Active energy ray-curable composition, cured product thereof, and article having cured coating film thereof
Through the specific formulation of active energy ray curable composition and protective film of the adhesive layer, the problem of deficit resistance, abrasion resistance and smoothness of the cured coating film is solved, and excellent antifouling and rub resistance is achieved. Injury, suitable for surfaces of various items.
Patent Information
- Application Number
- CN202010502833.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2012-11-02
- Filing Date
- 2013-10-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2033-10-30
AI Technical Summary
Although the cured coating film of the conventional active energy ray curable composition has excellent antifouling properties, it lacks abrasion resistance and smoothness, and it is difficult to meet the requirements of antifouling properties, abrasion resistance and smoothness at the same time.
By using specific composition formulations, including carbamate (meth)acrylate, polyfunctional (meth)acrylate and fluorine compounds with specific structures, by using aliphatic polyisocyanate and (meth)acrylic acid with hydroxyl groups The composition formed by the ester reaction forms a hard coating layer and a protective film of an adhesive layer is provided thereon, and cures with ultraviolet rays or ionizing radiation.
It realizes excellent anti-fouling, scratch resistance and smoothness of the cured coating film. It is suitable for the surface of various items as a hard coating agent, improving the anti-fouling and durability of the items.
Smart Images

Figure QLYQS_1 
Figure BDA0002524192660000061 
Figure BDA0002524192660000062
Abstract
Description
[0001] The present application is a divisional application of an application with a filing date of October 30, 2013, application number 201310524657.3, and invention name “Active energy ray-curable composition, cured product thereof, and article having cured coating film thereof”. Technical Field
[0002] The present invention relates to an active energy ray-curable composition capable of imparting excellent scratch resistance, antifouling property and smoothness to the surface of various articles, a cured product thereof and an article having a cured coating film thereof. Background Art
[0003] As for the active energy ray curable composition, since it has the characteristics of less thermal history to the coated substrate and excellent coating hardness and scratch resistance, it is used as a hard coating agent for imparting scratch resistance to the surface of plastic molded products that have the disadvantages of being soft and easily damaged. It should be noted that in order to impart antifouling properties to the cured coating film of the active energy ray curable composition, a fluorine compound having a perfluoropolyether group and a polymerizable group is proposed as a material added to the active energy ray curable composition (for example, refer to Patent Document 1.).
[0004] However, the cured coating film of the active energy ray-curable composition to which the fluorine compound described in Patent Document 1 is added has excellent antifouling properties, but has problems such as deterioration of scratch resistance and smoothness. Therefore, an active energy ray-curable composition is sought that can obtain a cured coating film having excellent antifouling properties, scratch resistance, and smoothness.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent No. 3963169 Summary of the invention
[0008] Problems to be solved by the invention
[0009] The problem to be solved by the present invention is to provide an active energy ray-curable composition capable of obtaining a cured coating film having excellent antifouling properties, scratch resistance and smoothness, a cured product thereof, and an article having the cured coating film thereof.
[0010] Methods used to solve problems
[0011] The present inventors have repeatedly conducted in-depth studies to solve the above-mentioned problems and have found that a cured coating film of an active energy ray-curable composition as described below has excellent antifouling properties, as well as excellent scratch resistance and smoothness, thereby completing the present invention. The active energy ray-curable composition contains specific tetrafunctional or higher-functional urethane (meth)acrylates, trifunctional or higher-functional (meth)acrylates, and fluorine compounds having a specific structure.
[0012] That is, the present invention relates to an active energy ray-curable composition, a cured product thereof, and an article having a cured coating film thereof, wherein the active energy ray-curable composition is characterized in that it contains a urethane (meth)acrylate (A), a multifunctional (meth)acrylate (B), and a fluorine compound (C), wherein the urethane (meth)acrylate (A) is a urethane (meth)acrylate having 4 or more (meth)acryloyl groups in one molecule obtained by reacting an aliphatic polyisocyanate (a1) with a (meth)acrylate (a2) having a hydroxyl group, the multifunctional (meth)acrylate (B) is a (meth)acrylate having 3 or more (meth)acryloyl groups in one molecule, and the fluorine compound (C) has a structure in which a polycyclosiloxane structure is bonded to both ends of a poly(perfluoroalkylene ether) chain via a divalent linking group, and a (meth)acryloyl group is bonded to the polycyclosiloxane structure via a divalent linking group. Furthermore, the present invention relates to a hard coating film in which a cured product of the active energy ray-curable composition is formed as a hard coating layer, and a protective film in which a pressure-sensitive adhesive layer is provided on the hard coating film.
[0013] Effects of the Invention
[0014] The active energy ray-curable composition of the present invention is extremely useful as a hard coating agent for protecting the surfaces of various articles because the cured coating film thereof has excellent antifouling properties and also excellent scratch resistance and smoothness. DETAILED DESCRIPTION
[0015] The active energy ray-curable composition of the present invention comprises a urethane (meth)acrylate (A) having 4 or more (meth)acryloyl groups in one molecule obtained by reacting an aliphatic polyisocyanate (a1) with a (meth)acrylate (a2) having a hydroxyl group, a multifunctional (meth)acrylate (B) having 3 or more (meth)acryloyl groups in one molecule, and a fluorine compound (C), wherein the urethane (meth)acrylate (A) is a urethane (meth)acrylate having 4 or more (meth)acryloyl groups in one molecule obtained by reacting an aliphatic polyisocyanate (a1) with a (meth)acrylate (a2) having a hydroxyl group, the multifunctional (meth)acrylate (B) is a multifunctional (meth)acrylate having 3 or more (meth)acryloyl groups in one molecule, and the fluorine compound (C) has a structure in which a polycyclosiloxane structure is bonded to both ends of a poly(perfluoroalkylene ether) chain via a divalent linking group, and a (meth)acryloyl group is bonded to the polycyclosiloxane structure via a divalent linking group.
[0016] In addition, in the present invention, "(meth)acrylate" means one or both of acrylate and methacrylate, and "(meth)acryloyl" means one or both of acryloyl and methacryloyl.
[0017] The urethane (meth)acrylate (A) is a urethane (meth)acrylate having four or more (meth)acryloyl groups in one molecule, obtained by reacting an aliphatic polyisocyanate (a1) with a (meth)acrylate (a2) having a hydroxyl group.
[0018] The aforementioned aliphatic polyisocyanate (a1) is a compound in which the parts other than the isocyanate group are composed of aliphatic hydrocarbons. Specific examples of the aliphatic polyisocyanate (a1) include aliphatic polyisocyanates (a1-1) such as hexamethylene diisocyanate, lysine diisocyanate, and lysine triisocyanate; and alicyclic polyisocyanates (a1-2) such as norbornane diisocyanate, isophorone diisocyanate, methylene bis (4-cyclohexyl isocyanate), 1,3-bis (isocyanatomethyl) cyclohexane, 2-methyl-1,3-diisocyanatocyclohexane, and 2-methyl-1,5-diisocyanatocyclohexane. It should be noted that a trimer obtained by trimerizing the aforementioned aliphatic polyisocyanate (a1-1) or alicyclic polyisocyanate (a1-2) can also be used as the aforementioned aliphatic polyisocyanate (a1). Among these aliphatic polyisocyanates (a1), hexamethylene diisocyanate as a diisocyanate of a straight-chain aliphatic hydrocarbon, norbornane diisocyanate and isophorone diisocyanate as an alicyclic diisocyanate are preferred because they can improve scratch resistance.
[0019] The aforementioned (meth)acrylate (a2) is a compound having a hydroxyl group and a (meth)acryloyl group. In order to make the aforementioned urethane (meth)acrylate (A) into a urethane (meth)acrylate having 4 or more (meth)acryloyl groups in one molecule, a compound having 2 or more (meth)acryloyl groups is preferred. As such (meth)acrylate (a2), for example, trimethylolpropane di(meth)acrylate, ethylene oxide-modified trimethylolpropane di(meth)acrylate, propylene oxide-modified trimethylolpropane di(meth)acrylate, glycerol di(meth)acrylate, bis(2-(meth)acryloyloxyethyl)hydroxyethyl isocyanurate, pentaerythritol tri(meth)acrylate, di(trimethylolpropane) tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, etc. can be cited. These (meth)acrylates (a2) can be used one by one relative to one of the aforementioned aliphatic polyisocyanates (a1), or two or more can be used in combination. Moreover, among these (meth)acrylates (a2), pentaerythritol tri(meth)acrylate and dipentaerythritol penta(meth)acrylate are preferred because they can improve the scratch resistance.
[0020] The reaction of the aforementioned aliphatic polyisocyanate (a1) and the aforementioned (meth)acrylate (a2) can be carried out by a conventional method of urethanization reaction. It should be noted that, in order to promote the progress of the urethanization reaction, it is preferred to carry out the urethanization reaction in the presence of a urethanization catalyst. As the aforementioned urethanization catalyst, for example, amine compounds such as pyridine, pyrrole, triethylamine, diethylamine, and dibutylamine; phosphorus compounds such as triphenylphosphine and triethylphosphine; organic tin compounds such as dibutyltin dilaurate, octyltin trilaurate, octyltin diacetate, dibutyltin diacetate, and octyltin, organic zinc compounds such as zinc octylate, etc.
[0021] The urethane (meth) acrylate (A) obtained in the urethanization reaction may be used alone or in combination of two or more. When two or more are used, it is preferred to use a urethane acrylate obtained by using norbornane diisocyanate as the aliphatic polyisocyanate (a1) and a urethane acrylate obtained by using isophorone diisocyanate as the aliphatic polyisocyanate (a1) in combination, because the scratch resistance can be improved.
[0022] The multifunctional (meth)acrylate (B) is a compound having three or more (meth)acryloyl groups in one molecule. Specific examples of the multifunctional (meth)acrylate (B) include trimethylolpropane tri(meth)acrylate, ethylene oxide-modified trimethylolpropane tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, di(trimethylolpropane) tri(meth)acrylate, di(trimethylolpropane) tetra(meth)acrylate, tri(2-(meth)acryloyloxyethyl)isocyanurate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, etc. These multifunctional (meth)acrylates (B) may be used alone or in combination of two or more. In addition, among these multifunctional (meth)acrylates (B), from the viewpoint of improving the scratch resistance of the cured coating film of the active energy ray-curable composition of the present invention, the (meth)acryloyl equivalent is preferably in the range of 50 to 200 g / eq., more preferably in the range of 70 to 150 g / eq., and still more preferably in the range of 80 to 120 g / eq. Specific examples of the multifunctional (meth)acrylate (B) having a (meth)acryloyl equivalent in the range of 80 to 200 g / eq. include pentaerythritol tetraacrylate (acryloyl equivalent: 88 g / eq.), dipentaerythritol hexa(meth)acrylate (acryloyl equivalent: 118 g / eq.), and the like.
[0023] The mass ratio [(A) / (B)] of the urethane (meth)acrylate (A) to the polyfunctional (meth)acrylate (B) is preferably in the range of 90 / 10 to 10 / 90, more preferably in the range of 80 / 20 to 20 / 80, and even more preferably in the range of 75 / 25 to 25 / 75, from the viewpoint of improving scratch resistance.
[0024] In addition, in addition to the aforementioned urethane (meth) acrylate (A) and the aforementioned multifunctional (meth) acrylate (B), the active energy ray-curable composition of the present invention may also contain other (meth) acrylates such as a mono (meth) acrylate having one (meth) acryloyl group in one molecule and a di (meth) acrylate having two (meth) acryloyl groups in one molecule, within a range that does not impair the effects of the present invention. When other (meth) acrylates are contained in the active energy ray-curable composition of the present invention, the amount thereof contained is preferably 40 parts by mass or less, and more preferably 20 parts by mass or less, relative to a total of 100 parts by mass of the aforementioned urethane (meth) acrylate (A) and the aforementioned multifunctional (meth) acrylate (B).
[0025] The fluorine compound (C) is a compound having a structure in which a polycyclosiloxane structure is bonded to both ends of a poly(perfluoroalkylene ether) chain via a bivalent linking group, and a (meth)acryloyl group is bonded to the polycyclosiloxane structure via a bivalent linking group. It should be noted that in the present invention, "poly(perfluoroalkylene ether)" is sometimes referred to as "perfluoropolyether".
[0026] Examples of the poly(perfluoroalkylene ether) chain possessed by the fluorine compound (C) include chains having a structure in which divalent fluorinated carbon groups having 1 to 3 carbon atoms and oxygen atoms are alternately linked. The divalent fluorinated carbon groups having 1 to 3 carbon atoms may be one or a combination of two or more, and specifically, a chain represented by the following structural formula (1) may be mentioned.
[0027]
[0028] (In the above general formula (1), X is the following formula (1-1) to (1-5), and X may be any one of the following formulas (1-1) to (1-5). In addition, two or more of the following formulas (1-1) to (1-5) may exist randomly or in blocks. In addition, n is an integer of 2 to 200 representing a repeating unit.)
[0029] -CF2- (1-1)
[0030] -CF2CF2- (1-2)
[0031] -CF2CF2CF2- (1-3)
[0032]
[0033] Among the aforementioned poly(perfluoroalkylene ether) chains, from the perspective of improving the antifouling properties of the cured coating film of the active energy ray-curable composition of the present invention, a poly(perfluoroalkylene ether) chain of a combination of a perfluoromethylene group represented by the aforementioned formula (1-1) and a perfluoroethylene group represented by the aforementioned formula (1-2) is preferred. Here, the molar ratio [(1-1) / (1-2)] of the perfluoromethylene group represented by the aforementioned formula (1-1) to the perfluoroethylene group represented by the aforementioned formula (1-2) is preferably in the range of 1 / 10 to 10 / 1. It should be noted that the value of n in the aforementioned general formula (1) is preferably in the range of 2 to 200, more preferably in the range of 10 to 100, and even more preferably in the range of 20 to 80.
[0034] Examples of the polycyclosiloxane structure of the fluorine compound (C) include a structure represented by the following general formula (2).
[0035]
[0036] (In the above general formula (2), R 1 Methyl, R 3 is a divalent organic group bonded to the poly(perfluoroalkylene ether) chain, R 4 is a monovalent organic group having a (meth)acryloyl group. In addition, m is an integer of 2 to 5.)
[0037] Among the aforementioned polycyclosiloxane structures, a cyclotetrasiloxane structure in which m in the aforementioned general formula (2) is 3 is preferred.
[0038] The divalent linking group that bonds the poly(perfluoroalkylene ether) chain to the polycyclosiloxane structure is not particularly limited as long as it is a divalent organic group, and examples thereof include a group represented by the following general formula (3).
[0039] -CH2-OY- (3)
[0040] (In the above general formula (3), Y is an alkylene group having 1 to 6 carbon atoms.)
[0041] The divalent linking group that bonds the polycyclosiloxane structure to the (meth)acryloyl group is not particularly limited as long as it is a divalent organic group, and examples thereof include a group represented by the following general formula (4).
[0042]
[0043] (In the above general formula (4), Z 1 , Z 2 and Z 3 Each is independently an alkylene group having 1 to 6 carbon atoms.)
[0044] Examples of the method for producing the fluorine compound (C) include a method of producing the fluorine compound (C) through the following steps (1) to (3).
[0045] (1) A step of reacting a compound having allyl groups at both ends of a poly(perfluoroalkylene ether) chain with a polycyclosiloxane compound having a hydrosilylation group in the presence of a platinum-based catalyst to obtain a compound having a polycyclosiloxane structure at both ends of the poly(perfluoroalkylene ether) chain.
[0046] (2) A step of reacting the compound obtained in (1) with allyloxyalkanol in the presence of a platinum-based catalyst to add a hydroxyl group to the polycyclosiloxane structure of the compound obtained in (1).
[0047] (3) A step of reacting the hydroxyl group added in (2) with a (meth)acrylate having an isocyanate group to introduce a (meth)acryloyl group.
[0048] The amount of the fluorine compound (C) in the active energy ray-curable composition of the present invention is preferably in the range of 0.05 to 5 parts by mass, more preferably in the range of 0.1 to 2 parts by mass, relative to 100 parts by mass of the total of the urethane (meth)acrylate (A), the multifunctional (meth)acrylate (B) and other (meth)acrylates optionally blended, from the perspective of being able to exhibit sufficient scratch resistance, antifouling properties and lubricity.
[0049] In addition, with respect to the active energy ray curable composition of the present invention, after being applied to a substrate, active energy rays can be irradiated to form a cured coating film. The active energy ray refers to ionizing radiations such as ultraviolet rays, electron beams, α rays, β rays, and γ rays. In the case of irradiating ultraviolet rays as active energy rays to form a cured coating film, it is preferred to add a photopolymerization initiator (D) to the active energy ray curable composition of the present invention to improve curability. In addition, a photosensitizer can be further added as needed to improve curability. On the other hand, in the case of using ionizing radiations such as electron beams, α rays, β rays, and γ rays, even without using a photopolymerization initiator (D) or a photosensitizer, rapid curing is also possible, so there is no need to particularly add a photopolymerization initiator (D) or a photosensitizer.
[0050] Examples of the photopolymerization initiator (D) include intramolecular cleavage photopolymerization initiators and dehydrogenation photopolymerization initiators. Examples of the intramolecular cleavage photopolymerization initiator include diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, oligo[2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone], benzyl dimethyl ketal, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropane-1-one, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, and 1-hydroxycyclohexylphenylketone. , 2-methyl-2-morpholino (4-thiomethylphenyl) propane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone and other acetophenone compounds; benzoin, benzoin methyl ether, benzoin isopropyl ether and other benzoin; acyl phosphine oxide compounds such as 2,4,6-trimethylbenzoin diphenylphosphine oxide and bis (2,4,6-trimethylbenzoyl)-phenylphosphine oxide; benzyl, methyl phenylglyoxylate and the like.
[0051] On the other hand, examples of dehydrogenation type photopolymerization initiators include benzophenone, methyl-4-phenylbenzophenone o-benzoylbenzoate, 4,4'-dichlorobenzophenone, hydroxybenzophenone, 4-benzoyl-4'-methyl-diphenyl sulfide, acryloyl benzophenone, 3,3',4,4'-tetrakis(tert-butylcarbonylperoxide)benzophenone, 3,3'-dimethyl-4-methoxybenzophenone, 2,4,6-trimethylbenzophenone, 4-methylbenzophenone and the like; 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2,4-di Thioxanthone compounds such as chlorothioxanthone; aminobenzophenone compounds such as Michler's ketone and 4,4'-diethylaminobenzophenone; 10-butyl-2-chloroacridone, 2-ethylanthraquinone, 9,10-phenanthrenequinone, camphorquinone, 1-[4-(4-benzoylphenylsulfanyl)phenyl]-2-methyl-2-(4-methylphenylsulfonyl)propan-1-one, etc. These photopolymerization initiators (D) may be used alone or in combination of two or more.
[0052] Examples of the photosensitizer include tertiary amine compounds such as diethanolamine, N-methyldiethanolamine, and tributylamine; urea compounds such as o-tolylthiourea; and sulfur compounds such as sodium diethyldithiophosphate and s-benzylisothiourea-p-toluenesulfonate.
[0053] The amount of the photopolymerization initiator and the photosensitizer used is preferably 0.05 to 20 parts by mass, more preferably 0.5 to 10% by mass, respectively, based on 100 parts by mass of the nonvolatile components in the active energy ray-curable composition of the present invention.
[0054] In addition, in addition to the above-mentioned components (A) to (D), the active energy ray-curable composition of the present invention may also contain, as required, additives such as polymerization inhibitors, surface conditioning agents, antistatic agents, defoaming agents, viscosity modifiers, light stabilizers, weathering stabilizers, heat stabilizers, ultraviolet absorbers, antioxidants, leveling agents, organic pigments, inorganic pigments, pigment dispersants, silica beads, organic beads, and inorganic fillers such as silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, and antimony pentoxide. These other compounds may be used alone or in combination of two or more.
[0055] The method for applying the active energy ray-curable composition of the present invention to a substrate varies depending on the application, and examples thereof include die coating, microgravure coating, gravure coating, roller coating, comma coating, air knife coating, kiss coating, spray coating, dip coating, spin coating, Wheeler coating, brush coating, full coating (full surface coating) using screen printing, wire bar coating, flow coating, and the like.
[0056] As the active energy ray that cures the active energy ray curable composition of the present invention, as described above, it is an ionizing radiation such as ultraviolet rays, electron beams, α rays, β rays, and γ rays. As a specific device for irradiating active energy rays, when ultraviolet rays are used, as the source of ultraviolet rays, low-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, electrodeless lamps (fusion lamps), chemical lamps, black light lamps, mercury-xenon lamps, short arc lamps, helium-cadmium lasers, argon lasers, sunlight, LEDs, etc. can be listed. In addition, when the substrate to which the active energy ray curable composition of the present invention is applied is a film substrate, if a xenon-flash lamp that is irradiated with flashing light is used, the effect of heat on the film substrate can be reduced, so it is preferred. On the other hand, when an electron beam is used, as the source of the electron beam, a scanning electron beam accelerator, a curtain electron beam accelerator, etc. can be listed.
[0057] When the active energy ray-curable composition of the present invention is irradiated with ultraviolet rays to form a cured coating film, the process can be carried out in an air atmosphere, but is preferably carried out in an atmosphere with an oxygen concentration of 5,000 ppm or less in order to obtain a cured coating film having better scratch resistance and smoothness.
[0058] The cured coating film of the active energy ray-curable composition of the present invention has excellent antifouling properties, and also excellent scratch resistance and smoothness. Therefore, by applying the active energy ray-curable composition of the present invention to the surface of various articles and curing it, it is possible to impart excellent antifouling properties, scratch resistance, and smoothness to the surface of various articles. Therefore, the active energy ray-curable composition of the present invention can be used as a hard coating agent having antifouling properties.
[0059] Articles to which the active energy ray-curable composition of the present invention can be applied include housings of household appliances such as televisions, refrigerators, washing machines, and air conditioners; housings of electronic devices such as personal computers, smart phones, mobile phones, digital cameras, and game consoles; interior materials of various vehicles such as automobiles and railway vehicles; various building materials such as decorative panels; woodworking materials such as furniture, artificial and synthetic leather; FRP baths; optical films of liquid crystal displays (LCDs) such as triacetylcellulose (TAC) films; prism sheets or diffusers as backlight components of LCDs; and various display screens (hard coatings, anti-corrosion coatings, etc.) such as plasma displays (PDPs) and organic EL displays. reflective layer); touch panels; screens of electronic terminals such as mobile phones and smart phones; transparent protective films for color filters (hereinafter referred to as "CF") for liquid crystal displays; optical recording media such as CDs, DVDs, and Blu-ray discs; transfer films for injection molding (IMD, IMF); rubber rollers for OA machines such as copiers and printers; glass surfaces of reading parts of OA machines such as copiers and scanners; optical lenses of cameras, video recorders, glasses, etc.; windshields and glass surfaces of clocks such as watches; windows of various vehicles such as cars and railway vehicles; protective glass or films for solar cells; various building materials such as decorative panels; window glass of houses; woodworking materials for furniture, etc.
[0060] The hard coating film of the present invention is a hard coating layer having the active energy ray curable composition of the present invention cured on at least one side of the film substrate. The aforementioned film substrate can use various commonly used resin film substrates, such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyethylene, polypropylene, cellophane, diacetyl cellulose, triacetyl cellulose, acetyl cellulose butyrate, cellulose acetate propionate, cycloolefin polymer, cycloolefin copolymer, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polystyrene, polycarbonate, polymethylpentene, polysulfone, polyetheretherketone, polyethersulfone, polyetherimide, polyimide, fluororesin, nylon, acrylic resin, etc. In particular, the resin films of polyethylene terephthalate, triacetyl cellulose, and acrylic resin are excellent in transparency and processability, so they can be preferably used.
[0061] In addition, the aforementioned film substrate can be a substrate consisting only of the above-mentioned resin film, and for the purpose of improving the adhesion with the active energy ray curable composition of the present invention, it can also be a film substrate provided with a primer on the aforementioned resin film. As the aforementioned primer, for example, a layer comprising a polyester resin, a polyurethane resin, an acrylic resin, etc. can be listed. In addition, for the purpose of improving the adhesion with the hard coat, the surface of the resin film can also be treated by using a sandblasting method, a solvent treatment method, etc., a surface concavoconvex treatment, a corona discharge treatment, a chromic acid treatment, a flame treatment, a hot air treatment, an ozone ultraviolet irradiation treatment, an oxidation treatment, etc.
[0062] The thickness of the film substrate is preferably in the range of 50 to 200 μm, more preferably in the range of 80 to 150 μm, and further preferably in the range of 90 to 130 μm. In the present invention, by setting the thickness of the film substrate in this range, curling can be easily suppressed even when a hard coating layer is provided on one side of the film substrate.
[0063] Furthermore, as the aforementioned film substrate, it is preferred to use a film substrate having an elastic modulus in the range of 3 to 7 GPa, and it is particularly preferred to use a film substrate in the range of 3 to 5 GPa. If the elastic modulus is within this range, deformation of the film substrate is not likely to occur when forming a protective film, cracks in the hard coating layer can be suppressed, and the hardness reduction of the hard coating surface can be easily suppressed. In addition, since the flexibility of the film substrate can be ensured, it is easy to follow a gentle curved surface when attaching the protective film described later.
[0064] The protective film of the present invention is a film having an adhesive layer on one side of the hard coating film. The adhesive layer can be provided by laminating the film substrate with an adhesive tape or by directly coating the adhesive layer on the side opposite to the hard coating surface of the film substrate.
[0065] The thickness of the adhesive layer of the protective film of the present invention is preferably in the range of 5 to 50 μm, more preferably in the range of 8 to 30 μm, and further preferably in the range of 10 to 25 μm. In the present invention, by setting the thickness of the adhesive layer to this range, excellent adhesion reliability is achieved, and the thickness can be maintained without significantly impairing the surface hardness of the hard coating film.
[0066] The adhesive used for the adhesive layer used in the present invention can be a known acrylic, rubber, silicone, etc. adhesive resin. Among them, from the viewpoint of adhesion to the film substrate, transparency, and weather resistance, an acrylic copolymer prepared by polymerizing a (meth)acrylate monomer having an alkyl group with 2 to 14 carbon atoms as a repeating unit as a main component is preferred.
[0067] Examples of the (meth)acrylic acid ester monomer having 2 to 14 carbon atoms include ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-hexyl acrylate, cyclohexyl acrylate, n-octyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, isononyl acrylate, isodecyl acrylate, lauryl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, n-octyl methacrylate, isooctyl methacrylate, 2-ethylhexyl methacrylate, isononyl methacrylate, isodecyl methacrylate, lauryl methacrylate, and the like.
[0068] Among the above-mentioned (meth)acrylate monomers, (meth)acrylic acid alkyl esters having an alkyl group with 4 to 9 carbon atoms are preferred, and alkyl acrylates further having an alkyl group with 4 to 9 carbon atoms are more preferred. Among the alkyl acrylates, n-butyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, isononyl acrylate, and ethyl acrylate are particularly preferred. By using (meth)acrylic acid alkyl esters having an alkyl group with a carbon number within this range, it is easy to ensure suitable adhesive force.
[0069] The content of the (meth)acrylate having 2 to 14 carbon atoms in the monomers constituting the acrylic copolymer used in the adhesive layer of the present invention is preferably 90 to 99% by mass, more preferably 90 to 96% by mass. By setting the content of the (meth)acrylate within this range, it is easy to ensure suitable adhesive strength.
[0070] In the acrylic copolymer, it is preferred to further use a (meth)acrylate monomer having a polar group such as a hydroxyl group, a carboxyl group, or an amide group, or a vinyl monomer having another polar group as a monomer component.
[0071] Examples of the (meth)acrylate monomer having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, hydroxypropyl (meth)acrylate, caprolactone-modified (meth)acrylate, polyethylene glycol mono (meth)acrylate, polypropylene glycol mono (meth)acrylate, etc. Among these, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 6-hydroxyhexyl (meth)acrylate are preferably used.
[0072] Examples of the (meth)acrylate monomer having a carboxyl group include acrylic acid, methacrylic acid, itaconic acid, maleic acid, crotonic acid, a dimer of acrylic acid or methacrylic acid, and ethylene oxide-modified succinic acid acrylate. Among these, acrylic acid is preferably used.
[0073] Examples of the (meth)acrylate monomer having an amide group include N-vinyl-2-pyrrolidone, N-vinyl caprolactam, acryloyl morpholine, acrylamide, N,N-dimethylacrylamide, and N-acryloyloxyethyl-3,4,5,6-tetrahydrophthalimide. Among these, N-vinyl-2-pyrrolidone, N-vinyl caprolactam, and acryloyl morpholine are preferably used.
[0074] Examples of the vinyl monomer having other polar groups include vinyl acetate, acrylonitrile, maleic anhydride, and itaconic anhydride.
[0075] The content of the monomer having a polar group is preferably 0.1 to 20% by weight, more preferably 1 to 13% by weight, and still more preferably 1.5 to 8% by weight of the monomer components constituting the acrylic copolymer. By containing the monomer having a polar group within this range, it is easy to adjust the cohesive force, holding power, and adhesiveness of the adhesive to a suitable range.
[0076] The weight average molecular weight Mw of the acrylic copolymer used in the adhesive layer is preferably 400,000 to 1,400,000, and more preferably 600,000 to 1,200,000. When the weight average molecular weight Mw of the acrylic copolymer is within this range, it is easy to adjust the adhesive force to a specific range.
[0077] The weight average molecular weight Mw can be measured by gel permeation chromatography (GPC). More specifically, the GPC measuring apparatus can be "SC8020" manufactured by Tosoh Corporation, and the weight average molecular weight Mw can be measured under the following GPC measuring conditions based on the polystyrene conversion value.
[0078] (GPC measurement conditions)
[0079] Sample concentration: 0.5 wt% (tetrahydrofuran solution)
[0080] Sample injection volume: 100μL
[0081] ·Eluent: Tetrahydrofuran (THF)
[0082] Flow rate: 1.0mL / min
[0083] Column temperature (measurement temperature): 40°C
[0084] ·Pillar: "TSKgel GMHHR-H" manufactured by Tosoh Corporation
[0085] Detector: Differential refractometer
[0086] Furthermore, in order to improve the cohesive force of the adhesive layer, it is preferred to add a crosslinking agent to the adhesive. As the crosslinking agent, for example, isocyanate crosslinking agents, epoxy crosslinking agents, chelate crosslinking agents, etc. can be listed. As the amount of the crosslinking agent added, it is preferably adjusted in a manner that the gel fraction of the adhesive layer is 25 to 80% by mass, more preferably adjusted in a manner that is 40 to 75% by mass, and most preferably adjusted in a manner that is 50 to 70% by mass. By adjusting the gel fraction to this range, the reduction in the surface pencil hardness when the protective film is attached to the substrate can be suppressed, and the adhesion can also be made sufficient. It should be noted that the gel fraction in the present invention is as follows: the cured adhesive layer is immersed in toluene, and the mass of the insoluble components remaining after being placed for 24 hours is measured after drying, and expressed as a percentage relative to the original mass.
[0087] In order to further improve the adhesive force of the adhesive layer, a tackifier resin may be added. When the adhesive resin is an acrylic copolymer, the amount of the tackifier resin added is preferably 10 to 60 parts by mass relative to 100 parts by mass of the acrylic copolymer. When the adhesive property is emphasized, the amount of the tackifier resin added is preferably 20 to 50 parts by mass.
[0088] In addition, in addition to the above, known and commonly used additives may be added to the adhesive. For example, in order to improve the adhesion to the glass substrate, a silane coupling agent is preferably added in a range of 0.001 to 0.005 parts by mass relative to 100 parts by mass of the adhesive. Furthermore, other additives such as plasticizers, softeners, fillers, pigments, flame retardants, etc. may be added as needed.
[0089] The protective film of the present invention can be applied to various purposes because it has suitable scratch resistance and smoothness, and is particularly preferably applied to the image display part of the image display device of the liquid crystal display (LCD), organic EL display, etc. In particular, even if it is thin, it can achieve suitable scratch resistance and smoothness, and is therefore suitable as a protective film for the image display part of the image display device of the portable electronic terminal with high requirements for miniaturization and thinness such as electronic notebooks, portable phones, smart phones, portable audio players, mobile personal computers, and tablet terminals. In such an image display device, for example, in an image display device of the structure described below, it is used by attaching it to the surface or back of the transparent panel, so as to prevent damage and prevent the transparent panel from scattering when it is damaged. The structure is that it has an image display module such as an LCD module and an organic EL module in its structure, and a transparent panel for protecting the image display module is provided on the upper part of the image display module.
[0090] Example
[0091] The present invention is described in more detail below by way of examples.
[0092] (Synthesis Example 1: Synthesis of urethane acrylate (A1))
[0093] In a flask equipped with a stirrer, a gas introduction tube, a cooling tube, and a thermometer, a mixture of pentaerythritol triacrylate (hereinafter referred to as "PE3A") and pentaerythritol tetraacrylate (hereinafter referred to as "PE4A") (PE3A / PE4A = 60 / 40 (mass ratio)) 549.1 parts by mass, 0.1 parts by mass of dibutyltin diacetate, 0.6 parts by mass of dibutylhydroxytoluene, 0.1 parts by mass of p-methoxyphenol, and 160 parts by mass of butyl acetate were added, and air was blown in, and the temperature was gradually raised while uniformly mixing. After reaching 60°C, 90.9 parts by mass of hexamethylene diisocyanate was added, and the mixture was reacted at 80°C for 5 hours to obtain a solution containing 80% by mass of nonvolatile components of urethane acrylate (A1) having 6 acryloyl groups in one molecule. In addition, in this solution, the non-volatile component contained 34.3 mass % of PE4A in addition to the urethane acrylate (A1).
[0094] (Synthesis Example 2: Synthesis of urethane acrylate (A2))
[0095] In a flask equipped with a stirrer, a gas introduction tube, a cooling tube and a thermometer, 250 parts by mass of butyl acetate, 206 parts by mass of norbornane diisocyanate, 0.5 parts by mass of p-methoxyphenol and 0.5 parts by mass of dibutyltin diacetate were added, and the temperature was raised to 70°C while blowing air, and then 795 parts by mass of a mixture of PE3A and PE4A (PE3A / PE4A=75 / 25 (mass ratio)) was added dropwise over 1 hour. After the addition was completed, the mixture was reacted at 70°C for 3 hours, and the reaction was further continued until 2250 cm-1 of the isocyanate group was -1 The infrared absorption spectrum of 1% disappeared, and a butyl acetate solution containing 80% by mass of nonvolatile components of urethane acrylate (A2) having 6 acryloyl groups in one molecule was obtained. It should be noted that in addition to urethane acrylate (A2), the nonvolatile components of the solution also contained 19.9% by mass of PE4A.
[0096] (Synthesis Example 3: Synthesis of urethane acrylate (A3))
[0097] In a flask equipped with a stirrer, a gas introduction tube, a cooling tube and a thermometer, 254 parts by mass of butyl acetate, 222 parts by mass of isophorone diisocyanate, 0.5 parts by mass of p-methoxyphenol and 0.5 parts by mass of dibutyltin diacetate were added, and the temperature was raised to 70°C while blowing air, and then 795 parts by mass of a mixture of PE3A and PE4A (PE3A / PE4A=75 / 25 (mass ratio)) was added dropwise over 1 hour. After the addition was completed, the mixture was reacted at 70°C for 3 hours, and the reaction was further continued until 2250 cm-1 of the isocyanate group was -1 The infrared absorption spectrum of 1% disappeared, and a solution containing 80% by mass of nonvolatile components of urethane acrylate (A3) having 6 acryloyl groups in one molecule was obtained. It should be noted that in addition to urethane acrylate (A3), the nonvolatile components of the solution also contained 19.5% by mass of PE4A.
[0098] (Synthesis Example 4: Synthesis of urethane acrylate (A4))
[0099] In a flask equipped with a stirrer, a gas introduction tube, a cooling tube, and a thermometer, 254 parts by mass of butyl acetate, 222 parts by mass of isophorone diisocyanate, 0.5 parts by mass of p-methoxyphenol, and 0.5 parts by mass of dibutyltin diacetate were added, and the temperature was raised to 70°C while blowing air, and then 369 parts by mass of bis(2-acryloyloxyethyl)hydroxyethyl isocyanurate and 398 parts by mass of a mixture of PE3A and PE4A (PE3A / PE4A=75 / 25 (mass ratio)) were added dropwise over 1 hour. After the addition was completed, the mixture was reacted at 70°C for 3 hours, and the reaction was further continued until 2250 cm-1 of the isocyanate group was -1 The infrared absorption spectrum of 1% disappeared, and a solution containing 80% by mass of nonvolatile components of urethane acrylate (A4) having 4 to 6 acryloyl groups in one molecule was obtained. It should be noted that the nonvolatile components of the solution contained 10.1% by mass of PE4A in addition to urethane acrylate (A4).
[0100] (Synthesis Example 5: Synthesis of urethane acrylate (A5))
[0101] In a flask equipped with a stirrer, a gas introduction tube, a cooling tube, and a thermometer, 242 parts by mass of a mixture of PE3A and PE4A (PE3A / PE4A=60 / 40 (mass ratio)), 0.23 parts by mass of p-methoxyphenol, 0.13 parts by mass of dibutyltin dilaurate, and 100 parts by mass of methyl ethyl ketone were added, and the temperature was raised to 75°C while blowing air, and then a mixed solution of 107 parts by mass of a trimer (isocyanurate) of hexamethylene diisocyanate ("Desmodur N3390BA" manufactured by Sumika Bayer Urethane Co., Ltd., non-volatile component: 90% by mass, NCO%: 19.6, NCO equivalent: 214 g / eq.) and 50 parts by mass of methyl ethyl ketone was added dropwise over 2 hours. After the addition was completed, the mixture was reacted at 75°C for 4 hours, and the reaction was further continued until the 2250 cm-1 of the isocyanate group was -1 The infrared absorption spectrum of 1% disappeared, and a solution containing 67.8% by mass of nonvolatile components of urethane acrylate (A5) having 9 acryloyl groups in one molecule was obtained. It should be noted that in addition to urethane acrylate (A5), the nonvolatile components of the solution also contained 28.6% by mass of PE4A.
[0102] (Synthesis Example 6: Synthesis of urethane acrylate (A6))
[0103] In a flask equipped with a stirrer, a gas introduction tube, a cooling tube and a thermometer, 436.7 parts by mass of a mixture of dipentaerythritol pentaacrylate (hereinafter referred to as "DPPA") and dipentaerythritol hexaacrylate (hereinafter referred to as "DPHA") (DPPA / DPHA = 60 / 40 (mass ratio)), 0.23 parts by mass of p-methoxyphenol, 0.13 parts by mass of dibutyltin dilaurate and 180 parts by mass of methyl ethyl ketone were added, and the temperature was raised to 75° C. while blowing air. Then, a mixed solution of 180 parts by mass of a trimer (isocyanurate) of isophorone diisocyanate ("Desmodur Z4470BA" manufactured by Sumika Bayer Urethane Co., Ltd., nonvolatile content: 70% by mass, NCO%: 11.7, NCO equivalent: 359 g / eq.) and 80 parts by mass of methyl ethyl ketone (hereinafter referred to as "MEK") was added dropwise over 2 hours. After the dropwise addition, the reaction was allowed to proceed at 75°C for 4 hours, and the reaction was further continued until the 2250 cm-1 wavelength of the isocyanate group -1 The infrared absorption spectrum of 15 acryloyl groups disappeared, and a solution containing 64.2% by mass of nonvolatile components of urethane acrylate (A5) having 15 acryloyl groups in one molecule was obtained. It should be noted that the nonvolatile components of the solution contained 31% by mass of DPHA in addition to urethane acrylate (A6).
[0104] (Synthesis Example 7: Synthesis of urethane acrylate (RA1))
[0105] In a flask equipped with a stirrer, a gas introduction tube, a cooling tube, and a thermometer, 58.4 parts by mass of 2-hydroxypropyl acrylate, 0.23 parts by mass of p-methoxyphenol, 0.13 parts by mass of dibutyltin dilaurate, and 100 parts by mass of methyl ethyl ketone were added, and the temperature was raised to 60° C. while blowing air, and then a mixed solution of 107 parts by mass of a trimer (isocyanurate) of hexamethylene diisocyanate ("Desmodur N3390BA" manufactured by Sumika Bayer Urethane Co., Ltd., nonvolatile component: 90% by mass, NCO%: 19.6, NCO equivalent: 214 g / eq.) and 50 parts by mass of methyl ethyl ketone was added dropwise over 2 hours. After the addition was completed, the mixture was reacted at 60° C. for 4 hours, and the reaction was further continued until the 2250 cm-1 of the isocyanate group was -1 The infrared absorption spectrum of disappeared, and a solution containing 71.8 mass % of nonvolatile components of urethane acrylate (RA1) having three acryloyl groups in one molecule was obtained.
[0106] (Synthesis Example 8: Synthesis of polymer (E1))
[0107] In a flask equipped with a stirrer, a gas introduction tube, a cooling tube, and a thermometer, 250 parts by mass of glycidyl methacrylate, 1.3 parts by mass of lauryl mercaptan, 1,000 parts by mass of methyl isobutyl ketone, and 7.5 parts by mass of 2,2'-azobisisobutyronitrile were added, and the temperature was raised to 90°C over 1 hour while stirring under a nitrogen gas stream, and the mixture was reacted at 90°C for 1 hour. Next, a mixed solution containing 750 parts by mass of glycidyl methacrylate, 3.7 parts by mass of lauryl mercaptan, and 22.5 parts by mass of 2,2'-azobisisobutyronitrile was added dropwise over 2 hours while stirring at 90°C, and the mixture was reacted at 100°C for 3 hours. Next, 10 parts by mass of 2,2'-azobisisobutyronitrile was added, and the mixture was further reacted at 100°C for 1 hour, and then the temperature was raised to about 120°C and the mixture was reacted for 2 hours. Cool to 60 ° C, replace the nitrogen inlet tube with an air inlet tube, add 507 parts by mass of acrylic acid, 2 parts by mass of p-methoxyphenol, and 5.4 parts by mass of triphenylphosphine, mix, bubble the reaction solution with air, and heat it to 110 ° C to react for 8 hours. Then, add 1.4 parts by mass of p-methoxyphenol, cool to room temperature, and add methyl isobutyl ketone in a manner such that the non-volatile component is 50% by mass to obtain a solution of an acrylic resin having an acryloyl group, i.e., a polymer (E1). It should be noted that the weight average molecular weight of the obtained polymer (E1) is 31,000 (converted to polystyrene using GPC), and the acryloyl equivalent is 300g / eq.
[0108] (Synthesis Example 9: Synthesis of fluorine compound (C1))
[0109] In a flask equipped with a stirrer and a cooling tube, 500 parts by mass of a perfluoropolyether having allyl groups at both ends represented by the following formula (5), 700 parts by mass of m-xylene hexafluoride, and 361 parts by mass of tetramethylcyclotetrasiloxane were added under a dry nitrogen atmosphere, and the temperature was raised to 90° C. while stirring. 0.442 parts by mass of a toluene solution of a chloroplatinic acid / vinylsiloxane complex (containing 1.1×10 -6 mol. ), and stirred for 4 hours while maintaining the internal temperature at 90°C or above. 1 After the disappearance of the allyl group of the raw material was confirmed by H-NMR spectrum, the solvent and excess tetramethylcyclotetrasiloxane were distilled off under reduced pressure, and the mixture was treated with activated carbon to obtain a perfluoropolyether compound (1) represented by the following formula (6) as a colorless transparent liquid.
[0110] H2C=CHCH2OCH2-Rf-CH2OCH2CH=CH2 (5)
[0111]
[0112] (In the formula, m / n is 0.9, and the sum of m and n is 45 as an average.)
[0113]
[0114] In a dry air atmosphere, 50 parts by mass of the perfluoropolyether compound (1) obtained as described above, 7.05 parts by mass of 2-allyloxyethanol, 50 parts by mass of m-ditrifluorotoluene, and 0.0442 parts by mass of a toluene solution of a chloroplatinic acid / vinylsiloxane complex (containing 1.1×10 -7 mol. ), stirred at 100°C for 4 hours. 1 After the disappearance of the Si-H group was confirmed by H-NMR spectrum and infrared absorption spectrum, the solvent and excess 2-allyloxyethanol were distilled off under reduced pressure and the mixture was treated with activated carbon to obtain a perfluoropolyether compound (2) represented by the following formula (7) as a pale yellow transparent liquid.
[0115]
[0116] In a dry air atmosphere, 50 parts by mass of the perfluoropolyether compound (2) obtained as described above, 50 parts by mass of tetrahydrofuran and 9 parts by mass of 2-acryloyloxyethyl isocyanate are mixed and heated to 50°C. Next, 0.05 parts by mass of dioctyltin laurate is added and stirred at 50°C for 24 hours. After the heating is completed, the fluorine compound (C1) in a pale yellow paste state represented by the following formula (8) is obtained by distilling under reduced pressure at 80°C and 0.27 kPa. A mixed solvent of methyl ethyl ketone and methyl isobutyl ketone (methyl ethyl ketone / methyl isobutyl ketone = 1 / 3 (mass ratio)) is added to the fluorine compound (C1) to prepare a fluorine compound (C1) solution having a non-volatile component of 20% by mass.
[0117]
[0118] Using the urethane acrylates (A1) to (A6), (RA1), the polymer (E1), and the fluorine compound (C1) obtained as described above, an active energy ray-curable composition was prepared as follows.
[0119] (Example 1)
[0120] 31.3 parts by mass of the solution containing urethane acrylate (A2) obtained in Synthesis Example 2 (containing 20 parts by mass of urethane acrylate (A2) and 5 parts by mass of PE4A), 31.3 parts by mass of the solution containing urethane acrylate (A3) obtained in Synthesis Example 3 (containing 20.1 parts by mass of urethane acrylate (A3) and 4.9 parts by mass of PE4A), 25 parts by mass of the solution containing urethane acrylate (A4) obtained in Synthesis Example 4 (containing 18 parts by mass of urethane acrylate (A4) and 2 parts by mass of PE4A), 30 parts by mass of a mixture of DPHA and DPPA (DPHA / DPPA=60 / 40 (mass ratio)), 1.5 parts by mass of a 20% by mass solution of a fluorine compound (C1) (0.3 parts by mass as the fluorine compound (C1)), and a photopolymerization initiator ("IRGACURE 9000" manufactured by BASF JAPAN CO., LTD.) were added. 184", 1-hydroxycyclohexyl phenyl ketone; hereinafter referred to as "photopolymerization initiator (D1)". 4.5 parts by mass of the reaction mixture was uniformly stirred and then diluted with ethyl acetate to prepare an active energy ray-curable composition (1) having a non-volatile component content of 40% by mass.
[0121] [Evaluation of coating appearance]
[0122] In order to determine whether the active energy ray-curable composition (1) obtained as described above can be used as a coating agent, the appearance was visually observed and the coating agent appearance was evaluated according to the following criteria.
[0123] ○: No turbidity or component separation.
[0124] ×: Cloudiness or component separation.
[0125] [Preparation of test piece film]
[0126] The active energy ray-curable composition (1) obtained as described above was applied onto the easily-adhesive treated surface of a polyethylene terephthalate film ("COSMOSHINEA 4100" manufactured by Toyobo Co., Ltd., thickness 100 μm) using a wire bar (#40), dried at 60°C for 1 minute, and then irradiated with an ultraviolet irradiation device ("MIDN-042-C1" manufactured by iGrafx Co., Ltd., lamp: 120 W / cm, high-pressure mercury lamp) in an air atmosphere at a light intensity of 0.5 J / cm 2 The ultraviolet rays were irradiated to obtain a test piece film having a cured coating film (hard coat layer) with a thickness of 10 μm.
[0127] [Evaluation of Cured Coating Film Appearance]
[0128] The surface of the cured coating film of the test piece film obtained as described above was visually observed, and the appearance of the cured coating film was evaluated according to the following criteria.
[0129] ○: There are no uneven coating, coating streaks, or stains.
[0130] △: Slight uneven coating, coating streaks, or stains.
[0131] ×: There are uneven coating, coating streaks, or dirt.
[0132] The test piece films obtained as described above were evaluated or measured for the following scratch resistance, water contact angle, oil-based ink repellency (antifouling property), and smoothness.
[0133] [Evaluation of scratch resistance]
[0134] The test piece film obtained as described above was cut into a 30 cm × 2 cm rectangle and fixed with a fixture in a flat friction tester (manufactured by Toyo Seiki Seisaku-sho Co., Ltd.) using steel wool #0000 at a load of 2 kg / cm 2 The test piece was subjected to 2000 reciprocating strokes, a stroke of 10 cm, a speed of 20 cm / sec, and the damage state of the test piece after the test was visually observed, and the abrasion resistance was evaluated according to the following criteria.
[0135] ◎: No damage.
[0136] ○: Less than 5 damaged fibers.
[0137] △: Although 5 or more strands were damaged, the entire surface of the test piece film was not damaged.
[0138] ×: The entire test piece film is damaged.
[0139] [Measurement of water contact angle]
[0140] The test piece film obtained as described above was cut into a 1×5 cm rectangle and fixed to a glass plate with a double-sided tape with the cured coating film on the front side. The contact angle of 4 to 4.5 μL of purified water was measured using an automatic contact angle meter "DROMP AMSTER500" manufactured by Kyowa Interface Science Co., Ltd.
[0141] [Evaluation of antifouling properties]
[0142] On the cured coating film of the test piece film obtained as described above, ink was applied in a circular shape using "UniMediax (black)" manufactured by Mitsubishi Pencil Co., Ltd., and the degree of ink repellency was visually observed. Based on the observation results, antifouling properties were evaluated according to the following criteria.
[0143] 5: Repels ink and appears in dot shape.
[0144] 4: Repel ink and appear in dots and lines.
[0145] 3: Repels ink and forms a line.
[0146] 2: Slightly repels ink.
[0147] 1: Does not repel ink.
[0148] [Evaluation of surface smoothness]
[0149] The surface of the cured coating film of the test piece film obtained as described above was rubbed with BEMCOT (manufactured by Asahi Kasei Fibers Corporation), and the smoothness was evaluated based on the degree of slipperiness at that time according to the following criteria.
[0150] ◎: Very slippery
[0151] ○: Slide
[0152] △: Not easy to slide
[0153] ×: No sliding
[0154] (Example 2)
[0155] 22.5 parts by mass of the solution containing urethane acrylate (A2) obtained in Synthesis Example 2 (containing 14.4 parts by mass of urethane acrylate (A2) and 3.6 parts by mass of PE4A), 22.5 parts by mass of the solution containing urethane acrylate (A3) obtained in Synthesis Example 3 (containing 14.5 parts by mass of urethane acrylate (A3) and 3.5 parts by mass of PE4A), and 17.5 parts by mass of the solution containing urethane acrylate (A4) obtained in Synthesis Example 4 (containing 12.6 parts by mass of urethane acrylate (A4) and 3.6 parts by mass of PE4A) were mixed. 1.4 parts by mass. ), 50 parts by mass of a mixture of DPHA and DPPA (DPHA / DPPA=60 / 40 (mass ratio)), 1.5 parts by mass of a 20% by mass solution of a fluorine compound (C1) (0.3 parts by mass as fluorine compound (C1)) and 4.5 parts by mass of a photopolymerization initiator (D1) were uniformly stirred and diluted with ethyl acetate to prepare an active energy ray-curable composition (2) having a non-volatile component content of 40% by mass. Using the obtained active energy ray-curable composition (2), a test piece film was prepared in the same manner as in Example 1, and the coating appearance, cured coating film appearance, scratch resistance, water contact angle, antifouling property and smoothness were evaluated or measured.
[0156] (Example 3)
[0157] 87.5 parts by mass of the solution containing urethane acrylate (A1) obtained in Synthesis Example 1 (containing 46 parts by mass of urethane acrylate (A1) and 24 parts by mass of PE4A), 30 parts by mass of a mixture of DPHA and DPPA (DPHA / DPPA=60 / 40 (mass ratio)), 1.5 parts by mass of a 20% by mass solution of a fluorine compound (C1) (0.3 parts by mass as fluorine compound (C1)) and 4.5 parts by mass of a photopolymerization initiator (D1) were uniformly stirred and diluted with ethyl acetate to prepare an active energy ray-curable composition (3) having a non-volatile component content of 40% by mass. Using the obtained active energy ray-curable composition (3), a test piece film was prepared in the same manner as in Example 1, and the coating appearance, cured coating film appearance, scratch resistance, water contact angle, antifouling property and smoothness were evaluated or measured.
[0158] (Example 4)
[0159] 62.5 parts by mass of the solution containing urethane acrylate (A1) obtained in Synthesis Example 1 (containing 32.8 parts by mass of urethane acrylate (A1) and 17.2 parts by mass of PE4A), 50 parts by mass of a mixture of DPHA and DPPA (DPHA / DPPA=60 / 40 (mass ratio)), 1.5 parts by mass of a 20% by mass solution of a fluorine compound (C1) (0.3 parts by mass as fluorine compound (C1)) and 4.5 parts by mass of a photopolymerization initiator (D1) were uniformly stirred and diluted with ethyl acetate to prepare an active energy ray-curable composition (4) having a non-volatile component content of 40% by mass. Using the obtained active energy ray-curable composition (4), a test piece film was prepared in the same manner as in Example 1, and the coating appearance, cured coating film appearance, scratch resistance, water contact angle, antifouling property and smoothness were evaluated or measured.
[0160] (Example 5)
[0161] 43.8 parts by mass of the solution containing urethane acrylate (A3) obtained in Synthesis Example 3 (containing 28.2 parts by mass of urethane acrylate (A3) and 6.8 parts by mass of PE4A), 50 parts by mass of a mixture of DPHA and DPPA (DPHA / DPPA=60 / 40 (mass ratio)), 15 parts by mass of hexanediol diacrylate (hereinafter referred to as "HDDA"), 1.5 parts by mass of a 20% by mass solution of a fluorine compound (C1) (0.3 parts by mass as fluorine compound (C1)) and 4.5 parts by mass of a photopolymerization initiator (D1) were uniformly stirred and diluted with ethyl acetate to prepare an active energy ray-curable composition (5) having a non-volatile component content of 40% by mass. Using the obtained active energy ray-curable composition (5), a test piece film was prepared in the same manner as in Example 1, and the coating appearance, cured coating film appearance, scratch resistance, water contact angle, antifouling property and smoothness were evaluated or measured.
[0162] (Example 6)
[0163] 56.3 parts by mass of the solution containing urethane acrylate (A3) obtained in Synthesis Example 3 (containing 36.2 parts by mass of urethane acrylate (A3) and 8.8 parts by mass of PE4A), 36.9 parts by mass of the solution containing urethane acrylate (A5) obtained in Synthesis Example 5 (containing 17.8 parts by mass of urethane acrylate (A5) and 7.2 parts by mass of PE4A), 30 parts by mass of a mixture of PE4A and PE3A (PE4A / PE3A=60 / 40 (mass ratio)), 1.5 parts by mass of a 20% by mass solution of a fluorine compound (C1) (0.3 parts by mass as the fluorine compound (C1)) and 4.5 parts by mass of a photopolymerization initiator (D1) were uniformly stirred and diluted with ethyl acetate to prepare an active energy ray-curable composition (6) having a non-volatile component content of 40% by mass. Using the obtained active energy ray-curable composition (6), a test piece film was prepared in the same manner as in Example 1, and then the coating appearance, cured coating film appearance, scratch resistance, water contact angle, antifouling property, and lubricity were evaluated or measured.
[0164] (Example 7)
[0165] 56.3 parts by mass of the solution containing urethane acrylate (A3) obtained in Synthesis Example 3 (containing 36.2 parts by mass of urethane acrylate (A3) and 8.8 parts by mass of PE4A), 38.9 parts by mass of the solution containing urethane acrylate (A6) obtained in Synthesis Example 6 (containing 17.2 parts by mass of urethane acrylate (A6) and 7.8 parts by mass of DPHA), 30 parts by mass of a mixture of PE4A and PE3A (PE4A / PE3A=60 / 40 (mass ratio)), 1.5 parts by mass of a 20% by mass solution of a fluorine compound (C1) (0.3 parts by mass as the fluorine compound (C1)) and 4.5 parts by mass of a photopolymerization initiator (D1) were uniformly stirred and diluted with ethyl acetate to prepare an active energy ray-curable composition (7) having a non-volatile component content of 40% by mass. Using the obtained active energy ray-curable composition (7), a test piece film was prepared in the same manner as in Example 1, and then the coating appearance, cured coating film appearance, scratch resistance, water contact angle, antifouling property, and lubricity were evaluated or measured.
[0166] (Example 8)
[0167] The active energy ray-curable composition (1) obtained in Example 1 was used, and the appearance, scratch resistance, water contact angle, antifouling property and smoothness of the cured coating film were evaluated or measured in the same manner as in Example 1, except that the curing conditions during the preparation of the test piece film, i.e., the air atmosphere, were changed to an atmosphere with an oxygen concentration of 5,000 ppm or less.
[0168] (Example 9)
[0169] The active energy ray-curable composition (2) obtained in Example 2 was used, and the curing conditions during the preparation of the test piece film, i.e., the air atmosphere, were changed to an atmosphere with an oxygen concentration of 5,000 ppm or less. The appearance, scratch resistance, water contact angle, antifouling property, and smoothness of the cured coating film were evaluated or measured in the same manner as in Example 1.
[0170] (Comparative Example 1)
[0171] An active energy ray-curable composition (R1) was obtained in the same manner as in Example 1 except that 1.5 parts by mass (0.3 parts by mass as fluorine compound (RC1)) having an acryloyl group at the end of the poly(perfluoroalkylene ether) chain ("OPTOOLDAC-HP" manufactured by Daikin Industries, Ltd., nonvolatile component: 20 parts by mass) was used instead of the fluorine compound (C1) used in Example 1. Using the obtained active energy ray-curable composition (R1), a test piece film was prepared in the same manner as in Example 1, and the coating appearance, cured coating film appearance, scratch resistance, water contact angle, antifouling property, and smoothness were evaluated or measured.
[0172] (Comparative Example 2)
[0173] 180 parts by mass of the solution of the polymer (E1) obtained in Synthesis Example 8, 10 parts by mass of a mixture of DPHA and DPPA (DPHA / DPPA=60 / 40 (mass ratio)), 1.5 parts by mass of a 20% by mass solution of a fluorine compound (C1) (0.3 parts by mass as fluorine compound (C1)) and 4.5 parts by mass of a photopolymerization initiator (D1) were uniformly stirred and diluted with ethyl acetate to prepare an active energy ray-curable composition (R2) having a non-volatile component content of 40% by mass. Using the obtained active energy ray-curable composition (R2), a test piece film was prepared in the same manner as in Example 1, and the coating appearance, cured coating film appearance, scratch resistance, water contact angle, antifouling property and smoothness were evaluated or measured.
[0174] (Comparative Example 3)
[0175] 97.5 parts by mass of the solution containing urethane acrylate (RA1) obtained in Synthesis Example 7 (70 parts by mass as urethane acrylate (RA1), 30 parts by mass of a mixture of DPHA and DPPA (DPHA / DPPA=60 / 40 (mass ratio)), 1.5 parts by mass of a 20% by mass solution of a fluorine compound (C1) (0.3 parts by mass as a fluorine compound (C1)) and 4.5 parts by mass of a photopolymerization initiator (D1) were uniformly stirred and diluted with ethyl acetate to prepare an active energy ray-curable composition (R3) having a non-volatile component content of 40% by mass. Using the obtained active energy ray-curable composition (R3), a test piece film was prepared in the same manner as in Example 1, and the coating appearance, cured coating film appearance, scratch resistance, water contact angle, antifouling property and smoothness were evaluated or measured.
[0176] (Comparative Example 4)
[0177] The active energy ray-curable composition (R1) obtained in Comparative Example 1 was used, and the appearance, scratch resistance, water contact angle, antifouling properties, and smoothness of the cured coating film were evaluated or measured in the same manner as in Example 1, except that the curing conditions during the preparation of the test piece film, i.e., the air atmosphere, were changed to an atmosphere with an oxygen concentration of 5,000 ppm or less.
[0178] (Comparative Example 5)
[0179] The appearance, scratch resistance, water contact angle, antifouling property and smoothness of the cured coating film were evaluated or measured in the same manner as in Example 1, except that the active energy ray-curable composition (R2) obtained in Comparative Example 2 was used and the curing conditions during the preparation of the test piece film, i.e., the air atmosphere, were changed to an atmosphere with an oxygen concentration of 5,000 ppm or less.
[0180] Table 1 shows the compositions and evaluation results of the active energy ray-curable compositions used in Examples 1 to 9 and Comparative Examples 1 to 5. It should be noted that all the compositions in Table 1 are described in terms of non-volatile component amounts, and for urethane acrylates (A1) to (A6), the amounts of PE4A or DPHA are described.
[0181] [Table 1]
[0182]
[0183] According to the evaluation results shown in Table 1, it can be confirmed that the active energy ray-curable compositions of the present invention, i.e., the compositions of Examples 1 to 9, have no problem in appearance as coating agents, and the appearance of the cured coating films thereof has no problem, and further, the surfaces of the cured coating films have excellent scratch resistance, antifouling properties, and smoothness. In addition, when the oxygen concentration is set to 5,000 ppm or less when preparing the cured coating films, it is confirmed that the scratch resistance and smoothness are further improved.
[0184] On the other hand, Comparative Example 1 is an example of an active energy ray-curable composition using a fluorine compound other than the fluorine compound (C) used in the present invention, and it was confirmed that the scratch resistance and smoothness were not sufficient. In addition, even in Comparative Example 4 in which the oxygen concentration during the curing of the active energy ray-curable composition was set to 5,000 ppm or less, it was also confirmed that the scratch resistance and smoothness were not sufficient.
[0185] Comparative Example 2 is an example of an active energy ray-curable composition using an acrylic resin having an acryloyl group instead of the urethane acrylate (A) used in the present invention, and it was confirmed that the appearance of the cured coating film had problems, and the scratch resistance and smoothness were not sufficient. In addition, even in Comparative Example 5 in which the oxygen concentration during the curing of the active energy ray-curable composition was set to 5,000 ppm or less, it was also confirmed that the appearance of the cured coating film had problems, and the scratch resistance and smoothness were not sufficient.
[0186] Comparative Example 3 is an example of an active energy ray-curable composition using a urethane acrylate having three acryloyl groups instead of the urethane acrylate (A) having four or more (meth) acryloyl groups used in the present invention. It was confirmed that the coating appearance and the cured coating film appearance were poor, and the scratch resistance, antifouling properties, and smoothness were also significantly deteriorated.
Claims
1. An active energy ray-curable composition, characterized in that: Contains urethane (meth)acrylate (A), multifunctional (meth)acrylate (B) and fluorine compound (C), wherein: The urethane (meth)acrylate (A) is a urethane (meth)acrylate having 4 or more (meth)acryloyl groups in one molecule obtained by reacting an aliphatic polyisocyanate (a1) with a (meth)acrylate (a2) having a hydroxyl group. The polyfunctional (meth)acrylate (B) is a polyfunctional (meth)acrylate having three or more (meth)acryloyl groups in one molecule. The fluorine compound (C) has a structure in which a polycyclosiloxane structure is bonded to both ends of a poly(perfluoroalkylene ether) chain via a divalent linking group, and a (meth)acryloyl group is bonded to the polycyclosiloxane structure via a divalent linking group. The urethane (meth)acrylate (A) is obtained by using a urethane acrylate obtained by using norbornane diisocyanate as the aliphatic polyisocyanate (a1) and a urethane acrylate obtained by using isophorone diisocyanate as the aliphatic polyisocyanate (a1). The divalent linking group that bonds the poly(perfluoroalkylene ether) chain to the polycyclosiloxane structure is a group represented by the following general formula (3): -CH2—O—Y-(3) Wherein, in the general formula (3), Y is an alkylene group having 1 to 6 carbon atoms; The divalent linking group that bonds the polycyclosiloxane structure to the (meth)acryloyl group is a group represented by the following general formula (4): Among them, in the general formula (4), Z 1 , Z 2 and Z 3 Each is independently an alkylene group having 1 to 6 carbon atoms; The multifunctional (meth)acrylate (B) is a mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate, or a mixture of pentaerythritol triacrylate and pentaerythritol tetraacrylate; The mass ratio (A) / (B) of the urethane (meth)acrylate (A) to the multifunctional (meth)acrylate (B) is 80 / 20 to 20 / 80, The amount of the fluorine compound (C) is 0.05 to 5 parts by mass based on 100 parts by mass of the total of the urethane (meth)acrylate (A), the polyfunctional (meth)acrylate (B), and optionally other (meth)acrylate compounds other than the urethane (meth)acrylate (A) and the polyfunctional (meth)acrylate (B).
2. The active energy ray-curable composition according to claim 1, wherein The multifunctional (meth)acrylate (B) is a mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate.
3. A solidified product, characterized in that: A cured product obtained by irradiating the active energy ray-curable composition according to claim 1 or 2 with active energy rays.
4. A solidified product, characterized in that: A cured product obtained by irradiating the active energy ray-curable composition according to claim 1 or 2 with ultraviolet rays in a gas atmosphere having an oxygen concentration of 5000 ppm or less.
5. An article, characterized in that: A cured coating film comprising the active energy ray-curable composition according to claim 1 or 2.
6. A hard coating film, characterized in that: A film substrate has a hard coat layer on at least one surface thereof, wherein the hard coat layer comprises a cured product of the active energy ray-curable composition according to claim 1 or 2.
7. The hard coating film according to claim 6, wherein The thickness of the hard coat layer is 1 μm to 20 μm, and the thickness of the substrate is 50 μm to 200 μm.
8. A protective film, characterized in that: The hard coating film according to claim 6 or 7 has an adhesive layer on one side.
9. The protective film according to claim 8, wherein: The thickness of the adhesive layer is 5 μm to 50 μm. 10 . The protective film according to claim 8 or 9 , which is used for protecting an image display portion of a portable electronic terminal.