Filling fire clay for assembling tundish upper water inlet iron shell and preparation method thereof

By using a specific proportion of filling fire mortar at the water inlet of the tundish, the problem of molten steel leakage is solved, the high temperature resistance and thermal shock stability of the equipment are improved, the service life is extended and safety hazards are reduced.

CN111348928BActive Publication Date: 2024-10-11WUXI NANFANG REFRACTORIES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010329145.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-04-23
Publication Date
2024-10-11
Estimated Expiration
2040-04-23

AI Technical Summary

Technical Problem

During the iron and steel metallurgical continuous casting process, the nozzle of the tundish is prone to steel penetration problems under the action of high-temperature molten steel, leading to equipment damage and safety hazards. Existing refractory materials are prone to micro-cracks under the action of temperature and pressure, causing molten steel to seep out. .

Method used

It is composed of brown corundum, 85 alumina, quartz, kyanite, ceramic plastic adhesive, Suzhou soil, spinel, potassium feldspar, methylcellulose, 92 magnesia, sodium alginate, starch and aluminum sol Fill the fire clay, through specific particle gradation and proportion, combined with aluminum sol liquid as a binding agent, stir and compact, naturally dry and then baked at low temperature in an oven to improve the heat resistance and impermeability of the material.

Benefits of technology

It effectively prevents leakage of molten steel, extends the service life of the nozzle of the tundish, improves the high temperature resistance and thermal shock stability of the equipment, and reduces the risk of accidents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004958845000000051
    Figure GDA0004958845000000051
  • Figure GDA0004958845000000061
    Figure GDA0004958845000000061
  • Figure GDA0004958845000000062
    Figure GDA0004958845000000062
Patent Text Reader

Abstract

The invention discloses a filling fireclay for assembling a tundish upper water shell, which contains the following components: brown corundum, 85 alumina, quartz, kyanite, ceramic plastic adhesive, Suzhou soil, spinel, potassium feldspar, methyl cellulose, 92 magnesium sand, sodium sea zeolite, starch, and aluminum sol; the weight percentage of each component is: 3-7% brown corundum, 3-7% 85 alumina, 65-75% quartz, 3-7% kyanite, 3-7% ceramic plastic adhesive, 2-5% Suzhou soil, 1-3% spinel, 1-2% potassium feldspar, 0.1-0.3% methyl cellulose, 2-5% 92 magnesium sand, 0.2-0.5% sodium sea zeolite, 0.3-0.7% starch, and 12-18% aluminum sol. The purpose of the invention is to provide a filling fireclay for assembling a tundish upper water shell, which has a new type of anti-seepage steel structure and can improve the life of tundish refractory materials and fundamentally solve the problem of steel seepage under high continuous casting conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of inorganic non-metallic refractory materials, and more specifically to filling fire clay for assembling an iron shell of a tundish upper nozzle and a preparation method thereof. Background Art

[0002] Continuous casting is the main process of steel metallurgical production at present. The tundish is the most important equipment in the continuous casting process. During the entire steel casting process, the tundish is in a fixed state, receiving molten steel from the ladle, and injecting the molten steel into the crystallizer according to the set casting speed through the valve formed by the stopper rod and the upper nozzle. The key components for controlling the flow rate, the stopper rod and the upper nozzle, are in contact with the molten steel with a temperature of more than 1500 degrees Celsius for a long time, so the quality of these two products must be guaranteed. In particular, the upper nozzle placed at the bottom of the tundish is subject to the static pressure of the high-temperature molten steel, the top force of the lower submerged nozzle from bottom to top, and the disturbance caused by the high-speed flow of high-temperature and high-density molten steel.

[0003] Usually, in some steel mills, when using the tundish water inlet, steel often seeps through the gap between the water inlet and the seat brick, affecting the normal production of the steel mill. In view of this situation that often occurs, we analyzed the water inlet, the seat brick, and the fire clay. We believe that the cause is that the drying and shrinkage of the fire clay during baking and use causes fine cracks. At the same time, during the steel pouring process, the high-temperature molten steel gradually seeps through the fine cracks in the fire clay due to the factors of the plug rod and the pressure of the molten steel. As time goes on, the molten steel eventually seeps into the mechanism, which will seriously damage the mechanism and cause greater equipment accidents and even personal safety accidents. The conventionally manufactured water inlet has a smooth upper surface of the inclined surface and a smooth inner wall surface of the seat brick. The fire clay is filled in the middle. Under the action of temperature and external force, the fire clay has penetrating fine cracks, resulting in steel seepage.

[0004] The continuous casting process of steel mills uses a tundish to hold molten steel. The refractory materials used in the tundish are called "functional refractory materials", which mainly include protective sleeves, stopper rods, nozzles, etc. There are two types of nozzles in the tundish: upper nozzle and lower nozzle, both of which play the role of circulating molten steel. The upper nozzle is embedded in the nozzle seat brick during the construction of the tundish dry material, and becomes one with the tundish; the lower nozzle is installed outside the bottom of the tundish, fixed by a fixing mechanism, and connected with the upper nozzle in a fixed slide. The function of the lower nozzle is to control the flow of molten steel and adjust the continuous casting speed by a different diameter from the upper nozzle. Therefore, the nozzle of the continuous casting tundish must be resistant to erosion by molten steel and high temperature, and on the other hand, it must have good thermal shock stability. Summary of the invention

[0005] In order to solve the above problems, the purpose of the present invention is to provide a new type of anti-seepage steel structure for filling fire clay for assembling the iron shell of the upper water outlet of the tundish, which can prolong the life of the tundish refractory material and fundamentally solve the problem of steel seepage under high continuous casting conditions.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] The filling fire clay for assembling the iron shell of the tundish upper nozzle is composed of the following components: brown corundum, 85 alumina, quartz, kyanite, ceramic plastic adhesive, Suzhou soil, spinel, potassium feldspar, methyl cellulose, 92 magnesium sand, sodium alginate, starch, and aluminum sol; the weight percentage of each component is: brown corundum 3-7%, 85 alumina 3-7%, quartz 65-75%, kyanite 3-7%, ceramic plastic adhesive 3-7%, Suzhou soil 2-5%, spinel 1-3%, potassium feldspar 1-2%, methyl cellulose 0.1-0.3%, 92 magnesium sand 2-5%, sodium alginate 0.2-0.5%, starch 0.3-0.7%, and aluminum sol 12-18%.

[0008] In some embodiments, brown corundum: Al 2 O 3 Content ≥95.0%, Fe 2 O 3 Content <1%、SiO 2 Content ≤1.20%, TiO 2 Content <3.8%, body density ≥3.8g / m3;

[0009] 85 Alumina: A l 2 O 3 Content ≥85.0%, Fe 2 O 3 Content<1.8%, T i O 2 Content <4.0%, body density ≥3.15g / m3;

[0010] Quartz: SiO 2 Content ≥97%, Fe 2 O 3 Content <0.5%;

[0011] Kyanite Al 2 O 3 Content ≥55.0%, Fe 2 O 3 Content<1.5%, T i O 2 Content ≤2%;

[0012] Ceramic plastic adhesive bulk density: 450g / L;

[0013] Suzhou soil: A l 2 O 3 Content 34~37%, Fe 2 O 3 Content ≤0.85%, SiO 2Content 47-50%;

[0014] Spinel Al 2 O 3 Content 75~77%, SiO 2 Content ≤0.20%, MgO content 21~23%, body density ≥

[0015] 3.25g / m3;

[0016] Potassium feldspar: A l 2 O 3 Content ≥12%, SiO 2 Content ≤1.20%;

[0017] Methylcellulose methoxy content 26-33%, water insoluble content ≤ 2.0%;

[0018] 92 magnesia: MgO content ≥ 92.0%, SiO 2 Content ≤4.20%, CaO content ≤2.0%; body density ≥3.18g / m3;

[0019] Sodium alginate: ash content 18.0-27.0%, water-insoluble matter ≤ 0.60%;

[0020] Starch moisture ≤14%, fineness ≥99%, ash content about 0.35%, protein content ≤0.55%;

[0021] Aluminum sol: Al 2O3 content ≥ 30%, P content < 20%, pH ≤ 4.

[0022] In some embodiments, the particle grading of each component is: brown corundum 1-0 mm, 85 alumina 0.5-0 mm, quartz 0.5-0 mm200 mesh, kyanite 180 mesh, ceramic plastic adhesive 200 mesh, Suzhou soil 200 mesh, spinel 325 mesh, potassium feldspar 200 mesh, methyl cellulose 100 mesh, 92 magnesium sand 325 mesh, sodium alginate 100 mesh, starch 200 mesh, and aluminum sol is liquid.

[0023] The particle size distribution of quartz is in percentage by weight:

[0024] 0.5~0mm 70~75%

[0025] 200 mesh 25~30%.

[0026] In some embodiments, a method for preparing a filling fire clay for assembling a tundish upper water shell is provided, wherein the components are as follows: brown corundum 3-7%, 85 alumina 3-7%, quartz 65-75%, kyanite 3-7%, ceramic plastic adhesive 3-7%, Suzhou soil 2-5%, spinel 1-3%, potassium feldspar 1-2%, methyl cellulose 0.1-0.3%, 92 magnesium sand 2-5%, sodium alginate 0 .2~0.5%, starch 0.3~0.7%, stir the mixture of the above particles and fine powder for 30 minutes, then add 12~18% aluminum sol liquid binder, add the amount of binder and set aside, fix the middle bag upper water inlet body brick on the operating platform, fix the positioning device, and then evenly spread the filling sealing fire mud on the inner surface of the iron shell, and then put it inside the upper water inlet brick, use a small hydraulic press to press the iron shell within the specified size, and then remove the remaining part of the fire mud for reuse. After natural drying for 8 hours, put it in a 200-degree oven and dry it for 20 to 25 hours. DETAILED DESCRIPTION

[0027] The filling fire clay for assembling the iron shell of the tundish upper water port contains the following components: brown corundum, 85 alumina, quartz, kyanite, ceramic plastic adhesive, Suzhou soil, spinel, potassium feldspar, methyl cellulose, 92 magnesium sand, sodium alginate, starch, and aluminum sol; the weight percentage of each component is: brown corundum 3-7%, 85 alumina 3-7%, quartz 65-75%, kyanite 3-7%, ceramic plastic adhesive 3-7%, Suzhou soil 2-5%, spinel 1-3%, potassium feldspar 1-2%, methyl cellulose 0.1-0.3%, 92 magnesium sand 2-5%, sodium alginate 0.2-0.5%, starch 0.3-0.7%, and aluminum sol 12-18%.

[0028] Brown corundum: Al 2 O 3 Content ≥95.0%, Fe 2 O 3 Content <1%、SiO 2 Content ≤1.20%, TiO 2 Content <3.8%, body density ≥3.8g / m3;

[0029] 85 Alumina: Al 2 O 3 Content ≥85.0%, Fe 2 O 3 Content<1.8%, T i O 2 Content <4.0%, body density ≥3.15g / m3;

[0030] Quartz: SiO2 Content ≥97%, Fe 2 O 3 Content <0.5%;

[0031] Kyanite A l 2 O 3 Content ≥55.0%, Fe 2 O 3 Content <1.5%、TiO 2 Content ≤2%;

[0032] Ceramic plastic adhesive bulk density: 450g / L;

[0033] Suzhou soil: Al 2 O 3 Content 34~37%, Fe 2 O 3 Content ≤0.85%, Si O 2 Content 47-50%;

[0034] Spinel Al 2 O 3 Content 75~77%, SiO 2 Content ≤ 0.20%, MgO content 21-23%, bulk density ≥ 3.25g / m3;

[0035] Potassium feldspar: Al 2 O 3 Content ≥12%, SiO 2 Content ≤1.20%;

[0036] Methylcellulose methoxy content 26-33%, water insoluble content ≤ 2.0%;

[0037] 92 magnesia: MgO content ≥ 92.0%, SiO 2 Content ≤4.20%, CaO content ≤2.0%; body density ≥3.18g / m3;

[0038] Sodium alginate: ash content 18.0-27.0%, water-insoluble matter ≤ 0.60%;

[0039] Starch moisture ≤14%, fineness ≥99%, ash content about 0.35%, protein content ≤0.55%;

[0040] Aluminum sol: Al 2 O 3 Content ≥30%, P content <20%, pH ≤4.

[0041] The particle grading of each component is: brown corundum 1-0mm, 85 alumina 0.5-0mm, quartz 0.5-0mm200 mesh, kyanite 180 mesh, ceramic plastic adhesive 200 mesh, Suzhou soil 200 mesh, spinel 325 mesh, potassium feldspar 200 mesh, methyl cellulose 100 mesh, 92 magnesia sand 325 mesh, sodium alginate 100 mesh, starch 200 mesh, and aluminum sol is liquid.

[0042] The particle size distribution of quartz is in percentage by weight:

[0043] 0.5~0mm 70~75%

[0044] 200 mesh 25~30%.

[0045] A method for preparing filling fire clay for assembling an iron shell of a tundish upper nozzle, comprising brown corundum, 85 alumina, quartz, kyanite, ceramic plastic adhesive, Suzhou soil, spinel, potassium feldspar, methyl cellulose, 92 magnesium sand, sodium alginate, starch and aluminum sol; the weight percentage of each component thereof is as follows: 3-7% brown corundum, 3-7% 85 alumina, 65-75% quartz, 3-7% kyanite, 3-7% ceramic plastic adhesive, 2-5% Suzhou soil, 1-3% spinel, 1-2% potassium feldspar, 0.1-0.3% methyl cellulose, 2-5% 92 magnesium sand, 0.2-0 .5%, starch 0.3-0.7%, stir the mixture of the above particles and fine powder for 30 minutes, then add 12-18% aluminum sol liquid binder, add the amount of binder and set aside, fix the middle bag upper water inlet body brick on the operating platform, fix the positioning device, and then evenly spread the filling sealing fire mud on the inner surface of the iron shell, and then put it inside the upper water inlet brick, use a small hydraulic press to press the iron shell within the specified size, and then remove the remaining part of the fire mud for reuse. After natural drying for 8 hours, put it in a 200-degree oven and dry it for 20-25 hours.

[0046] Ceramic plastic binder: An inorganic additive used for pressing, ramming and extrusion molding. Even if the amount added is small, it will have a plasticizing effect and enhance toughness. It uses mixed water to produce swelling, thereby producing a plasticizing effect, and can also increase the mechanical strength of the body.

[0047] The particle size required for quartz as a refractory material is generally 30% to 35% of particles larger than 1mm, 35% to 40% of particles 0.09 to 1mm, and the rest less than 0.09mm. The loosening and sintering ability of the siliceous body when heated depends on the nature and quantity of the coarse and fine particle sizes in the particle composition. The coarse particle transformation occurs to a large extent after the fine particle transformation and the silicon body begins to burn. Therefore, the volume expansion during the coarse particle transformation is the basic factor that causes the brick body to loosen and even crack. Therefore, it is hoped that there is a sufficient amount of fine particles in the brick to improve the sintering property of the brick.

[0048] Kyanite is a high-aluminum mineral with strong chemical corrosion resistance, high thermal shock mechanical strength, and irreversible thermal expansion. It is mainly because of its good refractoriness and corrosion resistance. More importantly, the volume expansion after heat flow will densify the castable, and this process is irreversible. Therefore, it is used more.

[0049] Alumina sol: It has good dispersibility and stability, high temperature resistance (greater than 1700℃), high bonding strength, suitable for rapid baking, high strength at medium and high temperatures, excellent thermal shock resistance and stability, etc. It is specially used to produce refractory bulk materials, such as castables, fire mud, repair materials, gunning materials, etc. In the corundum castable system, the impurity CaO introduced by cement bonding affects its high temperature performance. ASOL-2, as a binder, hardly introduces impurities, and its Al 2 O 3 Colloids promote sintering and improve high-temperature performance. In addition, compared with cement, it can achieve rapid baking, and is particularly suitable for prefabricated blocks in areas resistant to high-temperature fluid erosion. When ASOL-2 is used for repair materials and fire clay, it has good adhesion, rapid strength increase, and high high-temperature strength. It is particularly suitable for refractory fire clay and will not react with Fe impurities in the raw materials.

[0050] Plasticizer: A substance that can increase the plasticity of the mixed refractory mixture, or a substance that can improve the ability of the mixture (fire mud) to produce strain under stress. It is an additive used in plastic and ramming refractory materials. It is also used in some cast refractory materials. Plasticizer is a type of viscous substance or a type of surfactant.

[0051] Shrinkage-proofing agent: a substance that can prevent the shrinkage of refractory materials during heating and use after molding, also known as volume stabilizer or expansion agent. The amount of shrinkage-proofing agent added is generally a few percent of the total amount of ingredients. Its shrinkage-proofing principle is: 1. Thermal decomposition. The shrinkage-proofing agent undergoes pyrolysis after high temperature heating, and the molar volume of its product is greater than the molar volume of the original substance before pyrolysis, thereby compensating for the sintering shrinkage of the material. When kyanite is heated as an expansion agent, the following pyrolysis reaction occurs; due to the difference in molar volume before and after pyrolysis, a volume expansion effect of 10% to 12% can be produced, thereby compensating for the sintering shrinkage of the material. For example, clay and quartz powder in fire mud are added to compensate for the shrinkage by the volume expansion effect of mullite generated at high temperature. 3. Crystal transformation: Adding materials that can produce crystal transformation during high-temperature heating, and the molar volume of the transformed crystal is greater than the molar volume before the transformation, can also compensate for sintering shrinkage. For example, adding an appropriate amount of quartz powder to aluminum silicate fire clay or plastic can compensate for the sintering shrinkage of the matrix by taking advantage of the volume expansion (12.7% or 17.4%) when quartz is transformed into tridymite or cristobalite.

[0052] The basic production process of the invented product is: according to the formula of ratio 2 in Table 1, the raw materials brown corundum, 85 bauxite, and quartz are crushed and screened according to the ratio 2 in the table, and the remaining fine powder raw materials kyanite, ceramic plastic adhesive, Suzhou soil, spinel, potassium feldspar, methyl cellulose, 92 magnesium sand, sodium alginate, and starch are also mixed according to ratio 2. After the mixture of the above particles and fine powder ratios is stirred for 30 minutes, 15% of aluminum sol liquid binder is added. Depending on the on-site construction conditions, the amount of binder is reasonably added and reserved. The middle package upper nozzle body brick is fixed on the operating platform, the positioning device is fixed, and then the filling sealing fire mud is evenly distributed on the inner surface of the iron shell, and then it is put inside the upper nozzle brick. Use a small hydraulic press to press the iron shell within the specified size swing, and then remove the remaining part of the fire mud for reuse. After natural drying for 8 hours, put it in a 200-degree oven for drying for 20 to 25 hours.

[0053] Table 1:

[0054]

[0055]

[0056] Table 2:

[0057]

[0058]

[0059] The above are only some embodiments of the invention. It should be pointed out that for ordinary technicians in this field, other modifications and improvements can be made without departing from the creative concept of the utility model, which all belong to the protection scope of the utility model.

Claims

1. Fire clay for assembling the iron shell of the tundish upper nozzle, characterized in that: The invention is composed of the following components: brown corundum, 85 alumina, quartz, kyanite, ceramic plastic adhesive, Suzhou soil, spinel, potassium feldspar, methyl cellulose, 92 magnesium sand, sodium alginate, starch and aluminum sol; the weight percentage of each component is: 3-7% brown corundum, 3-7% 85 alumina, 65-75% quartz, 3-7% kyanite, 3-7% ceramic plastic adhesive, 2-5% Suzhou soil, 1-3% spinel, 1-2% potassium feldspar, 0.1-0.3% methyl cellulose, 2-5% 92 magnesium sand, 0.2-0.5% sodium alginate and 0.3-0.7% starch; and 12-18% aluminum sol as an external binder.

2. The filling fire clay for assembling the tundish upper nozzle iron shell according to claim 1, characterized in that: The brown corundum has Al2O3 content ≥95.0%, Fe2O3 content <1%, SiO2 content ≤1.20%, TiO2 content <3.8%, and bulk density ≥3.8g / m 3 ; The 85 alumina: Al2O3 content ≥85.0%, Fe2O3 content <1.8%, TiO2 content <4.0%, bulk density ≥3.15g / m 3 ; The quartz: SiO2 content ≥ 97%, Fe2O3 content < 0.5%; The kyanite: Al2O3 content ≥ 55.0%, Fe2O3 content < 1.5%, TiO2 content ≤ 2%; The ceramic plastic adhesive has a bulk density of 450 g / L; The Suzhou soil: Al2O3 content 34-37%, Fe2O3 content ≤0.85%, SiO2 content 47-50%; The spinel has an Al2O3 content of 75-77%, a SiO2 content of ≤0.20%, and a MgO content of 21-23%; a bulk density of ≥3.25 g / m 3 ; The potassium feldspar Al2O3 content is ≥12%, and the SiO2 content is ≤1.20%; The methyl cellulose has a methoxy content of 26-33% and a water-insoluble content of ≤2.0%; The 92 magnesia sand: MgO content ≥ 92.0%, SiO2 content ≤ 4.20%, CaO content ≤ 2.0%; bulk density ≥ 3.18 g / m 3 ; The sodium alginate: ash content 18.0-27.0%, water-insoluble matter ≤ 0.60%; The starch has a moisture content of ≤14%, a fineness of ≥99%, an ash content of about 0.35%, and a protein content of ≤0.55%; The aluminum sol has: Al2O3 content ≥30%, P content <20%, and pH ≤4.

3. The filling fire clay for assembling the tundish upper nozzle iron shell according to claim 2, characterized in that: The particle grading of each component is: brown corundum 1-0mm, 85 alumina 0.5-0mm, quartz 0.5-0mm, quartz 200 mesh, kyanite 180 mesh, ceramic plastic adhesive 200 mesh, Suzhou soil 200 mesh, spinel 325 mesh, potassium feldspar 200 mesh, methyl cellulose 100 mesh, 92 magnesia sand 325 mesh, sodium alginate 100 mesh, starch 200 mesh, and aluminum sol is liquid.

4. The filling fire clay for assembling the tundish upper nozzle iron shell according to claim 3, characterized in that: The particle size distribution of the quartz is as follows: 0.5~0mm70~75% 200 mesh 25~30%.

5. The method for preparing the filling fire clay for assembling the tundish upper nozzle iron shell according to any one of claims 1 to 4, characterized in that: The filling fire clay for assembling the tundish upper water shell is composed of the following components: brown corundum, 85 alumina, quartz, kyanite, ceramic plastic adhesive, Suzhou soil, spinel, potassium feldspar, methyl cellulose, 92 magnesium sand, sodium alginate, starch, and aluminum sol; the weight percentage of each component is: brown corundum 3-7%, 85 alumina 3-7%, quartz 65-75%, kyanite 3-7%, ceramic plastic adhesive 3-7%, Suzhou soil 2-5%, spinel 1-3%, potassium feldspar 1-2%, methyl cellulose 0.1-0.3%, 92 magnesium sand 2-5%, 0.2-0.5% sodium alginate and 0.3-0.7% starch are mixed in the above proportions and stirred for 30 minutes, then 12-18% aluminum sol liquid binder is added for later use. The middle bag upper nozzle body brick is fixed on the operating platform, the positioning device is fixed, and then the filling sealing fire mud is evenly distributed on the inner surface of the iron shell, and then put inside the upper nozzle brick. Use a small hydraulic press to press the iron shell within the specified size range, and then remove the remaining fire mud for reuse. After natural drying for 8 hours, put it in a 200-degree oven and dry it for 20-25 hours.