Positive electrode active material and secondary battery using the same

By coating the surface of the lithium composite oxide particles with ammonium phosphate compounds and polymers, the problems of decreasing discharge capacity and side reactions in the secondary battery are solved, and the improvement of high discharge capacity and cycling characteristics are achieved.

CN112018343BActive Publication Date: 2024-11-22PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010468508.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-13
Filing Date
2020-05-28
Publication Date
2024-11-22
Estimated Expiration
2040-05-28

AI Technical Summary

Technical Problem

The discharge capacity maintenance rate of the conventional secondary battery of the positive electrode active material decreases during the charge and discharge cycle, and the discharge capacity is insufficient, making it difficult to suppress side reactions in the nonaqueous electrolyte.

Method used

A positive electrode active material containing lithium composite oxide particles is used, and its surface is coated with an ammonium phosphate compound and a polymer with a specific structural unit. The reduction and dissolution of the lithium composite oxide are inhibited by the coating layer, thereby reducing the oxidative decomposition of the non-aqueous electrolyte.

Benefits of technology

The high discharge capacity and cycle characteristics of the secondary battery are improved, which suppresses the reduction of the discharge capacity maintenance rate and improves the cycle performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112018343B_ABST
    Figure CN112018343B_ABST
Patent Text Reader

Abstract

The present disclosure provides a positive electrode active material that can realize a secondary battery with a sufficiently high discharge capacity and suppress the reduction in the discharge capacity retention rate of the secondary battery. A positive electrode active material (10) in one technical solution of the present disclosure comprises particles (1) containing a lithium composite oxide and a coating layer (2) coating the particles (1), wherein the coating layer (2) contains an ammonium phosphate compound and a polymer having a structural unit represented by the following formula (1). #imgabs0# [In formula (1), R is a hydrogen atom or a methyl group. ]
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a positive electrode active material and a secondary battery using the positive electrode active material. Background Art

[0002] An electrolytic solution containing a nonaqueous solvent is called a nonaqueous electrolyte. In order to improve the cycle characteristics of a secondary battery including a nonaqueous electrolyte, it is important to suppress side reactions associated with the decomposition of the nonaqueous solvent.

[0003] In order to suppress the side reaction, various attempts have been made to improve the surface of the positive electrode active material which will become the reaction site of the side reaction. For example, Patent Document 1 discloses that in order to suppress the side reaction, a method of using mLi 1+x Al x Ti 2-x (PO 4 ) 3 The solid electrolyte represented by nLiOH covers the surface of the lithium composite oxide particles contained in the positive electrode active material.

[0004] Prior Art Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2018-206669 Summary of the invention

[0006] Problems to be solved by the invention

[0007] The discharge capacity retention rate of a secondary battery containing a conventional positive electrode active material may decrease significantly with repeated charge and discharge cycles. In addition, a secondary battery containing a conventional positive electrode active material may not have a sufficiently high discharge capacity.

[0008] Means for solving problems

[0009] A positive electrode active material according to a technical solution of the present disclosure comprises:

[0010] Particles comprising a lithium composite oxide; and a coating layer coating the particles,

[0011] The coating layer contains an ammonium phosphate compound and a polymer having a structural unit represented by the following formula (1).

[0012]

[0013] [In formula (1), R is a hydrogen atom or a methyl group.]

[0014] Effects of the Invention

[0015] The present disclosure provides a positive electrode active material capable of realizing a secondary battery having a sufficiently high discharge capacity and suppressing a decrease in the discharge capacity retention rate of the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a cross-sectional view of the positive electrode active material according to this embodiment.

[0017] Figure 2 It is a longitudinal cross-sectional view schematically showing a secondary battery including a positive electrode active material according to the present disclosure.

[0018] Figure 3 yes Figure 2 An enlarged cross-sectional view of a secondary battery in region III is shown. DETAILED DESCRIPTION

[0019] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings, but the present disclosure is not limited to the following embodiments.

[0020] (Embodiments of Positive Electrode Active Material)

[0021] Figure 1 is a cross-sectional view of the positive electrode active material 10 according to this embodiment. Figure 1 As shown, the positive electrode active material 10 includes a particle 1 and a coating layer 2. The coating layer 2 covers the particle 1. The coating layer 2 may cover the entire surface of the particle 1 or partially cover the surface of the particle 1. The coating layer 2 may be in a film shape or in an island shape. The coating layer 2 is in direct contact with the particle 1, for example.

[0022] Particle 1 contains lithium composite oxide. Particle 1 may contain lithium composite oxide as a main component. "Main component" refers to the component that is contained in the largest amount by weight in particle 1. Particle 1 may be substantially composed of lithium composite oxide. "Substantially composed of..." means that other components that would change the essential characteristics of the material mentioned are excluded. However, particle 1 may contain impurities in addition to lithium composite oxide. By particle 1 containing lithium composite oxide, positive electrode active material 10 can absorb and release lithium ions.

[0023] The lithium composite oxide is, for example, a metal oxide containing lithium and a transition metal. The lithium composite oxide contains, for example, at least one selected from nickel, cobalt, and manganese. The lithium composite oxide may contain at least one selected from nickel and cobalt. In other words, the lithium composite oxide may be a metal oxide containing lithium and at least one selected from nickel, cobalt, and manganese, or may be a metal oxide containing nickel, cobalt, and lithium. In the lithium composite oxide, the ratio of the number of nickel atoms to the total number of nickel, cobalt, and manganese atoms is, for example, 50% or more.

[0024] The lithium composite oxide has, for example, a crystal structure. The crystal structure of the lithium composite oxide is not particularly limited. The lithium composite oxide has, for example, a crystal structure belonging to the space group R-3m or C2 / m. In such a lithium composite oxide, the expansion and contraction of the lattice accompanying the charge and discharge of the secondary battery are small. Therefore, the lithium composite oxide is difficult to deteriorate in the non-aqueous electrolyte of the secondary battery. The secondary battery containing the lithium composite oxide has excellent cycle characteristics. In addition, the lithium composite oxide can form a secondary battery in a discharged state.

[0025] The coating layer 2 contains an ammonium phosphate compound and a polymer having a structural unit represented by the following formula (1). In this specification, a polymer including a structural unit represented by formula (1) may be referred to as "polymer P".

[0026]

[0027] [In formula (1), R is a hydrogen atom or a methyl group.]

[0028] Ammonium phosphate compounds are salts containing phosphate ions and ammonium ions. In this specification, ammonium ions include not only NH 4 + , also includes NH 4 + Primary ammonium ions, secondary ammonium ions and tertiary ammonium ions in which at least one hydrogen atom contained therein is replaced by a substituent. As the substituent contained in the ammonium ion, for example, a hydrocarbon group can be mentioned. The carbon number of the hydrocarbon group is, for example, greater than 1. The upper limit of the carbon number of the hydrocarbon group is not particularly limited, for example, 3. The hydrocarbon group can be chain-shaped or cyclic. The hydrocarbon group is, for example, a saturated aliphatic group. As saturated aliphatic groups, methyl, ethyl, propyl and the like can be mentioned. The hydrogen atoms contained in the hydrocarbon group can be substituted by halogen atoms such as fluorine atoms. In the ammonium phosphate compound, a part of the ammonium ions can be substituted by lithium ions.

[0029] The ammonium phosphate compound may be a compound represented by the following formula (2).

[0030] Li x (NR 4 ) 3-x PO 4 (2)

[0031] In formula (2), x satisfies the following relationship: 0.10≤x≤2.90. Multiple R are independently hydrogen atoms or a compound of the formula C α H β F γ A saturated aliphatic group represented by . In the saturated aliphatic group, α, β and γ are integers satisfying the following relationships: α≥1, β≥0, γ≥0 and β+γ=2α+1. In formula (2), all R may be hydrogen atoms.

[0032] In formula (2), the value of x can be determined, for example, by the following method. First, the positive electrode active material 10 is subjected to TG-GC / MS (Thermogravimetric Gas Chromatography-Mass Spectrometry) measurement. In the TG-GC / MS measurement, the ammonium phosphate compound contained in the positive electrode active material 10 is thermally decomposed to generate NH 3 Gas. By NH 3 Gas is quantitatively analyzed to determine the amount of ammonium ions contained in the ammonium phosphate compound. The amount of ammonium ions can be determined based on the obtained value by performing TG-GC / MS measurements on the positive electrode active material 10 five times. Next, the amount of phosphate ions contained in the ammonium phosphate compound is determined. The amount of phosphate ions contained in the ammonium phosphate compound can be determined, for example, by inductively coupled plasma (ICP) emission spectrometry. Based on the amount of ammonium ions and the amount of phosphate ions contained in the ammonium phosphate compound, the value of x can be calculated.

[0033] The value of x in formula (2) varies, for example, depending on the ratio of the weight of the coating layer 2 to the weight of the lithium composite oxide. There is a tendency that the value of x increases as the ratio decreases, and the value of x decreases as the ratio increases. The value of x may also vary depending on the conditions and surrounding environment when the coating layer 2 of the positive electrode active material 10 is produced.

[0034] As long as the polymer P contains the structural unit represented by formula (1), there is no particular limitation. The content of the structural unit represented by formula (1) in the polymer P may be 50 mol% or more, or 80 mol% or more. The polymer P may be substantially composed of the structural unit represented by formula (1). The polymer P may be lithium poly(meth)acrylate or lithium polyacrylate.

[0035] The weight average molecular weight of polymer P is not particularly limited. The weight average molecular weight of polymer P may be greater than 25,000, greater than 250,000, greater than 450,000, or greater than 1,000,000. There is a tendency that the greater the weight average molecular weight of polymer P, the lowering of the discharge capacity retention rate of the secondary battery is suppressed. The upper limit of the weight average molecular weight of polymer P is not particularly limited, for example, 3,000,000. The weight average molecular weight of polymer P may be greater than 25,000 and less than 1,000,000, or greater than 250,000 and less than 1,000,000.

[0036] The ratio of the weight of the ammonium phosphate compound to the weight of the polymer P in the coating layer 2 may be in any range as long as a single layer of the ammonium phosphate compound or a single layer of the polymer P is not formed. In the coating layer 2, the ratio of the weight of the ammonium phosphate compound to the weight of the polymer P is not particularly limited, and may be 1 / 9 or more and 9 / 1 or less, 2 / 8 or more and 8 / 2 or less, or 4 / 6 or more and 8 / 2 or less.

[0037] The ratio A of the weight of the coating layer 2 relative to the weight of the lithium composite oxide is not particularly limited. From the viewpoint of fully suppressing the side reaction between the lithium composite oxide and the non-aqueous solvent contained in the secondary battery, the ratio A can be 0.3% by weight or more. However, if the ratio A is too high, the movement of lithium ions between the lithium composite oxide and the non-aqueous solvent may be hindered. That is, if the ratio A is too high, the ammonium phosphate compound and the polymer P may sometimes act as resistance components, reducing the discharge capacity of the secondary battery. Therefore, the ratio A may be 2.0% by weight or less. The ratio A may be 0.3% by weight or more and 2.0% by weight or less.

[0038] The shape of the positive electrode active material 10 is, for example, particulate. In this specification, "particulate" includes spherical, ellipsoidal, scaly and fibrous. The average particle size of the positive electrode active material 10 is, for example, not less than 5 μm and not more than 50 μm. The average particle size of the positive electrode active material 10 refers to the particle size (D50) corresponding to a cumulative volume percentage of 50% in the particle size distribution measured by the laser diffraction scattering method.

[0039] The positive electrode active material 10 can be produced, for example, by the following method: First, a polymer Q including a structural unit represented by the following formula (3) is prepared.

[0040]

[0041] [In formula (3), R is a hydrogen atom or a methyl group.]

[0042] Next, a solution containing polymer Q is prepared. The solvent of the solution is, for example, water. Lithium hydroxide is added to the solution. As a result, the carboxyl groups contained in polymer Q are neutralized by lithium hydroxide to form polymer P. Then, the solution containing polymer P is concentrated using an evaporator or the like. The obtained concentrate is dried to obtain polymer P. Next, a solution containing polymer P and an ammonium phosphate compound is prepared. The solvent of the solution is, for example, water. Then, the solution is applied to particle 1. For example, the solution can be applied to particle 1 by mixing the solution with particle 1. Then, particle 1 coated with the solution is dried, thereby making it possible to produce positive electrode active material 10.

[0043] A secondary battery containing a conventional positive electrode active material undergoes a side reaction between the lithium composite oxide contained in the positive electrode active material and the non-aqueous solvent contained in the non-aqueous electrolyte during charging of the secondary battery. Specifically, as the positive electrode potential increases due to charging of the secondary battery, the reducing power of the lithium composite oxide increases. As a result, the transition metal contained in the lithium composite oxide is reduced and dissolved in the non-aqueous electrolyte. On the other hand, in the non-aqueous electrolyte, a portion of the non-aqueous solvent is oxidized and decomposed.

[0044] In contrast, the positive electrode active material 10 of the present embodiment imparts insulation to the surface of the particle 1 by means of the ammonium phosphate compound and the polymer P contained in the coating layer 2. The reduction and dissolution of the transition metal contained in the lithium composite oxide are suppressed by the coating layer 2. In particular, the dissolution of nickel, cobalt, manganese, etc., which are easily dissolved from the lithium composite oxide into the non-aqueous electrolyte, can also be suppressed by the coating layer 2. By suppressing the reduction and dissolution of the transition metal, the oxidative decomposition of the non-aqueous solvent is also suppressed. By suppressing the oxidative decomposition of the non-aqueous solvent, the reduction in the discharge capacity retention rate of the secondary battery is suppressed. In this way, the positive electrode active material 10 of the present embodiment improves the cycle characteristics of the secondary battery. In addition, the coating layer 2 is less likely to hinder the movement of lithium ions between the lithium composite oxide and the non-aqueous solvent. Therefore, a secondary battery with a sufficiently high discharge capacity can also be realized by the positive electrode active material 10.

[0045] (Embodiment of Secondary Battery)

[0046] Figure 2 Schematically shows a longitudinal cross-sectional view of a secondary battery 100 including a positive electrode active material according to the present disclosure. Figure 2 As shown, the secondary battery 100 is a cylindrical battery including a cylindrical battery case, a wound electrode group 14, and a non-aqueous electrolyte (not shown). The electrode group 14 is housed in the battery case and is in contact with the non-aqueous electrolyte.

[0047] The battery case is composed of a case body 15 which is a bottomed cylindrical metal container, and a sealing body 16 for sealing the opening of the case body 15. A gasket 27 is arranged between the case body 15 and the sealing body 16. The airtightness of the battery case is ensured by the gasket 27. Insulating plates 17 and 18 are arranged at both ends of the electrode group 14 in the winding axis direction of the electrode group 14 in the case body 15.

[0048] The housing body 15 has, for example, a recessed portion 21. The recessed portion 21 can be formed by partially pressing the side wall of the housing body 15 from the outside. The recessed portion 21 can be formed in an annular shape on the side wall of the housing body 15 along the circumferential direction of an imaginary circle defined by the housing body 15. In this case, the sealing body 16 is supported by, for example, the surface of the recessed portion 21 on the opening side.

[0049] The sealing body 16 includes a filter 22, a lower valve body 23, an insulating member 24, an upper valve body 25, and a cover 26. These members are stacked in sequence in the sealing body 16. The sealing body 16 is attached to the opening of the housing body 15 in such a manner that the cover 26 is located outside the housing body 15 and the filter 22 is located inside the housing body 15.

[0050] Each of the above-mentioned members constituting the sealing body 16 has, for example, a disk shape or a ring shape. The above-mentioned members are electrically connected to each other except for the insulating member 24 .

[0051] The electrode group 14 includes a positive electrode 11, a negative electrode 12, and a separator 13. The positive electrode 11, the negative electrode 12, and the separator 13 are all in a strip shape. The width direction of the strip-shaped positive electrode 11 and the negative electrode 12 is, for example, parallel to the winding axis of the electrode group 14. The separator 13 is arranged between the positive electrode 11 and the negative electrode 12. The positive electrode 11 and the negative electrode 12 are spirally wound with the separator 13 interposed between these electrodes.

[0052] When the cross section of the secondary battery 100 is viewed perpendicular to the winding axis of the electrode group 14 , the positive electrodes 11 and the negative electrodes 12 are alternately stacked in the radial direction of the virtual circle defined by the case body 15 with the separator 13 interposed therebetween.

[0053] The positive electrode 11 is electrically connected to the cap 26 also serving as a positive electrode terminal via the positive electrode lead 19. One end of the positive electrode lead 19 is connected, for example, to the vicinity of the center of the positive electrode 11 in the longitudinal direction of the positive electrode 11. The positive electrode lead 19 passes through a through hole formed in the insulating plate 17 and extends from the positive electrode 11 to the filter 22. The other end of the positive electrode lead 19 is welded, for example, to the surface of the filter 22 on the electrode group 14 side.

[0054] The negative electrode 12 is electrically connected to the case body 15 also serving as a negative electrode terminal via a negative electrode lead 20. One end of the negative electrode lead 20 is connected to, for example, an end of the negative electrode 12 in the longitudinal direction of the negative electrode 12. The other end of the negative electrode lead 20 is welded to the inner bottom surface of the case body 15, for example.

[0055] Hereinafter, the structure of the secondary battery 100 will be described in detail. The secondary battery 100 of the present embodiment can use known materials without particular limitation except for the positive electrode active material.

[0056] [Positive electrode 11]

[0057] Figure 3 yes Figure 2 FIG. 1 is an enlarged cross-sectional view of a secondary battery 100 in region III. Figure 3As shown, the positive electrode 11 has, for example, a positive electrode collector 30 and a positive electrode mixture layer 31. The positive electrode collector 30 and the positive electrode mixture layer 31 are, for example, strip-shaped. The positive electrode collector 30 has, for example, a pair of main surfaces facing each other. "Main surface" refers to the surface of the positive electrode collector 30 with the largest area. The positive electrode mixture layer 31 is, for example, formed on the positive electrode collector 30 and arranged on the surface of the positive electrode collector 30. The positive electrode collector 30 is, for example, in direct contact with the positive electrode mixture layer 31. As shown in FIG. Figure 3 As shown, in the positive electrode 11, two positive electrode mixture layers 31 may be formed on a pair of main surfaces of the positive electrode collector 30, respectively. In the positive electrode 11, only one positive electrode mixture layer 31 may be formed on one main surface of the positive electrode collector 30. In the positive electrode 11, the positive electrode mixture layer 31 may be formed only on one main surface of the positive electrode collector 30, in at least one selected from a region connected to the positive electrode lead 19 and a region not facing the negative electrode 12.

[0058] Examples of the material of the positive electrode current collector 30 include metal materials, such as stainless steel, iron, copper, and aluminum.

[0059] The positive electrode mixture layer 31 may contain the above-mentioned positive electrode active material as an essential component. The positive electrode mixture layer 31 may contain the positive electrode active material as a main component. The content of the positive electrode active material in the positive electrode mixture layer 31 is, for example, 80% by weight or more and 99.5% by weight or less. The positive electrode mixture layer 31 may further contain at least one selected from a conductive material and a binder as an arbitrary component. The positive electrode mixture layer 31 may contain additives other than the conductive material and the binder as needed.

[0060] The conductive material includes, for example, a carbon material. Examples of the carbon material include carbon black, carbon nanotubes, graphite, and the like. Examples of carbon black include acetylene black, Ketjen black, and the like. The positive electrode mixture layer 31 may include one or more conductive materials. Examples of the binder include fluororesins, polyacrylonitrile resins, polyimide resins, acrylic resins, polyolefin resins, rubber-like polymers, and the like. Examples of the fluororesins include polytetrafluoroethylene, polyvinylidene fluoride, and the like. The positive electrode mixture layer 31 may include one or more binders.

[0061] If necessary, a layer containing a conductive carbon material may be disposed between the positive electrode current collector 30 and the positive electrode mixture layer 31. Examples of the carbon material include the materials listed above with respect to the conductive material.

[0062] The positive electrode 11 can be produced, for example, by the following method. First, a slurry containing a material for the positive electrode mixture layer 31 and a dispersion medium is prepared. As the dispersion medium, at least one selected from water and an organic medium can be used. Next, the slurry is applied to the surface of the positive electrode collector 30. The obtained coating is dried and then rolled, thereby making the positive electrode 11. In the case where the positive electrode 11 has a layer containing a carbon material, the layer containing the carbon material is prepared before preparing the positive electrode mixture layer 31. The layer containing the carbon material can be produced, for example, by the following method. First, a dispersion containing a carbon material is prepared. The dispersion is applied to the surface of the positive electrode collector 30. The obtained coating is dried, thereby making the layer containing the carbon material.

[0063] [Negative electrode 12]

[0064] The negative electrode 12 includes a negative electrode current collector 40. Figure 3 As shown, in the secondary battery 100 in the discharge state, the negative electrode 12 is, for example, composed only of the negative electrode collector 40. At this time, it is easy for the secondary battery 100 to ensure a high volume energy density. In the present disclosure, the discharge state refers to a state in which the secondary battery 100 is discharged until a charge state (SOC: State of Charge) of less than 0.05×C when the rated capacity of the secondary battery 100 is defined as C. The discharge state refers to, for example, a state in which the secondary battery 100 is discharged at a constant current of 0.05C until the lower limit voltage of the secondary battery 100. The lower limit voltage of the secondary battery 100 is, for example, 2.5V.

[0065] The negative electrode collector 40 is usually composed of a conductive sheet. The material of the negative electrode collector 40 can be a metal material such as a metal or an alloy. As a metal material, for example, lithium metal and lithium alloys can be cited. The negative electrode collector 40 can be composed of lithium metal or a lithium alloy. The metal material can be a material that does not react with lithium. Such a material includes a material that does not react with at least one selected from lithium metal and lithium ions. More specifically, the metal material can be a material that does not form an alloy or an intermetallic compound with lithium. As such a metal material, for example, copper, nickel, iron and alloys containing these metal elements can be cited. The alloy can be a copper alloy, stainless steel, etc. From the perspective of having high conductivity and easily improving the capacity and charge and discharge efficiency of the secondary battery 100, the metal material can be at least one selected from copper and copper alloys. The negative electrode collector 40 can contain one or more of these metal materials. The negative electrode collector 40 can contain other conductive materials other than metal materials.

[0066] As the negative electrode current collector 40, foil, film, etc. can be used. The negative electrode current collector 40 can be porous. From the viewpoint of easily ensuring high conductivity, the negative electrode current collector 40 can be a metal foil, or a metal foil containing copper. Examples of metal foil containing copper include copper foil and copper alloy foil. The copper content in the metal foil can be 50% by weight or more, or 80% by weight or more. In particular, the metal foil can be a copper foil that essentially contains only copper as a metal. The thickness of the negative electrode current collector 40 is, for example, 5 μm or more and 20 μm or less.

[0067] In the case where the negative electrode 12 of the secondary battery 100 in the discharged state is composed only of the negative electrode collector 40, if the secondary battery 100 is charged, lithium metal will be precipitated on the negative electrode 12. In detail, if the secondary battery 100 is charged, the lithium ions contained in the non-aqueous electrolyte receive electrons from the negative electrode 12. As a result, the lithium ions are changed into lithium metal and precipitated on the negative electrode collector 40. The lithium ions contained in the non-aqueous electrolyte may be ions from a lithium salt added to the non-aqueous electrolyte, may be ions supplied from the positive electrode active material by charging the secondary battery 100, or may be both. The precipitated lithium metal is changed into lithium ions by the discharge of the secondary battery 100 and dissolved in the non-aqueous electrolyte.

[0068] In the secondary battery 100 in the discharged state, the negative electrode 12 may further include a negative electrode active material layer disposed on the surface of the negative electrode collector 40. The negative electrode active material layer contains a negative electrode active material. As the negative electrode active material, a negative electrode active material used in a known lithium ion battery can be used. As the negative electrode active material, for example, lithium metal, lithium alloys, and materials capable of reversibly absorbing and releasing lithium ions can be cited. As lithium alloys, lithium-aluminum alloys and the like can be cited.

[0069] As materials capable of reversibly absorbing and releasing lithium ions, carbon materials, inorganic materials, etc. can be cited. As carbon materials, for example, graphite, soft carbon, hard carbon, amorphous carbon, etc. can be cited. Inorganic materials, for example, include at least one selected from silicon and tin. As inorganic materials, for example, silicon monomer, silicon alloy, silicon compound, tin monomer, tin alloy, tin compound, etc. can be cited. The silicon compound and the tin compound can each be at least one selected from oxides and nitrides.

[0070] The negative electrode active material layer may further include a binder. As the binder, the above-mentioned materials listed for the positive electrode mixture layer 31 can be used. In addition to the negative electrode active material and the binder, the negative electrode active material layer may further include at least one selected from a conductive agent, a thickener, and other additives. The thickness of the negative electrode active material layer is not particularly limited, and in the secondary battery 100 in the discharged state, for example, it is greater than 30 μm and less than 300 μm.

[0071] The method for forming the negative electrode active material layer is not particularly limited. The negative electrode active material layer can be produced by depositing the negative electrode active material on the surface of the negative electrode collector 40 using a gas phase method such as electrolysis or evaporation. The negative electrode active material layer can also be produced by applying a negative electrode mixture containing a negative electrode active material and a binder to the surface of the negative electrode collector 40. The negative electrode mixture can contain other materials in addition to the negative electrode active material and the binder as needed.

[0072] When the negative electrode active material layer contains a material capable of absorbing and releasing lithium ions, the negative electrode active material layer absorbs lithium ions when the secondary battery 100 is charged, and releases lithium ions when the secondary battery 100 is discharged.

[0073] The negative electrode 12 may further include a protective layer. The protective layer is formed, for example, on the surface of the negative electrode current collector 40. When the negative electrode 12 has a negative electrode active material layer, the protective layer may be formed on the surface of the negative electrode active material layer. The protective layer enables the reaction on the surface of the negative electrode 12 to proceed more uniformly. The protective layer makes it easier for, for example, lithium metal to be precipitated more uniformly in the negative electrode 12.

[0074] As the material of the protective layer, a material that does not hinder lithium ion conduction is used. The protective layer is composed of, for example, at least one selected from organic and inorganic substances. As organic substances, polymers having lithium ion conductivity can be cited. Examples of such polymers include polyethylene oxide and polymethyl methacrylate. As inorganic substances, ceramics and solid electrolytes can be cited. As ceramics, SiO 2 、Al 2 O 3 , MgO, etc.

[0075] The solid electrolyte constituting the protective layer is not particularly limited, and examples thereof include sulfide-based solid electrolytes, phosphoric acid-based solid electrolytes, perovskite-based solid electrolytes, garnet-based solid electrolytes, etc. From the viewpoint of low cost and easy availability, the solid electrolyte may be at least one selected from a sulfide-based solid electrolyte and a phosphoric acid-based solid electrolyte.

[0076] The sulfide-based solid electrolyte is not particularly limited as long as it contains sulfur and has lithium ion conductivity. The sulfide-based solid electrolyte may contain S, Li, and other elements. As other elements, for example, at least one selected from P, Ge, B, Si, I, Al, Ga, and As can be cited. As sulfide-based solid electrolytes, Li 2 SP 2 S 5 、70Li 2 S-30P 2 S 5 、80Li2 S-20P 2 S 5 , Li 2 S-SiS 2 ,LiGe 0.25 P 0.75 S 4 wait.

[0077] The phosphoric acid-based solid electrolyte is not particularly limited as long as it contains a phosphoric acid component and has lithium ion conductivity. Examples of the phosphoric acid-based solid electrolyte include Li 1+X Al X Ti 2-X (PO 4 ) 3 , Li 1+X Al X Ge 2-X (PO 4 ) 3 In the above composition formula, X satisfies the following relationship, for example: 0<X<2. X may also satisfy the following relationship: 0<X≤1. 1+ X Al X Ti 2-X (PO 4 ) 3 For example, Li 1.5 Al 0.5 Ti 1.5 (PO 4 ) 3 .

[0078] [Diaphragm 13]

[0079] The separator 13 has, for example, ion permeability and insulation. As the separator 13, for example, a porous sheet can be used. As the separator 13, for example, microporous films, woven fabrics, and nonwoven fabrics can be cited. The material of the separator 13 is not particularly limited, and may be a polymer material.

[0080] As the polymer material, olefin resin, polyamide resin, cellulose, etc. can be mentioned. The olefin resin can contain a polymer containing at least one selected from ethylene and propylene as a monomer unit. The polymer can be a homopolymer or a copolymer. As the polymer, polyethylene, polypropylene, etc. can be mentioned.

[0081] The separator 13 may contain additives other than the polymer material as needed. Examples of the additives include inorganic fillers and the like.

[0082] [Non-aqueous electrolyte]

[0083] The non-aqueous electrolyte includes a non-aqueous solvent and a lithium salt. The lithium salt is dissolved in the non-aqueous solvent. The non-aqueous solvent is not particularly limited, and includes cyclic carbonates, chain carbonates, cyclic carboxylates, chain carboxylates, chain ethers, chain nitriles, etc. Cyclic carbonates, chain carbonates, carboxylates, etc. are compounds that are easily oxidized and decomposed. With the positive electrode active material of this embodiment, a non-aqueous solvent containing a compound that is easily oxidized and decomposed can be used.

[0084] As cyclic carbonate, for example, derivatives in which a part of hydrogen atoms contained in ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, vinylene ethylene carbonate and these compounds are substituted by fluoro groups can be enumerated. As derivatives with fluoro groups, fluoroethylene carbonate, trifluoropropylene carbonate etc. can be enumerated.

[0085] As the chain carbonate, for example, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate and derivatives in which a part of the hydrogen atoms contained in these compounds are substituted by fluorine groups can be cited. As the derivative having a fluorine group, fluorodimethyl carbonate, trifluoroethyl methyl carbonate etc. can be cited.

[0086] Examples of the cyclic carboxylic acid esters include γ-butyrolactone, γ-valerolactone, and derivatives of these compounds in which a part of hydrogen atoms contained therein are substituted with fluorine groups.

[0087] Examples of the chain carboxylic acid esters include methyl acetate, ethyl acetate, propyl acetate, dimethyl methyl acetate, trimethyl methyl acetate, methyl propionate, ethyl propionate, propyl propionate, and derivatives in which a part of hydrogen atoms contained in these compounds are substituted with fluorine groups. Examples of the derivatives having a fluorine group include ethyl trifluoroacetate and methyl trifluoropropionate.

[0088] The nonaqueous solvent may contain one or two or more of the above compounds.

[0089] As lithium salt, LiClO 4 , LiBF 4 、LiPF 6 、LiN(SO 2 F) 2 、LiN(SO 2 CF 3 ) 2 , lithium bis(oxalate)borate (LiBOB (Lithiumbis(oxalate)borate)), lithium difluorooxalateborate (LiDFOB (Lithiumdifluoro(oxalate)borate)), etc. The lithium salt may include, for example, LiBF 4 、LiPF 6 、LiN(SO 2 CF 3 )2 、LiN(SO 2 F) 2 From the viewpoint of further improving the ionic conductivity of the non-aqueous electrolyte, the lithium salt may include at least one selected from LiBF 4 、LiPF 6 、LiN(SO 2 F) 2 The concentration of the lithium salt in the non-aqueous electrolyte is not particularly limited, but is, for example, 0.5 mol / L or more and 3.5 mol / L or less.

[0090] The nonaqueous electrolyte may further include an additive. By means of the additive, a film may be formed on the negative electrode 12. By forming the film from the additive on the negative electrode 12, the charge and discharge reaction of the secondary battery 100 is easily and more uniformly carried out. Thus, in the secondary battery 100, a high discharge capacity can be ensured, and the cycle characteristics can be further suppressed from decreasing. As such an additive, vinylene carbonate, fluoroethylene carbonate, vinyl ethylene carbonate, etc. may be cited. The additive may include one or more of these compounds.

[0091] [other]

[0092] In the present disclosure, a cylindrical secondary battery 100 having a cylindrical battery case is described. However, the secondary battery 100 of the present embodiment is not limited to the above. The secondary battery 100 may be, for example, a square battery having a square battery case, a laminated battery having an outer body including an aluminum-containing laminate sheet, etc. The outer body of the laminated battery may contain a resin. Similarly, the electrode group 14 may not be a wound type. The electrode group 14 may be a stacked electrode group in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked via a separator.

[0093] (Example)

[0094] Hereinafter, the embodiments of the present disclosure will be described in more detail based on examples. The present disclosure is not limited to the following examples.

[0095] <Comparative Examples 1 to 3 and Examples 1 to 17>

[0096] [Manufacturing of Secondary Batteries]

[0097] Follow these steps to make a Figure 2 A secondary battery with the structure shown.

[0098] (1) Polymer P

[0099] First, polyacrylic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) having a weight average molecular weight of 1,000,000 is dissolved in pure water to obtain an aqueous solution. The carboxyl groups contained in the polyacrylic acid are neutralized by adding lithium hydroxide to the aqueous solution. Next, the obtained solution is concentrated using an evaporator. The obtained concentrate is dried at 105° C. for 12 hours using a vacuum dryer to obtain lithium polyacrylate (polymer P).

[0100] (2) Positive electrode active material

[0101] First, prepare the 1.2 Ni 0.133 Co 0.133 Mn 0.533 O 2 Particles formed of the lithium composite oxide represented. In Comparative Examples 1 and 2, the particles were used as positive electrode active materials. In Comparative Example 3, the particles used in Comparative Examples 1 and 2 were coated with lithium polyacrylate. In Examples 1 to 17, the particles used in Comparative Examples 1 and 2 were coated with triammonium phosphate and lithium polyacrylate. The coating of the particles was carried out by the following method. First, lithium polyacrylate and triammonium phosphate were mixed, and the weight ratio of triammonium phosphate to lithium polyacrylate was adjusted to the value shown in Table 1. Next, the obtained mixture was dissolved in pure water to obtain an aqueous solution. Then, the above-mentioned aqueous solution and the particles of the lithium composite oxide were added to an agate mortar, and they were kneaded so that in the obtained positive electrode active material, the ratio A of the weight of the coating layer to the weight of the lithium composite oxide was adjusted to the value shown in Table 1. At this time, the water contained in the aqueous solution evaporated, and triammonium phosphate and lithium polyacrylate precipitated. As a result, the particles of the lithium composite oxide were coated with the ammonium phosphate compound and lithium polyacrylate. The obtained particles were dried at 105°C under vacuum for 12 hours to obtain a positive electrode active material.

[0102] (3) Positive electrode

[0103] The positive electrode active material obtained in (2) above, acetylene black as a conductive material, and polyvinylidene fluoride as a binder are mixed in a mass ratio of 100:3:1. An appropriate amount of N-methyl-2-pyrrolidone is added to the obtained mixture as a dispersion medium. The mixture and the dispersion medium are stirred to prepare a positive electrode mixture slurry.

[0104] Next, prepare aluminum foil as a positive electrode collector. Apply a positive electrode mixture slurry to a pair of main surfaces of the aluminum foil. Dry the obtained coating film to obtain a dried product. Then, use a roller to compress the dried product in the thickness direction of the dried product. Cut the obtained laminate into a predetermined size to obtain a positive electrode having a positive electrode mixture layer on a pair of main surfaces of the positive electrode collector. Furthermore, a positive electrode mixture layer is not formed in a part of the main surface of the positive electrode collector. In this area, the positive electrode collector is exposed to the outside. In this area, one end of the aluminum positive electrode lead is welded and installed to the positive electrode collector.

[0105] (4) Negative electrode

[0106] A negative electrode was produced by cutting an electrolytic copper foil having a thickness of 12 μm into a predetermined size.

[0107] (5) Non-aqueous electrolytes

[0108] First, prepare the non-aqueous solvent and lithium salt shown in Table 1. The non-aqueous solvent is a mixture of two compounds. Table 1 also shows the volume ratio of the two compounds in the non-aqueous solvent. Next, the lithium salt is dissolved in the non-aqueous solvent to obtain a liquid non-aqueous electrolyte. The concentration of the lithium salt in the non-aqueous electrolyte is 1.0 mol / L. The non-aqueous solvent and lithium salt shown in Table 1 are as follows.

[0109] Non-aqueous solvents

[0110] (a) FEC: Fluoroethylene carbonate

[0111] (b) DMC: dimethyl carbonate

[0112] (c) MA: methyl acetate

[0113] Lithium salts

[0114] (d)LiPF 6 :Lithium hexafluorophosphate

[0115] (e) LiFSI: Lithium bissulfonyl imide

[0116] (6) Secondary battery

[0117] Under an inert gas atmosphere, the positive electrode obtained in (3) above and the negative electrode obtained in (4) above are stacked with a separator. As a separator, a microporous film made of polyethylene is used. In detail, the positive electrode, the separator, the negative electrode and the separator are stacked in this order. The obtained stack is spirally wound to produce an electrode group. The obtained electrode group is housed in a bag-shaped outer body. The outer body is composed of a laminated sheet having an Al layer. Next, a non-aqueous electrolyte is injected into the outer body and the outer body is sealed. Thus, the secondary batteries of Comparative Examples 1 to 3 and Examples 1 to 17 are obtained.

[0118] [Evaluation of Secondary Batteries]

[0119] The obtained secondary battery was subjected to a charge and discharge test in the following procedure to evaluate the discharge capacity and cycle characteristics of the secondary battery.

[0120] First, the secondary battery was charged in a thermostatic chamber at 25° C. Then, the secondary battery was discharged after a 20-minute pause. The conditions for charging and discharging the secondary battery were as follows.

[0121] (Charge)

[0122] First, constant current charging was performed at a current of 10 mA per square centimeter of the electrode area. Constant current charging was performed until the battery voltage of the secondary battery reached 4.7 V. Next, constant voltage charging was performed at a voltage of 4.7 V. Constant voltage charging was performed until the current value per square centimeter of the electrode area reached 1 mA.

[0123] (Discharge)

[0124] The constant current discharge was performed at a current of 10 mA per square centimeter of the electrode area until the battery voltage of the secondary battery reached 2.5V.

[0125] The above-mentioned charge and discharge is defined as 1 cycle. In the charge and discharge test, the above-mentioned charge and discharge are performed for 60 cycles. The discharge capacity of the secondary battery at the 1st cycle is defined as the initial discharge capacity. The ratio of the discharge capacity of the secondary battery at the 60th cycle to the initial discharge capacity is defined as the discharge capacity retention rate (%). The discharge capacity retention rate can be used as an indicator of the cycle characteristics of the secondary battery. The evaluation results of the secondary batteries of Comparative Examples 1 to 3 and Examples 1 to 17 are shown in Table 1. Table 1 also shows the non-aqueous solvent and lithium salt used for the non-aqueous electrolyte.

[0126] Table 1

[0127]

[0128] From the comparison of Comparative Examples 1 and 2 with Examples 1 to 17, it can be seen that in the case where the particles containing lithium composite oxides in the positive electrode active material are coated with a coating layer containing an ammonium phosphate compound and a polymer P, the reduction in the discharge capacity retention rate of the secondary battery containing the positive electrode active material is fully suppressed. In other words, the secondary battery containing the positive electrode active material has improved cycle characteristics. In addition, from the comparison of Comparative Example 3 with Examples 1 to 17, it can be seen that a secondary battery with a high initial discharge capacity can be obtained by including an ammonium phosphate compound in the coating layer. In Comparative Example 3, the coating layer composed only of lithium polyacrylate is hard and lacks flexibility. It is speculated that in Comparative Example 3, the hard coating layer acts as a resistance component that hinders the movement of lithium ions.

[0129] From the comparison of Comparative Examples 1 and 2, it can be seen that the non-aqueous solvent containing carboxylic acid ester has a tendency to reduce the discharge capacity maintenance rate of the secondary battery compared to the non-aqueous solvent composed of carbonate ester. However, from the comparison of Examples 12 and 13, it can be seen that the positive electrode active material of this embodiment can achieve a high discharge capacity maintenance rate even when the non-aqueous solvent contains carboxylic acid ester.

[0130] As can be seen from Examples 1 to 17, the ratio A of the weight of the coating layer to the weight of the lithium composite oxide can be 0.3 wt % or more and 2.0 wt % or less.

[0131] <Examples 18 to 20>

[0132] Secondary batteries of Examples 18 to 20 were prepared in the same manner as in Example 12 except that lithium polyacrylate having a weight average molecular weight shown in Table 2 was used. The obtained secondary batteries were subjected to the above-mentioned charge and discharge test to evaluate the discharge capacity and cycle characteristics of the secondary batteries. The results are shown in Table 2.

[0133] Table 2

[0134]

[0135] From the comparison of Examples 12 and 18 to 20 with Comparative Example 1, it can be seen that the positive electrode active material of the present embodiment improves the cycle characteristics of the secondary battery regardless of the weight average molecular weight of the lithium polyacrylate. In particular, it can be seen from Examples 12, 19 and 20 that when the weight average molecular weight of the lithium polyacrylate is 250,000 or more, the cycle characteristics of the secondary battery are further improved. Therefore, in the positive electrode active material of the present embodiment, the weight average molecular weight of the lithium polyacrylate can be 25,000 or more and 1,000,000 or less, or 250,000 or more and 1,000,000 or less.

[0136] Industrial Availability

[0137] The positive electrode active material disclosed in the present invention can improve the cycle characteristics of the secondary battery. Therefore, the secondary battery containing the positive electrode active material disclosed in the present invention can be used for various purposes such as electronic devices such as mobile phones, smart phones, and tablet terminals, electric vehicles including hybrid power, plug-in hybrid power, and household storage batteries combined with solar cells.

[0138] Description of Reference Numerals

[0139] 1 Particle

[0140] 2 Coating layer

[0141] 10. Positive electrode active material

[0142] 11 Positive electrode

[0143] 12 Negative electrode

[0144] 13 Diaphragm

[0145] 14 Electrode Group

[0146] 15 Shell body

[0147] 16 Sealing body

[0148] 17, 18 Insulation board

[0149] 19 Positive lead

[0150] 20 Negative lead

[0151] 21 recess

[0152] 22 Filters

[0153] 23 Lower valve body

[0154] 24 Insulation components

[0155] 25 Upper valve body

[0156] 26 Cover

[0157] 27 Gasket

[0158] 30 Positive electrode collector

[0159] 31. Positive electrode mixture layer

[0160] 40 Negative electrode collector

[0161] 100 Secondary batteries

Claims

1. A positive electrode active material having: Particles comprising a lithium composite oxide; and a coating layer coating the particles, The coating layer contains an ammonium phosphate compound and a polymer having a structural unit represented by the following formula (1): In formula (1), R is a hydrogen atom or a methyl group.

2. The positive electrode active material according to claim 1, The polymer is lithium polyacrylate.

3. The positive electrode active material according to claim 1, A ratio of the weight of the coating layer to the weight of the lithium composite oxide is 0.3 wt % or more and 2.0 wt % or less.

4. The positive electrode active material according to claim 1, The ratio of the weight of the ammonium phosphate compound to the weight of the polymer is 1 / 9 or more and 9 / 1 or less.

5. The positive electrode active material according to claim 1, The lithium composite oxide includes at least one selected from the group consisting of nickel, cobalt, and manganese.

6. The positive electrode active material according to claim 1, The lithium composite oxide has a crystal structure belonging to the space group R-3m or C2 / m.

7. A secondary battery comprising: A positive electrode comprising the positive electrode active material according to claim 1; a negative electrode comprising a negative electrode active material capable of occluding and releasing lithium ions; and A non-aqueous electrolyte includes a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent.

8. A secondary battery comprising: A positive electrode having a positive electrode current collector and a positive electrode mixture layer containing the positive electrode active material according to claim 1; a negative electrode having a negative electrode current collector; and a nonaqueous electrolyte comprising a nonaqueous solvent and a lithium salt dissolved in the nonaqueous solvent, During charge, lithium metal is deposited on the negative electrode current collector, and during discharge, the lithium metal is dissolved in the non-aqueous electrolyte.

9. The secondary battery according to claim 7, The lithium salt includes at least one selected from LiBF4, LiPF6, LiN(SO2CF3)2, LiN(SO2F)2, lithium bis(oxalatoborate), and lithium difluorooxalatoborate.

10. The secondary battery according to claim 8, The lithium salt includes at least one selected from LiBF4, LiPF6, LiN(SO2CF3)2, LiN(SO2F)2, lithium bis(oxalatoborate), and lithium difluorooxalatoborate.

11. The secondary battery according to claim 9, The concentration of the lithium salt in the non-aqueous electrolyte is 0.5 mol / L or more and 3.5 mol / L or less.

12. The secondary battery according to claim 10, The concentration of the lithium salt in the non-aqueous electrolyte is 0.5 mol / L or more and 3.5 mol / L or less.