Reactive silica-alumina matrix component composition for bottoms cracking catalysts
By developing a bottom residue cracking catalyst composition containing alumina, reactive silica and kaolin, the problem of high coke selectivity in existing catalysts is solved, and efficient cracking of light olefins and light cycle oils is achieved, and the catalyst is simplified Prepare and reduce costs.
Patent Information
- Application Number
- CN201880079490.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2017-12-11
- Filing Date
- 2018-12-10
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2038-12-10
AI Technical Summary
The existing catalysts have high coke selectivity during cracking, making it difficult to maximize the yield of light olefins and light circulating oils. At the same time, the preparation process is complex and the cost is high.
A bottom residue cracking catalyst composition is developed, including about 30% to 60% by weight of alumina, 2% to 20% by weight of reactive silica, 3% to 20% by weight of gum-soluble hydroaluminum ore and 10% by weight of % to 50 wt% of kaolin, microspheres are prepared by spray drying, for contacting with hydrocarbon feed and reducing coke yield.
It significantly reduces coke selectivity, improves the yield of light olefins and light cycle oils, simplifies the catalyst preparation process, and reduces production costs.
Smart Images

Figure CN111465446B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of priority to U.S. Provisional Patent Application No. 62 / 597,176, filed on December 11, 2017, the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0003] The present technology generally relates to petroleum refining catalysts. More specifically, the technology relates to bottoms cracking catalysts comprising alumina, a dopant, reactive silica, a component comprising peptizable gibbsite, colloidal silica, aluminum chlorohydrate, and kaolin, and methods of making and using such catalysts. Summary of the invention
[0004] In one aspect, the bottoms cracking catalyst composition comprises about 30 wt% to about 60 wt% alumina; greater than 0 to about 10 wt% of a dopant measured in the form of an oxide; about 2 wt% to about 20 wt% reactive silica; about 3 wt% to about 20 wt% of a component comprising peptized gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and about 10 wt% to about 50 wt% kaolin. In some embodiments, the dopant is doped onto the alumina, while in other embodiments, the dopant is mixed with the alumina. Additionally, in some embodiments, the alumina may be calcined alumina.
[0005] In another aspect, a method for preparing a bottoms cracking catalyst is provided, the method comprising forming an aqueous slurry containing, on a dry weight basis: about 30 wt % to about 60 wt % alumina; greater than 0 to about 10 wt % of a dopant measured as an oxide; about 2 wt % to about 20 wt % reactive silica; about 3 wt % to about 20 wt % of a component comprising peptizable gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and about 10 wt % to about 50 wt % kaolin, and spray drying the aqueous slurry to obtain microspheres.
[0006] In another aspect, a method for cracking a hydrocarbon feed is provided, the method comprising contacting the feed with a bottoms cracking catalyst comprising from about 30 wt% to about 60 wt% alumina; from greater than 0 to about 10 wt% of a dopant measured in oxide form; from about 2 wt% to about 20 wt% reactive silica; from about 3 wt% to about 20 wt% of a component comprising peptized gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and from about 10 wt% to about 50 wt% kaolin.
[0007] In another aspect, the bottoms cracking catalyst composition includes about 30 wt% to about 60 wt% alumina; greater than 0 to about 10 wt% rare earth carbonate; about 2 wt% to about 20 wt% reactive silica; about 3 wt% to about 20 wt% of a component comprising peptizable gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and about 10 wt% to about 50 wt% kaolin. The rare earth may be ytterbium, gadolinium, cerium, lanthanum, yttrium, or a mixture of any two or more thereof.
[0008] In another aspect, a method for preparing a bottoms cracking catalyst is provided, the method comprising forming an aqueous slurry containing, on a dry weight basis: about 30 wt% to about 60 wt% alumina; greater than 0 to about 10 wt% rare earth carbonate; about 2 wt% to about 20 wt% reactive silica; about 3 wt% to about 20 wt% of a component comprising peptizable gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and about 10 wt% to about 50 wt% kaolin, and spray drying the aqueous slurry to obtain microspheres. The rare earth may be ytterbium, gadolinium, cerium, lanthanum, yttrium, or a mixture of any two or more thereof.
[0009] In another aspect, a method for cracking a hydrocarbon feed is provided, the method comprising contacting the feed with a bottoms cracking catalyst, the cracking catalyst comprising about 30 wt% to about 60 wt% alumina; greater than 0 to about 10 wt% of a dopant measured in oxide form; about 2 wt% to about 20 wt% reactive silica; about 3 wt% to about 20 wt% of a component comprising peptizable gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and about 10 wt% to about 50 wt% kaolin. The rare earth may be ytterbium, gadolinium, cerium, lanthanum, yttrium, or a mixture of any two or more thereof.
[0010] In another aspect, the bottoms cracking catalyst composition comprises about 10 wt% to about 20 wt% of a rare earth exchanged Y zeolite; about 10 wt% to about 30 wt% of a binder comprising silica and gibbsite; about 30 wt% to about 60 wt% of an additive comprising alumina and optionally crystalline gibbsite; and about 10 wt% to about 50 wt% of kaolin. In such embodiments, the rare earth exchanged Y zeolite may comprise ytterbium, gadolinium, cerium, lanthanum, yttrium, or a mixture of any two or more thereof. In some embodiments, the rare earth exchanged Y zeolite comprises lanthanum. In such embodiments, the average particle size of the catalyst may be about 70-95 microns. In such embodiments, the mercury pore volume of the catalyst may be 0.3-0.56 cc / g, with a diameter ranging from 4 to 2,000 nm.
[0011] In another aspect, a method of preparing a bottoms cracking catalyst comprises forming an aqueous slurry containing, on a dry weight basis: about 10 wt% to about 20 wt% of a rare earth exchanged Y zeolite; about 10 wt% to about 30 wt% of a binder comprising silica and gibbsite; about 30 wt% to about 60 wt% of an additive comprising alumina and optionally crystalline gibbsite; and about 10 wt% to about 50 wt% of kaolin; and spray drying the aqueous slurry to obtain microspheres. The method may further comprise calcining the microspheres.
[0012] In another aspect, a method of cracking a hydrocarbon feed comprises contacting the feed with any of the above-described bottoms cracking catalysts. Such methods can result in a greater than 10% decrease in coke yield measured at 13 wt% bottoms when compared to contacting the feed with a catalyst exhibiting the same physical characteristics but not including the bottoms cracking catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 Catalytic product conversions for example catalyst blends (Blends 2, 4, and 6) and comparative catalyst blends (Blends 1, 3, and 5) as described in Example 2 are illustrated.
[0014] Figure 2 Graph of bottoms as a function of coke production for the illustrative and comparative catalyst blends described in Example 2.
[0015] Figure 3 Graph of hydrogen production as a function of product conversion for the illustrative and comparative catalyst blends described in Example 2.
[0016] Figure 4 Graph of dry gas production as a function of product conversion for the illustrative and comparative catalyst blends described in Example 2.
[0017] Figure 5 Graph of liquefied petroleum gas (LPG) production as a function of product conversion for the illustrative and comparative catalyst blends described in Example 2.
[0018] Figure 6 Graph of gasoline yield as a function of product conversion for the illustrative and comparative catalyst blends described in Example 2.
[0019] Figure 7 Graph of coke yield as a function of product conversion for the illustrative and comparative catalyst blends described in Example 2.
[0020] Figure 8 Graphs of light cycle oil (LCO) production and bottoms conversion as a function of coke selectivity for the illustrative and comparative catalyst blends described in Example 2. DETAILED DESCRIPTION
[0021] Various embodiments are described below. It should be noted that the specific embodiments are not intended to be exhaustive descriptions or as limitations on the broader aspects discussed herein. An aspect described in conjunction with a specific embodiment is not necessarily limited to the embodiment, and may be practiced with any other (one or more) embodiments.
[0022] As used herein, "about" will be understood by one of ordinary skill in the art and will vary to some extent depending on the context in which it is used. If a term is used that is not clear to one of ordinary skill in the art, then "about" will mean up to plus or minus 10% of the specific term, taking into account the context in which it is used.
[0023] Unless otherwise indicated herein or obviously contradictory to the content, the use of the terms "a / an" and "said" and similar references in the case of describing elements (especially in the case of the following claims) should be interpreted as including singular and plural. Unless otherwise indicated herein, the description of the value range herein is only intended to serve as a shorthand method for individually referring to each individual value belonging to the range, and each individual value is incorporated into this specification as if individually described herein. Unless otherwise indicated herein or otherwise obviously contradictory to the context, all methods described herein can be performed in any suitable order. Unless otherwise stated, the use of any and all examples or illustrative language (such as "such as") provided herein is only intended to better illustrate the embodiment and does not limit the scope of the claims. The language in the specification should not be understood to indicate any unrequired elements as necessary.
[0024] The product value of refinery products, such as gasoline, light olefins and light cycle oil, varies with time and / or location, but these are always more valuable than the bottoms fraction. Refineries need catalyst selections that will maximize each of these valuable fractions while minimizing the yield of low-value bottoms so that they can adjust the balanced catalyst composition at any time to maximize profitability. It is understood that zeolite cracking maximizes gasoline, while matrix cracking maximizes light olefins and light cycle oil (LCO). The inventors of the present invention have now developed catalyst additives for selective cracking bottoms with minimal coking and refinery needs to maximize LCO (diesel) and light olefins. In addition, the inventors of the technology described herein have found that bottoms cracking catalyst compositions exhibit unexpectedly low coke selectivity and are easier to prepare.
[0025] Provided herein are bottoms cracking catalyst compositions, methods for preparing bottoms cracking catalyst compositions, and methods for cracking hydrocarbon feeds. The compositions include dopant-stabilized alumina. The dopant may include a rare earth metal measured in oxide form. Although some embodiments contemplate the use of bottoms cracking catalyst compositions with zeolites, other embodiments are proposed that contain little or no zeolite.
[0026] In one aspect, a bottoms cracking catalyst composition is provided, comprising about 30 wt% to about 60 wt% alumina; greater than 0 to about 10 wt% of a dopant measured in the form of an oxide; about 2 wt% to about 20 wt% reactive silica; about 3 wt% to about 20 wt% of a component comprising peptized gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and about 10 wt% to about 50 wt% kaolin. In some embodiments, the dopant is doped onto the alumina, while in other embodiments, the dopant is mixed with the alumina. Additionally, in some embodiments, the alumina may be calcined alumina.
[0027] The bottoms cracking catalyst composition includes about 30 wt% to about 60 wt% alumina. This may include, but is not limited to, about 30 wt%, about 35 wt%, about 40 wt%, about 45 wt%, about 50 wt%, about 55 wt%, about 60 wt%, or a range between any two of these values. In some embodiments, the amount of alumina includes about 30 wt% to about 60 wt%, about 35 wt% to about 55 wt%, about 40 wt% to about 55 wt%, or about 45 wt% to about 55 wt%. Suitable types of alumina include, but are not limited to, γ-Al2O3, η-Al2O3, δ-Al2O3, θ-Al2O3, κ-Al2O3, and any combination of two or more thereof.
[0028] The bottoms cracking catalyst composition may contain alumina stabilized with a dopant. In some embodiments, the alumina is doped with a dopant by impregnation into, coating onto, or precipitating with the alumina.
[0029] In some embodiments, the bottoms cracking catalyst composition with dopant-stabilized alumina includes greater than 0 wt% to about 10 wt% of a dopant when measured in oxide form. Suitable amounts of dopant include, but are not limited to, greater than 0 to about 10 wt%, 0.01 wt% to about 7 wt%, about 0.1 wt% to about 5 wt%, or about 0.5 wt% to about 4 wt%. In some embodiments, the dopant is present in an amount of about 4 wt%.
[0030] The dopant may be a rare earth or alkaline earth metal oxide. For example, the dopant measured in oxide form may include ytterbium, gadolinium, cerium, lanthanum, yttrium, barium, magnesium, or a mixture of any two or more thereof. In some embodiments, the dopant is lanthanum. Without being bound by theory, it is believed that the rare earth material changes the acid site density of the catalyst, thereby reducing the coke selectivity.
[0031] In some embodiments, the bottoms cracking catalyst composition includes about 2 wt% to about 20 wt% reactive silica. For example, suitable amounts of reactive silica include, but are not limited to, about 2 wt% to about 20 wt%, about 5 wt% to 15 wt%, or about 7 wt% to about 12 wt%. Suitable types of reactive silica include, but are not limited to, colloidal silica, precipitated SiO2, SiO2 gel, volatile high surface area silica, zeolite, or a combination of two or more thereof. Without being bound by theory, it is believed that reactive silica provides the Si required to produce Bronsted acid sites while reducing or eliminating Lewis acid sites for making coke.
[0032] The bottom residue cracking catalyst composition includes about 3wt% to about 20wt% of components including peptized gibbsite, colloidal silica, hydrated aluminum chloride or any combination of two or more thereof. In some embodiments, the component includes colloidal silica and peptized gibbsite. Suitable amounts of the component include but are not limited to about 3wt%, about 5wt%, about 7wt%, about 10wt%, about 12wt%, about 15wt%, about 18wt%, about 20wt% or a range between any of these values. In some embodiments, the component is present in an amount of about 3wt% to about 18wt%, about 5wt% to about 15wt%, about 7wt% to about 12wt%. In some embodiments, the component includes about 5wt% to about 10wt% gibbsite and about 5wt% to 15wt% colloidal silica.
[0033] The bottom residue cracking catalyst composition includes about 10 wt% to about 50 wt% kaolin. For example, suitable amounts of kaolin include, but are not limited to, about 10 wt%, about 15 wt%, about 20 wt%, about 25 wt%, about 30 wt%, about 35 wt%, about 40 wt%, about 45 wt%, about 50 wt%, or a range between any two of these values. In some embodiments, the amount of kaolin present includes about 10 wt% to about 50 wt%, about 15 wt% to about 45 wt%, or about 20 wt% to about 30 wt%. In some embodiments, kaolin includes metakaolin (calcined kaolin to perform a strong endothermic reaction associated with dehydroxylation) and kaolin calcined under more severe conditions than those used to convert kaolin to metakaolin, i.e., calcined kaolin to perform a characteristic kaolin exothermic reaction, sometimes referred to as calcined kaolin in the form of spinel.
[0034] The average particle size of the bottoms cracking catalyst composition described in any of the embodiments herein is about 70 to about 95 microns. For example, suitable particle sizes include, but are not limited to, about 70 microns, about 75 microns, about 80 microns, about 85 microns, about 90 microns, about 95 microns, and ranges between any two of these values. In some embodiments, the particle size includes about 70 to about 95 microns, about 70 to about 85 microns, or about 70 to about 80 microns.
[0035] The bottoms cracking catalyst composition described in any of the embodiments herein has a mercury pore volume of 0.3 to 0.56 cc / g with a diameter range of 4 to 2,000 nm. For example, suitable mercury pore volume amounts include 0.30 cc / g, 0.35 cc / g, 0.40 cc / g, 0.45 cc / g, 0.50 cc / g, 0.56 cc / g, or a range between any two of these values. In some embodiments, the mercury pore volume includes an amount of 0.3 to 0.56 cc / g, 0.40 to 0.56 cc / g, or 0.45 to 0.56 cc / g.
[0036] The bottoms cracking catalyst described in any of the Examples herein has a BET ("Brunauer-Emmett-Teller") surface area of about 100 to about 200 m 2 / g. For example, the BET surface area includes, but is not limited to, about 100 to about 200 m 2 / g, about 125 to about 190m 2 / g or about 150 to about 180m 2 / g.
[0037] The bottoms cracking catalyst composition described in any embodiment herein may further include a zeolite. For example, suitable zeolites include, but are not limited to, Y zeolite, ultrastable Y, dealuminated Y (DeAl Y), ultrahydrophobic Y (UHPY), dealuminated silicon-rich zeolites (e.g., LZ-210), ZSM-5, ZSM-20, zeolite L, naturally occurring zeolites (e.g., faujasite, mordenite, etc.), zeolite beta, etc., and any combination of two or more thereof. In some embodiments, the zeolite is Y zeolite, or rare earth exchanged Y zeolite.
[0038] According to any embodiment, unless zeolite is explicitly included, the bottoms cracking catalyst composition may be substantially free of or free of zeolite. As used herein, "substantially free of" zeolite means that 0 wt% to about 10 wt% zeolite is present in the bottoms cracking catalyst. In some embodiments, substantially free of zeolite includes 0 wt% to about 5 wt%, 0 wt% to about 2 wt%, 0 wt% to about 1 wt%, 0 wt% to about 0.5 wt%, 0 wt% to about 0.05 wt%, or 0 wt% to about 0.01 wt% zeolite is present in the bottoms cracking catalyst. In some embodiments, the bottoms cracking catalyst does not contain zeolite. For example, the bottoms cracking catalyst has 0 wt% zeolite.
[0039] For the binder component, colloidal silica and peptized pseudo-gibbsites may be used, such as for gibbsite, Catapal or Disperal products, or for colloidal silica, small particle size colloidal silica or polysilicic acid, the former also known as ammonium polysilicate. As is known, for these colloidal or polymeric species, small particle sizes are preferred. For SiO2, less than is preferred, and freshly prepared (poly)silicic acid is most preferred. The aforementioned binder system is advantageous because it is substantially free of sodium, among other things. Thus, in any of the above embodiments, the composition may be substantially free of or free of sodium. As used herein, substantially free of sodium will mean that the composition has less than 0.5 wt% sodium. It is well known in the art to combine FCC catalysts with aluminum stabilized colloidal silica prepared by rapidly mixing together sodium silicate and alum in sulfuric acid, but this system contains sodium and is therefore less preferred, but does contain silica, and thus can be expected to function equivalently to the most preferred composition.
[0040] More generally, because the preferred binder system does not contain sodium, ion exchange and other processes can be avoided, and the (calcined) spray dried product is the final product. This means that the inventive catalyst is a useful vehicle for incorporating other known functional groups commonly used in catalytic cracking. Thus, small amounts of rare earth or alkaline earth metal vanadium traps or refractory oxide supported precious metal CO oxidation or NOx reduction catalysts and oxygen storage compounds are already known for surface coating onto monolithic supports for emission control, or small amounts of known SO x Oxidizing or adsorbing agents may all be added to the current formulation to obtain results as desired by one skilled in the art. ZSM-5 or other zeolites may also be added as described herein.
[0041] In another aspect, a method for preparing a bottoms cracking catalyst as described in any embodiment herein is provided. The method for preparing a bottoms cracking catalyst comprises forming an aqueous slurry containing, by dry weight, about 30 wt% to about 60 wt% alumina; greater than 0 to about 10 wt% of a dopant measured in the form of an oxide; about 2 wt% to about 20 wt% reactive silica; about 3 wt% to about 20 wt% of a component comprising peptized gibbsite, colloidal silica, hydrated aluminum chlorohydrate, or a combination of any two or more thereof; and about 10 wt% to about 50 wt% kaolin, and spray drying the aqueous slurry to obtain microspheres. In some embodiments, the dopant is doped onto the alumina, while in other embodiments, the dopant is mixed with the alumina. Additionally, in some embodiments, the alumina may be calcined alumina.
[0042] The methods described herein include forming an aqueous slurry containing the following as described herein in any embodiment herein: the alumina doped with the dopant measured in oxide form, reactive silica, a component including peptized gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof, and kaolin. For example, forming the aqueous slurry may include wet milling the doped or undoped alumina to improve attrition resistance.
[0043] Other particulate ingredients, such as zeolites or additives, may also be milled. Combinations of particulate ingredients may be premixed and then milled together. In some embodiments, suitable milling particle size targets include 90% less than 3 microns. Typically, gibbsite, bayerite, and calcined alumina are easy to mill. Peptized or partially peptized gibbsite may be difficult to mill or may not require milling. In some embodiments, peptization of gibbsite or pseudogibbsite will achieve particle size targets, including but not limited to 90% less than 3 microns. In some embodiments, the individual components may be pressed and milled together or separately and easily mixed in any order at an acidic pH. In some embodiments, the method includes adding colloidal SiO2 last. For example, colloidal SiO2 may have an alkaline pH and thereby react with the peptized alumina in the slurry. In some cases, the slurry thickens and may gel when SiO2 raises the overall pH of the mixture. In some embodiments, the colloidal SiO2 is Nalco 2326SiO2 and the peptizable gibbsite is PB-950 Catapal A or Catapal B.
[0044] In some embodiments, the forming is carried out under acidic pH conditions. In some embodiments, the forming is carried out at about pH 5, about pH 4, about pH 3, about pH 2.5, about pH 2, or a range between any two of these values.
[0045] In some embodiments, forming the aqueous slurry is performed at a temperature of at least about 10° C. For example, suitable temperatures include, but are not limited to, about 10° C., 15° C., 20° C., 25° C., 30° C., 35° C., 40° C., 45° C., 50° C., 55° C., 60° C., 65° C., 70° C., 75° C., 80° C., 85° C., 90° C., 95° C., or 100° C., or a range between any two of these values.
[0046] After forming the aqueous slurry, the method includes spray drying the aqueous slurry to obtain microspheres. In some embodiments, the microspheres include a particle size, BET surface area, and / or mercury pore volume as described in any embodiment herein. For example, the microspheres include a particle size of about 70 to about 95 microns, a BET surface area of about 100 to about 200 m 2 / g, and the mercury pore volume is 0.3 to 0.56 cc / g.
[0047] The methods described herein may further include static calcination of the microspheres. In some embodiments, the calcination is carried out at a temperature of about 400°C to about 850°C. Suitable temperatures for calcining the microspheres include, but are not limited to, calcination at a temperature of about 400°C to about 850°C, about 480°C to about 740°C, about 500°C to about 650°C, or about 600°C to about 700°C. In some embodiments, calcination is carried out at a temperature of about 400°C, 500°C, 525°C, 550°C, 575°C, 600°C, 625°C, 650°C, 675°C, 700°C, 725°C, 750°C, 775°C, 800°C, 825°C, or 850°C, or at a range between any two of these values.
[0048] In some embodiments, static calcination is performed for at least about 15 minutes ("min"). For example, suitable time periods for calcination include, but are not limited to, at least about 15 min, at least about 30 min, at least about 1 hour, or at least about 2 hours. In some embodiments, calcination is performed for about 15 min to about 5 hours, about 45 min to about 3 hours, or about 1 hour to about 2 hours.
[0049] In some embodiments, calcination is carried out in a rotary calciner. The rotary calcination may include a residence time of about 1 min to about 1 hour. For example, suitable rotary calcination residence times include, but are not limited to, about 1 min to about 1 hour, about 5 min to about 30 min, about 10 min to about 20 min. The rotary calcination may be carried out at the temperature described herein for static calcination. For example, suitable rotary calcination temperatures may be 400°C to about 850°C, about 480°C to about 740°C, about 500°C to about 650°C, or about 600°C to about 700°C.
[0050] In another related aspect, a method of cracking a hydrocarbon feed is provided, comprising contacting the feed with a bottoms cracking catalyst.Any of the bottoms cracking catalysts described in any of the embodiments herein can be used to catalytically crack a hydrocarbon feed.
[0051] A method for cracking a hydrocarbon feed comprises contacting the hydrocarbon feed with a bottoms cracking catalyst, the bottoms cracking catalyst composition comprising from about 30 wt% to about 60 wt% alumina; from greater than 0 to about 10 wt% of a dopant measured as an oxide; from about 2 wt% to about 20 wt% reactive silica; from about 3 wt% to about 20 wt% of a component comprising peptized gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and from about 10 wt% to about 50 wt% kaolin.
[0052] Cracking a hydrocarbon feed according to the process described herein results in at least a 10% decrease in coke yield at 13 wt% bottoms when compared to contacting the feed with a catalyst having the same physical characteristics but not including a bottoms cracking catalyst.
[0053] The method further includes adding a zeolite cracking component to a bottoms cracking catalyst to form a blend of catalysts. For example, suitable zeolite cracking components include zeolites as described herein. In some embodiments, the zeolite cracking component is Y zeolite. The ratio of the zeolite cracking component to the bottoms cracking component can be changed according to the feed needs of various gaseous oils or residual oils. The zeolite cracking component can be any known zeolite FCC catalyst. Particularly useful combinations include bottoms cracking catalysts blended with rich zeolites, and high-activity FCC catalysts blended with steamed ZSA / MSA having a (zeolite surface area / matrix surface area) ratio greater than about 2. Blends including similar portions of these high zeolite catalysts and bottoms cracking catalysts can produce ZSA / MSA values between 0.5 and about 1. The advantage of this type of formulation is that its lower activity can significantly reduce the FCC regenerator temperature in addition to increasing bottoms cracking and light olefin production. Cooling regenerators are particularly useful in resid feed applications because this avoids metallurgical limitations on operation, as well as reducing the rate of catalyst deactivation.Examples of useful high activity catalysts include those described in U.S. Pat. Nos. 6,656,347; 6,942,784; and 6,673,235, among others.
[0054] In some embodiments, a method of cracking a hydrocarbon feed includes a zeolite-free bottoms cracking catalyst.
[0055] In another aspect, provided herein are bottoms cracking catalyst compositions, methods of preparing bottoms cracking catalyst compositions, and methods of cracking hydrocarbon feeds. The compositions may include rare earth carbonates. The rare earth carbonates may be ytterbium carbonate, gadolinium carbonate, cerium carbonate, lanthanum carbonate, yttrium carbonate, or mixtures of any two or more thereof; in such embodiments, the bottoms cracking catalyst composition may include a zeolite, while in other embodiments, the bottoms cracking catalyst may contain little or no zeolite.
[0056] In one aspect, a bottoms cracking catalyst composition is provided, comprising about 30 wt% to about 60 wt% alumina; greater than 0 to about 10 wt% of a rare earth carbonate; about 2 wt% to about 20 wt% of reactive silica; about 3 wt% to about 20 wt% of a component comprising peptized gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and about 10 wt% to about 50 wt% of kaolin. In some embodiments, the dopant is doped onto the alumina, while in other embodiments, the dopant is mixed with the alumina. Additionally, in some embodiments, the alumina may be calcined alumina.
[0057] The bottoms cracking catalyst composition includes about 30 wt% to about 60 wt% alumina. This may include, but is not limited to, about 30 wt%, about 35 wt%, about 40 wt%, about 45 wt%, about 50 wt%, about 55 wt%, about 60 wt%, or a range between any two of these values. In some embodiments, the amount of alumina includes about 30 wt% to about 60 wt%, about 35 wt% to about 55 wt%, about 40 wt% to about 55 wt%, or about 45 wt% to about 55 wt%. Suitable types of alumina include, but are not limited to, γ-Al2O3, η-Al2O3, δ-Al2O3, θ-Al2O3, κ-Al2O3, and any combination of two or more thereof.
[0058] In some embodiments, the rare earth carbonate is present in the bottom residue cracking catalyst in an amount greater than 0 wt% to about 10 wt%. Suitable amounts of the rare earth carbonate include, but are not limited to, greater than 0 to about 10 wt%, 0.01 wt% to about 7 wt%, about 0.1 wt% to about 5 wt%, or about 0.5 wt% to about 4 wt%. In some embodiments, the rare earth carbonate is present in an amount of about 4 wt%.
[0059] The rare earth carbonate may be ytterbium carbonate, gadolinium carbonate, cerium carbonate, lanthanum carbonate, yttrium carbonate, or a mixture of any two or more thereof. In some embodiments, the rare earth carbonate is lanthanum carbonate. In other embodiments, the rare earth carbonate may be cerium carbonate.
[0060] In some embodiments, the bottoms cracking catalyst composition includes about 2 wt% to about 20 wt% reactive silica. For example, suitable amounts of reactive silica include, but are not limited to, about 2 wt% to about 20 wt%, about 5 wt% to 15 wt%, or about 7 wt% to about 12 wt%. Suitable types of reactive silica include, but are not limited to, colloidal silica, precipitated SiO2, SiO2 gel, volatile high surface area silica, zeolite, or a combination of two or more thereof. Without being bound by theory, it is believed that reactive silica provides the Si required to produce Bronsted acid sites while reducing or eliminating Lewis acid sites for making coke.
[0061] The bottom residue cracking catalyst composition includes about 3wt% to about 20wt% of components including peptized gibbsite, colloidal silica, hydrated aluminum chloride or any combination of two or more thereof. In some embodiments, the components are colloidal silica and peptized gibbsite. Suitable amounts of the components include, but are not limited to, about 3wt%, about 5wt%, about 7wt%, about 10wt%, about 12wt%, about 15wt%, about 18wt%, about 20wt% or a range between any one of these values. In some embodiments, the components are present in an amount of about 3wt% to about 18wt%, about 5wt% to about 15wt%, about 7wt% to about 12wt%.
[0062] The bottom residue cracking catalyst composition includes about 10 wt% to about 50 wt% kaolin. For example, suitable amounts of kaolin include, but are not limited to, about 10 wt%, about 15 wt%, about 20 wt%, about 25 wt%, about 30 wt%, about 35 wt%, about 40 wt%, about 45 wt%, about 50 wt%, or a range between any two of these values. In some embodiments, the amount of kaolin present includes about 10 wt% to about 50 wt%, about 15 wt% to about 45 wt%, or about 20 wt% to about 30 wt%. In some embodiments, kaolin includes metakaolin (calcined kaolin to perform a strong endothermic reaction associated with dehydroxylation) and kaolin calcined under more severe conditions than those used to convert kaolin to metakaolin, i.e., calcined kaolin to perform a characteristic kaolin exothermic reaction, sometimes referred to as calcined kaolin in the form of spinel.
[0063] The average particle size of the bottoms cracking catalyst composition described in any of the embodiments herein is about 70 to about 95 microns. For example, suitable particle sizes include, but are not limited to, about 70 microns, about 75 microns, about 80 microns, about 85 microns, about 90 microns, about 95 microns, and ranges between any two of these values. In some embodiments, the particle size includes about 70 to about 95 microns, about 70 to about 85 microns, or about 70 to about 80 microns.
[0064] The mercury pore volume of the bottoms cracking catalyst composition described in any of the embodiments herein may be 0.3 to 0.56 cc / g, with a diameter range of 4 to 2,000 nm. For example, suitable mercury pore volume amounts include 0.30 cc / g, 0.35 cc / g, 0.40 cc / g, 0.45 cc / g, 0.50 cc / g, 0.56 cc / g, or a range between any two of these values. In some embodiments, the mercury pore volume includes an amount of 0.3 to 0.56 cc / g, 0.40 to 0.56 cc / g, or 0.45 to 0.56 cc / g. If the alumina component is particulate alumina, or a non-peptizable or only partially peptizable hydrated alumina, then the mercury pore size distribution will include macropores. Conversely, if the alumina is fully or mostly peptizable, then the bottoms cracking catalyst will have very few or no macropores. Surprisingly, it has been found that enhancing bottoms cracking of gaseous oil feeds does not require macroporous and predominantly or completely peptized gibbsite to be effective.
[0065] The BET surface area of the bottoms cracking catalyst described in any of the embodiments herein may be from about 100 to about 200 m 2 / g. For example, the BET surface area includes, but is not limited to, about 100 to about 200 m 2 / g, about 125 to about 190m 2 / g or about 150 to about 180m 2 / g. And, while the surface area produced is useful for defining the present invention, the surface area of steaming is more indicative of its value in a refinery. Steaming conditions used included 1450F / 24h in 100% steam, or 1600F / 4h in 100% steam, which produced similar results. It is particularly preferred that the La-stabilized alumina produce a surface area of about 100m2 / g at 50% loading after steaming at 1600F / 4h. On the other hand, it was found that partially or fully peptized gibbsite produced a steaming surface area of 120 to 140m2 / g and also had a specific cracking activity that was 10%-20% higher than that of La-doped gamma alumina. The lower activity of La-doped alumina per unit surface area is consistent with the role of La as a steric inhibitor. However, unexpectedly, the coke selectivity of gibbsite continues to be acceptable. La carbonate can be added to these latter formulations without excessive loss of specific activity, while improving the overall catalyst activity by trapping vanadium.
[0066] The bottoms cracking catalyst composition described in any embodiment herein may further include a zeolite. For example, suitable zeolites include, but are not limited to, Y zeolite, ultrastable Y, dealuminated Y (DeAl Y), ultrahydrophobic Y (UHPY), dealuminated silicon-rich zeolites (e.g., LZ-210), ZSM-5, ZSM-20, zeolite L, naturally occurring zeolites (e.g., faujasite, mordenite, etc.), zeolite beta, etc., and any combination of two or more thereof. In some embodiments, the zeolite is Y zeolite, or rare earth exchanged Y zeolite. The amount of zeolite may range from 0 to about 10 wt % of the composition.
[0067] According to any embodiment, and unless expressly indicated to include zeolite, the bottoms cracking catalyst composition may be substantially free of, or free of, zeolite, unless the composition expressly states to include zeolite. As used herein, "substantially free of" zeolite means that 0 wt% to about 10 wt% zeolite is present in the bottoms cracking catalyst. In some embodiments, substantially free of zeolite includes 0 wt% to about 5 wt%, 0 wt% to about 2 wt%, 0 wt% to about 1 wt%, 0 wt% to about 0.5 wt%, 0 wt% to about 0.05 wt%, or 0 wt% to about 0.01 wt% zeolite is present in the bottoms cracking catalyst. In some embodiments, the bottoms cracking catalyst does not contain zeolite. For example, the bottoms cracking catalyst has 0 wt% zeolite.
[0068] For the binder component, colloidal silica and peptized pseudo-gibbsites may be used, such as for gibbsite, Catapal or Disperal products, or for colloidal silica, small particle size colloidal silica or polysilicic acid, the former also known as ammonium polysilicate. As is known, for these colloidal or polymeric species, small particle sizes are preferred. For SiO2, less than is preferred, and freshly prepared (poly)silicic acid is most preferred. The aforementioned binder system is advantageous because it is substantially free of sodium, among other things. Thus, in any of the above embodiments, the composition may be substantially free of or free of sodium. As used herein, substantially free of sodium will mean that the composition has less than 0.5 wt% sodium. It is well known in the art to combine FCC catalysts with aluminum stabilized colloidal silica prepared by rapidly mixing together sodium silicate and alum in sulfuric acid, but this system contains sodium and is therefore less preferred, but does contain silica, and thus can be expected to function equivalently to the most preferred composition.
[0069] More generally, because the preferred binder system does not contain sodium, ion exchange and other processes can be avoided, and the (calcined) spray dried product is the final product. This means that the inventive catalyst is a useful vehicle for incorporating other known functional groups commonly used in catalytic cracking. Thus, small amounts of rare earth or alkaline earth metal vanadium traps or refractory oxide supported precious metal CO oxidation or NOx reduction catalysts and oxygen storage compounds are already known for surface coating onto monolithic supports for emission control, or small amounts of known SO x Oxidizing or adsorbing agents may all be added to the current formulation to obtain results as desired by one skilled in the art.
[0070] In another aspect, a method of preparing a bottoms cracking catalyst as described in any of the embodiments herein is provided. The method of preparing the bottoms cracking catalyst comprises forming an aqueous slurry containing, by dry weight: about 30 wt% to about 60 wt% alumina; greater than 0 to about 10 wt% of a rare earth carbonate; about 2 wt% to about 20 wt% reactive silica, wherein about 3 wt% to about 20 wt% of a component comprising peptized gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and about 10 wt% to about 50 wt% kaolin, and spray drying the aqueous slurry to obtain microspheres. In the method, a dopant may be doped onto the alumina.
[0071] The methods described herein include forming an aqueous slurry containing alumina, rare earth carbonates, reactive silica, a component including peptized gibbsite, aluminum chlorohydrate, or a combination of any two or more thereof, and kaolin as described in any of the examples herein. For example, forming the aqueous slurry may include wet grinding the alumina to improve attrition resistance.
[0072] Other particulate ingredients may also be milled. Combinations of particulate ingredients may be premixed and then milled together. In some embodiments, suitable milling particle size targets include 90% less than 3 microns. Typically, gibbsite, bayerite, and calcined alumina are easy to mill. Peptized or partially peptized gibbsite may be difficult to mill or may not require milling. In some embodiments, peptization of gibbsite or pseudogibbsite will achieve particle size targets, including but not limited to 90% less than 3 microns. In some embodiments, the individual components may be pressed and milled together or separately and easily mixed in any order at an acidic pH. In some embodiments, the method includes adding colloidal SiO2 last. For example, colloidal SiO2 may have an alkaline pH and thereby react with the peptized alumina in the slurry. In some cases, the slurry thickens and may gel when SiO2 raises the total pH of the mixture. In some embodiments, the colloidal SiO2 is Nalco 2326SiO2, and the peptized gibbsite is PB-950Catapal A or Catapal B.
[0073] In some embodiments, the forming is carried out under acidic pH conditions. In some embodiments, the forming is carried out at about pH 5, about pH 4, about pH 3, about pH 2.5, about pH 2, or a range between any two of these values.
[0074] In some embodiments, the aqueous slurry is formed at a temperature of at least about 10° C. For example, suitable temperatures include, but are not limited to, about 10° C., 15° C., 20° C., 25° C., 30° C., 35° C., 40° C., 45° C., 50° C., 55° C., 60° C., 65° C., 70° C., 75° C., 80° C., 85° C., 90° C., 95° C., or 100° C., or a range between any two of these values.
[0075] After forming the aqueous slurry, the method includes spray drying the aqueous slurry to obtain microspheres. In some embodiments, the microspheres include a particle size, BET surface area, and / or mercury pore volume as described in any embodiment herein. For example, the microspheres include a particle size of about 70 to about 95 microns, a BET surface area of about 100 to about 200 m 2 / g, and the mercury pore volume is 0.3 to 0.56 cc / g.
[0076] The methods described herein may further include static calcination of the microspheres. In some embodiments, the calcination is carried out at a temperature of about 400°C to about 850°C. Suitable temperatures for calcining the microspheres include, but are not limited to, calcination at a temperature of about 400°C to about 850°C, about 480°C to about 740°C, about 500°C to about 650°C, or about 600°C to about 700°C. In some embodiments, calcination is carried out at a temperature of about 400°C, 500°C, 525°C, 550°C, 575°C, 600°C, 625°C, 650°C, 675°C, 700°C, 725°C, 750°C, 775°C, 800°C, 825°C, or 850°C, or at a range between any two of these values.
[0077] In some embodiments, static calcination is performed for at least about 15 minutes ("min"). For example, suitable time periods for calcination include, but are not limited to, at least about 15 min, at least about 30 min, at least about 1 hour, or at least about 2 hours. In some embodiments, calcination is performed for about 15 min to about 5 hours, about 45 min to about 3 hours, or about 1 hour to about 2 hours.
[0078] In some embodiments, calcination is carried out in a rotary calciner. The rotary calcination may include a residence time of about 1 min to about 1 hour. For example, suitable rotary calcination residence times include, but are not limited to, about 1 min to about 1 hour, about 5 min to about 30 min, about 10 min to about 20 min. The rotary calcination may be carried out at the temperature described herein for static calcination. For example, suitable rotary calcination temperatures may be 400°C to about 850°C, about 480°C to about 740°C, about 500°C to about 650°C, or about 600°C to about 700°C.
[0079] In another related aspect, a method of cracking a hydrocarbon feed is provided, comprising contacting the feed with a bottoms cracking catalyst.Any of the bottoms cracking catalysts described in any of the embodiments herein can be used to catalytically crack a hydrocarbon feed.
[0080] A method for cracking a hydrocarbon feed includes contacting the hydrocarbon feed with a bottoms cracking catalyst, the bottoms cracking catalyst comprising from about 30 wt% to about 60 wt% alumina; from greater than 0 to about 10 wt% rare earth carbonates measured as oxides; from about 2 wt% to about 20 wt% reactive silica; from about 3 wt% to about 20 wt% of a component including peptized gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and from about 10 wt% to about 50 wt% kaolin.
[0081] Cracking a hydrocarbon feed according to the process described herein results in at least a 10% decrease in coke yield at 13 wt% bottoms when compared to contacting the feed with a catalyst having the same physical characteristics but not including a bottoms cracking catalyst.
[0082] In some embodiments, a method of cracking a hydrocarbon feed includes a zeolite-free bottoms cracking catalyst.
[0083] In another aspect, the bottoms cracking catalyst composition includes a rare earth exchanged Y zeolite. In such embodiments, the rare earth element may be ytterbium, gadolinium, cerium, lanthanum, yttrium, or a mixture of any two or more thereof. The composition may include about 10 wt% to about 20 wt% of a rare earth exchanged Y zeolite; about 10 wt% to about 30 wt% of a binder comprising silica and gibbsite; about 30 wt% to about 60 wt% of an additive comprising alumina and optionally crystalline gibbsite; and about 10 wt% to about 50 wt% of kaolin.
[0084] The bottoms cracking catalyst composition includes about 30 wt% to about 60 wt% alumina. This may include, but is not limited to, about 30 wt%, about 35 wt%, about 40 wt%, about 45 wt%, about 50 wt%, about 55 wt%, about 60 wt%, or a range between any two of these values. In some embodiments, the amount of alumina includes about 30 wt% to about 60 wt%, about 35 wt% to about 55 wt%, about 40 wt% to about 55 wt%, or about 45 wt% to about 55 wt%. Suitable types of alumina include, but are not limited to, γ-Al2O3, η-Al2O3, δ-Al2O3, θ-Al2O3, κ-Al2O3, and any combination of two or more thereof.
[0085] In some embodiments, the bottoms cracking catalyst composition includes about 2 wt% to about 20 wt% reactive silica. For example, suitable amounts of reactive silica include, but are not limited to, about 2 wt% to about 20 wt%, about 5 wt% to 15 wt%, or about 7 wt% to about 12 wt%. Suitable types of reactive silica include, but are not limited to, colloidal silica, precipitated SiO2, SiO2 gel, volatile high surface area silica, zeolite, or a combination of two or more thereof. Without being bound by theory, it is believed that reactive silica provides the Si required to produce Bronsted acid sites while reducing or eliminating Lewis acid sites for making coke.
[0086] The bottom residue cracking catalyst composition includes about 3wt% to about 20wt% of components including peptized gibbsite, colloidal silica, hydrated aluminum chloride or any combination of two or more thereof. In some embodiments, the components are colloidal silica and peptized gibbsite. Suitable amounts of the components include, but are not limited to, about 3wt%, about 5wt%, about 7wt%, about 10wt%, about 12wt%, about 15wt%, about 18wt%, about 20wt% or a range between any one of these values. In some embodiments, the components are present in an amount of about 3wt% to about 18wt%, about 5wt% to about 15wt%, about 7wt% to about 12wt%.
[0087] The bottom residue cracking catalyst composition includes about 10 wt% to about 50 wt% kaolin. For example, suitable amounts of kaolin include, but are not limited to, about 10 wt%, about 15 wt%, about 20 wt%, about 25 wt%, about 30 wt%, about 35 wt%, about 40 wt%, about 45 wt%, about 50 wt%, or a range between any two of these values. In some embodiments, the amount of kaolin present includes about 10 wt% to about 50 wt%, about 15 wt% to about 45 wt%, or about 20 wt% to about 30 wt%. In some embodiments, kaolin includes metakaolin (calcined kaolin to perform a strong endothermic reaction associated with dehydroxylation) and kaolin calcined under more severe conditions than those used to convert kaolin to metakaolin, i.e., calcined kaolin to perform a characteristic kaolin exothermic reaction, sometimes referred to as calcined kaolin in the form of spinel.
[0088] The average particle size of the bottoms cracking catalyst composition described in any of the embodiments herein is about 70 to about 95 microns. For example, suitable particle sizes include, but are not limited to, about 70 microns, about 75 microns, about 80 microns, about 85 microns, about 90 microns, about 95 microns, and ranges between any two of these values. In some embodiments, the particle size includes about 70 to about 95 microns, about 70 to about 85 microns, or about 70 to about 80 microns.
[0089] The bottoms cracking catalyst composition described in any embodiment herein may have a mercury pore volume of 0.3 to 0.56 cc / g with a diameter range of 4 to 2,000 nm. For example, suitable mercury pore volume amounts include 0.30 cc / g, 0.35 cc / g, 0.40 cc / g, 0.45 cc / g, 0.50 cc / g, 0.56 cc / g, or a range between any two of these values. In some embodiments, the mercury pore volume includes an amount of 0.3 to 0.56 cc / g, 0.40 to 0.56 cc / g, or 0.45 to 0.56 cc / g.
[0090] In the case where the bottoms cracking catalyst comprises a rare earth exchanged Y zeolite, the BET surface area of the catalyst may be from about 200 to about 350 m 2 For example, the BET surface area includes, but is not limited to, about 220 to about 320 m2 / g, about 225 to about 310 m2 / g, or about 230 to about 300 m2 / g.
[0091] For the binder component, colloidal silica and peptized pseudo-gibbsites may be used, such as for gibbsite, Catapal or Disperal products, or for colloidal silica, small particle size colloidal silica or polysilicic acid, the former also known as ammonium polysilicate. As is known, for these colloidal or polymeric species, small particle sizes are preferred. For SiO2, less than is preferred, and freshly prepared (poly)silicic acid is most preferred. The aforementioned binder system is advantageous because it is substantially free of sodium, among other things. Thus, in any of the above embodiments, the composition may be substantially free of or free of sodium. As used herein, substantially free of sodium will mean that the composition has less than 0.5 wt% sodium. It is well known in the art to combine FCC catalysts with aluminum stabilized colloidal silica prepared by rapidly mixing together sodium silicate and alum in sulfuric acid, but this system contains sodium and is therefore less preferred, but does contain silica, and thus can be expected to function equivalently to the most preferred composition.
[0092] More generally, because the preferred binder system does not contain sodium, ion exchange and other processes can be avoided, and the (calcined) spray dried product is the final product. This means that the inventive catalyst is a useful vehicle for incorporating other known functional groups commonly used in catalytic cracking. Thus, small amounts of rare earth or alkaline earth metal vanadium traps or refractory oxide supported precious metal CO oxidation or NOx reduction catalysts and oxygen storage compounds are already known for surface coating onto monolithic supports for emission control, or small amounts of known SO x Oxidizing or adsorbing agents may all be added to the current formulation to obtain results as desired by one skilled in the art.
[0093] In another aspect, a method for preparing a bottoms cracking catalyst as described in any embodiment herein is provided. The method for preparing a bottoms cracking catalyst comprises forming an aqueous slurry containing, by dry weight, about 30 wt% to about 60 wt% alumina; greater than 0 to about 10 wt% of a rare earth carbonate; about 2 wt% to about 20 wt% of reactive silica; about 3 wt% to about 20 wt% of a component comprising peptized gibbsite, colloidal silica, hydrated aluminum chlorohydrate, or a combination of any two or more thereof; and about 10 wt% to about 50 wt% of kaolin, and spray drying the aqueous slurry to obtain microspheres. In some embodiments, the dopant is doped onto the alumina, while in other embodiments, the dopant is mixed with the alumina. Additionally, in some embodiments, the alumina may be calcined alumina.
[0094] The methods described herein include forming an aqueous slurry containing alumina, rare earth carbonates, reactive silica, a component including peptized gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof, and kaolin as described herein in any embodiment. For example, forming the aqueous slurry may include wet grinding the alumina to improve attrition resistance.
[0095] Other particulate ingredients may also be milled. Combinations of particulate ingredients may be premixed and then milled together. In some embodiments, suitable milling particle size targets include 90% less than 3 microns. Typically, gibbsite, bayerite, and calcined alumina are easy to mill. Peptized or partially peptized gibbsite may be difficult to mill or may not require milling. In some embodiments, peptization of gibbsite or pseudogibbsite will achieve particle size targets, including but not limited to 90% less than 3 microns. In some embodiments, the individual components may be pressed and milled together or separately and easily mixed in any order at an acidic pH. In some embodiments, the method includes adding colloidal SiO2 last. For example, colloidal SiO2 may have an alkaline pH and thereby react with the peptized alumina in the slurry. In some cases, the slurry thickens and may gel when SiO2 raises the total pH of the mixture. In some embodiments, the colloidal SiO2 is Nalco 2326SiO2, and the peptized gibbsite is PB-950Catapal A or Catapal B.
[0096] In some embodiments, the forming is carried out under acidic pH conditions. In some embodiments, the forming is carried out at about pH 5, about pH 4, about pH 3, about pH 2.5, about pH 2, or a range between any two of these values.
[0097] In some embodiments, forming the aqueous slurry is performed at a temperature of at least about 10° C. For example, suitable temperatures include, but are not limited to, about 10° C., 15° C., 20° C., 25° C., 30° C., 35° C., 40° C., 45° C., 50° C., 55° C., 60° C., 65° C., 70° C., 75° C., 80° C., 85° C., 90° C., 95° C., or 100° C., or a range between any two of these values.
[0098] After forming the aqueous slurry, the method includes spray drying the aqueous slurry to obtain microspheres. In some embodiments, the microspheres include a particle size, BET surface area, and / or mercury pore volume as described in any embodiment herein. For example, the microspheres include a particle size of about 70 to about 95 microns, a BET surface area of about 100 to about 200 m 2 / g, and a mercury pore volume of 0.3 to 0.56 cc / g. In the case where the bottoms cracking catalyst contains a rare earth exchanged Y zeolite, the BET surface area of the catalyst may be from about 200 to about 350 m 2 For example, the BET surface area includes, but is not limited to, about 220 to about 320 m2 / g, about 225 to about 310 m2 / g, or about 230 to about 300 m2 / g.
[0099] The methods described herein may further include static calcination of the microspheres. In some embodiments, the calcination is carried out at a temperature of about 400°C to about 850°C. Suitable temperatures for calcining the microspheres include, but are not limited to, calcination at a temperature of about 400°C to about 850°C, about 480°C to about 740°C, about 500°C to about 650°C, or about 600°C to about 700°C. In some embodiments, calcination is carried out at a temperature of about 400°C, 500°C, 525°C, 550°C, 575°C, 600°C, 625°C, 650°C, 675°C, 700°C, 725°C, 750°C, 775°C, 800°C, 825°C, or 850°C, or at a range between any two of these values.
[0100] In some embodiments, static calcination is performed for at least about 15 minutes ("min"). For example, suitable time periods for calcination include, but are not limited to, at least about 15 min, at least about 30 min, at least about 1 hour, or at least about 2 hours. In some embodiments, calcination is performed for about 15 min to about 5 hours, about 45 min to about 3 hours, or about 1 hour to about 2 hours.
[0101] In some embodiments, calcination is carried out in a rotary calciner. The rotary calcination may include a residence time of about 1 min to about 1 hour. For example, suitable rotary calcination residence times include, but are not limited to, about 1 min to about 1 hour, about 5 min to about 30 min, about 10 min to about 20 min. The rotary calcination may be carried out at the temperature described herein for static calcination. For example, suitable rotary calcination temperatures may be 400°C to about 850°C, about 480°C to about 740°C, about 500°C to about 650°C, or about 600°C to about 700°C.
[0102] In another related aspect, a method of cracking a hydrocarbon feed is provided, comprising contacting the feed with a bottoms cracking catalyst.Any of the bottoms cracking catalysts described in any of the embodiments herein can be used to catalytically crack a hydrocarbon feed.
[0103] A method for cracking a hydrocarbon feed includes contacting the hydrocarbon feed with a bottoms cracking catalyst, the bottoms cracking catalyst comprising from about 30 wt% to about 60 wt% alumina; from greater than 0 to about 10 wt% rare earth carbonates measured as oxides; from about 2 wt% to about 20 wt% reactive silica; from about 3 wt% to about 20 wt% of a component including peptized gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and from about 10 wt% to about 50 wt% kaolin.
[0104] Cracking a hydrocarbon feed according to the process described herein results in at least a 10% decrease in coke yield at 13 wt% bottoms when compared to contacting the feed with a catalyst having the same physical characteristics but not including a bottoms cracking catalyst.
[0105] The present technology thus generally described will be more readily understood by reference to the following examples, which are provided by way of illustration and are not intended to be limiting of the present technology.
[0106] Examples
[0107] Example 1. Sample catalysts (AE) were prepared as alumina loaded ladders according to the following steps: a lanthanum stabilized alumina matrix was wet milled 90% < ~3 μm and then spray dried a 15 wt% VF colloidal SiO2 sol and a 6.5% VF peptized pseudogibbsite binder system, each on a volatile-free (VF) basis. The remainder of the formulation consisted of alpha alumina and kaolin as listed in Table 1. The alumina was milled without pH adjustment, but in some cases it was adjusted to 4-5 pH after milling to reduce viscosity. Peptization of pseudogibbsite was performed as directed by the manufacturer with an aging period of several hours or preferably overnight. Commercial colloidal silica was used as is and was slowly added to the combined slurry as the last component. The other ingredients were combined in the order listed in Table 1. Spray drying was conducted on a pressure atomization single fluid nozzle dryer with a slurry solids of about 20 wt%. The sample catalysts were calcined at 1300°F and steam was turned off at 1450°F for 24 hours. The formulations and properties of exemplary catalysts AE are provided in Table 1. Comparative catalyst (F) was prepared according to the procedure described above, which has typical properties of replacing inert kaolin activity regulating microspheres. Samples C, D and E produce high surface area along with acceptable bulk density and attrition resistance.
[0108] Table 1. Formulation
[0109]
[0110]
[0111] ABD is the abbreviation for apparent (or descending) bulk density, g / mL.
[0112] AJAR is an abbreviation for Air Jet Loss Rate by ASTM 5757 between 1 hour and 5 hours.
[0113] AJI is the Air Jet Index, an abbreviation for the total wt% loss between 0 hours and 5 hours.
[0114] MSA is the abbreviation for matrix surface area.
[0115] HgTPV is an abbreviation for total mercury pore volume with diameters ranging from 4 to 2,000 nm.
[0116] Example 2. Catalytic evaluation of catalyst blends. Catalytic evaluation of catalyst blends was performed to evaluate the effect of changing only the overall physical and chemical properties of the catalyst blend on catalytic performance. Table 2 shows the ACE test formulations of exemplary catalyst blends including a bottoms cracking catalyst composition (Sample D) as described in Example 1. Sample D is blended with a commercially available clay-based in-situ zeolite component of relatively high steaming ZSA / MSA (SZ / M) to match other clay-based in-situ zeolite components of lower SZ / M. In the case of the 0.25SZ / M target, no clay-based in-situ control is available, so Comparative Blend 5 also contains 44% of Sample D, while the corresponding Example Blend 6 contains 78% of Sample D. All catalysts were steamed at 1450°F for 24 hours, respectively, and then blended as described for the ACE test. Blends were prepared at constant total surface area (TSA), ABD, and three levels of SZ / M (Table 2). Only the clay-based in-situ zeolite component contained zeolite. Higher density (Clay MS, Comparative F in Table 1) and lower density inert kaolin active conditioning microspheres were used to balance the surface area and bulk density of the blend. In cases where the blend properties are so well matched, it would be unexpected to find any performance differences.
[0117] Table 2. Comparative and Example Blend Ratios and Properties
[0118]
[0119] The example and comparative catalyst blends were evaluated using an Advanced Catalyst Evaluation (ACE) fluidized bed. Figure 1 The example catalyst blends (blends 2, 4, and 6) and the comparative catalyst blends (1, 3, and 5) are shown to have about the same activity. The ACE results in Table 3 show that the example compositions have 11%-24% less coke at constant bottoms compared to the comparative examples. Specifically, the example catalyst blends with Sample D catalyst (Example 1) at 13 wt%, 17 wt%, and 20 wt% bottoms yields show a 3.5% to 5.6% reduction in coke compared to the comparative catalyst blends ( Figure 2 ) Coke selectivity is 11%, 24% and 15% lower. Figure 2 Table 3 also shows the relative coke reduction at different bottoms conversions because the activity of the catalyst changes when SZ / M changes. Steaming Unit Size (SUCS) vs. Comparative Blend 1 and Example Blends 4 and 6 And comparison blend 3 Same as, but with instance blend 2 The difference is shown. Low SUCS indicates low zeolite activity, reduces the Z / M activity ratio, and potentially increases coke selectivity. Thus, this difference in SUCS between Example Blend 2 and Comparative Blend 1 explains the small difference in benefit.
[0120] Figure 3 , Figure 4 , Figure 5 , Figure 6 , Figure 7 and Figure 8 The yields of different products LCO, H2, dry gas, liquefied petroleum gas (LPG) and gasoline are shown respectively. As can be seen in the figure, the example catalyst blends (blends 2, 4 and 6) with sample D catalyst show up to 2% higher gasoline yield and lower LPG, H2 and dry gas yield. Figure 7 It is shown that for the comparative blends (blends 1, 3 and 5) as SZ / M decreases, coke increases systematically; using the catalyst of the present technology, the coke increase is less. In other words, the exemplary catalyst blends (2, 4 and 6) increase conversion at constant coke and SZ / M due to improved coke selectivity. Figure 8 It is shown that the ratio of LCO production to bottoms conversion at a constant coke yield of 2.5 wt% increases by 2% (Z / M=1.06), 15% (Z / M=0.5) and 12% (Z / M=0.25).
[0121] Table 3. Comparisons with Example Blends.
[0122] Comparison of blends Blend 1 Blend 3 Blend 5 Example Blends Blend 2 Blend 4 Blend 6 Bottom residue Wt% 13.00 17.00 20.00 Reduce coke % -11% -24% -15%
[0123] Example 3. Bottoms Catalyst Formulation with Rare Earth Carbonate and No Zeolite The following table shows the range of materials used to form the bottoms catalyst.
[0124] Element Wide range Lanthanum carbonate (or cerium carbonate) >0-10wt% <![CDATA[SiO2 binder]]> 2wt%-20wt% Peptized gibbsite PB-950 3wt%-15wt% Alpha Alumina 0wt%-20wt% Kaolin 10wt%-50wt% characteristic BET surface area, new <![CDATA[100-200m 2 / g]]> HgTPV, 40-20,000A Diameter 0.41-0.55mL / g Average particle size 70-95 microns <![CDATA[Na2O]]> <h2 style=";text-align:left;direction:ltr"><0.2wt%<h2 style=";text-align:left;direction:ltr">
[0125] Example 4. Bottoms catalyst formulation based on rare earth exchanged Y zeolite.
[0126] Rare earth exchanged Y zeolite 15.0% N1 40.0% Nalco 2326 15.0% PB950-peptized 6.5% Crystalline gibbsite 10% Hydrated Kaolin 13.5%
[0127] Paragraph A1. A bottoms cracking catalyst composition comprising: about 30 wt% to about 60 wt% alumina; greater than 0 to about 10 wt% of a dopant measured in oxide form, the dopant comprising ytterbium, gadolinium, cerium, lanthanum, yttrium, barium, magnesium, or a mixture of any two or more thereof; about 2 wt% to about 20 wt% reactive silica; about 3 wt% to about 20 wt% of a component comprising peptized gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and about 10 wt% to about 50 wt% kaolin. In some embodiments, the dopant is doped onto the alumina, while in other embodiments, the dopant is mixed with the alumina. Additionally, in some embodiments, the alumina may be calcined alumina.
[0128] Paragraph A1. The catalyst of Paragraph A1, comprising a dopant present in an amount of about 0.1 wt% to about 5 wt% of the composition measured as the oxide.
[0129] Paragraph A3. The catalyst of any of paragraphs A1 or A2, wherein the dopant is present in an amount of about 4 wt %.
[0130] Paragraph A4. The catalyst of Paragraph A1, wherein the dopant comprises lanthanum.
[0131] Paragraph A5. The catalyst of any of Paragraphs A1 to A4, wherein the dopant is impregnated into, coated onto, or co-precipitated with the alumina.
[0132] Paragraph A6. The catalyst of any of Paragraphs A1 to A5, having an average particle size of about 70-95 microns.
[0133] Paragraph A7. The catalyst of any of Paragraphs A1 to A6, having a mercury pore volume of 0.3-0.56 cc / g and a diameter range of 4 to 2,000 nm.
[0134] Paragraph A8. The catalyst of any of Paragraphs A1 to A7, further comprising a zeolite in the composition.
[0135] Paragraph A9. The catalyst of Paragraph A8, wherein the zeolite is Y zeolite.
[0136] Paragraph A10. The catalyst of any of Paragraphs A1 to A8, which is free of zeolite.
[0137] Paragraph A10a. The catalyst of any of Paragraphs A1 to A10, wherein the alumina is calcined alumina.
[0138] Paragraph A11. A method for preparing a bottoms cracking catalyst comprising
[0139] An aqueous slurry is formed containing, by dry weight:
[0140] about 30 wt % to about 60 wt % alumina;
[0141] from greater than 0 to about 10 weight percent of a dopant, measured as an oxide, comprising ytterbium, gadolinium, cerium, lanthanum, yttrium, barium, magnesium, or a mixture of any two or more thereof;
[0142] about 2 wt % to about 20 wt % reactive silica;
[0143] about 3 wt% to about 20 wt% of a component comprising peptizable gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and
[0144] about 10 wt % to about 50 wt % kaolin, and
[0145] The aqueous slurry was spray dried to obtain microspheres.
[0146] Paragraph A 12. The method of Paragraph A11, further comprising calcined microspheres.
[0147] Paragraph A13. A method of cracking a hydrocarbon feed comprising contacting the feed with a fluid catalytic cracking (FCC) catalyst comprising a zeolite component and a bottoms cracking catalyst comprising:
[0148] about 30 wt % to about 60 wt % alumina;
[0149] for aluminum oxide, greater than 0 to about 10 weight percent of a dopant measured as an oxide, the dopant comprising ytterbium, gadolinium, cerium, lanthanum, yttrium, barium, magnesium, or a mixture of any two or more thereof;
[0150] about 2 wt % to about 20 wt % reactive silica;
[0151] about 3 wt% to about 20 wt% of a component comprising peptizable gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and
[0152] About 10 wt % to about 50 wt % kaolin.
[0153] Paragraph A14. The method of Paragraph A13, wherein the catalyst comprises a dopant in an amount of about 0.1 wt % to about 5 wt % measured as the oxide.
[0154] Paragraph A15. The method of Paragraph A13, wherein the rare earth element comprises lanthanum.
[0155] Paragraph A16. The process of any of paragraphs A13 to 1A5, wherein the process results in a decrease in coke yield measured at 13 wt% bottoms of greater than 10% when compared to contacting the feed with a catalyst having the same physical properties but not including a bottom cracking catalyst.
[0156] Paragraph A17. The method of any of paragraphs A13-1A6, wherein the zeolite comprises Y zeolite.
[0157] Paragraph A19. The process of any of paragraphs A13-A16, wherein the FCC catalyst comprises at least 15 wt% bottoms cracking catalyst.
[0158] Paragraph A20. The process of Paragraph A19, wherein the FCC catalyst comprises at least 50 wt% of a zeolite component.
[0159] Paragraph A21. The process of any of paragraphs A13-A16, wherein the FCC catalyst comprises 15 wt% to 50 wt% of the bottoms cracking catalyst, or wherein the FCC catalyst comprises 85 wt% to 50 wt% of the zeolite component.
[0160] Paragraph A22. The process of any of paragraphs A13-A16, wherein the FCC catalyst comprises 15 wt% to 80 wt% bottoms cracking catalyst and 85 wt% to 20 wt% zeolite and optionally other clay-based components.
[0161] Paragraph A23. The process of any of paragraphs A13-A22, wherein the FCC catalyst further comprises a vanadium capture agent, or a crystalline gibbsite nickel capture agent.
[0162] Paragraph A25. A bottoms cracking catalyst composition comprising:
[0163] about 30 wt % to about 60 wt % alumina;
[0164] from greater than 0 to about 10 weight percent of a rare earth carbonate, measured as an oxide, comprising ytterbium carbonate, gadolinium carbonate, cerium carbonate, lanthanum carbonate, yttrium carbonate, or a mixture of any two or more thereof;
[0165] about 2 wt % to about 20 wt % reactive silica;
[0166] about 3 wt% to about 20 wt% of a component comprising peptizable gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and
[0167] About 10 wt % to about 50 wt % kaolin.
[0168] Paragraph A26. The catalyst of paragraph 25, comprising a rare earth carbonate present in an amount from about 0.1 wt % to about 5 wt % of the composition.
[0169] Paragraph A27. The catalyst of any of paragraphs A25 or A26, wherein the rare earth carbonate is present in an amount of about 4 wt %.
[0170] Paragraph A28. The catalyst of any of paragraphs A25 to A27, wherein the rare earth element comprises lanthanum.
[0171] Paragraph A29. The catalyst of any of paragraphs A25 to A28, having an average particle size of about 70-95 microns.
[0172] Paragraph A30. The catalyst of any of paragraphs A25 to A29, having a mercury pore volume of 0.3-0.56 cc / g and a diameter range of 4 to 2,000 nm.
[0173] Paragraph A31. A bottoms cracking catalyst composition comprising:
[0174] about 10 wt % to about 20 wt % of a rare earth exchanged Y zeolite;
[0175] about 10 wt % to about 30 wt % of a binder comprising silica and gibbsite;
[0176] about 30 wt % to about 60 wt % of an additive comprising alumina and optionally crystalline gibbsite; and
[0177] About 10 wt % to about 50 wt % kaolin.
[0178] Paragraph A32. The bottoms cracking catalyst composition of paragraph A31, wherein the rare earth exchanged Y zeolite can include ytterbium, gadolinium, cerium, lanthanum, yttrium, or a mixture of any two or more thereof.
[0179] Paragraph A33. A bottoms cracking catalyst composition according to paragraph A31 or A32, wherein the rare earth exchanged Y zeolite comprises lanthanum.
[0180] Paragraph A34. A bottoms cracking catalyst composition according to paragraph A31, A32, or A33, having an average particle size of about 70-95 microns.
[0181] Paragraph A35. The bottoms cracking catalyst composition of any of paragraphs A31 to A34 may have a mercury pore volume of 0.3-0.56 cc / g and a diameter range of 4 to 2,000 nm.
[0182] Paragraph A36. A method for preparing a bottoms cracking catalyst, the method comprising:
[0183] An aqueous slurry is formed containing, by dry weight:
[0184] about 10 wt % to about 20 wt % of a rare earth exchanged Y zeolite;
[0185] about 10 wt % to about 30 wt % of a binder comprising silica and gibbsite;
[0186] about 30 wt % to about 60 wt % of an additive comprising alumina and optionally crystalline gibbsite; and
[0187] about 10 wt % to about 50 wt % kaolin; and
[0188] The aqueous slurry was spray dried to obtain microspheres.
[0189] Paragraph A37. The method of Paragraph A36, further comprising calcining the microspheres.
[0190] Paragraph A38. The method of paragraph A36 or A37, wherein the Y zeolite is exchanged with about 1 wt % to 10 wt % rare earth.
[0191] Paragraph A39. A method of cracking a hydrocarbon feed comprising contacting the feed with a bottoms cracking catalyst according to any of paragraphs A31 to A35.
[0192] While certain embodiments have been illustrated and described, it will be appreciated that changes and modifications may be made therein in accordance with the knowledge of one skilled in the art without departing from the technology in its broader aspects as defined in the following claims.
[0193] The embodiments described in the illustrative description may be suitably practiced in the absence of any element or elements, limitation or limitations, not specifically disclosed herein. Thus, for example, the terms "comprising," "including," "containing," and the like should be read broadly and not restrictively. Furthermore, the terms and expressions employed herein have been used as terms of description and not of limitation, and it is not intended that such terms and expressions be used to exclude any equivalents of the features shown and described, or portions thereof, but it should be recognized that various modifications may be made within the scope of the claimed technology. Furthermore, the phrase "consisting essentially of" will be understood to include those elements specifically recited and those additional elements that do not significantly affect the basic and novel characteristics of the claimed technology. The phrase "consisting of" does not include any unspecified elements.
[0194] According to the specific embodiments described in this application, the present disclosure is not limited. As will be apparent to those skilled in the art, many modifications and changes can be made without departing from its spirit and scope. In addition to those listed herein, according to the foregoing description, functionally equivalent methods and compositions within the scope of the present disclosure are apparent to those skilled in the art. Such modifications and changes are intended to fall within the scope of the appended claims. The present disclosure is only limited by the terms of the appended claims together with the full range of equivalents authorized by the claims. It should be understood that the present disclosure is not limited to specific methods, reagents, compound compositions or biological systems that can certainly vary. It should also be understood that the terms used herein are only for the purpose of describing specific embodiments and are not intended to be restrictive.
[0195] In addition, where features or aspects of the disclosure are described in terms of Markush groups, those skilled in the art will recognize that the disclosure is also thereby described in terms of any individual member or subgroup of members of the Markush group.
[0196] As will be understood by those skilled in the art, for any and all purposes, particularly for providing written descriptions, all ranges disclosed herein also encompass any and all possible subranges and subrange combinations thereof. Any listed range can be easily identified as fully describing and enabling the same range to be split into at least equal two, three, four, five, ten, etc. As a non-limiting example, each range discussed herein can be easily split into a lower third, a middle third, and an upper third, etc. As will be understood by those skilled in the art, all languages such as "at most", "at least", "greater than", "less than", etc. include the numerical values narrated and refer to the ranges that can be subsequently split into subranges as discussed above. Finally, as will be understood by those skilled in the art, ranges include each individual member.
[0197] All publications, patent applications, issued patents, and other documents referenced in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, issued patent, or other document was specifically and individually indicated to be incorporated by reference in its entirety. Definitions contained in the text incorporated by reference shall not be construed to the extent they conflict with a definition in this disclosure.
[0198] Other embodiments are set forth in the following claims.
Claims
1. A bottoms cracking catalyst composition comprising: 30wt% to 60wt% alumina; greater than 0 to 10 wt% of a dopant measured as an oxide, the dopant comprising ytterbium, gadolinium, cerium, lanthanum, yttrium, barium, magnesium, or a mixture of any two or more thereof; 2 wt% to 20 wt% reactive silica; 3 wt% to 20 wt% of a component comprising peptizable gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and 10 wt% to 50 wt% kaolin; The bottoms cracking catalyst composition comprises 0% to 10% by weight zeolite.
2. The bottoms cracking catalyst composition of claim 1 comprising said dopant present in an amount of from 0.1 wt% to 5 wt% of said composition measured as oxide.
3. The bottoms cracking catalyst composition of claim 1 or 2, wherein the dopant is present in an amount of about 4 wt%, wherein "about" shall mean up to plus or minus 10% of the particular term.
4. The bottoms cracking catalyst composition of claim 1, wherein the dopant comprises lanthanum.
5. The bottoms cracking catalyst composition according to any one of claims 1 to 4, wherein the dopant is impregnated into the alumina, or coated onto the alumina, or the dopant is co-precipitated with the alumina.
6. A bottoms cracking catalyst composition according to any one of claims 1 to 5, having an average particle size of 70-95 microns.
7. A bottoms cracking catalyst composition according to any one of claims 1 to 6 having a mercury pore volume of 0.3-0.56 cc / g and a diameter ranging from 4 to 2,000 nm.
8. A bottoms cracking catalyst composition according to any one of claims 1 to 7 which is free of zeolite.
9. The bottoms cracking catalyst composition according to any one of claims 1 to 8, wherein the alumina is calcined alumina.
10. The bottoms cracking catalyst composition of claim 1, wherein the bottoms cracking catalyst composition contains 0 wt% to 5 wt% zeolite.
11. The bottoms cracking catalyst composition of claim 10, wherein the bottoms cracking catalyst composition contains 0 wt% to 2 wt% zeolite.
12. The bottoms cracking catalyst composition of claim 11, wherein the bottoms cracking catalyst composition contains 0 wt% to 1 wt% zeolite.
13. The bottoms cracking catalyst composition of claim 12, wherein the bottoms cracking catalyst composition contains 0 wt% to 0.5 wt% zeolite.
14. The bottoms cracking catalyst composition of claim 13, wherein the bottoms cracking catalyst composition contains 0 wt% to 0.05 wt% zeolite.
15. The bottoms cracking catalyst composition of claim 14, wherein the bottoms cracking catalyst composition contains 0 wt% to 0.01 wt% zeolite.
16. A method of preparing a bottoms cracking catalyst composition comprising forming an aqueous slurry containing, by dry weight: 30wt% to 60wt% alumina; For the aluminum oxide, greater than 0 to 10 wt% of a dopant measured in oxide form, the dopant comprising ytterbium, gadolinium, cerium, lanthanum, yttrium, barium, or a mixture of any two or more thereof; 2 wt% to 20 wt% reactive silica; 3 wt% to 20 wt% of a component comprising peptizable gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and 10 wt% to 50 wt% kaolin, and spray drying the aqueous slurry to obtain microspheres; The bottoms cracking catalyst composition comprises 0% to 10% by weight zeolite.
17. The method of claim 16, further comprising calcining the microspheres.
18. The method of claim 16, wherein the alumina is calcined alumina.
19. The process of claim 16, wherein the bottoms cracking catalyst composition contains 0 wt% to 5 wt% zeolite.
20. The process of claim 19, wherein the bottoms cracking catalyst composition contains 0 wt% to 2 wt% zeolite.
21. The process of claim 20 wherein the bottoms cracking catalyst composition contains 0 wt% to 1 wt% zeolite.
22. The process of claim 21 wherein the bottoms cracking catalyst composition contains 0 wt% to 0.5 wt% zeolite.
23. The process of claim 22, wherein the bottoms cracking catalyst composition contains 0 wt% to 0.05 wt% zeolite.
24. The process of claim 23, wherein the bottoms cracking catalyst composition contains 0 wt% to 0.01 wt% zeolite.
25. A method of cracking a hydrocarbon feed comprising contacting the feed with a fluid catalytic cracking catalyst comprising a zeolite component and a bottoms cracking catalyst composition comprising: 30wt% to 60wt% alumina; greater than 0 to 10 wt% of a dopant measured as an oxide, the dopant comprising ytterbium, gadolinium, cerium, lanthanum, yttrium, barium, magnesium, or a mixture of any two or more thereof; 2 wt% to 20 wt% reactive silica; 3 wt% to 20 wt% of a component comprising peptizable gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and 10 wt% to 50 wt% kaolin; The bottoms cracking catalyst composition comprises 0% to 10% by weight zeolite.
26. The process of claim 25, wherein the bottoms cracking catalyst composition comprises the dopant in an amount of 0.1 wt% to 5 wt% measured as the oxide.
27. The method of claim 26, wherein the rare earth element comprises lanthanum.
28. The process of any one of claims 25 to 27, wherein the process results in a decrease in coke yield measured at 13 wt% bottoms of greater than 10% when compared to contacting the feed with a catalyst having the same physical characteristics but not including the bottoms cracking catalyst composition.
29. The method of any one of claims 25 to 28, wherein the zeolite comprises Y zeolite.
30. The process of any one of claims 25 to 29, wherein the fluid catalytic cracking catalyst comprises at least 15 wt% of the bottoms cracking catalyst composition.
31. The process of claim 30, wherein the fluid catalytic cracking catalyst comprises at least 50 wt% of the zeolite component.
32. The process of any one of claims 25 to 28, wherein the fluid catalytic cracking catalyst comprises from 15 wt% to 80 wt% of the bottoms cracking catalyst composition.
33. The process of claim 32, wherein the fluid catalytic cracking catalyst comprises from 50 wt% to 80 wt% of the bottoms cracking catalyst composition.
34. The process according to any one of claims 25 to 28, wherein the fluid catalytic cracking catalyst comprises 15 wt% to 50 wt% of the bottoms cracking catalyst composition and 85 wt% to 50 wt% of the zeolite component and optionally other clay-based components.
35. A process according to any one of claims 25 to 34, wherein the fluid catalytic cracking catalyst additionally comprises a vanadium catch agent, or a crystalline gibbsite nickel catch agent.
36. The method of any one of claims 25 to 35, wherein the alumina is calcined alumina.
37. The process of claim 25 wherein the bottoms cracking catalyst composition comprises from 0 wt% to 5 wt% zeolite.
38. The process of claim 37 wherein the bottoms cracking catalyst composition comprises from 0 wt% to 2 wt% zeolite.
39. The process of claim 38, wherein the bottoms cracking catalyst composition contains 0 wt% to 1 wt% zeolite.
40. The process of claim 39 wherein the bottoms cracking catalyst composition comprises from 0 wt% to 0.5 wt% zeolite.
41. The process of claim 40 wherein the bottoms cracking catalyst composition comprises from 0 wt% to 0.05 wt% zeolite.
42. The process of claim 41 wherein the bottoms cracking catalyst composition comprises 0 wt% to 0.01 wt% zeolite.
43. A bottoms cracking catalyst composition comprising: 30wt% to 60wt% alumina; greater than 0 to 10 wt% of a rare earth carbonate comprising ytterbium carbonate, gadolinium carbonate, cerium carbonate, lanthanum carbonate, yttrium carbonate, or a mixture of any two or more thereof; 2 wt% to 20 wt% reactive silica; 3 wt% to 20 wt% of a component comprising peptizable gibbsite, colloidal silica, aluminum chlorohydrate, or a combination of any two or more thereof; and 10 wt% to 50 wt% kaolin; The bottoms cracking catalyst composition comprises 0% to 10% by weight zeolite.
44. A bottoms cracking catalyst composition according to claim 43 comprising said rare earth carbonate present in an amount of from 0.1 wt% to 5 wt% of said composition measured as the oxide.
45. The bottoms cracking catalyst composition of claim 43 or 44, wherein the rare earth element comprises lanthanum.
46. A bottoms cracking catalyst composition according to any one of claims 43 to 45 having an average particle size of 70 to 95 microns.
47. A bottoms cracking catalyst composition according to any one of claims 43 to 46 having a mercury pore volume of 0.3-0.56 cc / g and a diameter range of 4 to 2,000 nm.
48. The bottoms cracking catalyst composition of any one of claims 43 to 47, wherein the alumina is calcined alumina.
49. The bottoms cracking catalyst composition of claim 43, wherein the bottoms cracking catalyst composition comprises 0 wt% to 5 wt% zeolite.
50. The bottoms cracking catalyst composition of claim 49, wherein the bottoms cracking catalyst composition comprises 0 wt% to 2 wt% zeolite.
51. The bottoms cracking catalyst composition of claim 50, wherein the bottoms cracking catalyst composition comprises 0 wt% to 1 wt% zeolite.
52. The bottoms cracking catalyst composition of claim 51, wherein the bottoms cracking catalyst composition comprises 0 wt% to 0.5 wt% zeolite.
53. The bottoms cracking catalyst composition of claim 52, wherein the bottoms cracking catalyst composition comprises 0 wt% to 0.05 wt% zeolite.
54. The bottoms cracking catalyst composition of claim 53, wherein the bottoms cracking catalyst composition comprises 0 wt% to 0.01 wt% zeolite.
Citation Information
Patent Citations
Structurally enhanced cracking catalysts
US6656347B2
Fluidizing cracking catalyst and method for reducing NOx emissions during fluid catalytic cracking
CN101503632A
Process for making improved zeolite catalysts from peptized aluminas
CN102791374A
Metal passivator additive and process for preparing
CN103037966A
Stabilized dual zeolite single particle catalyst composition and a process thereof
US20030166453A1