A formaldehyde-purifying EB-cured PET facing cabinet door panel

Through electron beam curing technology and multi-layer structural design, formaldehyde purification coatings with components such as chitin and nano silicon powder have been used to solve the problems of formaldehyde release and insufficient performance during the curing of wooden cabinet door panels, and achieve efficient formaldehyde purification and surface performance improvement , meets environmental protection and performance needs.

CN118636253BActive Publication Date: 2024-12-06DEHUA TB NEW DECORATION MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411106561.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-12-06
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

During the curing process, existing wooden cabinet door panels have problems such as formaldehyde emission, high energy consumption, serious pollution and insufficient curing degree, which affects indoor air quality and product performance.

Method used

Formaldehyde purification coatings that combine electron beam curing technology with chitin, nano-silicon powder, alumina and boric acid powder are improved through a multi-layer structural design including a dextile-free coating adhesive and a photocatalyst PET film layer to improve formaldehyde purification and surface performance.

Benefits of technology

The formaldehyde purification, pollution resistance, wear resistance, impact resistance, fingerprint resistance and other properties of the cabinet door panel are significantly improved, and the formaldehyde emission is reduced, achieving high surface performance and environmentally friendly production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118636253B_ABST
    Figure CN118636253B_ABST
Patent Text Reader

Abstract

The invention relates to a formaldehyde-purifying EB-cured PET facing cabinet door panel, comprising the steps of preparing an electron beam-cured formaldehyde-purifying coating, preparing an aldehyde-free coating adhesive, preparing a PET film layer, and coating the cabinet door panel with an EB-cured formaldehyde-purifying coating. An EB electron beam-cured formaldehyde-purifying and reinforcing modifier different from a conventional cabinet door panel is added as a surface functional material, and a photocatalyst medium PET film layer, an aldehyde-free coating adhesive, a multi-layer structure of a plate material, and purification of formaldehyde in the air are combined to obtain a formaldehyde-purifying EB-cured PET facing cabinet door panel that is wear-resistant, corrosion-resistant, high-hardness, anti-fouling, anti-impact, anti-yellowing, anti-fingerprint, and is green, ecological, and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of furniture, and in particular to the field of a formaldehyde-purified EB-cured PET facing cabinet door panel. Background Art

[0002] Wood-based panels include natural wood-based panels and a large number of wood-based panels (plywood, particleboard, fiberboard, etc.), which are widely used in furniture, building materials and other fields. In the production process of wood-based panels, wood-based panels that have not undergone the final finishing process are called plain panels. After the surface of the plain panels is painted and cured, they can form colorful, diverse tones, and varied patterns of decorative coatings, as well as protective coatings with high surface performance and high adhesion.

[0003] The current status of indoor air quality is a focal issue of social concern. Excessive concentrations of formaldehyde, TVOC and bacteria seriously affect people's physical and mental health. At present, the main indoor decorative panels are: blockboard, plywood, density board, integrated wood, particle board, fireproof board, decorative veneer, ecological board, etc. Indoor decorative panels such as paint, latex paint or adhesives contain formaldehyde, VOCs and other harmful gases. Studies have shown that the release period of indoor formaldehyde is generally 3 to 15 years. Living in a space containing harmful gases such as formaldehyde for a long time will cause great harm to the human body.

[0004] In addition, conventional cabinet door panels have a variety of coatings on their surface, and the general curing method is thermal curing or UV curing. However, when using the heating curing method, a large amount of heat or electricity is consumed during the curing process of the liquid coating, and the energy cannot be used efficiently; at the same time, the thermal curing process uses coatings containing a large amount of solvents, and the solvents evaporate when heated, and the volatile organic compounds (VOCs) in them are released into the air, causing serious air pollution. In addition, the microstructure of the thermally cured paint is a two-dimensional linear interlaced structure, and the curing can still be improved, and it cannot bring a high-strength, anti-fouling and anti-scratch wood surface.

[0005] The UV curing process is an alternative to thermal curing. It triggers a radiation chemical reaction in the coating through UV irradiation, generates reactive free radicals or ions, and then triggers chain growth (polymerization / cross-linking, etc.), so that the liquid coating forms a film quickly and solidifies. Since UV curing coatings use little or no solvent, UV curing can reduce VOCs emissions during the curing production process and reduce energy consumption. However, due to the limitations of the UV curing principle, when curing thick or colored coatings containing metal powder or inorganic fillers, it is difficult for UV light to penetrate the entire coating, and multiple UV curing processes are required, which increases the complexity of the production line and the space occupied by the production line, and reduces the controllability of product quality. During UV curing, the high temperature of the UV lamp itself and the infrared section of its emission spectrum will cause the irradiated object to heat up and deform, especially when processing large-area thin plates, there will be product deformation problems, quality problems and production safety hazards. In addition, the photoinitiator used in UV curing is expensive and will also bring health risks. The structure of UV-curing materials is mostly a 2.5-dimensional dendritic cross-linked structure with a degree of curing of around 40-70%. Insufficient curing will affect the performance of subsequent related products. Summary of the invention

[0006] The technical purpose of the present invention is to solve the problems in the background technology and provide a formaldehyde-purified EB-cured PET veneer cabinet door panel.

[0007] The above technical objectives of the present invention are achieved through the following technical solutions:

[0008] A formaldehyde-purified EB-cured PET facing cabinet door panel comprises the following process steps:

[0009] Step S1 Preparation of electron beam cured formaldehyde purification coating: adding a certain amount of EB electron beam cured formaldehyde purification and enhancement modifier fine powder into a mixed solution of acrylic emulsion and waterborne polyurethane emulsion at 40-60°C, mixing and stirring evenly at a constant temperature, and storing for standby after the material particles are evenly dispersed;

[0010] Step S2: Formaldehyde-free coating adhesive preparation:

[0011] S21 lignin purification: dissolve the lignin cake in sodium hydroxide solution, stir and mix evenly, extract the supernatant by centrifugation, adjust the pH value of the supernatant with dilute sulfuric acid, and then filter, wash and dry to obtain lignin powder;

[0012] S22 Preparation of formaldehyde-free coating adhesive: dissolving the purified lignin in sodium hydroxide solution, stirring and heating to a constant temperature, adding glyoxal, cooling after the reaction is completed to obtain lignin glyoxal, stirring and mixing the obtained lignin glyoxal with polymer 4,4 / -diphenylmethane diisocyanate PMDI to obtain a formaldehyde-free coating adhesive;

[0013] Step S3: Preparation of the photocatalyst medium PET film layer: polyethylene terephthalate particles, i.e., PET fine powder particles, are melted, mixed with an appropriate amount of nano titanium dioxide, and then extruded and cooled to form a PET film layer;

[0014] Step S4: coating of cabinet door panels: the cabinet door panels are of a multi-layer structure, and the coated multi-layer structure includes a bonding layer outside the core panel, a photocatalyst medium PET film layer and an EB-cured formaldehyde purification layer; the bonding layer adopts the formaldehyde-free coating adhesive prepared in step S2, and the EB-cured formaldehyde purification layer adopts the formaldehyde-purifying electron beam-cured coating prepared in step S1.

[0015] EB stands for electron beam, so EB curing is also electron beam curing. In this scheme, under the electron beam environment, nitrogen molecules are in a plasma state. Under high energy, plasma nitrogen instantly reacts with Si, Al and B in nano-silicon, alumina and boric acid coated on the surface enhancement modifier coating of the plate to form silicon nitride Si. 3 N 4 , aluminum nitride AlN and boron nitride BN, silicon nitride, aluminum nitride, boron nitride are all high hardness ceramic materials with anti-fouling, wear-resistant and anti-fingerprint properties. These nitrogen compounds evenly distributed in the outer layer of the coating have the effect of high surface performance and high adhesion strength.

[0016] Chitosan is the only animal cellulose discovered so far. It is an organic natural substance containing a large amount of active amino groups and a large molecular weight. It has a stable unsaturated positive charge structure and has a strong ability to adsorb small molecular free substances and decompose formaldehyde. Nanosilicon has a strong negative electric field and can adsorb gas molecules such as formaldehyde in the air to the surface of the board. Then the active amino groups in chitosan decompose these substances into water molecules and oximes.

[0017] Preferably, the main components of the EB electron beam curing formaldehyde purification and enhancement modifier in step S1 are chitosan, nano-silicon powder, alumina and boric acid or borax powder; during the production process, 3-10 parts of chitosan, 1-5 parts of nano-silicon powder, 1-3 parts of alumina powder, and 1-5 parts of boric acid or borax powder are mixed evenly for later use, and the above-mentioned mixed fine powder is gradually added to the acrylic acid and water-based polyurethane mixed emulsion and heated and stirred evenly.

[0018] The invention has the advantages of mixing a small amount of chitin, nano silicon powder, aluminum oxide and boric acid or borax powder into the emulsion coating, which can greatly enhance the formaldehyde purification and anti-fouling, wear-resistant, yellowing-resistant, impact-resistant, anti-fingerprint and other properties of the board surface under electron beam irradiation, and has the characteristics of small addition amount, moderate cost and easy operation.

[0019] Preferably, during the lignin purification process in step S21 of step S2, the dissolved mass volume concentration of the lignin cake and the sodium hydroxide solution is 80-150 g / L, the concentration of sodium hydroxide is 1 mol / L, the mixture is stirred and then centrifuged at 4000-4500 rpm for 5 min to obtain a supernatant suspension, the suspension is heated to a constant temperature of 75-90°C and maintained for 2 h, then vacuum filtered and washed twice, and finally dried at 50°C for 12-30 h to obtain purified lignin powder.

[0020] Preferably, in the preparation process of the formaldehyde-free coating adhesive in step S22, 15-40 parts of purified lignin powder are dissolved in a stirring container filled with sodium hydroxide, and glyoxal is gradually added during stirring, the mass fraction of glyoxal is 60-85 parts, and lignin glyoxal is obtained after mixing evenly; in the preparation of the formaldehyde-free coating adhesive, lignin glyoxal is 40-60 parts, and the rest is PMDI.

[0021] The advantage of the present invention is that glyoxal is the simplest dialdehyde with two adjacent carbon groups. Formaldehyde is classified as a carcinogenic, mutagenic and re-toxic substance by ECHA (European Chemical Agency), and the measured LD value is 500-800 mg / kg, which is one order of magnitude lower than glyoxal (2960-8979 mg / kg). In addition, there are multiple ways to produce glyoxal from bio-based raw materials or intermediates, including sugars, ethanol and ethylene glycol. In addition, glyoxal, as a non-volatile, biodegradable and low-cost monomer, has been proven to be a suitable substitute for formaldehyde. By mixing lignin-glyoxal resin with 10-60% PMDI, the synthesized adhesive has sufficient internal bonding strength required for various grades of wood board applications, and also avoids the emission of formaldehyde pollutants.

[0022] Preferably, in the process of preparing the PET film layer in step S3, the mass fraction of ethylene terephthalate particles, ie, PET fine powder particles, is 75-95 parts, and the mass fraction of nano-titanium dioxide is 5-25 parts.

[0023] The advantage of the present invention is that nano titanium dioxide is combined with the PET film. When light shines through the surface layer onto the PET film layer, under suitable air humidity, the PET film layer generates radiation waves that assist in the decomposition of formaldehyde and other molecular structures, further improving the effect of purifying formaldehyde.

[0024] Preferably, during the paint coating process of the cabinet door panel in step S4, the multi-layer specific structure of the cabinet door panel is that the core panel is coated with an adhesive layer, a photocatalyst medium PET film layer, and an EB-cured formaldehyde purification layer in sequence. After the surface coating is applied, the entire system is placed in a nitrogen environment of more than 99.9% for electron beam curing.

[0025] Preferably, a hole is provided at the connection between the core plate and the adhesive layer, porous alumina is arranged in the hole, and the thickness of the core plate is 10-18 mm.

[0026] Preferably, the coating amount of the adhesive layer is 20-50 g / m 2 The thickness of the photocatalyst medium PET film layer is 0.10-0.30 mm, and the coating amount of the EB curing formaldehyde purification layer is 10-30 g / m 2 .

[0027] The advantage of adopting the present invention is that through the multi-layer bonding structure of the cabinet door panel, the surface layer is reinforced with formaldehyde purification and EB-cured formaldehyde purification layer, the obtained cabinet door panel can be more solid, and the surface is endowed with high surface properties such as formaldehyde purification and scratch resistance and fingerprint resistance.

[0028] The advantage of adopting the present invention is that holes 11 are provided on the core board 1, and the gaps generated when the base materials are glued can be filled with porous alumina 12 to ensure the strength of the board. The porous alumina 12 is applied to the board to absorb moisture or reducing substances in the environment through the pores of the board, thereby achieving the effect of regulating the dryness and humidity of the air.

[0029] The invention has the advantage that the purifier uses chitin and nano silicon wafers, which can effectively eliminate free formaldehyde in the ambient air; the strong negative electric field of the nano silicon wafer can adsorb small molecules such as formaldehyde, and the active amino groups in the chitin quickly decompose the formaldehyde into water molecules, thereby ensuring the effective purification rate of formaldehyde.

[0030] In summary, the present invention has the following beneficial effects:

[0031] 1. Through the addition of chitosan, nano-silicon powder, alumina and boric acid powder in the formaldehyde purification and enhanced modified additive coating formula, under the radiation of EB high-energy electron beam, the formaldehyde purification and wear resistance, corrosion resistance, high hardness, anti-fouling, impact resistance, anti-yellowing, anti-fingerprint and other properties of home cabinet door panels can be greatly improved, and the process remains green and environmentally friendly;

[0032] 2. The design of the core board and formaldehyde-free coating adhesive gives the coating high strength and formaldehyde-free release effect, providing basic support for the product's formaldehyde purification performance and high surface performance of EB curing; the designed photocatalyst PET film, under suitable air humidity, the radiation waves generated by the PET film layer have an auxiliary decomposition effect on formaldehyde and other molecular structures, further improving the effect of formaldehyde purification;

[0033] 3. The formaldehyde-purified EB-cured PET facing cabinet door panel prepared by the scheme of the present invention is ecologically pollution-free, has a suitable production cost, a simple process, and can be mass-produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] FIG1 is a schematic structural diagram of a formaldehyde-purified EB-cured PET facing cabinet door panel;

[0035] FIG2 is a schematic diagram of the structure of a core board of a formaldehyde-purified EB-cured PET facing cabinet door board;

[0036] FIG3 is an enlarged schematic diagram of point A in the core plate structure;

[0037] Among them, 1. core board; 11. holes; 12. porous alumina; 2. bonding layer; 3. photocatalyst medium PET film layer; 4. EB curing formaldehyde purification layer. DETAILED DESCRIPTION

[0038] The following specific embodiments are merely explanations of the present invention and are not limitations of the present invention. After reading this specification, those skilled in the art may make modifications to the embodiments without any creative contribution as needed. However, such modifications are protected by the patent law as long as they are within the scope of the claims of the present invention. Example 1

[0039] Step S1 Preparation of electron beam cured formaldehyde purification coating paint: a certain amount of EB electron beam curing enhancement modifier fine powder is mixed and stirred evenly in a mixed solution of 40°C acrylic emulsion and aqueous polyurethane emulsion at a constant temperature, and the material particles are evenly dispersed and stored for later use. The main components of the EB electron beam curing enhancement modifier are chitosan, nano-silicon powder, alumina and boric acid or borax powder; during the production process, 3 parts of chitosan, 1 part of nano-silicon powder, 1 part of alumina powder, and 1 part of boric acid or borax powder are mixed evenly for later use, and the above-mentioned mixed fine powder is gradually added to the mixed emulsion of acrylic acid and aqueous polyurethane and heated and stirred evenly.

[0040] Step S21 lignin purification: dissolve the lignin cake in the sodium hydroxide solution and stir to mix evenly. During the lignin purification process, the dissolved mass volume concentration of the lignin cake and the sodium hydroxide solution is 80 g / L, and the concentration of sodium hydroxide is 1 mol / L. After mixing and stirring, centrifuge at 4000 rpm for 5 min to obtain a supernatant suspension. The pH of the supernatant is adjusted with dilute sulfuric acid. The suspension is heated to 75°C and kept at a constant temperature for 2 hours, then vacuum filtered and washed twice, and finally dried at 50°C for 12 hours to obtain purified lignin powder;

[0041] Step S22 preparation of formaldehyde-free coating adhesive: dissolve 15 parts of the purified lignin mentioned above in a stirring container filled with 1M sodium hydroxide, stir and heat to a constant temperature, gradually add glyoxal, the mass fraction of glyoxal is 85 parts, mix and stir, and after the reaction is completed, cool to obtain lignin glyoxal, stir the obtained lignin glyoxal with polymer 4,4 / -diphenylmethane diisocyanate pMDI to obtain a formaldehyde-free coating adhesive, and after mixing evenly, obtain lignin glyoxal, of which lignin glyoxal is 40 parts and the rest is pMDI.

[0042] Step S3 Preparation of photocatalyst medium PET film layer: polyethylene terephthalate particles, i.e. PET fine powder particles, are melted and mixed with a proper amount of nano titanium dioxide, and then extruded and cooled to form a PET film layer; wherein the mass fraction of PET fine powder particles is 75 parts, and the mass fraction of nano titanium dioxide is 25 parts.

[0043] Step S4: coating of cabinet door panels: the cabinet door panels are multi-layer structures, and the coated multi-layer structures include a bonding layer outside the core panel, a photocatalyst medium PET film layer and an EB-cured formaldehyde purification layer; the bonding layer adopts the formaldehyde-free coating adhesive prepared in step S2, and the EB-cured formaldehyde purification layer adopts the formaldehyde-purifying electron beam-cured coating prepared in step S1; during the coating of the door panel coating, the multi-layer structure of the cabinet door panel is specifically that the bonding layer 2, the photocatalyst medium PET film layer 3, the bonding layer 2 and the EB-cured formaldehyde purification layer 4 are sequentially coated on the core panel 1, and after the EB-cured formaldehyde purification layer 4 is coated, the whole system is placed in a nitrogen N2 environment of more than 99.9% for electron beam curing; a hole 11 is provided at the top of the connection between the core panel 1 and the bonding layer 2, and a porous aluminum oxide 12 is arranged in the hole 11, and the thickness of the core panel is 10 mm; the coating amount of the bonding layer is 20 g / m 2 The thickness of the photocatalyst medium PET film layer is 0.10mm, and the coating amount of the EB curing formaldehyde purification layer is 10g / m 2 . Example 2

[0044] Step S1 Preparation of electron beam cured formaldehyde purification coating paint: a certain amount of EB electron beam curing enhancement modifier fine powder is mixed and stirred evenly in a mixed solution of 60°C acrylic emulsion and aqueous polyurethane emulsion at a constant temperature, and the material particles are evenly dispersed and stored for later use. The main components of the EB electron beam curing enhancement modifier are chitin, nano silicon powder, alumina and boric acid or borax powder; during the production process, 10 parts of chitosan, 5 parts of nano silicon powder, 3 parts of alumina powder, and 5 parts of boric acid or borax powder are mixed evenly for later use, and the above-mentioned mixed fine powder is gradually added to the mixed emulsion of acrylic acid and aqueous polyurethane and heated and stirred evenly.

[0045] Step S21 lignin purification: dissolve the lignin cake in the sodium hydroxide solution and stir to mix evenly. During the purification of lignin, the dissolved mass volume concentration of the lignin cake and the sodium hydroxide solution is 150 g / L, and the concentration of sodium hydroxide is 1 mol / L. After mixing and stirring, centrifuge at 4500 rpm for 5 min to obtain a supernatant suspension. The pH of the supernatant is adjusted with dilute sulfuric acid. The suspension is heated to 90°C and kept at a constant temperature for 2 hours, then vacuum filtered and washed twice, and finally dried at 50°C for 30 hours to obtain purified lignin powder;

[0046] Step S22 preparation of formaldehyde-free coating adhesive: dissolve 40 parts of the purified lignin mentioned above in a stirring container filled with 1M sodium hydroxide, stir and heat to a constant temperature, gradually add glyoxal, the mass fraction of glyoxal is 60 parts, mix and stir, and after the reaction is completed, cool to obtain lignin glyoxal, stir the obtained lignin glyoxal with polymer 4,4 / -diphenylmethane diisocyanate pMDI to obtain a formaldehyde-free coating adhesive, and after mixing evenly, obtain lignin glyoxal, of which lignin glyoxal is 60 parts and the rest is pMDI.

[0047] Step S3 Preparation of photocatalyst medium PET film layer: polyethylene terephthalate particles, i.e. PET fine powder particles, are melted and mixed with a proper amount of nano titanium dioxide, and then extruded and cooled to form a PET film layer; wherein the mass fraction of PET fine powder particles is 95 parts, and the mass fraction of nano titanium dioxide is 5 parts.

[0048] Step S4: coating of cabinet door panels: the cabinet door panels are multi-layer structures, and the coated multi-layer structures include a bonding layer outside the core panel, a photocatalyst medium PET film layer and an EB-cured formaldehyde purification layer; the bonding layer adopts the formaldehyde-free coating adhesive prepared in step S2, and the EB-cured formaldehyde purification layer adopts the formaldehyde-purifying electron beam-cured coating prepared in step S1; during the coating of the door panel coating, the multi-layer structure of the cabinet door panel is specifically that the bonding layer 2, the photocatalyst medium PET film layer 3, the bonding layer 2 and the EB-cured formaldehyde purification layer 4 are sequentially coated on the core panel 1, and after the EB-cured formaldehyde purification layer 4 is coated, the entire system is placed in a nitrogen N2 environment of more than 99.9% for electron beam curing; a hole 11 is provided at the top of the connection between the core panel 1 and the bonding layer 2, and a porous aluminum oxide 12 is arranged in the hole 11, and the thickness of the core panel is 18 mm; the coating amount of the bonding layer is 50 g / m 2 The thickness of the photocatalyst medium PET film layer is 0.30mm, and the coating amount of the EB curing formaldehyde purification layer is 30g / m 2 . Example 3

[0049] Step S1 Preparation of electron beam cured formaldehyde purification coating paint: a certain amount of EB electron beam curing enhancement modifier fine powder is mixed and stirred evenly in a mixed solution of 50°C acrylic emulsion and aqueous polyurethane emulsion at a constant temperature, and the material particles are evenly dispersed and stored for later use. The main components of the EB electron beam curing enhancement modifier are chitin, nano silicon powder, alumina and boric acid or borax powder; during the production process, 6.5 parts of chitin, 4 parts of nano silicon powder, 1.5 parts of alumina powder, and 3.2 parts of boric acid or borax powder are mixed evenly for later use, and the above mixed fine powder is gradually added to the acrylic acid and aqueous polyurethane mixed emulsion and heated and stirred evenly.

[0050] Step S21 lignin purification: dissolve the lignin cake in the sodium hydroxide solution and stir to mix evenly. During the lignin purification process, the dissolved mass volume concentration of the lignin cake and the sodium hydroxide solution is 100 g / L, and the concentration of sodium hydroxide is 1 mol / L. After mixing and stirring, centrifuge at 4500 rpm for 5 min to obtain a supernatant suspension. The pH of the supernatant is adjusted with dilute sulfuric acid. The suspension is heated to 80°C and kept at a constant temperature for 2 hours, then vacuum filtered and washed twice, and finally dried at 50°C for 24 hours to obtain purified lignin powder;

[0051] Step S22 preparation of formaldehyde-free coating adhesive: dissolve 30 parts of the above-mentioned purified lignin in a stirring container filled with 1M sodium hydroxide, stir and heat to a constant temperature, gradually add glyoxal, the mass fraction of glyoxal is 70 parts, mix and stir, and after the reaction is completed, cool to obtain lignin glyoxal, stir the obtained lignin glyoxal with polymer 4,4 / -diphenylmethane diisocyanate pMDI to obtain a formaldehyde-free coating adhesive, and after mixing evenly, obtain lignin glyoxal, of which lignin glyoxal is 48 parts and the rest is pMDI.

[0052] Step S3: Preparation of photocatalyst medium PET film layer: polyethylene terephthalate particles, i.e. PET fine powder particles, are melted and mixed with a proper amount of nano titanium dioxide, and then extruded and cooled to form a PET film layer; wherein the mass fraction of PET fine powder particles is 85 parts, and the mass fraction of nano titanium dioxide is 15 parts.

[0053] Step S4: coating of cabinet door panels: the cabinet door panels are multi-layer structures, and the coated multi-layer structures include a bonding layer outside the core panel, a photocatalyst medium PET film layer and an EB-cured formaldehyde purification layer; the bonding layer adopts the formaldehyde-free coating adhesive prepared in step S2, and the EB-cured formaldehyde purification layer adopts the formaldehyde-purifying electron beam-cured coating prepared in step S1; during the coating of the door panel coating, the multi-layer structure of the cabinet door panel is specifically that the bonding layer 2, the photocatalyst medium PET film layer 3, the bonding layer 2 and the EB-cured formaldehyde purification layer 4 are sequentially coated on the core panel 1, and after the EB-cured formaldehyde purification layer 4 is coated, the whole system is placed in a nitrogen N2 environment of more than 99.9% for electron beam curing; a hole 11 is provided at the top of the connection between the core panel 1 and the bonding layer 2, and a porous aluminum oxide 12 is arranged in the hole 11, and the thickness of the core panel is 15 mm; the coating amount of the bonding layer is 38 g / m 2 The thickness of the photocatalyst medium PET film layer is 0.20mm, and the coating amount of the EB curing formaldehyde purification layer is 18.5g / m 2 . Example 4

[0054] Step S1 Preparation of electron beam cured formaldehyde purification coating paint: a certain amount of EB electron beam curing enhancement modifier fine powder is mixed and stirred evenly in a mixed solution of 50°C acrylic emulsion and aqueous polyurethane emulsion at a constant temperature, and the material particles are evenly dispersed and stored for later use. The main components of the EB electron beam curing enhancement modifier are chitin, nano-silicon powder, alumina and boric acid or borax powder; during the production process, 5 parts of chitosan, 3 parts of nano-silicon powder, 2.8 parts of alumina powder, and 3 parts of boric acid or borax powder are mixed evenly for later use, and the above-mentioned mixed fine powder is gradually added to the mixed emulsion of acrylic acid and aqueous polyurethane and heated and stirred evenly.

[0055] Step S21 lignin purification: dissolve the lignin cake in the sodium hydroxide solution and stir to mix evenly. During the lignin purification process, the dissolved mass volume concentration of the lignin cake and the sodium hydroxide solution is 110 g / L, and the concentration of sodium hydroxide is 1 mol / L. After mixing and stirring, centrifuge at 4500 rpm for 5 min to obtain a supernatant suspension. The pH of the supernatant is adjusted with dilute sulfuric acid. The suspension is heated to 80°C and kept at a constant temperature for 2 hours, then vacuum filtered and washed twice, and finally dried at 50°C for 18 hours to obtain purified lignin powder;

[0056] Step S22 preparation of formaldehyde-free coating adhesive: dissolve 25 parts of the purified lignin mentioned above in a stirring container filled with 1M sodium hydroxide, stir and heat to a constant temperature, gradually add glyoxal, the mass fraction of glyoxal is 75 parts, mix and stir, and after the reaction is completed, cool to obtain lignin glyoxal, stir the obtained lignin glyoxal with polymer 4,4 / -diphenylmethane diisocyanate pMDI to obtain a formaldehyde-free coating adhesive, and after mixing evenly, obtain lignin glyoxal, of which lignin glyoxal is 45 parts and the rest is pMDI.

[0057] Step S3 Preparation of photocatalyst medium PET film layer: polyethylene terephthalate particles, i.e. PET fine powder particles, are melted and mixed with a proper amount of nano titanium dioxide, and then extruded and cooled to form a PET film layer; wherein the mass fraction of PET fine powder particles is 75 parts, and the mass fraction of nano titanium dioxide is 25 parts.

[0058] Step S4: coating of cabinet door panels: the cabinet door panels are multi-layer structures, and the coated multi-layer structures include a bonding layer outside the core panel, a photocatalyst medium PET film layer and an EB-cured formaldehyde purification layer; the bonding layer adopts the formaldehyde-free coating adhesive prepared in step S2, and the EB-cured formaldehyde purification layer adopts the formaldehyde-purifying electron beam-cured coating prepared in step S1; during the coating of the door panel coating, the multi-layer structure of the cabinet door panel is specifically that the bonding layer 2, the photocatalyst medium PET film layer 3, the bonding layer 2 and the EB-cured formaldehyde purification layer 4 are sequentially coated on the core panel 1, and after the EB-cured formaldehyde purification layer 4 is coated, the entire system is placed in a nitrogen N2 environment of more than 99.9% for electron beam curing; a hole 11 is provided at the top of the connection between the core panel 1 and the bonding layer 2, and a porous aluminum oxide 12 is arranged in the hole 11, and the thickness of the core panel is 14 mm; the coating amount of the bonding layer is 40 g / m 2 The thickness of the photocatalyst medium PET film layer is 0.19mm, and the coating amount of the EB curing formaldehyde purification layer is 25g / m 2 . Example 5

[0059] Step S1 Preparation of electron beam cured formaldehyde purification coating paint: a certain amount of EB electron beam curing enhancement modifier fine powder is mixed and stirred evenly in a mixed solution of 50°C acrylic emulsion and aqueous polyurethane emulsion at a constant temperature, and the material particles are evenly dispersed and stored for later use. The main components of the EB electron beam curing enhancement modifier are chitin, nano silicon powder, alumina and boric acid or borax powder; during the production process, 8.8 parts of chitin, 4 parts of nano silicon powder, 2 parts of alumina powder, and 2.5 parts of boric acid or borax powder are mixed evenly for later use, and the above mixed fine powder is gradually added to the acrylic acid and aqueous polyurethane mixed emulsion and heated and stirred evenly.

[0060] Step S21 lignin purification: dissolve the lignin cake in the sodium hydroxide solution and stir to mix evenly. During the purification of lignin, the dissolved mass volume concentration of the lignin cake and the sodium hydroxide solution is 120 g / L, and the concentration of sodium hydroxide is 1 mol / L. After mixing and stirring, centrifuge at 4500 rpm for 5 min to obtain a supernatant suspension. The pH of the supernatant is adjusted with dilute sulfuric acid. The suspension is heated to 85°C and kept at a constant temperature for 2 hours, then vacuum filtered and washed twice, and finally dried at 50°C for 22 hours to obtain purified lignin powder;

[0061] Step S22 preparation of formaldehyde-free coating adhesive: dissolve 27 parts of the above-mentioned purified lignin in a stirring container filled with 1M sodium hydroxide, stir and heat to a constant temperature, gradually add glyoxal, the mass fraction of glyoxal is 73 parts, mix and stir, and after the reaction is completed, cool to obtain lignin glyoxal, stir the obtained lignin glyoxal with polymer 4,4 / -diphenylmethane diisocyanate pMDI to obtain a formaldehyde-free coating adhesive, and after mixing evenly, obtain lignin glyoxal, of which lignin glyoxal is 50 parts and the rest is pMDI.

[0062] Step S3 Preparation of photocatalyst medium PET film layer: polyethylene terephthalate particles, i.e. PET fine powder particles, are melted and mixed with a proper amount of nano titanium dioxide, and then extruded and cooled to form a PET film layer; wherein the mass fraction of PET fine powder particles is 80 parts, and the mass fraction of nano titanium dioxide is 20 parts.

[0063] Step S4: coating of cabinet door panels: the cabinet door panels are multi-layer structures, and the coated multi-layer structures include a bonding layer outside the core panel, a photocatalyst medium PET film layer and an EB-cured formaldehyde purification layer; the bonding layer adopts the formaldehyde-free coating adhesive prepared in step S2, and the EB-cured formaldehyde purification layer adopts the formaldehyde-purifying electron beam-cured coating prepared in step S1; during the coating of the door panel coating, the multi-layer structure of the cabinet door panel is specifically that the bonding layer 2, the photocatalyst medium PET film layer 3, the bonding layer 2 and the EB-cured formaldehyde purification layer 4 are sequentially coated on the core panel 1, and after the EB-cured formaldehyde purification layer 4 is coated, the whole system is placed in a nitrogen N2 environment of more than 99.9% for electron beam curing; a hole 11 is provided at the top of the connection between the core panel 1 and the bonding layer 2, and a porous aluminum oxide 12 is arranged in the hole 11, and the thickness of the core panel is 14 mm; the coating amount of the bonding layer is 29 g / m 2 The thickness of the photocatalyst medium PET film layer is 0.15mm, and the coating amount of the EB curing formaldehyde purification layer is 19g / m 2 . Comparative Example 1

[0064] Different from the embodiment, the cabinet door panel of this comparative example is coated with only one adhesive layer and a PET film layer, and the PET film layer does not contain nano-grade titanium dioxide. Specific parameters are:

[0065] Step S11 lignin purification: dissolve the lignin cake in the sodium hydroxide solution and stir to mix evenly. During the lignin purification process, the dissolved mass volume concentration of the lignin cake and the sodium hydroxide solution is 100 g / L, and the concentration of sodium hydroxide is 1 mol / L. After mixing and stirring, centrifuge at 4500 rpm for 5 min to obtain a supernatant suspension. The pH of the supernatant is adjusted with dilute sulfuric acid. The suspension is heated to 80°C and kept at a constant temperature for 2 hours, then vacuum filtered and washed twice, and finally dried at 50°C for 24 hours to obtain purified lignin powder;

[0066] Step S12 preparation of formaldehyde-free coating adhesive: dissolve 30 parts of the purified lignin mentioned above in a stirring container filled with 1M sodium hydroxide, stir and heat to a constant temperature, gradually add glyoxal, the mass fraction of glyoxal is 70 parts, mix and stir, and after the reaction is completed, cool to obtain lignin glyoxal, stir the obtained lignin glyoxal with polymer 4,4 / -diphenylmethane diisocyanate pMDI to obtain a formaldehyde-free coating adhesive, and after mixing evenly, obtain lignin glyoxal, of which lignin glyoxal is 48 parts and the rest is pMDI.

[0067] Step S2: Apply the adhesive layer on the cabinet door panel: Apply the adhesive on the base core panel 1 with a coating amount of 34 g / m 2 ; The structure of the core plate 1 is the same as that in the above embodiment. Comparative Example 2

[0068] Different from the embodiment, this comparative example is a conventional cabinet door panel on the market, which has neither an EB-cured formaldehyde purification layer nor a photocatalyst medium layer, and the gluing method and materials are also different from those in the embodiment.

[0069] The cabinet door panels obtained in the above-mentioned embodiments and comparative examples were subjected to hardness test, surface wear resistance test, yellowing resistance test and formaldehyde emission level evaluation.

[0070] The hardness test method is to use a Mitsubishi test pencil of specified 1H, sharpen the pencil until the cylindrical lead core is exposed for about 3mm (be careful not to damage the lead core), hold the pencil at a 90-degree angle to the 400-grit paper, and keep circling on the sandpaper to rub the end face of the lead core until the end face is flat and the edge of the lead core is sharp. Install it on a special pencil hardness tester, apply a load of 500gf to the tip of the pencil, and the front end of the pencil core contacts the surface to be tested. The angle between the pencil core and the surface to be tested is 45°. Push the pencil forward at a speed of 0.5mm / s~lmm / s for about 5m (try to test on the sample surface when the sample length is less than 5m), draw 5 lines in total, and rotate the pencil about 60° for each line. After the test is completed, use an eraser to erase the black pencil scratches on the paint coating surface and compare them with the test sample. The judgment standard is that no indentation or scratches are allowed on the outer surface, and indentations that can be restored within 24 hours are not judged. Problem: small scratches at the starting position (1 / 5 of the total length) are allowed.

[0071] The method of wear test is to use a special wear tester and a special paper tape produced by the manufacturer, apply a load of 175g, and drive the paper tape to rub the surface of the sample for a specified number of consecutive turns. This test must be carried out in a room with a humidity of 40% to 60%. The paper tape is stored in an environment of 40% ± 5% humidity and 24℃ ± 2℃. Put the paper tape into the paper supply wheel of the wear tester, and be careful not to put the paper tape upside down; the paper tape is only rubbed once with the inner surface, and it needs to be stored in a drying oven if it is not used for more than 4 hours: install and fix the sample, keep it parallel to the horizontal plane, and the sample tested area cannot be suspended, and ensure that there is a physical object filled inside: adjust the balance bar so that the gravity pressed on the surface of the oil coating is exactly 175g, and rub 250 times. The judgment standard is to observe with a magnifying glass, and it is passed if the substrate is not exposed.

[0072] The yellowing resistance test method is to use an ultraviolet light source to irradiate the sample for 200 hours of continuous illumination. The judgment level is divided into 1-5 levels. Level 1 means that under the specified test conditions, the color of the material is almost unchanged, maintaining the original color, and has extremely high yellowing resistance; Level 2 means that the color of the material changes slightly during the test, but the change is minor and has little impact on the overall aesthetics; Level 3 means that under the test conditions, the color of the material changes significantly, but it can still maintain a certain aesthetics; Level 4 means that the color of the material changes significantly after the test, which has a great impact on the aesthetics, but it can still be used; Level 5 means that the color of the material changes very seriously after the test, which seriously affects the aesthetics and use value, and it is almost impossible to continue to use.

[0073] The formaldehyde emission level evaluation method is E 1 、E 0 、E NF Level, among which E NF The best level, formaldehyde release limit ≤ 0.025mg / m 3 .

[0074] In addition, the anti-fingerprint performance of the door panels was visually observed by pressing the sample surface with fingers to ensure that the fingerprints were clearly visible. The fingerprints were carefully observed, and the number, shape and depth of fingerprints were recorded. The sample surface was scored based on the number of fingerprints on a scale of 1-10, with higher scores indicating worse anti-fingerprint performance.

[0075]

[0076] Regarding formaldehyde release, the formaldehyde release of Examples 1-5 is less than 0.015 mg / m 3 , reaching E NFThe test conditions of Example 3 can be used to obtain the EB-cured PET decorative cabinet door panel with the best performance, and the other example samples have excellent anti-scratch hardness, anti-fingerprint, anti-yellowing, anti-fouling, wear-resistant, corrosion-resistant and formaldehyde purification performance, which can well meet the performance requirements of cabinet panels in daily life and people's demands for home health and safety.

Claims

1. A process for producing a formaldehyde-purified EB-cured PET facing cabinet door panel, characterized in that The process steps include: Step S1 Preparation of electron beam cured formaldehyde purification coating: Add a certain amount of EB electron beam cured formaldehyde purification and enhancement modifier fine powder into a mixed solution of acrylic emulsion and waterborne polyurethane emulsion at 40-60° C., mix and stir evenly at a constant temperature, and store and reserve after the material particles are evenly dispersed; Step S2 Formaldehyde-free coating adhesive preparation: S21 lignin purification: dissolve the lignin cake in sodium hydroxide solution, stir and mix evenly, extract the supernatant by centrifugation, adjust the pH value of the supernatant with dilute sulfuric acid, and then filter, wash and dry to obtain lignin powder; S22 Preparation of formaldehyde-free coating adhesive: dissolving the purified lignin in sodium hydroxide solution, stirring and heating to a constant temperature, adding glyoxal, cooling after the reaction is completed to obtain lignin glyoxal, stirring and mixing the obtained lignin glyoxal with polymer 4,4'-diphenylmethane diisocyanate PMDI to obtain a formaldehyde-free coating adhesive; Step S3: Preparation of the photocatalyst medium PET film layer: polyethylene terephthalate particles, i.e. PET fine powder particles, are melted, mixed with a proper amount of nano titanium dioxide, and then extruded and cooled to form a PET film layer; Step S4: coating the cabinet door panel: the cabinet door panel is a multi-layer structure, and the coated multi-layer structure includes a bonding layer outside the core board, a photocatalyst medium PET film layer and an EB-cured formaldehyde purification layer; the bonding layer adopts the formaldehyde-free coating adhesive prepared in step S2, and the EB-cured formaldehyde purification layer adopts the formaldehyde-purifying electron beam-cured coating prepared in step S1; The main components of the EB electron beam curing formaldehyde purification and enhancement modifier in step S1 are chitin, nano silicon powder, aluminum oxide and boric acid or borax powder; during the production process, 3-10 parts of chitin, 1-5 parts of nano silicon powder, 1-3 parts of aluminum oxide powder, and 1-5 parts of boric acid or borax powder are mixed evenly for later use, and the mixed fine powder is gradually added to the acrylic acid and waterborne polyurethane mixed emulsion and heated and stirred evenly; In step S4, during the coating process of the cabinet door panel, the multi-layer structure of the cabinet door panel specifically comprises a core panel (1) coated with an adhesive layer (2), a photocatalytic medium PET film layer (3), and an EB-cured formaldehyde purification layer (4) in sequence; After the EB-cured formaldehyde purification layer (4) coating is applied, the entire system is placed in a nitrogen environment with a nitrogen content of more than 99.9% for electron beam curing.

2. The manufacturing process of a formaldehyde-purified EB-cured PET facing cabinet door panel according to claim 1, characterized in that: In the process of lignin purification in step S21, the dissolved mass volume concentration of lignin cake and sodium hydroxide solution is 80-150g / L, the concentration of sodium hydroxide is 1mol / L, the mixture is stirred and centrifuged, and the supernatant suspension is obtained by centrifugation at 4000-4500rpm for 5min. The suspension is heated to 75-90℃ and kept at a constant temperature for 2h, then vacuum filtered and washed twice, and finally dried at 50℃ After 12-30 hours, purified lignin powder is obtained.

3. The manufacturing process of a formaldehyde-purified EB-cured PET facing cabinet door panel according to claim 2, characterized in that: In the preparation process of the formaldehyde-free coating adhesive in step S22, 15-40 parts of purified lignin powder are dissolved in a stirring container filled with sodium hydroxide, and glyoxal is gradually added during stirring, the mass fraction of glyoxal is 60-85 parts, and lignin glyoxal is obtained after mixing evenly; in the preparation of the formaldehyde-free coating adhesive, lignin glyoxal is 40-60 parts, and the rest is PMDI.

4. The manufacturing process of a formaldehyde-purified EB-cured PET facing cabinet door panel according to claim 1, characterized in that: In the preparation process of the PET film layer in step S3, the mass fraction of ethylene terephthalate particles, i.e., PET fine powder particles, is 75-95 parts, and the mass fraction of nano-titanium dioxide is 5-25 parts.

5. The manufacturing process of a formaldehyde-purified EB-cured PET facing cabinet door panel according to claim 4, characterized in that: A hole (11) is provided at the connection between the core plate (1) and the adhesive layer (2), and porous aluminum oxide (12) is arranged in the hole (11). The thickness of the core plate is 10-18 mm.

6. The manufacturing process of a formaldehyde-purified EB-cured PET facing cabinet door panel according to claim 5, characterized in that: The coating amount of the adhesive layer is 20-50 g / ㎡, the thickness of the photocatalyst medium PET film layer is 0.10-0.30 mm, and the coating amount of the EB-cured formaldehyde purification layer is 10-30 g / ㎡.