Photosensitive resin composition, photosensitive resin film and pattern forming method

By using the polymer of general formula (c) as a thermal cross-linking agent and an alkali-soluble polyimide precursor in the photosensitive resin, combined with a photoacid generator, the problem in the existing technology that the photosensitive resin is difficult to simultaneously improve chemical resistance is solved. Solve the problems of sensitivity and sensitivity, and achieve a photosensitive resin composition with high sensitivity and low stress, which is suitable for surface protection and insulating layers of semiconductor devices.

CN111812943BActive Publication Date: 2024-10-11WUHAN ROUXIAN SCIENCE & TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010788700.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-07
Publication Date
2024-10-11
Estimated Expiration
2040-08-07

AI Technical Summary

Technical Problem

It is difficult for existing photosensitive resins to maintain high sensitivity and low stress while improving chemical resistance and mechanical properties, especially as the demand for patterning and fine processing in semiconductor device manufacturing increases and the use of small molecule cross-linking agents Limits its exposure sensitivity and chemical resistance.

Method used

A polymer with general formula (c) is used as a thermal cross-linking agent, combined with an alkali-soluble polyimide precursor and a photoacid generator to form a highly sensitive photosensitive resin composition. Through the cross-linking structure of the thermal cross-linking agent and alkali The imide ring structure of the soluble resin improves the chemical resistance and low-stress characteristics of the film, and improves exposure sensitivity through an appropriate amount of photoacid generator.

Benefits of technology

It can significantly improve the exposure sensitivity of photosensitive resin while improving chemical resistance and low stress, and provides excellent light transmittance and mechanical properties. It is suitable for surface protective films of semiconductor components and insulation of organic electroluminescent components. layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111812943B_ABST
    Figure CN111812943B_ABST
Patent Text Reader

Abstract

The present invention discloses a photosensitive resin composition, a photosensitive resin film and a pattern forming method. The photosensitive resin composition comprises an alkali-soluble resin, a photoacid generator and a thermal crosslinking agent. The alkali-soluble resin of the present invention mainly comprises an alkali-soluble polyimide precursor represented by the general formula (a). The alkali-soluble resin can form a polymer having an imide ring or other cyclic structure by heating or catalysis. When the alkali-soluble resin is combined with a polymer represented by the general formula (c) as a thermal crosslinking agent, the sensitivity can be improved while improving the heat resistance and chemical resistance of the cured film, and the film has excellent properties such as low stress. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to a photosensitive resin composition, a photosensitive resin film and a pattern forming method, which are suitable for surface protection films of semiconductor elements, interlayer insulating films, insulating films of organic electroluminescent elements, etc. Background Art

[0002] Since polyimide resin not only has excellent heat resistance and insulation, but also has low stress and high elongation after film formation, it is widely used in surface protection films of semiconductor components, interlayer insulation films, insulation layers of organic electroluminescent components, etc. However, with the continuous improvement of the requirements of the semiconductor industry, the requirements for patterned fine processing of protection films, insulation films, planarization films, etc. are also constantly increasing.

[0003] Since semiconductor device manufacturing processes involve many steps and organic solvents are frequently used, photosensitive resins are required to have high chemical resistance and mechanical properties in addition to sensitivity. The introduction of flexible groups into the polyimide backbone can reduce the stress of the cured film, but there is a disadvantage that it is difficult to give the cured film sufficient mechanical properties.

[0004] On the other hand, the use of crosslinking agents can improve chemical resistance. However, some small molecule crosslinking agents, such as small molecule thermal crosslinking agents with polyalkoxymethyl or hydroxymethyl groups, still have difficulty in giving the cured film sufficient chemical resistance; for example, CN111133382A discloses a photosensitive resin composition, which uses a crosslinking agent containing polyalkoxymethyl or hydroxymethyl groups, but the scheme further limits the thermal crosslinking agent to have phenolic hydroxyl groups, and the hydroxymethyl and / or alkoxymethyl groups are located at the ortho position of the phenolic hydroxyl groups, and the photosensitive resin also introduces a compound with a phenolic hydroxyl group, and the chemical resistance is improved by the reaction of the thermal crosslinking agent with the phenolic hydroxyl compound. On the other hand, some thermal crosslinking agents containing aromatic groups, such as polyphenol epoxy resins, absorb ultraviolet light during the exposure process after being introduced as additives, thereby reducing their exposure sensitivity. Summary of the invention

[0005] The object of the present invention is to provide a highly sensitive photosensitive resin composition, which uses a polymer represented by general formula (c) as a thermal crosslinking agent, and is combined with a suitable alkali-soluble resin and a photoacid generator to improve the chemical resistance of the cured film while improving the sensitivity, and has excellent properties such as low stress.

[0006] Specifically, the alkali-soluble resin of the present invention mainly includes an alkali-soluble polyimide precursor represented by the general formula (a). The alkali-soluble resin can form a polymer having an imide ring or other cyclic structure by heating or catalysis. When combined with a poly(glycidyl acrylate) thermal crosslinking agent, it provides low stress characteristics to the cured film, which not only significantly improves the exposure sensitivity, but also has excellent heat resistance and chemical resistance.

[0007] The first aspect of the present invention provides a photosensitive resin composition, comprising (A) an alkali-soluble resin, wherein the alkali-soluble resin is composed of a repeating unit represented by formula (a):

[0008]

[0009] In formula (a), R 11 and R 12 represents a divalent to hexavalent organic group having 2 to 40 carbon atoms; R1 and R2 represent a hydrogen atom or an organic group having 1 to 20 carbon atoms; m represents an integer in the range of 10 to 100000, and p, q, h, and g represent integers satisfying 0≤p+q+h+g≤4;

[0010] (B) photoacid generator;

[0011] (C) a thermal crosslinking agent, the thermal crosslinking agent comprising a repeating unit represented by formula (c):

[0012]

[0013] In formula (c), R3 represents a hydrogen atom or a monovalent organic group having 1 to 4 carbon atoms, R4 represents a divalent organic group having 1 to 10 carbon atoms; and n represents an integer in the range of 4 to 200.

[0014] Wherein, R of the general formula (a) 11 One or more selected from the following structural formulas:

[0015]

[0016] wherein R is each independently an alkyl group having 1 to 20 carbon atoms, a fluoroalkyl group, an alkoxy group, an ester group, a nitro group, a cyano group or a halogen group; x, y and z are each independently an integer from 0 to 4; A represents a direct bond, -CO-, -CH2-, -C2H4-, -O-, -C3H6-, -C3F6-, -SO2-, -S-, or -Si(CH3)2-; and J represents a direct bond, -COO-, -CONH-, -CH2-, -C2H4-, -O-, -C3H6-, -C3F6-, -SO2-, -S-, -Si(CH3)2-, -OSi(CH3)2O-, -C6H4-, -C6H4-O-C6H4-, -C6H4-C3H6-C6H4-, or -C6H4-C3F6-C6H4-.

[0017] Wherein, R of the general formula (a) 12 Selected from two or more of the following structural formulas:

[0018]

[0019] , and a diamine residue structure having a siloxane structure;

[0020] wherein R is each independently an alkyl group having 1 to 20 carbon atoms, a fluoroalkyl group, an alkoxy group, an ester group, a nitro group, a cyano group or a halogen group; x, y and z are each independently an integer from 0 to 4; B represents a direct bond, -CO-, -CH2-, -C2H4-, -O-, -C3H6-, -C3F6-, -SO2-, -S-, or any one of -Si(CH3)2-; and Z represents a direct bond, -COO-, -CONH-, -CH2-, -C2H4-, -O-, -C3H6-, -C3F6-, -SO2-, -S-, -Si(CH3)2-, -O Si(CH3)2O-, -C6H4-, -C6H4-O-C6H4-, -C6H4-C3H6-C6H4-, or -C6H4-C3F6-C6H4-.

[0021] Among them, R of the general formula (a) 11 and / or R 12 It comprises a structure containing sulfone group substitution, wherein the molar amount of the structural unit containing sulfone group substitution accounts for 5-20% of the total molar amount of the structural unit of the general formula (a).

[0022] Among them, R of the general formula (a) 11 and / or R 12 The fluorine-containing substituted structure comprises a total molar amount of the fluorine-containing substituted structure unit and the sulfone-containing substituted structure unit, which accounts for 40-90% of the total molar amount of the structure unit of the general formula (a).

[0023] The weight average molecular weight of the thermal crosslinking agent is 1000-20000; based on 100 parts by mass of the alkali-soluble resin, the mass of the thermal crosslinking agent is 1-20 parts by mass.

[0024] Wherein, the photoacid generator is a diazonaphthoquinone compound, and based on 100 parts by mass of the alkali-soluble resin, the mass of the photoacid generator is 3-40 parts by mass.

[0025] Wherein, the photoacid generator is selected from one or two of the following structures:

[0026]

[0027] Where Q is hydrogen, And Q is not entirely hydrogen.

[0028] Wherein, the end of the alkali-soluble resin further includes a group represented by formula (e-1) and / or formula (e-2):

[0029] Formula (e-1): -NH-R5, wherein R5 represents a monovalent organic group containing a hydroxyl group, a carboxyl group, a benzenesulfonic acid group, a pyrimidine group, a phenol group or a thiophenol group;

[0030] Formula (e-2): -CO-R6, wherein R6 represents a monovalent organic group containing a carboxyl group, a phenol group, a thiophenol group, a hydroxyl group, a mercapto group, or a benzenesulfonic acid group.

[0031] A second aspect of the present invention provides a photosensitive resin film, which is prepared from the above-mentioned photosensitive resin composition.

[0032] Furthermore, under the condition that the film thickness is 10 μm, the transmittance of i-ray (365 nm wavelength) is ≥91%, the transmittance of h-ray (405 nm wavelength) is ≥93%, and the transmittance of g-ray (436 nm wavelength) is ≥95%, and the minimum exposure required for exposure under these conditions is ≤40 mJ / cm 2 .

[0033] A third aspect of the present invention provides a pattern forming method, which uses the above-mentioned photosensitive resin composition to form a pattern having a resin coating, comprising the following steps:

[0034] Step 1: coating the above-mentioned photosensitive resin composition on a substrate to form a photosensitive resin coating, and then pre-baking on a hot plate at 80-120° C. for 2-60 minutes to form a photosensitive film;

[0035] Step 2: using an exposure mask to expose the photosensitive film;

[0036] Step 3: removing the exposed portion of the photosensitive film with an alkaline developer and developing the film;

[0037] Step 4: Curing the developed film at a temperature of 100° C. to 300° C. to obtain a cured film.

[0038] The photosensitive resin composition and pattern forming method provided by the present invention have the following beneficial effects:

[0039] The high-sensitivity photosensitive resin film composition provided by the present invention uses a polymer represented by general formula (c) as a thermal crosslinking agent, and is combined with a suitable alkali-soluble resin and a photoacid generator. It can improve the sensitivity while giving the cured film excellent properties such as chemical resistance and low stress. In particular, when combined with an alkali-soluble resin containing a sulfone group, it has significantly improved light transmittance and better overall performance. DETAILED DESCRIPTION

[0040] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Photosensitive resin films can be applied to surface protection films of semiconductor elements, interlayer insulating films, insulating films of organic electroluminescent elements, etc., and are mainly prepared from photosensitive resin compositions.

[0042] <Photosensitive resin composition>

[0043] (A) Alkali-soluble resin

[0044] The alkali solubility in the present invention means that it is soluble in alkaline aqueous solutions such as tetramethylammonium hydroxide, choline, triethylamine, dimethylaminopyridine, monoethanolamine, diethylaminoethanol, sodium hydroxide, potassium hydroxide, and sodium carbonate.

[0045] The first aspect of the present invention provides a photosensitive resin composition, comprising (A) an alkali-soluble resin, wherein the alkali-soluble resin is composed of a repeating unit represented by formula (a):

[0046]

[0047] In formula (a), R 11 and R 12 represents a divalent to hexavalent organic group having 2 to 40 carbon atoms; R1 and R2 represent a hydrogen atom or an organic group having 1 to 20 carbon atoms; m represents an integer in the range of 10 to 100,000, and p, q, h, and g represent integers satisfying 0≤p+q+h+g≤4.

[0048] Based on the consideration of the fluidity of the photosensitive resin before film formation and the toughness after film formation, the weight average molecular weight of the alkali-soluble resin of the present invention is preferably in the range of 5000-80000. If the weight average molecular weight of the alkali-soluble resin is higher than 80000, it is not conducive to the coating process of the resin composition. If the weight average molecular weight of the alkali-soluble resin is lower than 5000, it does not have good toughness. The weight average molecular weight of the alkali-soluble resin is preferably in the range of 8000-60000.

[0049] Furthermore, in consideration of the effect of the alkali-soluble resin during development, the value of p+q+h+g is preferably 2 or 4, wherein both p and h are 0.

[0050] R in the formula 11 It can be derived from tetracarboxylic acid, tetracarboxylic dianhydride, tetracarboxylic acid diester dichloride, etc. In the present invention, tetracarboxylic dianhydride is preferred. 11 represents a tetracarboxylic acid residue, and preferred structures of the tetracarboxylic acid residue include the following:

[0051]

[0052] wherein R is each independently an alkyl group having 1 to 20 carbon atoms, a fluoroalkyl group, an alkoxy group, an ester group, a nitro group, a cyano group or a halogen group; x, y and z are each independently an integer from 0 to 4; A represents a direct bond, -CO-, -CH2-, -C2H4-, -O-, -C3H6-, -C3F6-, -SO2-, -S-, or -Si(CH3)2-; and J represents a direct bond, -COO-, -CONH-, -CH2-, -C2H4-, -O-, -C3H6-, -C3F6-, -SO2-, -S-, -Si(CH3)2-, -OSi(CH3)2O-, -C6H4-, -C6H4-O-C6H4-, -C6H4-C3H6-C6H4-, or -C6H4-C3F6-C6H4-.

[0053] Specifically, the following structures can be cited, and some of the hydrogen atoms in these structures can be substituted with an alkyl group having 1 to 20 carbon atoms, a fluoroalkyl group, an alkoxy group, an ester group, a nitro group, a cyano group, a fluorine atom or a chlorine atom:

[0054]

[0055]

[0056] J represents a direct bond, -COO-, -CONH-, -CH2-, -C2H4-, -O-, -C3H6-, -C3F6-, -SO2-, -S-, -Si(CH3)2-, -OSi(CH3)2O-, -C6H4-, -C6H4-O-C6H4-, -C6H4-C3H6-C6H4-, or any one of -C6H4-C3F6-C6H4-.

[0057] R in the formula 12 Preferably it is derived from a diamine. 12 represents a diamine residue, and preferred structures of the diamine residue include the following:

[0058]

[0059] , and a diamine residue structure having a siloxane structure;

[0060] wherein R is each independently an alkyl group having 1 to 20 carbon atoms, a fluoroalkyl group, an alkoxy group, an ester group, a nitro group, a cyano group or a halogen group; x, y and z are each independently an integer from 0 to 4; B represents a direct bond, -CO-, -CH2-, -C2H4-, -O-, -C3H6-, -C3F6-, -SO2-, -S-, or any one of -Si(CH3)2-; and Z represents a direct bond, -COO-, -CONH-, -CH2-, -C2H4-, -O-, -C3H6-, -C3F6-, -SO2-, -S-, -Si(CH3)2-, -O Si(CH3)2O-, -C6H4-, -C6H4-O-C6H4-, -C6H4-C3H6-C6H4-, or -C6H4-C3F6-C6H4-.

[0061] Specifically, the following structures can be cited, and some of the hydrogen atoms in these structures can be substituted with an alkyl group having 1 to 20 carbon atoms, a fluoroalkyl group, an alkoxy group, an ester group, a nitro group, a cyano group, a fluorine atom or a chlorine atom:

[0062]

[0063] Z represents any one of a direct bond, -COO-, -CONH-, -CH2-, -C2H4-, -O-, -C3H6-, -C3F6-, -SO2-, -S-, -Si(CH3)2-, -OSi(CH3)2O-, -C6H4-, -C6H4-O-C6H4-, -C6H4-C3H6-C6H4-, and -C6H4-C3F6-C6H4-.

[0064] Among these, the diamine residue is more preferably a structure containing a sulfone group or a trifluoromethyl group, and specifically may be:

[0065] as well as

[0066]

[0067] Wherein, Z is a sulfone group.

[0068] As a preferred example of the present invention, the diamine preferably uses the following two diamines:

[0069]

[0070] The inventors have found that the thermal crosslinking agent of the present invention is combined with the hydroxyl-containing polyamic acid composed of the two diamines, and the photosensitive resin has high sensitivity and excellent light transmittance, and has high elongation and low stress as well as excellent heat resistance and chemical resistance after film formation.

[0071] In addition, in order to improve the adhesion of the resin to the substrate and the resistance of the resin to oxygen plasma and ultraviolet ozone treatment, a small amount of diamine with a siloxane structure can be added as a diamine component, such as 1,3-bis(3-aminopropyl)tetramethyldisiloxane, 1,3-bis(4-anilino)tetramethyldisiloxane, etc. The molar amount of the diamine is preferably 1-30% of the total molar amount of the diamine. In order to improve the adhesion of the resin to the substrate and the resistance to oxygen plasma and ultraviolet ozone treatment, the content is not less than 1% of the total molar amount of the diamine; considering the solubility of the resin in alkaline aqueous solution, the content is preferably less than 30% of the total molar amount of the diamine.

[0072] Furthermore, as the diamine of the present invention, at least two kinds of the above-mentioned diamines are preferred.

[0073] Through comprehensive research on the sensitivity, transmittance, stress, heat resistance, chemical resistance and other aspects of photosensitive resins, the inventors found that the molar amount of structural units containing sulfone substitution in the anhydride residues and / or diamine residues accounts for 5-20% of the total molar amount of structural units of the general formula (a), which can control the volatile matter during curing to be less, and the sensitivity and transmittance of the resin are the best.

[0074] More preferably, the anhydride residue and / or diamine residue may include a fluorine-containing substituted structure and a sulfone-containing substituted structure at the same time, and the total molar amount of the fluorine-containing substituted structural unit and the sulfone-containing substituted structural unit accounts for 40-90% of the total molar amount of the structural unit of the general formula (a), and the comprehensive performance of the resin is better.

[0075] As can be seen from the above description, the structure represented by the general formula (a) of the present invention is mainly composed of the above-mentioned acid anhydride and diamine structural units. The end of the alkali-soluble resin of the present invention also includes a capping group. By adjusting the type and amount of the capping agent, the dissolution rate of the resin in the alkaline aqueous solution can be easily adjusted.

[0076] The end of the alkali-soluble resin further includes a group represented by formula (e-1) and / or formula (e-2):

[0077] Formula (e-1): -NH-R5, wherein R5 represents a monovalent organic group containing a hydroxyl group, a carboxyl group, a benzenesulfonic acid group, a pyrimidine group, a phenol group or a thiophenol group;

[0078] Formula (e-2): -CO-R6, wherein R6 represents a monovalent organic group containing a carboxyl group, a phenol group, a thiophenol group, a hydroxyl group, a mercapto group, or a benzenesulfonic acid group.

[0079] Preferred examples of the monoamines include the following: 5-amino-8-hydroxyquinoline, 1-hydroxy-7-aminonaphthalene, 1-hydroxy-6-aminonaphthalene, 1-hydroxy-5-aminonaphthalene, 1-hydroxy-4-aminonaphthalene, 2-hydroxy-7-aminonaphthalene, 2-hydroxy-6-aminonaphthalene, 2-hydroxy-5-aminonaphthalene, 2-hydroxy-3-aminonaphthalene, 1-carboxy-7-aminonaphthalene, 1-carboxy-6-aminonaphthalene, 1-carboxy-5-aminonaphthalene, 2-carboxy-7-aminonaphthalene, 2-carboxy-6-aminonaphthalene, 6-aminonaphthalene, 2-carboxy-5-aminonaphthalene, 2-aminobenzoic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, 4-aminosalicylic acid, 5-aminosalicylic acid, 6-aminosalicylic acid, 2-aminobenzenesulfonic acid, 3-aminobenzenesulfonic acid, 4-aminobenzenesulfonic acid, 3-amino-4,6-dihydroxypyrimidine, 2-aminophenol, 3-aminophenol, 4-aminophenol, 2-amino-4-tert-butylphenol, 2-aminothiophenol, 3-aminothiophenol, 4-aminothiophenol, etc.

[0080] Preferred examples of monoanhydrides, monocarboxylic acids and acid chlorides include anhydrides such as phthalic anhydride, maleic anhydride, nadic anhydride, cyclohexanedicarboxylic anhydride and 3-hydroxyphthalic anhydride. Monocarboxylic acids such as 3-carboxyphenol, 4-carboxyphenol, 3-carboxythiophenol, 4-carboxythiophenol, 1-hydroxy-7-carboxynaphthalene, 1-hydroxy-6-carboxynaphthalene, 1-hydroxy-5-carboxynaphthalene, 1-mercapto-7-carboxynaphthalene, 1-mercapto-6-carboxynaphthalene, 1-mercapto-5-carboxynaphthalene, 3-carboxybenzenesulfonic acid and 4-carboxybenzenesulfonic acid. And monoacyl chloride compounds obtained by chlorinating the carboxyl groups of the compounds listed above.

[0081] When a monoamine is added as an end-capping agent, its content is preferably in the range of 1-60 mol% of the mole number of the diamine, more preferably 5-50 mol%, and more preferably 10-40%. When an acid anhydride, a monocarboxylic acid, or an acid chloride is added as an end-capping agent, its content is preferably in the range of 1-60 mol% of the mole number of the dicarboxylic acid, more preferably 5-50 mol%, and more preferably 10-40%. When the content of the end-capping agent is within such a range, the photosensitive resin composition obtained has moderate viscosity and excellent film properties.

[0082] As an example of the present invention, the alkali-soluble resin is prepared from the following monomers:

[0083]

[0084] In the alkali-soluble resin, 0.2 mol of 3-aminophenol and 0.1 mol of pyromellitic dianhydride constitute a capping structure; the three diamines and acid anhydrides listed above constitute the structure shown in the general formula (a), wherein the molar amount of the structural unit containing sulfone substitution (0.2 mol) accounts for 11.1% of the total molar amount (1.8 mol) of the structural unit of the general formula (a); the total molar amount (0.85 mol) of the structural unit containing fluorine substitution (0.65 mol) and the structural unit containing sulfone substitution accounts for 47.22% of the total molar amount (1.8 mol) of the structural unit of the general formula (a).

[0085] (Polyimide)

[0086] The photosensitive resin composition of the present invention may also include polyimide, which can be obtained by imidization of a polyimide precursor represented by the general formula (a). Therefore, on the basis of the acid anhydride and diamine disclosed in the present invention, the polyimide prepared from the acid anhydride monomer and diamine monomer of the present invention, and the alkali-soluble resin of the polyimide-polyimide precursor are also within the protection scope of the present invention.

[0087] (B) Photoacid generator

[0088] The photosensitive composition of the present invention has photosensitivity by containing a photoacid generator (B). The photoacid generator has the characteristic of generating acid by light irradiation, so that the solubility of the light-irradiated part in the alkaline aqueous solution is increased. As the photoacid generator, there are diazonium quinone compounds, sulfonium salts, phosphonium salts, diazonium salts, iodonium salts, etc. These photoacid generators are used in combination with alkali-soluble resins when not irradiated with light and show excellent dissolution inhibition effects. The present invention preferably uses diazonium quinone compounds, and the diazonium quinone compounds can be cited as: compounds obtained by bonding diazonium quinone sulfonic acid with polyhydroxy compounds by ester bonds; compounds obtained by bonding diazonium quinone sulfonic acid with polyamino compounds by sulfonamide bonds; compounds obtained by bonding diazonium quinone sulfonic acid with polyhydroxy polyamino compounds by ester bonds or sulfonamide bonds; compounds obtained by bonding diazonium quinone sulfonic acid with polyhydroxy polyamino compounds by ester bonds and sulfonamide bonds, etc. The present invention can be prepared by reacting diazonium quinone sulfonyl chloride with polyhydroxy compounds.

[0089] The functional groups of these polyhydroxy compounds and polyamino compounds may not be completely substituted with diazonaphthoquinone groups. The inventors have found that when the substitution with the diazonaphthoquinone groups is 50 mol% or more, the solubility in the alkaline developer will not become too high, and the contrast with the unexposed part can be obtained, and the desired pattern can be obtained. Therefore, the present invention preferably replaces more than 50 mol% of the functional groups with diazonaphthoquinone groups; on the other hand, considering the solubility of the diazonaphthoquinone compound in the solvent, it is preferred that less than 95 mol% of the functional groups are replaced with diazonaphthoquinone groups. By using such diazonaphthoquinone compounds, a positive photosensitive film having photosensitivity to the i-line (365 nm), h-line (405 nm), and g-line (436 nm) of a mercury lamp, which are common ultraviolet rays, can be obtained.

[0090] Examples of the polyhydroxy compound in the photoacid generator include, but are not limited to, 2,6-dimethoxymethyl-4-tert-butylphenol, 2,6-dimethoxymethyl-p-cresol, 2,6-diacetoxymethyl-p-cresol, naphthol, tetrahydroxybenzophenone, methyl gallate, bisphenol A, bisphenol E, methylene bisphenol, etc. Examples of the polyamino compound include, but are not limited to, 1,4-phenylenediamine, 1,3-phenylenediamine, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfide, etc. In addition, examples of the polyhydroxy polyamino compound include, but are not limited to, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 3,3'-dihydroxybenzidine, etc.

[0091] The diazonaphthoquinone-4-sulfonyl ester compound has absorption in the i-line region of the mercury lamp and is suitable for i-line exposure. The absorption of the diazonaphthoquinone-5-sulfonyl ester compound extends to the g-line region of the mercury lamp and is suitable for g-line exposure. In the present invention, both the diazonaphthoquinone-5-sulfonyl group and the diazonaphthoquinone-4-sulfonyl group can be preferably used. In addition, a diazonaphthoquinone-4-sulfonyl ester compound using both the diazonaphthoquinone-5-sulfonyl group and the diazonaphthoquinone-4-sulfonyl group in the same molecule can also be obtained, and the diazonaphthoquinone-4-sulfonyl ester compound and the diazonaphthoquinone-5-sulfonyl ester compound can also be mixed and used.

[0092] The naphthoquinone diazo compound prepared by using the polyhydroxyphenol compound and the naphthoquinone diazo sulfonyl ester compound can be used alone or in combination of two or more. The present invention preferably uses two or more photoacid generators. By adjusting the composition and content of the multiple photoacid generators, a greater dissolution rate ratio between the exposed part and the unexposed part can be obtained, resulting in a highly sensitive photosensitive film.

[0093] The molecular weight of the diazonaphthoquinone compound of the present invention is preferably in the range of 300-4000. When the molecular weight of the diazonaphthoquinone compound is greater than 4000, the diazonaphthoquinone compound is prone to insufficient thermal decomposition during subsequent heat treatment, which may reduce the heat resistance, mechanical properties, adhesion, etc. of the film.

[0094] Based on 100 parts by mass of the alkali-soluble resin, the mass of the photoacid generator is 3-40 parts by mass, preferably 10-30 parts by mass.

[0095] As a preferred example of the present invention, the photoacid generator is a combination of the following two structures:

[0096]

[0097] Where Q is hydrogen, And Q is not entirely hydrogen.

[0098] More preferably, the molar ratio of the diazonaphthoquinone group to Q is 70% or more.

[0099] (C) Thermal crosslinking agent

[0100] The thermal crosslinking agent is one of the key points of the present invention. When the photosensitive resin is heat-treated, the thermal crosslinking agent can form a crosslinking structure between the resins, which can not only reduce the shrinkage rate of the film during curing, but also improve the chemical resistance of the film after thermal curing.

[0101] The thermal crosslinking agent used in the present invention comprises a repeating unit represented by formula (c):

[0102]

[0103] In formula (c), R3 represents a hydrogen atom or a monovalent organic group having 1 to 4 carbon atoms, R4 represents a divalent organic group having 1 to 10 carbon atoms; and n represents an integer in the range of 4 to 200.

[0104] Preferably, the thermal crosslinking of the present invention comprises a repeating unit represented by formula (c'):

[0105] Wherein R4' represents a divalent organic group having 0 to 9 carbon atoms.

[0106] That is, in the repeating unit of the thermal crosslinking agent, the group for

[0107] The thermal crosslinking agent of the present invention is obtained by self-polymerization of vinyl-containing glycidyl esters or copolymerization with other vinyl compounds. The monomers for synthesizing such thermal crosslinking agents preferably include: glycidyl methacrylate, glycidyl ethacrylate, glycidyl acrylate, etc., but are not limited to these. The thermal crosslinking agent can be used alone or in combination of two or more. The inventors have found through extensive research that the alkyl flexible chain of the above general formula not only provides low stress characteristics to the cured film, but also the polyepoxy groups on the side chains provide excellent chemical resistance to the cured film through the crosslinking effect. More preferably, when the polyglycidyl acrylate thermal crosslinking agent is matched with a sulfone-containing polyimide precursor, the exposure sensitivity of the pre-baked film is more significantly improved.

[0108] For the thermal crosslinking agent of the present invention, in order to provide the film with better mechanical properties and chemical resistance, the molecular weight of the thermal crosslinking agent should be greater than 1000, and in order to maintain low stress and high elongation of the film, the molecular weight of the crosslinking agent needs to be less than 20000. Therefore, the weight average molecular weight of the thermal crosslinking agent is preferably 1000-20000, more preferably 1000-5000.

[0109] Furthermore, in order to improve mechanical properties and heat resistance, the content of the thermal crosslinking agent is preferably more than 1 part, and more preferably more than 2 parts, based on 100 parts of the resin content. In order to maintain low stress of the film, the content of the thermal crosslinking agent is preferably less than 20 parts, and more preferably less than 10 parts. The amount of the thermal crosslinking agent used in the present invention is preferably 1-20 parts by mass, and most preferably 2-10 parts by mass.

[0110] As a suitable solvent for the reaction, the solvent used to form the above composition can be directly used, or other suitable solvents can be used. There is no particular limitation on the solvent, which is usually an organic solvent suitable for dissolving the monomer and precursor and having no side reactions. Examples of the solvent include, but are not limited to, γ-butyrolactone, dimethyl sulfoxide (DMSO), dimethylformamide (DMF), N-methyl 2-pyrrolidone (NMP), ethyl acetate, chloroform, tetrahydrofuran (THF), acetone, etc.

[0111] <Photosensitive resin film>

[0112] A second aspect of the present invention provides a photosensitive resin film, which is formed from the photosensitive resin composition.

[0113] Preferably, under the condition that the film thickness is 10 μm, the transmittance of i-ray (365 nm wavelength) is ≥91%, the transmittance of h-ray (405 nm wavelength) is ≥93%, and the transmittance of g-ray (436 nm wavelength) is ≥95%, and the minimum exposure required for exposure under these conditions is ≤40 mJ / cm 2 .

[0114] The photosensitive resin film of the present invention exhibits the following properties: excellent light transmittance, high temperature resistance, chemical resistance, low shrinkage, and low stress. Due to the excellent heat resistance, chemical resistance, low stress, and low thermal expansion coefficient of the film of the present invention, it can be used as a surface protection film of a semiconductor element, an interlayer insulating film, an insulating film of an organic electroluminescent element, etc.

[0115] <Pattern Formation Method Using Photosensitive Resin Composition>

[0116] A third aspect of the present invention provides a pattern forming method, which comprises the following steps:

[0117] Step 1: coating the photosensitive resin composition on the substrate to form a photosensitive resin coating, and then pre-baking on a hot plate at 80-120° C. for 2-60 minutes to form a photosensitive film;

[0118] Step 2: using an exposure mask to expose the photosensitive film;

[0119] Step 3: removing the exposed portion of the photosensitive film with an alkaline developer and developing the film;

[0120] Step 4: Curing the developed film at a temperature of 100° C. to 300° C. to obtain a cured film.

[0121] First, in step 1, a photosensitive resin is coated on a substrate to make it uniform in thickness. Examples of substrates may include substrates, silicon wafers, substrates with a metal coating on the surface by ion sputtering or electroplating, etc.; the coating method may be dip coating, spin coating, roller coating, slit coating, spray coating, etc., and these methods may be combined; in order to make the coating thickness more uniform, the present invention may use a coating machine to control the uniform film thickness, but is not limited thereto. It is preferred to form the film by pre-baking, and the pre-baking conditions are pre-baking on a hot plate at 80-120°C for 2-60 minutes.

[0122] Steps 2 and 3 are exposure and development steps, wherein the exposure radiation preferably has a wavelength of 190nm to 500nm and an exposure dose of 10-5000mJ / cm 2 .

[0123] Step 4: Curing the patterned resin film. The curing process, especially the temperature change under high temperature conditions, has a great influence on the cross-linking degree of the resin film, and also directly affects the properties of the cured film, such as heat resistance, mechanical strength, etc. In the present invention, the developed film is cured at a temperature of 100° C. to 300° C. to obtain a cured film.

[0124] The most preferred embodiment is: placing the developed film under a nitrogen flow at 100°C, heating it to 250-270°C at a heating rate of 1-10°C / min, and curing it at 250-270°C for 60-100 minutes, naturally cooling it to room temperature 25°C, separating the coating from the substrate, and obtaining a cured film.

[0125] The above and other advantages of the present invention may be better understood through the following examples, but the following examples are not intended to limit the scope of the present invention.

[0126] <Preparation of Sulfone-containing Diamine / Anhydride Monomer>

[0127] (Synthesis Example 1) Synthesis of a hydroxyl-containing diamine compound (HSHA)

[0128] Under a dry nitrogen stream, 14.015 g (0.05 mol) of 3,3′-diamino-4,4′-dihydroxydiphenyl sulfone (BAHS) was dissolved in 100 mL of acetone, and 17.4 g (0.3 mol) of propylene oxide was added to the acetone, and the temperature was cooled to -15°C. 100 mL of acetone containing 20.4 g (0.11 mol) of 3-nitrobenzoyl chloride was added dropwise. The addition process lasted for 30 minutes. After the addition was completed, the mixture was reacted at -15°C for 4 hours, and then returned to room temperature. The precipitated solid was filtered and vacuum dried at 80°C.

[0129] 30 g of the obtained light yellow solid was dissolved in 500 mL of ethanol, 0.75 g of 5% palladium carbon was added, the temperature was raised to 85° C. and refluxed, and then 75 mL of an ethanol solution containing 25 mL of hydrazine hydrate was added dropwise. The dropping process lasted for 3 hours. After the addition was completed, the reaction was continued for 2 hours, and then the catalyst was filtered off, the ethanol was evaporated off, and the mixture was washed with a mixed solution of ethyl acetate and petroleum ether (ethyl acetate: petroleum ether=1:2), and vacuum dried at 50° C. to obtain a hydroxyl-containing diamine compound (HSHA) represented by the following formula.

[0130]

[0131] (Synthesis Example 2) Synthesis of a Hydroxyl-Containing Diamine Compound (PHSHA)

[0132] By replacing 3-nitrobenzoyl chloride in Synthesis Example 1 with 4-nitrobenzoyl chloride, a hydroxyl-containing diamine compound (PHSHA) represented by the following formula can be obtained:

[0133]

[0134] (Synthesis Example 3) Synthesis of Sulfone-containing Acid Anhydride Compound

[0135] <Preparation of alkali-soluble resin>

[0136] (Synthesis Example 4) Synthesis of alkali-soluble resin (a1-1)

[0137] Under a dry nitrogen flow, 10.36 g (0.02 mol) of HSHA, 39.23 g (0.065 mol) of 2,2′-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 1.24 g (0.005 mol) of 1,3-bis(3-aminopropyl)tetramethyldisiloxane, and 2.18 g (0.02 mol) of 3-aminophenol were dissolved in 200 g of N-methyl-2-pyrrolidone, and 31.02 g (0.1 mol) of 3,3′,4,4′-diphenylethertetracarboxylic dianhydride (ODPA) was added thereto. The mixture was reacted at 40° C. for 2 hours, then heated to 50° C. for 3 hours, and then the solution was dripped into 2 L of deionized water for sufficient precipitation, and the polymer solid precipitate was collected by filtration. The solid was then washed three times with 2 L of deionized water and vacuum dried at 50° C. to obtain a polyimide precursor (a1-1).

[0138] (Synthesis Example 5-8) Synthesis of Alkali-Soluble Resins a1-2, a2-1, a3-1 and a4-1

[0139] By adopting the same process as in Synthesis Example 4, different diamine monomers are selected to react with anhydride to obtain polyimide precursors with different effects. The raw materials and amounts of each monomer are summarized in Table 1, wherein the amounts of all materials are molar amounts.

[0140] Table 1 Composition and dosage of each monomer in the preparation of alkali-soluble resin precursors in Synthesis Examples 4-8

[0141]

[0142] Here, ODPA* refers to 0.02 mol of 3,3',4,4'-diphenylsulfone tetracarboxylic acid dianhydride and 0.08 mol of ODPA, and the sulfone-containing anhydride is used as a structural unit constituting the general formula (a), and its proportion is 22.2%.

[0143] <Synthesis of Photoacid Generator>

[0144] (Synthesis Example 9) Synthesis of Diazonaphthoquinone Compound (b1-1)

[0145] Under a dry nitrogen stream, 42.45 g (0.1 mol) of TrisP-PA (trade name, manufactured by Honshu Chemical Industry Co., Ltd.) and 75.23 g (0.28 mol) of naphthoquinone diazide-5-sulfonyl chloride were dissolved in 1000 g of 1,4-dioxane. While the reaction system was cooled with ice, a liquid mixed with 150 g of 1,4-dioxane and 30.36 g (0.3 mol) of triethylamine was added dropwise so that the temperature in the system did not exceed 10°C. After the addition, the mixture was stirred at 30°C for 2 hours, the triethylamine salt was filtered, and the filtrate was added to 7 L of pure water to obtain a precipitate. The precipitate is collected by filtration, washed with hydrochloric acid having a solid content of 1%, and then further washed twice with 5L of pure water. Finally, it is dried in a vacuum oven at 50°C for 24 hours to obtain a diazonaphthoquinone compound (b1-1) represented by the following formula, wherein an average of 2.8 of the 3 unit amounts of Q are substituted by diazonaphthoquinone-5-sulfonate groups.

[0146] Q Overall, H=2.8:0.2

[0147] By changing the added amount of diazonaphthoquinone-5-sulfonyl chloride in Synthesis Example 9 to 64.48 g (0.24 mol), a diazonaphthoquinone compound (b1-2) in which an average of 2.4 diazonaphthoquinone-5-sulfonate groups are substituted in 3 units of Q can be obtained. By changing the added amount of diazonaphthoquinone-5-sulfonyl chloride in Synthesis Example 9 to 53.74 g (0.20 mol), a diazonaphthoquinone compound (b1-3) in which an average of 2.0 diazonaphthoquinone-5-sulfonate groups are substituted in 3 units of Q can be obtained.

[0148] (Synthesis Example 10) Synthesis of Diazonaphthoquinone Compound (b2-1)

[0149] Under a dry nitrogen stream, 30.61 g (0.1 mol) of TrisP-HAP (trade name, manufactured by Honshu Chemical Industry Co., Ltd.) and 75.23 g (0.28 mol) of diazonaphthoquinone-4-sulfonyl chloride were dissolved in 1000 g of 1,4-dioxane. While the reaction system was cooled with ice, a liquid mixed with 150 g of 1,4-dioxane and 30.36 g (0.3 mol) of triethylamine was added dropwise so that the temperature in the system did not exceed 10°C. After the addition, the mixture was stirred at 30°C for 2 hours, the triethylamine salt was filtered, and the filtrate was added to 7 L of pure water to obtain a precipitate. The precipitate is collected by filtration, washed with hydrochloric acid having a solid content of 1%, and then further washed twice with 5L of pure water. Finally, it is dried in a vacuum oven at 50°C for 24 hours to obtain a diazonaphthoquinone compound (b2-1) represented by the following formula, wherein an average of 2.8 of the 3 unit amounts of Q are substituted by diazonaphthoquinone-4-sulfonate groups.

[0150] Q Overall, H=2.8:0.2

[0151] By changing the added amount of diazonaphthoquinone-4-sulfonyl chloride in Synthesis Example 10 to 64.48 g (0.24 mol), a diazonaphthoquinone compound (b2-2) in which an average of 2.4 diazonaphthoquinone-4-sulfonate groups are substituted in 3 units of Q can be obtained. By changing the added amount of diazonaphthoquinone-4-sulfonyl chloride in Synthesis Example 8 to 53.74 g (0.20 mol), a diazonaphthoquinone compound (b2-3) in which an average of 2.0 diazonaphthoquinone-4-sulfonate groups are substituted in 3 units of Q can be obtained.

[0152] <Synthesis of Thermal Crosslinking Agent>

[0153] (Synthesis Example 11) Synthesis of thermal crosslinking agent (c1-1)

[0154] 10 g of glycidyl acrylate was dissolved in 100 mL of a mixture of water and tetrahydrofuran in a volume ratio of 1:1, and placed in a sealed reactor that excludes oxygen. 1 g of sodium dithionite and 0.2 g of sodium bicarbonate were added, and the mixture was stirred and polymerized at 35° C. for 8 hours. n-hexane was added to the reaction solution to precipitate the polymer, which was separated and dried to obtain 9.6 g of polyglycidyl acrylate, i.e., a thermal crosslinking agent (c1-1). The weight average molecular weight thereof was measured by gel permeation chromatography to be 4569.

[0155] By replacing the glycidyl acrylate in Synthesis Example 11 with glycidyl methacrylate, polyglycidyl methacrylate, namely the thermal crosslinking agent (c1-2), can be obtained. The weight average molecular weight thereof is 2550 as measured by gel permeation chromatography.

[0156] <Preparation of Photosensitive Resin>

[0157] Example 1

[0158] 10 g of an alkali-soluble resin (a1-1), 0.6 g of a diazonaphthoquinone compound (b1-1), 1.4 g of a diazonaphthoquinone compound (b2-1), and 0.7 g of a thermal crosslinking agent (c1-1) were added to 80 g of γ-butyrolactone to obtain a varnish D1 of a positive photosensitive resin composition.

[0159] Example 2-17

[0160] By adopting the same process as in Example 1, different alkali-soluble resins, photoacid generators and thermal crosslinking agents are selected to obtain photosensitive resins with different effects. The raw materials and amounts of each component are summarized in Table 2, where the amounts of all materials are in mass (g).

[0161] Comparative Examples 1-5

[0162] By adopting the same process as in Example 1, different alkali-soluble resins, photoacid generators and thermal crosslinking agents are selected to obtain photosensitive resins with different effects. The raw materials and amounts of each component are summarized in Table 2, where the amounts of all materials are in mass (g).

[0163] Table 2 Preparation ingredients of photosensitive resins of Examples 1-17 and Comparative Examples 1-5

[0164]

[0165] Among them, if there is no special explanation, the amount of each component is the default value in the first row; in Example 11, (c1-1)* is a small molecular weight poly(glycidyl acrylate) (weight average molecular weight is 563); in Example 17, the photoacid generator uses a single composition photoacid generator (b1-1).

[0166] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and functional group modifications can be made without departing from the monomer reaction principle of the present invention. These improvements and functional group modifications should also be regarded as the scope of protection of the present invention.

[0167] Test Method

[0168] (1) Light transmittance

[0169] The visible light transmittance of the photosensitive resin film was measured using a UV spectrophotometer (Cary100, Varian). (2) Coefficient of linear thermal expansion (CTE)

[0170] The CTE of the photosensitive resin film was measured by a thermal mechanical analyzer (Q400, TA instrument) at a heating rate of 5°C / min, with the values ​​in the range of 50-250°C as the measured values.

[0171] (3) Glass transition temperature (Tg)

[0172] The glass transition temperature was measured by differential scanning calorimetry (DSC822) in a nitrogen atmosphere at a heating rate of 5 °C / min.

[0173] (4) Thermogravimetric analysis (TGA)

[0174] Thermogravimetric analysis was performed using a thermogravimetric analyzer (Mettler TGA / SDTA851) in a nitrogen atmosphere with a heating rate of 10°C / min.

[0175] (5) Stress evaluation

[0176] The varnish was evenly dropped on the silicon wafer, spun evenly at a speed of 300 r / min using a coater, and then pre-baked on a hot plate at 110°C for 4 minutes, exposed and developed, and then heated from 100°C to 250°C at a rate of 5°C / min, and cured at 250°C for 1 hour to obtain a film thickness of 10 μm. The silicon wafer was taken out when the temperature became below 50°C, and the stress of the cured film was confirmed using a stress measuring device FLX2908 (manufactured by KLA Tencor).

[0177] (6) Chemical resistance

[0178] The varnish was evenly dropped on the silicon wafer, and the varnish was evenly spun at a speed of 300 r / min using a sizing machine, and then pre-baked on a hot plate at 110°C for 4 minutes, and then exposed and developed. Then, the temperature was raised from 100°C to 250°C at 5°C / min, and then cured at 250°C for 1 hour to obtain a film thickness of 10μm. When the temperature became below 50°C, the silicon wafer was taken out and the film thickness was measured. Then, the wafer was immersed in a solvent of dimethyl sulfoxide (DMSO) at 70°C for 100 minutes. The wafer taken out of the solvent was washed with pure water, and then the film thickness was measured again. The case where the absolute value of the change rate was greater than 15% and the case of cured film peeling was evaluated as insufficient (D), the case within 15% and greater than 10% was evaluated as qualified (C), the case within 10% and greater than 5% was evaluated as good (B), and the case within 5% was evaluated as better (A).

[0179] (7) Evaluation of sensitivity

[0180] The resolution pattern of the produced developed film was observed using a Zeiss confocal microscope, and the exposure amount (i-line illuminometer value) at which a 20 μm line and space pattern with a width of 1:1 was formed was taken as the sensitivity.

[0181] Table 3 Test performance of Examples 1-17 and Comparative Examples 1-5

[0182] Table 3-1

[0183]

[0184]

[0185] It can be clearly seen from the results in Table 3 that after HSHA and PHSHA as monomers of polyimide precursors participate in the polymerization reaction, the transmittance of the cured film at 365nm and 405nm is significantly improved, but the sulfone content is too high, which is easy to affect the thermal expansion coefficient of the film. When the appropriate amount of thermal crosslinking agents c1-1 and c1-2 replace the small molecule thermal crosslinking agent, not only the thermal expansion coefficient of the cured film is reduced, the glass transition temperature and thermal weight loss temperature of the cured film are increased, but also the transmittance of the cured film is further improved.

[0186] Table 3-2

[0187]

[0188] It can also be seen from Table 3 that the different proportions of hydrogen substituents of Q in the diazonaphthoquinone compound also have a significant effect on the exposure sensitivity of the pre-baked film, and different diazonaphthoquinone compounds combined and matched have an effect on the exposure sensitivity of the pre-baked film, among which b1-1 and b2-2 can achieve better results when matched. It can also be found that when polyacrylate glycidyl ester thermal crosslinkers and polyimide precursors containing HSHA or PHSHA are matched, the exposure sensitivity of the pre-baked film is more significantly improved. In addition, comparison of data shows that the thermal crosslinkers c1-1 and c1-2 have the best comprehensive performance when combined with the above-mentioned alkali-soluble resin and photoacid generator: their alkyl flexible chains not only provide low stress characteristics to the cured film, but also the polyepoxy groups on the side chains of the thermal crosslinkers c1-1 and c1-2 provide excellent chemical resistance to the cured film through the crosslinking effect.

[0189] Although the present invention has been described in detail above by means of general description, specific implementation methods and tests, it is obvious to those skilled in the art that some modifications or improvements may be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A photosensitive resin composition, characterized in that It comprises (A) an alkali-soluble resin, wherein the alkali-soluble resin is composed of a repeating unit represented by formula (a); In formula (a), R 11 and R 12 represents a divalent to hexavalent organic group having 2 to 40 carbon atoms; R1 and R2 represent a hydrogen atom or an organic group having 1 to 20 carbon atoms; m represents an integer in the range of 10 to 100000, and p, q, h, and g represent integers satisfying 0≤p+q+h+g≤4; R of the formula (a) 11 and / or R 12 Including a structure containing sulfone group substitution, wherein the molar amount of the structural unit containing sulfone group substitution accounts for 5-20% of the total molar amount of the structural unit of formula (a); (B) photoacid generator; (C) a thermal crosslinking agent, the thermal crosslinking agent comprising a repeating unit represented by formula (c): In formula (c), R3 represents a hydrogen atom or a monovalent organic group having 1 to 4 carbon atoms, and R4 is R4' represents a divalent organic group having 0 to 9 carbon atoms; n represents an integer in the range of 4 to 200; The weight average molecular weight of the thermal crosslinking agent is 1000-20000; Based on 100 parts by mass of the alkali-soluble resin, the thermal crosslinking agent is 1-20 parts by mass, and the photoacid generator is 3-40 parts by mass.

2. The photosensitive resin composition according to claim 1, characterized in that R of the formula (a) 11 One or more selected from the following structural formulas: wherein R is each independently an alkyl group having 1 to 20 carbon atoms, a fluoroalkyl group, an alkoxy group, an ester group, a nitro group, a cyano group or a halogen group; x, y and z are each independently an integer from 0 to 4; A represents a direct bond, -CO-, -CH2-, -C2H4-, -O-, -C3H6-, -C3F6-, -SO2-, -S-, or any one of -Si(CH3)2-; and J represents a direct bond, -COO-, -CONH-, -CH2-, -C2H4-, -O-, -C3H6-, -C3F6-, -SO2-, -S-, -Si(CH3)2-, -OSi(CH3)2O-, -C6H4-, -C6H4-O-C6H4-, -C6H4-C3H6-C6H4-, or -C6H4-C3F6-C6H4-.

3. The photosensitive resin composition according to claim 1, characterized in that R of the formula (a) 12 Selected from two or more of the following structural formulas: , and a diamine residue structure having a siloxane structure; wherein R is each independently an alkyl group having 1 to 20 carbon atoms, a fluoroalkyl group, an alkoxy group, an ester group, a nitro group, a cyano group or a halogen group, and x, y, and z are each independently an integer from 0 to 4; B represents a direct bond, -CO-, -CH2-, -C2H4-, -O-, -C3H6-, -C3F6-, -SO2-, -S-, or any one of -Si(CH3)2-; and Z represents a direct bond, -COO-, -CONH-, -CH2-, -C2H4-, -O-, -C3H6-, -C3F6-, -SO2-, -S-, -Si(CH3)2-, -OSi(CH3)2O-, -C6H4-, -C6H4-O-C6H4-, -C6H4-C3H6-C6H4-, or -C6H4-C3F6-C6H4-.

4. The photosensitive resin composition according to any one of claims 1 to 3, characterized in that: The photoacid generator is a naphthoquinone diazide compound.

5. The photosensitive resin composition according to claim 1, characterized in that: The end of the alkali-soluble resin further includes a group represented by formula (e-1) and / or formula (e-2): Formula (e-1): -NH-R5, wherein R5 represents a monovalent organic group containing a hydroxyl group, a carboxyl group, a benzenesulfonic acid group, a pyrimidine group, a phenol group or a thiophenol group; Formula (e-2): -CO-R6, wherein R6 represents a monovalent organic group containing a carboxyl group, a phenol group, a thiophenol group, a hydroxyl group, a mercapto group, or a benzenesulfonic acid group.

6. A photosensitive resin film, characterized in that: The photosensitive resin film is prepared from the photosensitive resin composition according to any one of claims 1 to 5.

7. The photosensitive resin film according to claim 6, characterized in that: Under the condition of film thickness of 10μm, the transmittance of i-ray is ≥91%, the transmittance of h-ray is ≥93%, the transmittance of g-ray is ≥95%, and the minimum exposure required for exposure under this condition is ≤40mJ / cm 2 .

8. A pattern forming method, characterized in that: The following steps are involved: Step 1: coating the photosensitive resin composition according to any one of claims 1 to 5 on a substrate to form a photosensitive resin coating, and then pre-baking on a hot plate at 80-120° C. for 2-60 minutes to form a photosensitive film; Step 2: using an exposure mask to expose the photosensitive film; Step 3: removing the exposed portion of the photosensitive film with an alkaline developer and developing the film; Step 4: Curing the developed film at a temperature of 100° C. to 300° C. to obtain a cured film.