw hole (8), and the fixing piece fixes one end of the conductor (3) and exposes it in the blind hole; the other end of the conductor (3) is sealed through the through hole (2) and extends into the cavity of the body (4); The body (4) is a columnar body consisting of a hollow pentagonal prism (9) and a hollow cylinder (10); the inner wall of the cylinder (10) is threaded; the blind hole with the screw hole (8) is the first blind hole (7), and the rest are the second blind holes (11); the first blind hole (7) and the second blind hole (11) are both located on each edge face of the outer wall of the pentagonal prism (9); The first blind holes (7) and the second blind holes (11) are each grouped in five and are evenly arranged along the radial direction of the pentagonal prism (9); The centers of the five blind holes in each group are cocircular; The connecting hole (6) is a threaded hole, and the plug (5) has threads matching the threaded hole; the fixing member is a nylon bolt (1), and the connection between the nylon bolt (1) and the wire (3) is sealed with a sealant; the screw hole (8) is an M5 threaded hole, and the diameter of the through hole (2) is 2 mm; The five first blind holes (7) have the same diameter and different depths; the five second blind holes (11) have the same diameter and different depths; and the first blind hole (7) and the second blind hole (11) have the same diameter.

2. The oilfield wellbore under-scale corrosion test device according to claim 1, characterized in that: The diameters of the first blind hole (7) and the second blind hole (11) are both 30 mm, and the depths of the blind holes on the five facets are 2 mm, 4 mm, 6 mm, 8 mm and 10 mm respectively.

3. The oilfield wellbore under-scale corrosion test device according to claim 1, characterized in that: The conductor (3) is a thin copper wire with an insulating skin, and the length of the conductor (3) is 18 to 22 cm.

4. The oilfield wellbore under-scale corrosion test device according to claim 1, characterized in that: The plugging head (5) is made of polytetrafluoroethylene, and the body (4) is made of carbon steel.

5. A method for using an oilfield wellbore under-scale corrosion test device, characterized in that: The method of using the wellbore under-scale corrosion test device as described in any one of claims 1 to 4 comprises the following steps: Step 1: Connect the oilfield wellbore under-scale corrosion test device Screw in nylon bolts (1) into a group of five first blind holes (7) on the body (4) away from the cylinder (10) and connect one end of the wire (3) to each of them. After one end of the wire (3) is firmly connected, tighten the nylon bolt (1). Then, pass the other end of the wire (3) through the through hole (2) into the inner cavity of the pentagonal prism (9). After all five wires are passed through, bind them together and tighten the plug (5) to seal them. Apply sealant to the connection between the nylon bolt (1) and the wire (3) and the outer surface of the through hole (2). Step 2: Lowering the oilfield wellbore corrosion test device into the well The cylindrical internal threaded portion of the oilfield wellbore corrosion test device body (4) connected in step 1 is connected to the screen pipe at the bottom of the oil well pump and tightened, and the oilfield wellbore corrosion test device is lowered into the bottom of the wellbore with the oil pipe along with the oil well pump; Step 3: Recover the oilfield wellbore under-scale corrosion experimental device After the completion of step 2, the oilfield wellbore under-scale corrosion experimental device is retrieved from the well after a predetermined suspension period; Step 4: Collect and analyze solid sediment Analyze the solid sediments of different thicknesses deposited in the first blind holes (7) at different depths on the oilfield wellbore underscale corrosion experimental device recovered in step 3; Step 5: Analyze the recovered oilfield wellbore under-scale corrosion test device The sediment in the second blind hole (11) without the conductor is cleaned up, and the second blind hole (11) is cut open along the center line to observe the morphology and depth of the corrosion pit; the first blind hole (7) with the conductor is tested by an electrochemical system to analyze the effect on the corrosion under the carbon steel scale, and the experimental data are summarized and analyzed to obtain the extent and cause of the corrosion under the scale of the wellbore.

6. The method for using the oilfield wellbore under-scale corrosion test device according to claim 5, characterized in that: The predetermined suspension period in step three is greater than 3 months.