Semiconductor chip manufacturing method
By using an adhesive sheet with non-expandable and expandable base material layers in the manufacturing of semiconductor chips, the expansion of the expandable particles is used to generate unevenness, which solves the problem of insufficient adhesion of the thermally expandable adhesive layer and realizes the production of semiconductor chips. Efficient manufacturing and efficient separation improve production efficiency.
Patent Information
- Application Number
- CN201980030707.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-04-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-04-26
AI Technical Summary
In the existing semiconductor chip manufacturing methods, the insufficient adhesive force of the thermally expandable adhesive layer causes the semiconductor wafer to be insufficiently fixed, which easily causes chip end defects, and is difficult to separate at one time during the peeling process, and may lead to contamination of the support, affecting the Production efficiency.
Adopting an adhesive sheet with a non-expandable base material layer and an expandable base material layer, the expansion of the expandable particles creates unevenness on the surface of the adhesive layer, reducing the contact area with the support, improving the adhesive force, and improving the separation process This makes the adhesive sheet easy to separate and avoids contamination of the support body.
It effectively suppresses end defects of the semiconductor chip, improves the yield, realizes easy separation of the support and the adhesive sheet, omits the cleaning process of the support, and improves production efficiency.
Smart Images

Figure CN112088421B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for manufacturing a semiconductor chip. Background Art
[0002] In the manufacturing process of semiconductor chips, various processes are often performed with the semiconductor wafer attached to a support using an adhesive sheet.
[0003] The adhesive sheet used in this case is required to have properties that allow the semiconductor wafer to be sufficiently fixed during processing and can be easily peeled from the support after processing.
[0004] As a PSA sheet that can meet such a demand, a heat-peelable PSA sheet having a heat-expandable PSA layer containing heat-expandable particles is known.
[0005] For example, Patent Document 1 discloses a method in which a heat-expandable double-sided adhesive sheet having a heat-expandable adhesive layer containing heat-expandable microspheres on one side of a substrate and an adhesive layer on the other side is used, the heat-expandable adhesive layer is pasted to a support, and an adherend such as a wafer is pasted to the adhesive layer on the other side to process the adherend.
[0006] According to Patent Document 1, by using the above-mentioned heat-peelable double-sided PSA sheet, the smoothness of the adherend surface can be maintained during processing of the adherend, and the stress when peeling the double-sided PSA sheet after processing can be reduced, thereby making it easy to peel without damaging the adherend.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2003-292916 Summary of the invention
[0010] Problem that the invention aims to solve
[0011] In the method for processing an adherend described in Patent Document 1, the heat-expandable adhesive layer of the double-sided adhesive sheet is attached to a support, and the adherend is bonded to the other adhesive layer to process the adherend.
[0012] However, the heat-expandable adhesive layer of the double-sided adhesive sheet used in the processing method of Patent Document 1 contains heat-expandable microspheres, and therefore has a tendency to have lower adhesive strength with a support than an adhesive layer not containing heat-expandable microspheres.
[0013] The reduction in adhesion to the support body is the main cause of various problems caused by insufficient fixation of the adherend to the support body. For example, in chip processing methods such as pre-dicing and stealth dicing, which grind the back of the wafer to separate into chips, the end of the obtained chip may be damaged due to insufficient fixation to the support body.
[0014] In Patent Document 1, when peeling a double-sided PSA sheet from a support, heat treatment is performed to expand heat-expandable microspheres, thereby forming irregularities on the surface of the heat-expandable PSA layer to reduce the contact area with the support, thereby reducing the adhesive force and causing peeling.
[0015] However, in the above-mentioned stripping method, when the double-sided adhesive sheet is stripped from the support, a little adhesive force may remain sometimes, so it is difficult to strip in some cases. In addition, after stripping, a part of the heat-expandable adhesive layer may remain on the surface of the support sometimes, requiring a cleaning process for the support, which may become the main reason causing the productivity to decrease.
[0016] It should be noted that in order to prevent contamination of the support, it is also possible to consider selecting a resin with low adhesion as the adhesive resin constituting the heat-expandable adhesive layer, but in this case, as described above, there may be a disadvantage that the adherend cannot be fully fixed to the adherend during processing of the adherend.
[0017] The object of the present invention is to provide a method for manufacturing a semiconductor chip, which can suppress end defects of the semiconductor chip and improve the yield, and can easily separate the support body from the adhesive sheet to which it is attached at one time. At the same time, it can also suppress the contamination of the support body after separation, thereby omitting the cleaning process of the support body.
[0018] Solutions to the problem
[0019] The present inventors have found that the above problems can be solved by using a PSA sheet having a first PSA layer and a second PSA layer on both sides of a substrate having at least a non-expandable substrate layer and an expandable substrate layer containing expandable particles in a process of dividing a semiconductor wafer to produce semiconductor chips.
[0020] That is, the present invention relates to the following [1] to
[11] .
[0021] [1] A method for producing a semiconductor chip, which is a method for producing a semiconductor chip from a semiconductor wafer using an adhesive sheet, the adhesive sheet comprising a substrate (Y) and a first adhesive layer (X1) and a second adhesive layer (X2) on both sides of the substrate (Y), wherein the substrate (Y) comprises at least an expandable substrate layer (Y1) containing expandable particles and a non-expandable substrate layer (Y2),
[0022] The adhesive sheet can generate irregularities on the adhesive surface of the first adhesive layer (X1) due to the expansion of the expandable particles.
[0023] The method for manufacturing the semiconductor chip comprises the following steps (1) to (3):
[0024] Step (1): a step of attaching the adhesive surface of the first adhesive layer (X1) to a rigid support and attaching the adhesive surface of the second adhesive layer (X2) to a surface of a semiconductor wafer;
[0025] Step (2): a step of dividing the semiconductor wafer to obtain a plurality of semiconductor chips.
[0026] Step (3): a step of expanding the expandable particles to separate the plurality of semiconductor chips bonded to the second adhesive layer (X2) at the interface P between the rigid support and the first adhesive layer (X1).
[0027] [2] A method for manufacturing a semiconductor chip according to the above-mentioned [1], wherein the above-mentioned adhesive sheet has a first adhesive layer (X1) on the above-mentioned expandable substrate layer (Y1) side of the above-mentioned substrate (Y), and has the above-mentioned second adhesive layer (X2) on the above-mentioned non-expandable substrate layer (Y2) side of the substrate (Y).
[0028] [3] The method for manufacturing a semiconductor chip according to [1] above, wherein the substrate (Y) comprises the expandable substrate layer (Y1), a non-expandable substrate layer (Y2-1) provided on the first adhesive layer (X1) side of the expandable substrate layer (Y1), and a non-expandable substrate layer (Y2-2) provided on the second adhesive layer (X2) side of the expandable substrate layer (Y1),
[0029] The storage modulus E' of the non-expandable base layer (Y2-1) when the expandable particles expand is lower than the storage modulus E' of the non-expandable base layer (Y2-2) when the expandable particles expand.
[0030] [4] The method for manufacturing a semiconductor chip according to [1] or [2], wherein the non-expandable substrate layer (Y2) is located farther from the first adhesive layer (X1) than the expandable substrate layer (Y1), and the non-expandable substrate layer (Y2) is not present between the expandable substrate layer (Y1) and the first adhesive layer (X1).
[0031] The storage modulus E' of the non-expandable base layer (Y2) when the expandable particles expand is larger than the storage modulus E' of the expandable base layer (Y1) when the expandable particles expand.
[0032] [5] The method for manufacturing a semiconductor chip according to any one of [1] to [4] above, wherein in step (3), when the expandable particles are expanded, separation does not occur between the layers constituting the adhesive sheet.
[0033] [6] The method for manufacturing a semiconductor chip according to any one of [1] to [5] above, further comprising the following step (4):
[0034] Step (4): After separation from the hard support in step (3), the back surfaces of the plurality of semiconductor chips opposite to the circuit surfaces are attached to a transfer tape, and then the adhesive sheet is removed from the semiconductor chips, wherein the transfer tape has a base film and has an adhesive layer and / or a bonding agent layer.
[0035] [7] The method for manufacturing a semiconductor chip according to any one of [1] to [6] above, wherein the expandable particles are heat-expandable particles having an expansion starting temperature (t) of 60 to 270°C.
[0036] [8] A method for manufacturing a semiconductor chip according to [7] above, wherein the expansion of the heat-expandable particles is performed by heating the heat-expandable particles at a temperature between "expansion starting temperature (t) + 10°C" and "expansion starting temperature (t) + 60°C".
[0037] [9] The method for manufacturing a semiconductor chip according to [7] or [8], wherein the expandable substrate layer (Y1) is a heat-expandable substrate layer (Y1-1) containing the heat-expandable particles, and the heat-expandable substrate layer (Y1-1) has a storage modulus E'(23) at 23°C of 1.0×10 6 Pa or above.
[0038]
[10] The method for manufacturing a semiconductor chip according to any one of [1] to [9] above, wherein the volume change rate (%) of the non-expandable base material layer (Y2) is less than 2 volume %.
[0039]
[11] A method for manufacturing a semiconductor chip according to any one of [1] to
[10] above, wherein step (2) is a step of grinding the back side of the semiconductor wafer having a modified region which is opposite to the circuit surface and on which no circuit is formed, thereby dividing the semiconductor wafer into a plurality of semiconductor chips.
[0040] Effects of the Invention
[0041] According to the method for manufacturing a semiconductor chip of the present invention, end defects of the obtained semiconductor chip can be suppressed to improve the yield, and the support body and the adhesive sheet to which they are attached can be easily separated at one time. At the same time, the contamination of the support body after separation can be suppressed, thereby omitting the cleaning process of the support body, thereby improving productivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] [ Figure 1 ] A cross-sectional schematic diagram of an adhesive sheet showing an example of the structure of the adhesive sheet used in the method for manufacturing a semiconductor chip of the present invention.
[0043] [ Figure 2 ] A schematic cross-sectional view of steps (1) to (3) of the method for manufacturing a semiconductor chip of the present invention.
[0044] [ Figure 3 ] A schematic cross-sectional view of steps (4) to (6) of the method for manufacturing a semiconductor chip of the present invention.
[0045] Explanation of symbols
[0046] 1a, 1b Adhesive sheet
[0047] (X1) 1st adhesive layer
[0048] (X2) Second adhesive layer
[0049] (Y) Base material
[0050] (Y1) Expandable base material layer
[0051] (Y2) Non-expandable base material layer
[0052] (Y2-1) First non-expandable base material layer
[0053] (Y2-2) Second non-expandable base material layer
[0054] 50 Hard support
[0055] 60 semiconductor wafer
[0056] 61 Circuit surface
[0057] 62 Back
[0058] 70 Semiconductor Chip
[0059] 71 Circuit board
[0060] 72 Back
[0061] 80 Transfer belt
[0062] 81 Base film
[0063] 82 adhesive layer DETAILED DESCRIPTION
[0064] In this specification, whether a target layer is an "expandable layer" or a "non-expandable layer" is determined based on the volume change rate before and after the treatment calculated by the following formula after the treatment for expansion for 3 minutes.
[0065] Volume change rate (%) = {(volume of the above layer after treatment - volume of the above layer before treatment) / volume of the above layer before treatment} × 100
[0066] That is, if the volume change rate is 5 volume % or more, the layer is judged to be an "expandable layer", and if the volume change rate is less than 5 volume %, the layer is judged to be a "non-expandable layer".
[0067] In addition, as "treatment for expansion", when the expandable particles are heat-expandable particles, for example, a heating treatment for 3 minutes may be performed at the expansion starting temperature (t) of the heat-expandable particles.
[0068] In the present specification, the "active ingredient" refers to the ingredients contained in the target composition excluding the diluent solvent.
[0069] The weight average molecular weight (Mw) is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene, and specifically, is a value measured by the method described in Examples.
[0070] In this specification, for example, "(meth)acrylic acid" means both "acrylic acid" and "methacrylic acid", and the same applies to other similar terms.
[0071] In addition, regarding the preferred numerical range (e.g., the range of the content, etc.), the lower limit and upper limit described in the segment can be independently combined. For example, according to the description of "preferably 10 to 90, more preferably 30 to 60", the "preferable lower limit (10)" and the "more preferably upper limit (60)" can also be combined to obtain "10 to 60".
[0072] [Method for manufacturing semiconductor chip of the present invention]
[0073] The method for manufacturing a semiconductor chip of the present invention (hereinafter also referred to as the "manufacturing method of the present invention") is a method for manufacturing a semiconductor chip from a semiconductor wafer using an adhesive sheet, wherein the adhesive sheet has a substrate (Y) and has a first adhesive layer (X1) and a second adhesive layer (X2) on both sides of the substrate (Y), respectively, wherein the substrate (Y) has at least an expandable substrate layer (Y1) containing expandable particles and a non-expandable substrate layer (Y2), and the adhesive sheet can produce projections and depressions on the adhesive surface of the first adhesive layer (X1) by the expansion of the above-mentioned expandable particles.
[0074] Furthermore, the production method of the present invention includes the following steps (1) to (3).
[0075] Step (1): A step of attaching the adhesive surface of the first adhesive layer (X1) to a rigid support and attaching the adhesive surface of the second adhesive layer (X2) to the surface of a semiconductor wafer.
[0076] Step (2): a step of dividing the semiconductor wafer to obtain a plurality of semiconductor chips.
[0077] Step (3): a step of expanding the expandable particles to separate the plurality of semiconductor chips bonded to the second adhesive layer (X2) at the interface P between the rigid support and the first adhesive layer (X1).
[0078] [Constitution of the Pressure-Sensitive Adhesive Sheet Used in the Production Method of the Present Invention]
[0079] Figure 1 This is a schematic cross-sectional view of a PSA sheet showing an example of the structure of the PSA sheet used in the production method of the present invention.
[0080] The pressure-sensitive adhesive sheet used in the production method of the present invention can be exemplified by Figure 1 As shown in (a), a pressure-sensitive adhesive sheet 1a comprises a substrate (Y) having at least an expandable substrate layer (Y1) and a non-expandable substrate layer (Y2), and a first pressure-sensitive adhesive layer (X1) and a second pressure-sensitive adhesive layer (X2) on both surfaces of the substrate (Y).
[0081] Figure 1 The substrate (Y) of the pressure-sensitive adhesive sheet 1a shown in (a) has a structure in which an expandable substrate layer (Y1) and a non-expandable substrate layer (Y2) are directly laminated, but the substrate (Y) may have other structures.
[0082] For example, you can also Figure 1 Like the substrate (Y) of the pressure-sensitive adhesive sheet 1b shown in (b), the first non-thermally expandable substrate layer (Y2-1) and the second non-thermally expandable substrate layer (Y2-2) are provided on both sides of the expandable substrate layer (Y1).
[0083] In addition, the pressure-sensitive adhesive sheet used in one embodiment of the present invention may be configured such that a release material is further laminated on the pressure-sensitive adhesive surface of the first pressure-sensitive adhesive layer (X1) and the pressure-sensitive adhesive surface of the second pressure-sensitive adhesive layer (X2).
[0084] In this configuration, a release material having both surfaces subjected to release treatment is laminated on the adhesive surface of one of the first adhesive layer (X1) and the second adhesive layer (X2) and rolled into a roll.
[0085] These release materials are provided to protect the adhesive surfaces of the first adhesive layer (X1) and the second adhesive layer (X2), and are removed when the adhesive sheet is used.
[0086] In addition, for example, Figure 1 In the adhesive sheet 1a shown in (a), when the peeling force when peeling off the peeling material stacked on the first adhesive layer (X1) and the peeling force when peeling off the peeling material stacked on the second adhesive layer (X2) are of the same level, sometimes the peeling materials on both sides need to be pulled outward to peel off, causing the adhesive sheet 1a to be cut and peeled off along with the two peeling materials.
[0087] Therefore, it is preferable to use two kinds of release materials designed to have different release forces from mutually adhered pressure-sensitive adhesive layers, as the release material laminated on the first pressure-sensitive adhesive layer (X1) and the release material laminated on the second pressure-sensitive adhesive layer (X2).
[0088] The PSA sheet used in the production method of the present invention is adjusted so that projections and depressions can be generated on the adhesive surface of the first PSA layer (X1) due to the expansion of the expandable particles.
[0089] For example, in Figure 1 The pressure-sensitive adhesive sheet 1a shown in (a) has a structure in which a first pressure-sensitive adhesive layer (X1) is laminated on an expandable base layer (Y1) containing expandable particles, and a second pressure-sensitive adhesive layer (X2) is laminated on a non-expandable base layer (Y2).
[0090] In the adhesive sheet 1a, when the expandable particles in the expandable substrate layer (Y1) expand, unevenness is generated on the surface of the expandable substrate layer (Y1), and the first adhesive layer (X1) in contact with the surface is lifted up by the unevenness. As a result, unevenness is also generated on the adhesive surface of the first adhesive layer (X1).
[0091] In the production method of the present invention, as in the above step (1), the adhesive surface of the first adhesive layer (X1) is attached to a rigid support.
[0092] Furthermore, in the above-mentioned step (3), when the expandable particles are expanded, projections and depressions are generated on the adhesive surface of the first adhesive layer (X1), thereby reducing the contact area with the rigid support body, so that the rigid support body and the first adhesive layer (X1) can be easily separated at one time with a very small force at the interface P.
[0093] Furthermore, when the expandable particles are expanded, the expandable base layer (Y1) and the non-expandable base layer (Y2) can be easily separated at one time with a very small force at the interface.
[0094] On the other hand, as in the above step (1), the surface of the semiconductor wafer is adhered to the adhesive surface of the second adhesive layer (X2), and in the step (2), the semiconductor wafer is divided to obtain a plurality of semiconductor chips. Then, as specified in the above step (3), when the expandable particles are expanded, the plurality of semiconductor chips on the second adhesive layer (X2) can be separated at the interface P between the hard support and the first adhesive layer (X1) while being adhered.
[0095] That is, when separating from the rigid support, the plurality of semiconductor chips must be held on the second adhesive layer (X2) of the adhesive sheet.
[0096] For this purpose, the adhesive surface of the second adhesive layer (X2) is preferably adjusted to suppress the formation of irregularities so that the adhesive force does not decrease even when the expandable particles expand.
[0097] For example, in Figure 1 In the pressure-sensitive adhesive sheet 1a shown in (a), a non-expandable base layer (Y2) is provided on the surface of the expandable base layer (Y1) opposite to the first pressure-sensitive adhesive layer (X1), and a second pressure-sensitive adhesive layer (X2) is laminated on the surface of the non-expandable base layer (Y2).
[0098] In the adhesive sheet 1a, when the expandable particles expand, the stress from the expandable substrate layer (Y1) side caused by the expansion of the expandable particles is absorbed by the non-expandable substrate layer (Y2) due to the presence of the non-expandable substrate layer (Y2). As a result, the formation of unevenness on the adhesive surface of the second adhesive layer (X2) laminated on the non-expandable substrate layer (Y2) is suppressed, so that the semiconductor chip attached to the adhesive surface can be held.
[0099] It should be noted that in Figure 1 In the pressure-sensitive adhesive sheet 1b shown in (b), the storage elastic modulus E' of the first non-expandable base layer (Y2-1) is preferably adjusted to be low so that when the expandable particles expand, irregularities are formed on the adhesive surface of the first pressure-sensitive adhesive layer (X1).
[0100] On the other hand, the storage elastic modulus E' of the second non-heat-expandable base layer (Y2-2) is preferably adjusted to be high so that the formation of irregularities on the adhesive surface of the second adhesive layer (X2) is suppressed when the expandable particles expand.
[0101] That is, the storage modulus E' of the first non-expandable base layer (Y2-1) when the expandable particles expand is preferably adjusted to be lower than the storage modulus E' of the second non-heat-expandable base layer (Y2-2) when the expandable particles expand.
[0102] It should be noted that, when a double-sided adhesive sheet having an expandable adhesive layer containing expandable particles is used as described in Patent Document 1, the expandable adhesive layer is attached to a rigid support, and a semiconductor wafer is attached to the adhesive layer on the other side to manufacture a semiconductor chip, the expandable adhesive layer attached to the rigid support contains expandable particles, and therefore its adhesive strength tends to become insufficient.
[0103] Due to the reduced adhesive force of the expandable adhesive layer to the rigid support, the semiconductor wafer cannot be sufficiently fixed to the rigid support. For example, when the semiconductor wafer is divided into a plurality of semiconductor chips, the end of the obtained chip may be damaged.
[0104] In addition, when using the Stealth Dicing (registered trademark, the same below) method to manufacture semiconductor chips, it is necessary to set a modified area inside the semiconductor wafer, and the more the number of modified areas increases, the easier it is to cause the semiconductor wafer to warp. Here, if the semiconductor wafer is not sufficiently fixed to the hard support, the warping of the semiconductor wafer cannot be completely suppressed, which will become the main cause of chip breakage, etc.
[0105] On the other hand, it is also conceivable that the above-mentioned disadvantages can be avoided by selecting an adhesive resin so that the adhesive layer or expandable adhesive layer for bonding the semiconductor wafer has high adhesive strength.
[0106] However, when the adhesive layer to which the semiconductor wafer is bonded has high adhesive strength, it may become difficult to peel the obtained plurality of semiconductor chips from the adhesive layer.
[0107] In addition, when the expandable adhesive layer has a high adhesive force, when the expandable particles are expanded and the double-sided adhesive sheet is peeled off from the rigid support, a part of the expandable adhesive layer may remain on the surface of the rigid support, and a cleaning process of the support may be required, which may also be a major cause of reduced productivity. In addition, a certain degree of force is required to peel off the double-sided adhesive sheet attached to the rigid support, and it is sometimes difficult to peel off easily at one time.
[0108] On the other hand, the adhesive sheet used in the manufacturing method of the present invention has a substrate (Y) having at least an expandable substrate layer (Y1) containing expandable particles and a non-expandable substrate layer (Y2), and is adjusted so that when the expandable particles expand, projections and depressions are formed on the adhesive surface of the first adhesive layer (X1).
[0109] Therefore, the first adhesive layer (X1) attached to the rigid support does not need to contain expandable particles, so the semiconductor wafer can be sufficiently fixed to the rigid support, and disadvantages such as chip edge chipping can be effectively suppressed, thereby improving the yield.
[0110] Furthermore, when the rigid support and the attached pressure-sensitive adhesive sheet are separated, they can be easily separated at one time, and contamination of the rigid support after separation can be suppressed, thereby omitting the support cleaning step and improving productivity.
[0111] Furthermore, the degree of freedom in selecting the adhesive composition as the material for forming the first adhesive layer (X1) and the second adhesive layer (X2) is also high.
[0112] [Various properties of adhesive sheets]
[0113] The adhesive sheet used in one embodiment of the present invention produces projections and depressions on the adhesive surface of the first adhesive layer (X1) adhered to the rigid support body due to the expansion of the expandable particles, thereby being easily separated at one time with a very small force at the interface P between the rigid support body and the first adhesive layer (X1).
[0114] Here, in the PSA sheet used in one embodiment of the present invention, the peeling force (F) when the expandable particles are expanded and separated at the interface P is 1 ), usually 0 to 2000 mN / 25 mm, preferably 0 to 1000 mN / 25 mm, more preferably 0 to 150 mN / 25 mm, further preferably 0 to 100 mN / 25 mm, and still further preferably 0 to 50 mN / 25 mm.
[0115] It should be noted that the peeling force (F 1 ) is 0 mN / 25 mm, the peel force may be too small to be measured even if the peel force is measured by the method described in the examples.
[0116] On the other hand, when a plurality of semiconductor chips are produced from a semiconductor wafer before the expandable particles expand, the higher the adhesive force of the first adhesive layer (X1) is, the more preferably it is from the viewpoint of suppressing chip edge defects and improving the yield.
[0117] From the above viewpoints, in the PSA sheet used in one embodiment of the present invention, the peeling force (F) when the expandable particles separate at the interface P before expansion is 0 ), preferably 0.05 to 10.0 N / 25 mm, more preferably 0.1 to 8.0 N / 25 mm, further preferably 0.15 to 6.0 N / 25 mm, and further preferably 0.2 to 4.0 N / 25 mm.
[0118] It should be noted that the above peeling force (F 0 ) can also be regarded as the adhesive force of the first adhesive layer (X1) with respect to the rigid support.
[0119] In the pressure-sensitive adhesive sheet used in one embodiment of the present invention, the peel force (F 1 ) and peeling force (F 0 ) ratio [(F 1 ) / (F 0 )] is preferably 0 to 0.9, more preferably 0 to 0.8, further preferably 0 to 0.5, and further preferably 0 to 0.2.
[0120] It should be noted that the peeling force (F 1 ) is a value measured in an environment where the expandable particles expand. For example, when the expandable particles are heat-expandable particles, the peeling force (F 1 ) as long as the temperature is above the expansion starting temperature (t) of the heat-expandable particles.
[0121] On the other hand, as a test piece for the peeling force (F 0 ) is preferably at a temperature at which the expandable particles do not expand, and is basically room temperature (23° C.).
[0122] Among them, the peel force (F 1 ) and peeling force (F 0 ) are based on the method described in the Examples.
[0123] In addition, in the pressure-sensitive adhesive sheet used in one embodiment of the present invention, the pressure-sensitive adhesive strength of the second pressure-sensitive adhesive layer (X2) at room temperature (23° C.) is preferably 0.1 to 10.0 N / 25 mm, more preferably 0.2 to 8.0 N / 25 mm, further preferably 0.4 to 6.0 N / 25 mm, and further preferably 0.5 to 4.0 N / 25 mm.
[0124] In the present specification, the adhesive force of the second pressure-sensitive adhesive layer (X2) refers to a value measured by the method described in Examples.
[0125] Hereinafter, each layer constituting the pressure-sensitive adhesive sheet used in one embodiment of the present invention will be described.
[0126] <Base material (Y)>
[0127] The substrate (Y) of the pressure-sensitive adhesive sheet used in one embodiment of the present invention includes at least an expandable substrate layer (Y1) containing expandable particles and a non-expandable substrate layer (Y2).
[0128] In addition, as the base material (Y), it can be Figure 1 The structure in which the expandable substrate layer (Y1) and the non-expandable substrate layer (Y2) are laminated one by one, as in the pressure-sensitive adhesive sheet 1a shown in (a), may also be as follows: Figure 1 Like the pressure-sensitive adhesive sheet 1b shown in (b), a first non-thermally expandable substrate layer (Y2-1) and a second non-thermally expandable substrate layer (Y2-2) are provided on both surfaces of an expandable substrate layer (Y1).
[0129] The substrate (Y) of the pressure-sensitive adhesive sheet used in one embodiment of the present invention may have a structure in which an adhesive layer is provided between an expandable substrate layer (Y1) and a non-expandable substrate layer (Y2).
[0130] For example, Figure 1 In the case of the structure of the pressure-sensitive adhesive sheet 1b shown in (b), an adhesive layer may be provided between the expandable substrate layer (Y1) and the first non-heat-expandable substrate layer (Y2-1) and / or the second non-heat-expandable substrate layer (Y2-2).
[0131] By providing the adhesive layer, the interlayer adhesion between the expandable base layer (Y1) and the non-expandable base layer (Y2) can be improved.
[0132] The adhesive layer can be formed of a conventional adhesive or an adhesive composition which is a material for forming the first adhesive layer (X1) and the second adhesive layer (X2).
[0133] In one embodiment of the present invention, from the viewpoint of obtaining a pressure-sensitive adhesive sheet in which projections and recesses are generated on the adhesive surface of the first pressure-sensitive adhesive layer (X1) due to the expansion of expandable particles, while on the other hand, the formation of projections and recesses is suppressed on the adhesive surface of the second pressure-sensitive adhesive layer (X2), the substrate (Y) is preferably a material having an expandable substrate layer (Y1) and a non-expandable substrate layer (Y2) on at least the outermost surface.
[0134] As an embodiment of the present invention, Figure 1 The pressure-sensitive adhesive sheet 1a shown in (a) includes a substrate (Y), an expandable substrate layer (Y1), an adhesive layer, and a non-expandable substrate layer (Y2) laminated in this order.
[0135] Examples of the material for forming the adhesive layer include the same materials as the adhesive composition described later as the material for forming the adhesive layer of the transfer tape.
[0136] In addition, both the expandable base material layer (Y1) and the non-expandable base material layer (Y2) constituting the base material (Y) are non-adhesive layers.
[0137] In the present invention, when determining whether or not a layer is a non-adhesive layer, if the probe viscosity value measured based on JIS Z0237:1991 with respect to the surface of the target layer is less than 50 mN / 5 mmφ, the layer is determined to be a “non-adhesive layer”.
[0138] The probe tack values of the surfaces of the expandable substrate layer (Y1) and the non-expandable substrate layer (Y2) of the pressure-sensitive adhesive sheet (I) used in one embodiment of the present invention are each independently lower than 50 mN / 5 mmφ, preferably lower than 30 mN / 5 mmφ, more preferably lower than 10 mN / 5 mmφ, and further preferably lower than 5 mN / 5 mmφ.
[0139] In addition, in this specification, the specific method of measuring the probe viscosity value of the surface of the heat-expandable substrate can utilize the method described in the Examples.
[0140] In the pressure-sensitive adhesive sheet used in one embodiment of the present invention, the thickness of the substrate (Y) is preferably 15 to 2000 μm, more preferably 25 to 1500 μm, further preferably 30 to 1000 μm, and further preferably 40 to 500 μm.
[0141] The thickness of the expandable base material (Y1) before the expandable particles expand is preferably 10 to 1000 μm, more preferably 20 to 700 μm, further preferably 25 to 500 μm, and further preferably 30 to 300 μm.
[0142] The thickness of the non-expandable substrate (Y2) is preferably 10 to 1000 μm, more preferably 20 to 700 μm, further preferably 25 to 500 μm, and further preferably 30 to 300 μm.
[0143] It should be noted that in this manual, Figure 1 When a plurality of expandable substrates (Y1) or non-expandable substrates (Y2) are present with other layers interposed therebetween, as in the pressure-sensitive adhesive sheet 1b shown in (b), the thickness of the expandable substrate (Y1) or non-expandable substrate (Y2) refers to the thickness of each layer.
[0144] In the pressure-sensitive adhesive sheet used in one embodiment of the present invention, the thickness ratio [(Y1) / (Y2)] of the expandable substrate layer (Y1) to the non-heat-expandable substrate layer (Y2) before the expandable particles expand is preferably 0.02 to 200, more preferably 0.03 to 150, and even more preferably 0.05 to 100.
[0145] In the adhesive sheet used in one embodiment of the present invention, the thickness ratio [(Y1) / (X1)] of the expandable base layer (Y1) before the expandable particles expand and the first adhesive layer (X1) directly laminated with the expandable base layer (Y1) is preferably 0.2 or more, more preferably 0.5 or more, further preferably 1.0 or more, and further preferably 5.0 or more, and is preferably 1000 or less, more preferably 200 or less, further preferably 60 or less, and further preferably 30 or less.
[0146] In addition, in the adhesive sheet used in one embodiment of the present invention, the thickness ratio [(Y2) / (X2)] between the non-expandable substrate layer (Y2) and the second adhesive layer (X2) directly laminated with the non-expandable substrate layer (Y2) is preferably 0.1 or more, more preferably 0.2 or more, and further preferably 0.3 or more, and is preferably 20 or less, more preferably 10 or less, and further preferably 5 or less.
[0147] Hereinafter, the expandable base material layer (Y1) and the non-expandable base material layer (Y2) constituting the base material (Y) will be described.
[0148] <Expandable Base Material Layer (Y1)>
[0149] The expandable base material layer (Y1) constituting the base material (Y) is a layer containing expandable particles and capable of expanding by a predetermined expansion treatment.
[0150] The content of expandable particles in the expandable substrate layer (Y1) is preferably 1 to 40 mass %, more preferably 5 to 35 mass %, further preferably 10 to 30 mass %, and further preferably 15 to 25 mass %, relative to the total mass (100 mass %) of the expandable substrate layer (Y1).
[0151] It should be noted that, from the viewpoint of improving the interlayer adhesion between the expandable base layer (Y1) and other layers laminated therewith, the surface of the expandable base layer (Y1) may be subjected to surface treatment by oxidation, embossing, or the like, adhesion-facilitating treatment, or primer treatment.
[0152] Examples of the oxidation method include corona discharge treatment, plasma discharge treatment, chromic acid treatment (wet method), hot air treatment, ozone, and ultraviolet irradiation treatment. Examples of the roughening method include sandblasting and solvent treatment.
[0153] The expandable particles contained in the expandable substrate layer (Y1) may be any particles that expand by a given treatment, and examples thereof include heat-expandable particles that expand by heating to a given temperature or above, and UV-expandable particles that expand by generating gas inside the particles by absorbing a given amount of ultraviolet rays.
[0154] The maximum volume expansion ratio of the expandable particles is preferably 1.5 to 100 times, more preferably 2 to 80 times, further preferably 2.5 to 60 times, and further preferably 3 to 40 times.
[0155] The average particle size of the expandable particles before expansion at 23° C. is preferably 3 to 100 μm, more preferably 4 to 70 μm, further preferably 6 to 60 μm, and further preferably 10 to 50 μm.
[0156] It should be noted that the average particle size of the expandable particles is the volume median particle size (D 50 ) refers to the particle size at which the cumulative volume frequency calculated from the particles with the smallest particle size among the expandable particles is equivalent to 50% in the particle distribution of the expandable particles measured using a laser diffraction particle size distribution measuring device (for example, manufactured by Malvern, product name "Mastersizer 3000").
[0157] The 90% particle size (D 90 ), preferably 10 to 150 μm, more preferably 20 to 100 μm, further preferably 25 to 90 μm, and further preferably 30 to 80 μm.
[0158] It should be noted that the 90% particle size (D 90 ) refers to the particle size corresponding to 90% of the cumulative volume frequency calculated starting from the particles with the smallest particle size among the expandable particles in the particle distribution of the expandable particles measured using a laser diffraction particle size distribution measuring apparatus (e.g., manufactured by Malvern, product name “Mastersizer 3000”).
[0159] In one embodiment of the present invention, the expandable particles are preferably heat-expandable particles having an expansion starting temperature (t) of 60 to 270°C.
[0160] That is, the expandable substrate layer (Y1) is preferably a heat-expandable substrate layer (Y1-1) containing heat-expandable particles having an expansion starting temperature (t) of 60 to 270°C, and more preferably the heat-expandable substrate layer (Y1-1) satisfies the following condition (1).
[0161] Condition (1): At the expansion starting temperature (t) of the heat-expandable particles, the storage modulus E'(t) of the heat-expandable substrate layer (Y1-1) is 1.0×10 7 Below Pa.
[0162] In addition, in this specification, the storage modulus E' of the heat-expandable base material layer (Y1-1) at a given temperature represents a value measured by the method described in the Examples.
[0163] The condition (1) described above can be considered to be an index representing the rigidity of the heat-expandable base material layer (Y1-1) immediately before the heat-expandable particles expand.
[0164] That is, as long as the heat-expandable substrate layer (Y1-1) has a degree of softness that satisfies the above-mentioned condition (1) when the heat-expandable particles expand, it is easy to form unevenness on the surface of the heat-expandable substrate layer (Y1-1), and it is easy to generate unevenness on the bonding surface of the first adhesive layer (X1). As a result, the hard support body and the first adhesive layer (X1) can be easily separated at one time with a very small force at the interface P.
[0165] From the above viewpoints, the storage modulus E'(t) of the heat expandable substrate layer (Y1-1) defined by the condition (1) is preferably 9.0×10 6 Pa or less, more preferably 8.0×10 6 Pa or less, more preferably 6.0×10 6 Pa or less, more preferably 4.0×10 6 Below Pa.
[0166] In addition, from the viewpoint of suppressing the flow of the heat-expandable particles after expansion, improving the shape retention of the irregularities generated on the surface of the heat-expandable substrate layer (Y1-1), and making it easy to generate irregularities on the bonding surface of the first adhesive layer (X1), the storage modulus E'(t) of the heat-expandable substrate layer (Y1-1) defined by the condition (1) is preferably 1.0×10 3 Pa or more, more preferably 1.0×10 4 Pa or more, more preferably 1.0×10 5 Pa or above.
[0167] Furthermore, the heat-expandable base layer (Y1-1) preferably satisfies the following condition (2), and more preferably satisfies the condition (2) in addition to the above condition (1).
[0168] Condition (2): The storage modulus E'(23) of the heat-expandable substrate layer (Y1-1) at 23°C is 1.0×10 6 Pa or above.
[0169] By obtaining a heat-expandable substrate layer (Y1-1) that satisfies the above-mentioned condition (2), it is possible to prevent displacement when the semiconductor chip is attached to the adhesive surface of the second adhesive layer (X2), and it is also possible to prevent the semiconductor chip from excessively sinking into the second adhesive layer (X2).
[0170] From the above viewpoints, the storage modulus E'(23) of the heat expandable substrate layer (Y1-1) defined by the above condition (2) is preferably 5.0×10 6 ~5.0×10 12 Pa, more preferably 1.0×10 7 ~1.0×10 12 Pa, more preferably 5.0×10 7 ~1.0×10 11 Pa, and more preferably 1.0×10 8 ~1.0×10 10 Pa.
[0171] The heat-expandable particles contained in the heat-expandable base material layer (Y1-1) are preferably heat-expandable particles having an expansion starting temperature (t) of 60 to 270°C.
[0172] In addition, in this specification, the expansion starting temperature (t) of the heat-expandable particle|grains shows the value measured by the following method.
[0173] [Method for measuring expansion starting temperature (t) of heat-expandable particles]
[0174] 0.5 mg of heat-expandable particles to be measured were placed in an aluminum cup having a diameter of 6.0 mm (inner diameter of 5.65 mm) and a depth of 4.8 mm, and an aluminum cap (diameter of 5.6 mm, thickness of 0.1 mm) was placed on the cup to prepare a sample.
[0175] The height of the sample was measured using a dynamic viscoelasticity measuring device while applying a force of 0.01 N to the sample from the upper part of the aluminum cover using an indenter. Then, while applying a force of 0.01 N using an indenter, the sample was heated from 20°C to 300°C at a heating rate of 10°C / min, and the displacement of the indenter in the vertical direction was measured. The displacement start temperature in the positive direction was taken as the expansion start temperature (t).
[0176] The heat-expandable particles are preferably microencapsulated foaming agents comprising an outer shell formed of a thermoplastic resin and an inner component which is encapsulated by the outer shell and vaporizes when heated to a predetermined temperature.
[0177] Examples of the thermoplastic resin constituting the outer shell of the microencapsulated foaming agent include vinylidene chloride-acrylonitrile copolymer, polyvinyl alcohol, polyvinyl butyral, polymethyl methacrylate, polyacrylonitrile, polyvinylidene chloride, and polysulfone.
[0178] Examples of the inner component enclosed by the outer shell include propane, butane, pentane, hexane, heptane, octane, nonane, decane, isobutane, isopentane, isohexane, isoheptane, isooctane, isononane, isodecane, cyclopropane, cyclobutane, cyclopentane, cyclohexane, cycloheptane, cyclooctane, neopentane, dodecane, isododecane, cyclotridecane, hexylcyclohexane, tridecane, tetradecane, pentadecane, hexadecane, heptadecane, octadecane, nonadecane, Isotridecane, 4-methyldodecane, isotetradecane, isopentadecane, isohexadecane, 2,2,4,4,6,8,8-heptamethylnonane, isoheptadecane, isooctadecane, isononadecane, 2,6,10,14-tetramethylpentadecane, cyclotridecane, heptylcyclohexane, n-octylcyclohexane, cyclopentadecane, nonylcyclohexane, decylcyclohexane, pentadecylcyclohexane, hexadecylcyclohexane, heptadecane, octadecylcyclohexane, etc.
[0179] These internal components may be used alone or in combination of two or more.
[0180] The expansion starting temperature (t) of the heat-expandable particles can be adjusted by appropriately selecting the type of the contained components.
[0181] The expandable base material layer (Y1) is preferably formed from a resin composition (y) containing a resin and expandable particles.
[0182] The resin composition (y) may contain a substrate additive as necessary within a range not impairing the effects of the present invention.
[0183] Examples of the additive for the substrate include ultraviolet absorbers, light stabilizers, antioxidants, antistatic agents, slip agents, antiblocking agents, and colorants.
[0184] In addition, these additives for substrates may be used alone or in combination of two or more.
[0185] When these additives for base materials are contained, the content of each additive for base materials is preferably 0.0001 to 20 parts by mass, more preferably 0.001 to 10 parts by mass, based on 100 parts by mass of the resin.
[0186] As described above, the expandable particles contained in the resin composition (y) as a material for forming the expandable base layer (Y1) are preferably heat-expandable particles.
[0187] The content of the expandable particles is preferably 1 to 40% by mass, more preferably 5 to 35% by mass, further preferably 10 to 30% by mass, and further preferably 15 to 25% by mass, based on the total amount (100% by mass) of the active ingredients of the resin composition (y).
[0188] The resin contained in the resin composition (y) as a material for forming the expandable base material layer (Y1) may be a non-adhesive resin or an adhesive resin.
[0189] That is, even if the resin contained in the resin composition (y) is an adhesive resin, as long as the adhesive resin undergoes a polymerization reaction with a polymerizable compound during the process of forming the expandable substrate layer (Y1) from the resin composition (y), the resulting resin becomes a non-adhesive resin, and the expandable substrate layer (Y1) containing the resin is non-adhesive.
[0190] The weight average molecular weight (Mw) of the resin contained in the resin composition (y) is preferably 1,000 to 1,000,000, more preferably 1,000 to 700,000, and even more preferably 1,000 to 500,000.
[0191] When the resin is a copolymer having two or more structural units, the form of the copolymer is not particularly limited, and may be any of a block copolymer, a random copolymer and a graft copolymer.
[0192] The content of the resin is preferably 50 to 99 mass %, more preferably 60 to 95 mass %, further preferably 65 to 90 mass %, and further preferably 70 to 85 mass % based on the total amount (100 mass %) of the active ingredients of the resin composition (y).
[0193] In one embodiment of the present invention, from the viewpoint of obtaining an expandable base material layer (Y1) that easily forms irregularities on the surface when the expandable particles expand, the resin contained in the resin composition (y) preferably contains one or more selected from acrylic urethane resins and olefin resins.
[0194] Moreover, as said acrylic urethane resin, the following resin (U1) is preferable.
[0195] An acrylic urethane resin (U1) obtained by polymerizing a urethane prepolymer (UP) and a vinyl compound containing (meth)acrylate.
[0196] [Acrylic urethane resin (U1)]
[0197] Examples of the urethane prepolymer (UP) forming the main chain of the acrylic urethane resin (U1) include reaction products of polyols and polyisocyanates.
[0198] In addition, the urethane prepolymer (UP) is preferably a prepolymer obtained by further subjecting the prepolymer to a chain extension reaction using a chain extender.
[0199] Examples of the polyol used as a raw material of the urethane prepolymer (UP) include alkylene polyols, ether polyols, ester polyols, ester amide polyols, ester-ether polyols, and carbonate polyols.
[0200] These polyols may be used alone or in combination of two or more.
[0201] As the polyol used in one embodiment of the present invention, diol is preferred, ester diol, alkylene diol, and carbonate diol are more preferred, and ester diol and carbonate diol are further preferred.
[0202] Examples of the ester diol include polycondensates of one or more selected from the following diols and one or more selected from the following dicarboxylic acids and their anhydrides. The diols include alkane diols such as 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, and 1,6-hexanediol, and alkylene glycols such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol. The dicarboxylic acids include phthalic acid, isophthalic acid, terephthalic acid, naphthalene dicarboxylic acid, 4,4-diphenyl dicarboxylic acid, diphenylmethane-4,4'-dicarboxylic acid, succinic acid, adipic acid, azelaic acid, sebacic acid, chlorobridgeic acid, maleic acid, fumaric acid, itaconic acid, cyclohexane-1,3-dicarboxylic acid, cyclohexane-1,4-dicarboxylic acid, hexahydrophthalic acid, hexahydroisophthalic acid, hexahydroterephthalic acid, and methylhexahydrophthalic acid.
[0203] Specific examples thereof include polyethylene adipate diol, polybutylene adipate diol, poly-1,6-hexanediol adipate diol, poly-1,6-hexanediol isophthalate diol, poly-neopentyl adipate diol, polyethylene propylene adipate diol, polyethylene butylene adipate diol, poly-1,6-hexanediol adipate diol, polyethylene diglycol adipate diol, poly(polytetramethylene ether) adipate diol, poly(3-methylpentanediol adipate) diol, polyethylene azelaic acid diol, polyethylene sebacate diol, polybutylene azelaic acid diol, polybutylene sebacate diol, and poly-neopentyl terephthalate diol.
[0204] Examples of the alkylene glycol include alkane glycols such as 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, and 1,6-hexanediol; alkylene glycols such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol; polyalkylene glycols such as polyethylene glycol, polypropylene glycol, and polybutylene glycol; polyoxyalkylene glycols such as polytetramethylene glycol; and the like.
[0205] Examples of the carbonate diol include 1,4-tetramethylene carbonate diol, 1,5-pentamethylene carbonate diol, 1,6-hexamethylene carbonate diol, 1,2-propylene carbonate diol, 1,3-propylene carbonate diol, 2,2-dimethylpropylene carbonate diol, 1,7-heptamethylene carbonate diol, 1,8-octamethylene carbonate diol, and 1,4-cyclohexane carbonate diol.
[0206] Examples of the polyisocyanate used as a raw material of the urethane prepolymer (UP) include aromatic polyisocyanates, aliphatic polyisocyanates, and alicyclic polyisocyanates.
[0207] These polyisocyanates may be used alone or in combination of two or more.
[0208] These polyisocyanates may be trimethylolpropane adduct-type modified products, biuret-type modified products obtained by reacting with water, or isocyanurate-type modified products containing an isocyanurate ring.
[0209] Among these, the polyisocyanate used in one embodiment of the present invention is preferably a diisocyanate, and more preferably at least one selected from 4,4′-diphenylmethane diisocyanate (MDI), 2,4-toluene diisocyanate (2,4-TDI), 2,6-toluene diisocyanate (2,6-TDI), hexamethylene diisocyanate (HMDI), and alicyclic diisocyanates.
[0210] Examples of the alicyclic diisocyanate include 3-isocyanate methyl-3,5,5-trimethylcyclohexyl isocyanate (isophorone diisocyanate, IPDI), 1,3-cyclopentane diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, methyl-2,4-cyclohexane diisocyanate, and methyl-2,6-cyclohexane diisocyanate, and isophorone diisocyanate (IPDI) is preferred.
[0211] In one embodiment of the present invention, the urethane prepolymer (UP) forming the main chain of the acrylic urethane resin (U1) is preferably a linear urethane prepolymer which is a reaction product of a diol and a diisocyanate and has ethylenically unsaturated groups at both ends.
[0212] Examples of a method for introducing ethylenically unsaturated groups into both terminals of the linear urethane prepolymer include a method of reacting a terminal NCO group of a linear urethane prepolymer obtained by reacting a diol with a diisocyanate compound with a hydroxyalkyl (meth)acrylate.
[0213] Examples of the hydroxyalkyl (meth)acrylate include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate.
[0214] The vinyl compound forming the side chain of the acrylic urethane resin (U1) contains at least (meth)acrylate.
[0215] As the (meth)acrylate, at least one selected from alkyl (meth)acrylates and hydroxyalkyl (meth)acrylates is preferred, and a combination of an alkyl (meth)acrylate and a hydroxyalkyl (meth)acrylate is more preferred.
[0216] When an alkyl (meth)acrylate and a hydroxyalkyl (meth)acrylate are used in combination, the blending ratio of the hydroxyalkyl (meth)acrylate to 100 parts by mass of the alkyl (meth)acrylate is preferably 0.1 to 100 parts by mass, more preferably 0.5 to 30 parts by mass, further preferably 1.0 to 20 parts by mass, and further preferably 1.5 to 10 parts by mass.
[0217] The number of carbon atoms of the alkyl group of the alkyl (meth)acrylate is preferably 1 to 24, more preferably 1 to 12, further preferably 1 to 8, and further preferably 1 to 3.
[0218] Examples of the hydroxyalkyl (meth)acrylate include the same hydroxyalkyl (meth)acrylates as those used for introducing ethylenically unsaturated groups into both terminals of the linear urethane prepolymer.
[0219] Examples of vinyl compounds other than (meth)acrylates include aromatic hydrocarbon vinyl compounds such as styrene, α-methylstyrene, and vinyl toluene; vinyl ethers such as methyl vinyl ether and ethyl vinyl ether; polar group-containing monomers such as vinyl acetate, vinyl propionate, (meth)acrylonitrile, N-vinyl pyrrolidone, (meth)acrylic acid, maleic acid, fumaric acid, itaconic acid, and (meth)acrylamide; and the like.
[0220] These compounds may be used alone or in combination of two or more.
[0221] The content of the (meth)acrylate in the vinyl compound is preferably 40 to 100 mass %, more preferably 65 to 100 mass %, further preferably 80 to 100 mass %, and further preferably 90 to 100 mass %, based on the total amount (100 mass %) of the vinyl compound.
[0222] The total content of the alkyl (meth)acrylate and the hydroxyalkyl (meth)acrylate in the vinyl compound is preferably 40 to 100% by mass, more preferably 65 to 100% by mass, further preferably 80 to 100% by mass, and further preferably 90 to 100% by mass, based on the total amount (100% by mass) of the vinyl compound.
[0223] In the acrylic urethane resin (U1) used in one embodiment of the present invention, the content ratio of the structural unit (u11) derived from the urethane prepolymer (UP) to the structural unit (u12) derived from the vinyl compound [(u11) / (u12)] is preferably 10 / 90 to 80 / 20, more preferably 20 / 80 to 70 / 30, further preferably 30 / 70 to 60 / 40, and further preferably 35 / 65 to 55 / 45 in terms of mass ratio.
[0224] [Olefin resin]
[0225] Examples of the olefin-based resin preferably used as the resin contained in the resin composition (y) include polymers having at least a structural unit derived from an olefin monomer.
[0226] The olefin monomer is preferably an α-olefin having 2 to 8 carbon atoms, and specific examples thereof include ethylene, propylene, butene, isobutylene, and 1-hexene.
[0227] Among these, ethylene and propylene are preferred.
[0228] Specific examples of olefin resins include ultra-low density polyethylene (VLDPE, density: 880 kg / m 3 Above and below 910kg / m 3 ), low-density polyethylene (LDPE, density: 910kg / m 3 Above and below 915kg / m 3 ), medium density polyethylene (MDPE, density: 915kg / m 3 Above and below 942kg / m 3 ), high-density polyethylene (HDPE, density: 942kg / m 3The above), polyethylene resins such as linear low-density polyethylene; polypropylene resin (PP); polybutene resin (PB); ethylene-propylene copolymer; olefin elastomer (TPO); ethylene-vinyl acetate copolymer (EVA); ethylene-propylene-(5-ethylidene-2-norbornene) and other olefin terpolymers; and the like.
[0229] In one embodiment of the present invention, the olefin-based resin may be a modified olefin-based resin further subjected to one or more modifications selected from the group consisting of acid modification, hydroxy modification, and acrylic modification.
[0230] For example, examples of the acid-modified olefin resin obtained by acid-modifying an olefin resin include a modified polymer obtained by graft-polymerizing an unsaturated carboxylic acid or an anhydride thereof to the above-mentioned unmodified olefin resin.
[0231] Examples of the unsaturated carboxylic acid or anhydride thereof include maleic acid, fumaric acid, itaconic acid, citraconic acid, glutaconic acid, tetrahydrophthalic acid, aconitic acid, (meth)acrylic acid, maleic anhydride, itaconic anhydride, glutaconic anhydride, citraconic anhydride, aconitic anhydride, norbornene dicarboxylic anhydride, and tetrahydrophthalic anhydride.
[0232] In addition, the unsaturated carboxylic acid or its anhydride may be used alone or in combination of two or more.
[0233] Examples of the acrylic-modified olefin resin obtained by subjecting an olefin resin to acrylic modification include a modified polymer obtained by graft-polymerizing an alkyl (meth)acrylate as a side chain to the above-mentioned unmodified olefin resin as a main chain.
[0234] The number of carbon atoms of the alkyl group of the alkyl (meth)acrylate is preferably 1-20, more preferably 1-16, and even more preferably 1-12.
[0235] Examples of the alkyl (meth)acrylate include the same compounds as those which can be selected as the monomer (a1′) described later.
[0236] Examples of the hydroxy-modified olefin-based resin obtained by subjecting an olefin-based resin to hydroxyl group modification include modified polymers obtained by graft-polymerizing a hydroxyl-containing compound onto the above-mentioned unmodified olefin-based resin as a main chain.
[0237] Examples of the hydroxyl-containing compounds include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and unsaturated alcohols such as vinyl alcohol and allyl alcohol.
[0238] (Resins other than acrylic urethane resins and olefin resins)
[0239] In one embodiment of the present invention, the resin composition (y) may contain a resin other than the acrylic urethane resin and the olefin resin within a range not impairing the effects of the present invention.
[0240] Examples of such resins include vinyl resins such as polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl acetate copolymer, and ethylene-vinyl alcohol copolymer; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polystyrene; acrylonitrile-butadiene-styrene copolymer; cellulose triacetate; polycarbonate; polyurethane that does not belong to acrylic urethane resins; polymethylpentene; polysulfone; polyetheretherketone; polyethersulfone; polyphenylene sulfide; polyimide resins such as polyetherimide and polyimide; polyamide resins; acrylic resins; fluorine resins, etc.
[0241] Among them, from the viewpoint of forming an expandable base material layer (Y1) that easily forms surface irregularities when the expandable particles expand, it is preferred that the content of resins other than the acrylic urethane resin and the olefin resin in the resin composition (y) is small.
[0242] The content ratio of resins other than acrylic urethane resins and olefin resins is preferably less than 30 parts by mass, more preferably less than 20 parts by mass, more preferably less than 10 parts by mass, further preferably less than 5 parts by mass, and further preferably less than 1 part by mass, relative to 100 parts by mass of the total amount of resins contained in the resin composition (y).
[0243] [Solvent-free resin composition (y1)]
[0244] One embodiment of the resin composition (y) is a solvent-free resin composition (y1) containing an oligomer having an ethylenically unsaturated group and a weight average molecular weight (Mw) of 50,000 or less, an energy beam polymerizable monomer, and the above-mentioned thermally expandable particles without adding a solvent.
[0245] Although no solvent is blended in the solvent-free resin composition (y1), the energy-ray polymerizable monomer contributes to the improvement of the plasticity of the oligomer.
[0246] By irradiating a coating film formed of a solvent-free resin composition (y1) with energy rays, it is easy to form an expandable base layer (Y1) that easily forms irregularities on the surface when the expandable particles expand, and in particular, it is easy to form a heat-expandable base layer (Y1-1) that satisfies the above-mentioned conditions (1) and (2).
[0247] The type, shape, and amount (content) of the expandable particles to be blended in the solvent-free resin composition (y1) are the same as those of the resin composition (y), as described above.
[0248] The weight average molecular weight (Mw) of the oligomer contained in the solvent-free resin composition (y1) is 50,000 or less, preferably 1,000 to 50,000, more preferably 2,000 to 40,000, further preferably 3,000 to 35,000, and further preferably 4,000 to 30,000.
[0249] The oligomer may be any oligomer having an ethylenically unsaturated group and having a weight average molecular weight of 50,000 or less among the resins contained in the resin composition (y), and is preferably the urethane prepolymer (UP).
[0250] In addition, as this oligomer, a modified olefin resin having an ethylenically unsaturated group may also be used.
[0251] The total content of the above-mentioned oligomers and energy-ray polymerizable monomers in the solvent-free resin composition (y1) is preferably 50 to 99 mass %, more preferably 60 to 95 mass %, further preferably 65 to 90 mass %, and further preferably 70 to 85 mass %, relative to the total amount (100 mass %) of the solvent-free resin composition (y1).
[0252] Examples of energy-ray polymerizable monomers include alicyclic polymerizable compounds such as isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxy (meth)acrylate, cyclohexyl (meth)acrylate, adamantyl (meth)acrylate, and tricyclodecyl acrylate; aromatic polymerizable compounds such as phenyl hydroxypropyl acrylate, benzyl acrylate, and phenol ethylene oxide-modified acrylate; and heterocyclic polymerizable compounds such as tetrahydrofurfuryl (meth)acrylate, morpholine acrylate, N-vinyl pyrrolidone, and N-vinyl caprolactam.
[0253] These energy ray polymerizable monomers may be used alone or in combination of two or more.
[0254] The blending ratio of the oligomer to the energy-beam-polymerizable monomer (oligomer / energy-beam-polymerizable monomer) is preferably 20 / 80 to 90 / 10, more preferably 30 / 70 to 85 / 15, and even more preferably 35 / 65 to 80 / 20.
[0255] In one embodiment of the present invention, it is preferred that the solvent-free resin composition (y1) further contains a photopolymerization initiator.
[0256] By containing a photopolymerization initiator, the curing reaction can be sufficiently advanced by irradiation with energy rays having relatively low energy.
[0257] Examples of the photopolymerization initiator include 1-hydroxycyclohexyl phenyl ketone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzyl phenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyronitrile, bibenzyl, diacetyl, and 8-chloroanthraquinone.
[0258] These photopolymerization initiators may be used alone or in combination of two or more.
[0259] The amount of the photopolymerization initiator to be added is preferably 0.01 to 5 parts by mass, more preferably 0.01 to 4 parts by mass, and even more preferably 0.02 to 3 parts by mass, based on the total amount (100 parts by mass) of the oligomer and the energy ray polymerizable monomer.
[0260] <Non-expandable substrate layer (Y2)>
[0261] Examples of the material for forming the non-expandable base material layer (Y2) constituting the base material (Y) include paper materials, resins, and metals.
[0262] Examples of the paper material include thin paper, medium-quality paper, premium paper, impregnated paper, coated paper, art paper, sulphate paper, and glass paper.
[0263] Examples of the resin include polyolefin resins such as polyethylene and polypropylene; vinyl resins such as polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl acetate copolymer, and ethylene-vinyl alcohol copolymer; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polystyrene; acrylonitrile-butadiene-styrene copolymer; cellulose triacetate; polycarbonate; polyurethane resins such as polyurethane and acrylic modified polyurethane; polymethylpentene; polysulfone; polyetheretherketone; polyethersulfone; polyphenylene sulfide; polyimide resins such as polyetherimide and polyimide; polyamide resins; acrylic resins; fluorine resins, etc.
[0264] Examples of the metal include aluminum, tin, chromium, and titanium.
[0265] These forming materials may be composed of one kind or two or more kinds may be used in combination.
[0266] Examples of the non-expandable base material layer (Y2) formed by combining two or more materials include a material obtained by laminating a paper material with a thermoplastic resin such as polyethylene, and a material obtained by forming a metal film on the surface of a resin film or sheet containing a resin.
[0267] Examples of the method for forming the metal layer include a method of depositing the metal by PVD such as vacuum deposition, sputtering, or ion plating, and a method of attaching a metal foil made of the metal using a common adhesive.
[0268] It should be noted that, from the viewpoint of improving the interlayer adhesion between the non-expandable substrate layer (Y2) and other laminated layers, when the non-expandable substrate layer (Y2) contains a resin, the surface of the non-expandable substrate layer (Y2) may be subjected to a surface treatment by an oxidation method, a convexo-relief method, or the like, an adhesion-facilitating treatment, or a primer treatment, similarly to the above-mentioned expandable substrate layer (Y1).
[0269] Furthermore, when the non-expandable base layer (Y2) contains a resin, it may contain the above-mentioned base material additive which may be contained in the resin composition (y) together with the resin.
[0270] It is preferred that the non-expandable substrate layer (Y2) is present at a position farther from the first adhesive layer (X1) than the expandable substrate layer (Y1), the non-expandable substrate layer (Y2) does not exist between the expandable substrate layer (Y1) and the first adhesive layer (X1), and the storage modulus E' of the non-expandable substrate layer (Y2) when the expandable particles expand is greater than the storage modulus E' of the expandable substrate layer (Y1) when the expandable particles expand. In this way, since there is no non-expandable substrate layer (Y2) between the expandable substrate layer (Y1) and the first adhesive layer (X1), the unevenness generated on the surface of the expandable substrate layer (Y1) due to the expansion of the expandable particles is transferred to the first adhesive layer (X1) without the non-expandable substrate layer (Y2) being interposed therebetween, and unevenness is easily generated on the adhesive surface of the first adhesive layer (X1). In addition, when the expandable particles expand, since the storage modulus E' of the non-expandable substrate layer (Y2) is greater than the storage modulus E' of the expandable substrate layer (Y1), it is possible to suppress the generation of irregularities on the surface of the non-expandable substrate layer (Y2) side of the expandable substrate layer (Y1) when the expandable particles expand. As a result, it becomes easy to generate irregularities on the surface of the first adhesive layer (X1) side of the expandable substrate layer (Y1), and therefore, irregularities are also easy to generate on the adhesive surface of the first adhesive layer (X1).
[0271] As described above, from the viewpoint of making it easy to generate irregularities on the adhesive surface of the first adhesive layer (X1), the storage elastic modulus E' of the non-expandable base layer (Y2) when the expandable particles expand is preferably 1.0 MPa or more. From the viewpoint of the ease of the pasting and peeling operations, from the viewpoint of making it easy to generate irregularities on the adhesive surface of the second adhesive layer (X2), or from the viewpoint of the ease of handling of the roll, it is preferably 1.0×10 3 MPa or less. From this viewpoint, the storage elastic modulus E' of the non-expandable base material layer (Y2) when the expandable particles expand is preferably 1.0 to 5.0 × 10 2 MPa, more preferably 1.0×10 1 ~1.0×10 2 MPa, more preferably 5.0×10 1 ~1.0×10 3 MPa.
[0272] In addition, from the above viewpoints and from the viewpoint of preventing the semiconductor wafer from being displaced when being attached to the adhesive surface of the second adhesive layer (X2), the storage modulus E'(23) of the non-expandable substrate layer (Y2) at 23°C is preferably 5.0×10 1 ~5.0×10 4 MPa, more preferably 1.0×10 2 ~1.0×10 4 MPa, more preferably 5.0×10 2 ~5.0×10 3 MPa.
[0273] The non-expandable base material layer (Y2) is a non-expandable layer determined by the above-mentioned method.
[0274] Therefore, the volume change rate (%) of the non-expandable substrate layer (Y2) which can be calculated by the above formula is less than 5 volume %, preferably less than 2 volume %, more preferably less than 1 volume %, further preferably less than 0.1 volume %, and further preferably less than 0.01 volume %.
[0275] In addition, the non-expandable substrate layer (Y2) may contain heat-expandable particles as long as the volume change rate is within the above range. For example, by selecting the resin contained in the non-expandable substrate layer (Y2), the volume change rate can be adjusted to the above range even if heat-expandable particles are contained.
[0276] However, the smaller the content of the heat-expandable particles in the non-expandable base material layer (Y2), the more preferably.
[0277] As a specific content of the heat-expandable particles, it is usually less than 3 mass%, preferably less than 1 mass%, more preferably less than 0.1 mass%, further preferably less than 0.01 mass%, and further preferably less than 0.001 mass%, relative to the total mass (100 mass%) of the non-expandable substrate layer (Y2).
[0278] <First Adhesive Layer (X1), Second Adhesive Layer (X2)>
[0279] The pressure-sensitive adhesive sheet used in one embodiment of the present invention includes a first pressure-sensitive adhesive layer (X1) and a second pressure-sensitive adhesive layer (X2).
[0280] In the production method of the present invention, the adhesive surface of the first adhesive layer (X1) is bonded to the hard support, and the adhesive surface of the second adhesive layer (X2) is bonded to the semiconductor wafer.
[0281] The first adhesive layer (X1) is required to have a property that the expandable particles contained in the expandable base layer (Y1) have high adhesion to the rigid support before expansion, and that the semiconductor wafer can be sufficiently fixed to the rigid support.
[0282] From this viewpoint, the shear storage modulus G'(23) of the first pressure-sensitive adhesive layer (X1) at 23°C is preferably 1.0×10 8 Pa or less, more preferably 5.0×10 7 Pa or less, more preferably 1.0×10 7 Below Pa.
[0283] On the other hand, it is also required to have rigidity to such an extent that the irregularities generated on the surface of the expandable base layer (Y1) when the expandable particles in the expandable base layer (Y1) expand can also be formed on the bonding surface of the first adhesive layer (X1).
[0284] From this viewpoint, the shear storage modulus G'(23) of the first pressure-sensitive adhesive layer (X1) at 23°C is preferably 1.0×10 4 Pa or more, more preferably 5.0×10 4 Pa or more, more preferably 1.0×10 5 Pa or above.
[0285] In addition, the second adhesive layer (X2) is required to have good adhesion not only to the semiconductor wafer but also to the semiconductor chip obtained by dividing the semiconductor wafer, and it is also necessary to suppress the excessive sinking of the semiconductor chip into the second adhesive layer (X2).
[0286] From these viewpoints, the shear storage modulus G'(23) of the second pressure-sensitive adhesive layer (X2) at 23°C is preferably 1.0×10 4 ~1.0×10 8 Pa, more preferably 5.0×10 4 ~5.0×10 7 Pa, more preferably 1.0×10 5 ~1.0×10 7 Pa.
[0287] In addition, in this specification, the shear storage modulus G'(23) of the first adhesive layer (X1) and the second adhesive layer (X2) refers to the value measured by the method described in the Examples.
[0288] The thickness of the first pressure-sensitive adhesive layer (X1) is preferably 1 to 60 μm, more preferably 2 to 50 μm, further preferably 3 to 40 μm, and further preferably 5 to 30 μm.
[0289] The thickness of the second pressure-sensitive adhesive layer (X2) is preferably 1 to 60 μm, more preferably 2 to 50 μm, further preferably 3 to 40 μm, and further preferably 5 to 30 μm.
[0290] The first adhesive layer (X1) and the second adhesive layer (X2) can be formed from an adhesive composition (x) containing an adhesive resin.
[0291] Furthermore, the pressure-sensitive adhesive composition (x) may contain pressure-sensitive adhesive additives such as a cross-linking agent, a tackifier, a polymerizable compound, and a polymerization initiator, as necessary.
[0292] Hereinafter, each component contained in the adhesive composition (x) will be described.
[0293] (Adhesive resin)
[0294] The adhesive resin used in one embodiment of the present invention may be any resin that has adhesiveness on its own and is a polymer having a weight average molecular weight (Mw) of 10,000 or more.
[0295] The weight average molecular weight (Mw) of the adhesive resin used in one embodiment of the present invention is preferably 10,000 to 2,000,000, more preferably 20,000 to 1,500,000, and even more preferably 30,000 to 1,000,000 from the viewpoint of improving adhesive strength.
[0296] Specific examples of the adhesive resin include rubber resins such as acrylic resins, urethane resins, and polyisobutylene resins, polyester resins, olefin resins, silicone resins, and polyvinyl ether resins.
[0297] These adhesive resins may be used alone or in combination of two or more.
[0298] When these adhesive resins are copolymers having two or more structural units, the form of the copolymer is not particularly limited, and may be any of a block copolymer, a random copolymer, and a graft copolymer.
[0299] The adhesive resin used in one embodiment of the present invention may be an energy-ray-curable adhesive resin in which a polymerizable functional group is introduced into a side chain of the above-mentioned adhesive resin.
[0300] For example, by forming the second adhesive layer (X2) from an energy-ray-curable adhesive composition containing an energy-ray-curable adhesive resin, the adhesive force can be reduced by irradiating energy rays, so that the obtained semiconductor chip can be easily picked up from the second adhesive layer (X2).
[0301] Examples of the polymerizable functional group include a (meth)acryloyl group and a vinyl group.
[0302] In addition, examples of energy rays include ultraviolet rays and electron beams, and ultraviolet rays are preferred.
[0303] The material for forming the pressure-sensitive adhesive layer whose adhesive strength can be reduced by irradiating energy rays may be an energy-ray-curable pressure-sensitive adhesive composition containing a monomer or oligomer having a polymerizable functional group.
[0304] It is preferred that these energy-ray-curable pressure-sensitive adhesive compositions further contain a photopolymerization initiator.
[0305] By containing a photopolymerization initiator, the curing reaction can be sufficiently advanced even by irradiation with energy rays having relatively low energy.
[0306] Examples of the photopolymerization initiator include the same ones as those blended in the above-mentioned solvent-free resin composition (y1).
[0307] The content of the photopolymerization initiator is preferably 0.01 to 10 parts by mass, more preferably 0.03 to 5 parts by mass, and even more preferably 0.05 to 2 parts by mass, based on 100 parts by mass of the energy-ray-curable adhesive resin or 100 parts by mass of the monomer or oligomer having a polymerizable functional group.
[0308] In one embodiment of the present invention, from the viewpoint of exhibiting excellent adhesive force, the adhesive resin preferably contains an acrylic resin. In particular, by forming the first adhesive layer (X1) from an adhesive composition containing an acrylic resin, it is possible to easily form irregularities on the surface of the first adhesive layer.
[0309] The content of the acrylic resin in the adhesive resin is preferably 30 to 100% by mass, more preferably 50 to 100% by mass, further preferably 70 to 100% by mass, and further preferably 85 to 100% by mass, relative to the total amount (100% by mass) of the adhesive resin contained in the adhesive composition (x).
[0310] The content of the adhesive resin is preferably 35 to 100 mass %, more preferably 50 to 100 mass %, further preferably 60 to 98 mass %, and further preferably 70 to 95 mass %, relative to the total amount (100 mass %) of the active ingredients of the adhesive composition (x).
[0311] (Crosslinking agent)
[0312] In one embodiment of the present invention, when the adhesive composition (x) contains an adhesive resin having a functional group, it is preferred that the adhesive composition (x) further contains a crosslinking agent.
[0313] The crosslinking agent is a component that reacts with the adhesive resin having a functional group to crosslink the adhesive resins with the functional group serving as a crosslinking starting point.
[0314] Examples of the crosslinking agent include isocyanate crosslinking agents, epoxy crosslinking agents, aziridine crosslinking agents, and metal chelate crosslinking agents.
[0315] These cross-linking agents may be used alone or in combination of two or more.
[0316] Among these crosslinking agents, isocyanate crosslinking agents are preferred from the viewpoints of improving cohesive force and thus adhesive force, and from the viewpoints of easy availability and the like.
[0317] The content of the crosslinking agent can be appropriately adjusted according to the number of functional groups of the adhesive resin, but is preferably 0.01 to 10 parts by mass, more preferably 0.03 to 7 parts by mass, and even more preferably 0.05 to 5 parts by mass based on 100 parts by mass of the adhesive resin having functional groups.
[0318] (Thickener)
[0319] In one embodiment of the present invention, the pressure-sensitive adhesive composition (x) may further contain a tackifier from the viewpoint of further improving the adhesive strength.
[0320] In this specification, the "tackifier" refers to an oligomer having a weight average molecular weight (Mw) of less than 10,000 among components that assist in improving the adhesive strength of the above-mentioned adhesive resin, and is a component different from the above-mentioned adhesive resin.
[0321] The weight average molecular weight (Mw) of the tackifier is preferably 400 to 10,000, more preferably 500 to 8,000, and even more preferably 800 to 5,000.
[0322] Examples of the tackifier include rosin-based resins, terpene-based resins, styrene-based resins, C5-based petroleum resins obtained by copolymerizing C5 fractions such as pentene, isoprene, piperine, and 1,3-pentadiene generated by thermal decomposition of naphtha, C9-based petroleum resins obtained by copolymerizing C9 fractions such as indene and vinyltoluene generated by thermal decomposition of naphtha, and hydrogenated resins obtained by hydrogenating these resins.
[0323] The softening point of the tackifier is preferably 60 to 170°C, more preferably 65 to 160°C, and even more preferably 70 to 150°C.
[0324] In addition, in this specification, the "softening point" of a tackifier means the value measured based on JIS K 2531.
[0325] The tackifiers may be used alone or in combination of two or more tackifiers having different softening points, structures, etc.
[0326] Furthermore, when two or more tackifiers are used, it is preferred that the weighted average of the softening points of the tackifiers fall within the above range.
[0327] The content of the tackifier is preferably 0.01 to 65 mass %, more preferably 0.1 to 50 mass %, further preferably 1 to 40 mass %, and further preferably 2 to 30 mass % based on the total amount (100 mass %) of the active ingredients of the adhesive composition (x).
[0328] (Additives for adhesives)
[0329] In one embodiment of the present invention, the adhesive composition (x) may contain adhesive additives used in conventional adhesives in addition to the above-mentioned additives within a range that does not impair the effects of the present invention.
[0330] Examples of such adhesive additives include antioxidants, softeners (plasticizers), rust preventives, pigments, dyes, retarders, reaction accelerators (catalysts), ultraviolet absorbers, and antistatic agents.
[0331] In addition, these adhesive additives may be used individually or in combination of 2 or more types.
[0332] When these adhesive additives are contained, the content of each adhesive additive is preferably 0.0001 to 20 parts by mass, more preferably 0.001 to 10 parts by mass, based on 100 parts by mass of the adhesive resin.
[0333] It should be noted that the first adhesive layer (X1) and the second adhesive layer (X2) are preferably non-expandable adhesive layers. Therefore, it is more preferred that the content of expandable particles in the adhesive composition (x) as a forming material of the first adhesive layer (X1) and the second adhesive layer (X2) is as small as possible.
[0334] The content of the expandable particles is preferably less than 1 mass %, more preferably less than 0.1 mass %, further preferably less than 0.01 mass %, and further preferably less than 0.001 mass %, relative to the total amount (100 mass %) of the active ingredients of the adhesive composition (x) or relative to the total mass (100 mass %) of the first adhesive layer (X1) and the second adhesive layer (X2).
[0335] <Peeling Material>
[0336] The pressure-sensitive adhesive sheet used in one embodiment of the present invention may further have a release material laminated on the pressure-sensitive adhesive surfaces of the first pressure-sensitive adhesive layer (X1) and the second pressure-sensitive adhesive layer (X2).
[0337] As the release material, a release sheet subjected to double-sided release treatment, a release sheet subjected to single-sided release treatment, or the like can be used. Examples of the release material include a release material substrate coated with a release agent.
[0338] Examples of the release material substrate include papers such as high-quality paper, glassine paper, and kraft paper; plastic films such as polyester resin films such as polyethylene terephthalate resin, polybutylene terephthalate resin, and polyethylene naphthalate resin; and olefin resin films such as polypropylene resin and polyethylene resin.
[0339] Examples of the release agent include silicone-based resins, olefin-based resins, isoprene-based resins, butadiene-based resins and other rubber-based elastomers, long-chain alkyl-based resins, alkyd-based resins, and fluorine-based resins.
[0340] The thickness of the release material is not particularly limited, but is preferably 10 to 200 μm, more preferably 25 to 170 μm, and even more preferably 35 to 80 μm.
[0341] [Each step of the method for manufacturing a semiconductor chip of the present invention]
[0342] The manufacturing method of the present invention is a method for manufacturing a semiconductor chip from a semiconductor wafer using the above-mentioned adhesive sheet, wherein the method comprises the following steps (1) to (3).
[0343] Step (1): A step of attaching the adhesive surface of the first adhesive layer (X1) to a rigid support and attaching the adhesive surface of the second adhesive layer (X2) to the surface of a semiconductor wafer.
[0344] Step (2): a step of dividing the semiconductor wafer to obtain a plurality of semiconductor chips.
[0345] Step (3): a step of expanding the expandable particles to separate the plurality of semiconductor chips bonded to the second adhesive layer (X2) at the interface P between the rigid support and the first adhesive layer (X1).
[0346] The method for manufacturing a semiconductor chip of the present invention can be applied to either a so-called stealth dicing method or a pre-dicing method.
[0347] In addition, the production method according to one embodiment of the present invention preferably further includes the following step (4), and more preferably includes the following steps (4) to (6).
[0348] Step (4): After separation from the hard support in step (3), the back surfaces of the plurality of semiconductor chips opposite to the circuit surfaces are attached to a transfer tape, and then the adhesive sheet is removed from the semiconductor chips, wherein the transfer tape has a base film and has an adhesive layer and / or a bonding agent layer.
[0349] Step (5): a step of stretching the transfer tape in the MD direction to increase the intervals between the plurality of semiconductor chips.
[0350] Step (6): A step of separating a plurality of semiconductor chips from the transfer tape to obtain semiconductor chips.
[0351] Figure 2 is a schematic cross-sectional view of steps (1) to (3) of the method for manufacturing a semiconductor chip of the present invention, Figure 3 It is a schematic cross-sectional view of steps (4) to (6).
[0352] Below, refer to Figure 2 and 3 Steps (1) to (4) are described.
[0353] <Step (1)>
[0354] Figure 2 (a) is a schematic cross-sectional view of step (1), showing the use of Figure 1 The adhesive sheet 1 a shown in (a) is in a state where a semiconductor wafer 60 is attached to a hard support 50 .
[0355] In step (1), the adhesive surface of the first adhesive layer (X1) of the adhesive sheet 1a is preferably adhered to the hard support 50, and the adhesive surface of the second adhesive layer (X2) is preferably adhered to the circuit surface 61 of the semiconductor wafer 60 where the circuit is formed.
[0356] It should be noted that in Figure 2 In the figure, the use of Figure 1 In the embodiment of the adhesive sheet 1a shown in (a), when using an adhesive sheet having other structures, it is also preferred to stack the hard support body, the adhesive sheet and the semiconductor chip in sequence, and adhere the adhesive surface of the first adhesive layer (X1) of the adhesive sheet to the hard support body, and adhere the adhesive surface of the second adhesive layer (X2) to the circuit surface of the semiconductor chip.
[0357] The rigid support is preferably attached to the entire adhesive surface of the first adhesive layer (X1) of the adhesive sheet. Therefore, the rigid support is preferably in a plate shape.
[0358] The surface area of the hard support to which the first adhesive layer (X1) is attached is preferably as follows: Figure 2 As shown, it is equal to or larger than the area of the adhesive surface of the first adhesive layer (X1).
[0359] The material constituting the hard support body includes, for example: metal materials such as SUS; non-metallic inorganic materials such as glass and silicon wafers; resin materials such as epoxy resin, ABS resin, acrylic resin, engineering plastics, special engineering plastics, polyimide resin, polyamide-imide resin; composite materials such as glass epoxy resin, etc. Among these, SUS, glass, and silicon wafers are preferred.
[0360] In addition, as an engineering plastic, nylon, polycarbonate (PC), polyethylene terephthalate (PET), etc. are mentioned.
[0361] Examples of the special engineering plastics include polyphenylene sulfide (PPS), polyethersulfone (PES), and polyetheretherketone (PEEK).
[0362] The thickness of the rigid support is preferably 20 μm or more and 50 mm or less, and more preferably 60 μm or more and 20 mm or less.
[0363] The Young's modulus of the rigid support is preferably 1.0 GPa or more, more preferably 5.0 GPa or more, further preferably 10 GPa or more, and further preferably 20 GPa or more, from the viewpoint of improving the performance of preventing chip breakage.
[0364] In addition, in this specification, the Young's modulus of a rigid support body is a value measured at room temperature (25 degreeC) based on the static Young's modulus test method of JIS Z2280:1993.
[0365] The surface of the semiconductor wafer to be attached to the adhesive surface of the second adhesive layer (X2) is preferably a circuit surface on which a circuit is formed.
[0366] On the other hand, the surface of the semiconductor chip opposite to the circuit surface (hereinafter also referred to as the "back side") is preferably a flat surface without circuits, electrodes, etc. because it will be ground and the semiconductor wafer will be divided into multiple semiconductor chips in a subsequent process.
[0367] By attaching the adhesive surface of the second adhesive layer (X2) to the circuit surface of the semiconductor wafer, the circuit surface can be protected.
[0368] The semiconductor wafer used in the manufacturing method of the present invention can be obtained by forming a circuit on one surface of a semiconductor wafer made of silicon, SiC (silicon carbide), gallium, arsenic, etc. by etching, lift-off, etc.
[0369] It should be noted that the semiconductor wafer needs to be processed to form a modified region inside the semiconductor wafer for stealth dicing and to form grooves in the thickness direction from the surface of the semiconductor wafer for pre-dicing.
[0370] The circuit surface of the semiconductor wafer that has been subjected to these treatments in advance can be pasted on the adhesive surface of the second adhesive layer (X2). In addition, in this process, after the circuit surface of the semiconductor wafer that has not been subjected to these treatments is pasted on the adhesive surface of the second adhesive layer (X2), these treatments can be performed from the back side of the semiconductor wafer.
[0371] In particular, the process for forming a modified region inside the semiconductor wafer suitable for stealth dicing is preferably performed after the circuit surface of the semiconductor wafer is attached to the adhesive surface of the second adhesive layer (X2).
[0372] By performing a modified region formation process after adhering the circuit surface of the semiconductor chip to the adhesive surface of the second adhesive layer (X2), the semiconductor chip can be adhered to a hard support body via the adhesive sheet, thereby effectively suppressing the warping of the semiconductor chip that may occur after the modified region is formed.
[0373] In the case of manufacturing semiconductor chips by stealth dicing, as a process for forming a modified region inside a semiconductor wafer, a method of forming a modified region based on multiphoton absorption can be cited, in which the back side of the semiconductor wafer is used as a laser incident surface, a focal point is directed to the inside of the workpiece, and laser is irradiated. When the modified region is formed, a crack line extending from the modified region along the thickness direction of the semiconductor wafer is also formed.
[0374] On the other hand, the process for forming grooves in the thickness direction from the surface of the semiconductor wafer suitable for the dicing-before method may be performed before or after the semiconductor wafer is attached to the second adhesive layer (X2).
[0375] When semiconductor chips are manufactured by the dicing-before method, as a process for forming grooves from the surface of the semiconductor wafer in the thickness direction, there can be mentioned a method of performing dicing using a known wafer dicing apparatus or the like.
[0376] It should be noted that step (1) is preferably performed in an environment where the expandable particles do not expand.
[0377] For example, when heat-expandable particles are used as expandable particles, step (1) may be carried out under a temperature condition lower than the expansion starting temperature (t) of the heat-expandable particles. Specifically, it is preferably carried out in an environment of 0 to 80° C. (when the expansion starting temperature (t) is 60 to 80° C., in an environment lower than the expansion starting temperature (t)).
[0378] <Step (2)>
[0379] Step (2) is a step of dividing the semiconductor wafer to obtain a plurality of semiconductor chips.
[0380] As a method of dividing a semiconductor wafer, a method of grinding the back surface of the semiconductor wafer to separate the semiconductor wafer into a plurality of semiconductor chips is preferable.
[0381] Figure 2 (b) is a schematic cross-sectional view of a case where the back surface 62 of the semiconductor wafer 60 is ground and singulated into a plurality of semiconductor chips.
[0382] For example, in the stealth dicing method, this step is a step of grinding the back surface of the semiconductor wafer having the reformed region, which is opposite to the circuit surface and on which no circuit is formed, to divide the semiconductor wafer into a plurality of semiconductor chips.
[0383] In the stealth dicing method, the modified region is a brittle portion of the semiconductor wafer, so the back of the semiconductor wafer is ground to reduce its thickness, or the force applied by grinding causes the semiconductor wafer to be damaged and singulated into semiconductor chips. As a result, the semiconductor wafer is split along the modified region and crack line and singulated into multiple semiconductor chips.
[0384] In the pre-dicing method, this step is a step of grinding the back surface of the semiconductor wafer having grooves formed in advance in the thickness direction, which is opposite to the circuit surface and has no circuit formed thereon, to divide the semiconductor wafer into a plurality of semiconductor chips.
[0385] In the pre-cutting method, the groove formed in the semiconductor wafer is a groove whose depth is less than the thickness of the semiconductor wafer. Here, in this process, the semiconductor wafer is ground to be at least as thin as the bottom of the groove, and the groove becomes a cut through the wafer, and the semiconductor wafer is divided and singulated into a plurality of semiconductor chips.
[0386] As described above, in the manufacturing method of the present invention, the first adhesive layer (X1) attached to the rigid support does not need to contain expandable particles, so the back grinding for dividing the semiconductor wafer can be performed while the semiconductor wafer is fully fixed to the rigid support. As a result, the disadvantages such as end defects of the obtained semiconductor chip can be effectively suppressed, and the yield rate in the manufacture of semiconductor chips can be improved.
[0387] In addition, in step (2), it is also preferable to carry out in an environment where the expandable particles do not expand.
[0388] For example, when heat-expandable particles are used as expandable particles, step (2) may be carried out under a temperature condition lower than the expansion starting temperature (t) of the heat-expandable particles. Specifically, it is preferably carried out in an environment of 0 to 80° C. (when the expansion starting temperature (t) is 60 to 80° C., in an environment lower than the expansion starting temperature (t)).
[0389] <Step (3)>
[0390] Step (3) is a step of expanding the expandable particles to separate the plurality of semiconductor chips bonded to the second adhesive layer (X2) at the interface P between the rigid support and the first adhesive layer (X1).
[0391] Figure 2 (c) shows a state where the expandable particles in the expandable base material layer (Y1) are expanded and separated at the interface P between the rigid support body 50 and the first adhesive layer (X1).
[0392] like Figure 2 As shown in (c), in this process, when the expandable particles are expanded, they are separated from the hard support body 50 at the interface P while maintaining the state of the plurality of semiconductor chips adhered to the second adhesive layer (X2), but it is further preferred that no separation occurs between the layers constituting the above-mentioned adhesive sheet.
[0393] In this step, the method for expanding the expandable particles can be appropriately selected according to the type of the expandable particles.
[0394] For example, when heat-expandable particles are used as expandable particles, the heat-expandable particles are subjected to a heat treatment at a temperature equal to or higher than the expansion starting temperature (t) of the heat-expandable particles to expand the heat-expandable particles.
[0395] At this time, the above-mentioned "temperature above the expansion starting temperature (t)" is preferably above "expansion starting temperature (t) + 10°C" and below "expansion starting temperature (t) + 60°C", and more preferably above "expansion starting temperature (t) + 15°C" and below "expansion starting temperature (t) + 40°C".
[0396] In the manufacturing method of the present invention, an adhesive sheet having an expandable base material layer (Y1) containing expandable particles is used and adjusted so that projections and depressions can be formed on the adhesive surface of the first adhesive layer (X1) adhered to a rigid support body by the expansion of the expandable particles, thereby enabling separation at the interface P between the rigid support body and the first adhesive layer (X1).
[0397] Therefore, contamination of the hard support body, such as a portion of the first pressure-sensitive adhesive layer (X1) remaining on the surface of the hard support body after separation, can be suppressed, and the hard support body cleaning step can be omitted, thereby achieving improved productivity.
[0398] <Step (4)>
[0399] Step (4) is a step of attaching the back surfaces of the plurality of semiconductor chips opposite to the circuit surface to a transfer tape after separation from the above-mentioned hard support in step (3), and then removing the above-mentioned adhesive sheet from the semiconductor chips, wherein the transfer tape has a base film and has an adhesive layer and / or a bonding agent layer.
[0400] Figure 3 (a) shows a state where the adhesive sheet 1 a is removed from the semiconductor chips 70 after the back surfaces 72 of the plurality of semiconductor chips 70 are attached to the transfer tape 80 .
[0401] In this step, when the second adhesive layer (X2) of the adhesive sheet 1a is a layer formed of an energy-ray-curable adhesive composition, the adhesive strength of the second adhesive layer (X2) can be reduced by irradiating with energy rays, thereby removing the adhesive sheet 1a.
[0402] It should be noted that the energy ray irradiated to reduce the adhesive force of the second adhesive layer (X2) is preferably irradiated from the adhesive sheet side.
[0403] After the adhesive sheet 1 a is removed, the circuit surfaces 71 of the plurality of semiconductor chips 70 are exposed, and the back surfaces 72 are affixed to the transfer tape 80 .
[0404] The transfer tape 80 is designed to be stretched by being pulled in the MD direction, and is an adhesive tape designed to increase the intervals between the plurality of semiconductor chips 70 .
[0405] The transfer tape used in one embodiment of the present invention is a transfer tape having a base film and a pressure-sensitive adhesive layer and / or an adhesive layer. Specific configurations thereof include, for example, the following aspects (1) to (3).
[0406] (1) A transfer tape in which a base film and an adhesive layer are laminated in this order.
[0407] (2) A transfer tape in which a base film and an adhesive layer are laminated in this order.
[0408] (3) A transfer tape in which a base film, a pressure-sensitive adhesive layer and an adhesive layer are laminated in this order.
[0409] Figure 3 2 shows a case where the transfer tape of the form (1) described above is used, and shows a state where the back surfaces 72 of a plurality of semiconductor chips 70 are attached to the adhesive layer 82 of the transfer tape 80 formed by laminating a base film 81 and an adhesive layer 82 in this order.
[0410] (Base film)
[0411] Examples of the base film constituting the transfer tape include resin films comprising one or more resins selected from polyvinyl chloride resins, polyester resins (such as polyethylene terephthalate), acrylic resins, polycarbonate resins, polyethylene resins, polypropylene resins, acrylonitrile-butadiene-styrene resins, polyimide resins, polyurethane resins, and polystyrene resins.
[0412] The base film constituting the transfer belt preferably contains a thermoplastic elastomer, a rubber-based material, or the like, and more preferably contains a thermoplastic elastomer.
[0413] Examples of the thermoplastic elastomer include urethane elastomers, olefin elastomers, vinyl chloride elastomers, polyester elastomers, styrene elastomers, acrylic elastomers, and amide elastomers.
[0414] The base film may have a single-layer structure or a multi-layer structure in which two or more layers are stacked.
[0415] In addition, the base film may further contain various additives such as pigments, dyes, flame retardants, plasticizers, antistatic agents, lubricants, and fillers.
[0416] The thickness of the base film constituting the transfer belt is preferably 20 to 300 μm, more preferably 30 to 250 μm, and even more preferably 40 to 200 μm.
[0417] (Adhesive layer)
[0418] The adhesive layer constituting the transfer tape may be a layer formed by an adhesive composition (x) which is a forming material for the above-mentioned first adhesive layer (X1) and the second adhesive layer (X2), but is preferably an energy-ray-curable adhesive layer formed by the above-mentioned energy-ray-curable adhesive composition which is suitable as a forming material for the second adhesive layer (X2).
[0419] When the pressure-sensitive adhesive layer constituting the transfer tape is an energy-ray-curable pressure-sensitive adhesive layer, the workability of the pickup step (6) becomes good.
[0420] However, when irradiating energy rays when removing the adhesive sheet in step (4), it is preferred to irradiate energy rays when removing the adhesive sheet from the adhesive sheet side so as not to reduce the adhesive strength of the energy-ray-curable adhesive layer of the transfer tape.
[0421] The thickness of the pressure-sensitive adhesive layer constituting the transfer tape is preferably 1 to 100 μm, more preferably 3 to 50 μm, and even more preferably 5 to 40 μm.
[0422] (Adhesive layer)
[0423] The adhesive layer constituting the transfer tape is preferably a layer formed of an adhesive composition containing a binder resin and a thermosetting component.
[0424] Examples of the binder resin include acrylic resins, polyester resins, urethane resins, acrylic urethane resins, silicone resins, rubber-based polymers, and phenoxy resins, and acrylic resins are preferred.
[0425] As the thermosetting component, an epoxy resin and a thermosetting agent are preferably contained.
[0426] The thickness of the adhesive layer constituting the transfer tape is preferably 1 to 100 μm, more preferably 5 to 75 μm, and even more preferably 5 to 50 μm.
[0427] <Step (5)>
[0428] Step (5) is a step of stretching the transfer tape in the MD direction to increase the intervals between the plurality of semiconductor chips.
[0429] like Figure 3 As shown in (b), by stretching the transfer tape 80 in the MD direction to increase the intervals between the plurality of semiconductor chips 70, it is possible to improve the pickup performance in the subsequent process.
[0430] <Step (6)>
[0431] Step (6) is a step of separating a plurality of semiconductor chips from the transfer tape to obtain semiconductor chips.
[0432] Figure 3 (c) shows a state where a plurality of semiconductor chips 70 are obtained by picking up in this process using the transfer tape of the embodiment (1) above.
[0433] Here, when the transfer tape used has an energy ray-curable adhesive layer, the adhesive force can be reduced by irradiating the energy ray, thereby improving the pickup property.
[0434] In addition, at this time, it is preferable to irradiate energy rays from the base film side.
[0435] When the transfer tape of the form (2) or (3) mentioned above is used as the transfer tape, when picking up in this process, the adhesive layer remains adhered to the back side of the semiconductor chip, and a semiconductor chip with an adhesive layer can be obtained, thereby omitting the bonding process.
[0436] Example
[0437] The present invention will be specifically described with reference to the following examples, but the present invention is not limited to the following examples. It should be noted that the physical property values in the following preparation examples and examples are values measured by the following methods.
[0438] <Weight average molecular weight (Mw)>
[0439] The values measured using a gel permeation chromatography apparatus (manufactured by Tosoh Corporation, product name "HLC-8020") under the following conditions and converted in terms of standard polystyrene were used.
[0440] (Measurement conditions)
[0441] Column: A column made by connecting "TSK guard column HXL-L", "TSK gel G2500HXL", "TSK gelG2000HXL", and "TSK gel G1000HXL" (all manufactured by Tosoh Corporation) in this order
[0442] Column temperature: 40℃
[0443] ·Developing solvent: tetrahydrofuran
[0444] Flow rate: 1.0mL / min
[0445] <Measurement of Thickness of Each Layer>
[0446] The measurement was performed using a constant pressure thickness gauge manufactured by TECLOCK Co., Ltd. (model: "PG-02J", standard: in accordance with JIS K6783, Z1702, and Z1709).
[0447] <Storage modulus E' of the heat-expandable substrate layer (Y1)>
[0448] The formed heat-expandable base material layer (Y1) was made into a size of 5 mm in length×30 mm in width×200 μm in thickness, and after removing the release material, the obtained material was used as a test sample.
[0449] The storage modulus E' of the test sample at a given temperature was measured using a dynamic viscoelasticity measuring apparatus (manufactured by TA INSTRUMENTS, product name "DMAQ800") under the conditions of test start temperature 0°C, test end temperature 300°C, heating rate 3°C / min, frequency 1 Hz, and amplitude 20 μm.
[0450] <Shear Storage Modulus G' of the First Adhesive Layer (X1) and the Second Adhesive Layer (X2)>
[0451] The formed first adhesive layer (X1) and second adhesive layer (X2) were cut into a circle with a diameter of 8 mm, and then the release material was removed and the layers were laminated to prepare a sample with a thickness of 3 mm. This sample was used as a test sample.
[0452] The shear storage modulus G' of the test sample at a given temperature was measured by a torsional shear method using a viscoelasticity measuring device (manufactured by Anton Paar, device name "MCR300") at a test start temperature of 0°C, a test end temperature of 300°C, a heating rate of 3°C / min, and a frequency of 1 Hz.
[0453] <Probe stickiness value>
[0454] The substrate layer to be measured was cut into a square with a side length of 10 mm, and then left to stand in an environment of 23° C. and 50% RH (relative humidity) for 24 hours to obtain a sample to be used as a test sample.
[0455] The probe tack value of the surface of the test sample was measured in an environment of 23° C. and 50% RH (relative humidity) using a tack tester (manufactured by Nippon Tokusakushoku Co., Ltd., product name “NTS-4800”) in accordance with JIS Z0237:1991.
[0456] Specifically, a stainless steel probe with a diameter of 5 mm was subjected to a contact load of 0.98 N / cm for 1 second. 2 After contacting the surface of the test sample, the force required to separate the probe from the surface of the test sample at a speed of 10 mm / sec was measured, and the obtained value was taken as the probe adhesion value of the test sample.
[0457] <Measurement of Adhesive Strength of Second Adhesive Layer (X2)>
[0458] A 50 μm thick PET film (manufactured by Toyobo Co., Ltd., product name “COSMOSHINE A4100”) was laminated on the adhesive surface of the second adhesive layer (X2) formed on the release film to prepare a substrate-attached adhesive sheet.
[0459] Then, the release film was removed, and the exposed adhesive surface of the second adhesive layer (X2) was attached to a stainless steel plate (SUS304 360 polish) as an adherend, and left to stand in an environment of 23°C and 50% RH (relative humidity) for 24 hours. Then, the adhesive strength at 23°C was measured in the same environment based on JIS Z0237:2000 using a 180° peeling method at a tensile speed of 300 mm / min.
[0460] <Young's modulus of the rigid support>
[0461] The static Young's modulus test method was measured at room temperature (25° C.) based on JIS Z2280:1993.
[0462] Preparation Example 1 (Synthesis of acrylic urethane resin)
[0463] (1) Synthesis of urethane prepolymer
[0464] In a reaction container under a nitrogen atmosphere, isophorone diisocyanate was added to 100 parts by mass (solid content ratio) of a polycarbonate diol having a weight average molecular weight of 1,000 so that the equivalent ratio of the hydroxyl group of the polycarbonate diol to the isocyanate group of the isophorone diisocyanate was 1 / 1, and then 160 parts by mass of toluene was added, and the reaction was carried out at 80° C. for 6 hours or more under a nitrogen atmosphere while stirring until the isocyanate group concentration reached a theoretical amount.
[0465] Next, a solution prepared by diluting 1.44 parts by mass (solid content ratio) of 2-hydroxyethyl methacrylate (2-HEMA) in 30 parts by mass of toluene was added, and the reaction was further carried out at 80° C. for 6 hours until the isocyanate groups at both terminals disappeared, thereby obtaining a urethane prepolymer having a weight average molecular weight of 29,000.
[0466] (2) Synthesis of acrylic urethane resin
[0467] Into a reaction container under a nitrogen atmosphere, 100 parts by mass (solid content ratio) of the urethane prepolymer obtained in Production Example 1, 117 parts by mass (solid content ratio) of methyl methacrylate (MMA), 5.1 parts by mass (solid content ratio) of 2-hydroxyethyl methacrylate (2-HEMA), 1.1 parts by mass (solid content ratio) of 1-thioglycerol, and 50 parts by mass of toluene were added, and the temperature was raised to 105° C. while stirring.
[0468] Then, a solution prepared by diluting 2.2 parts by mass (solid content ratio) of a radical initiator (manufactured by Nippon Seika Co., Ltd., product name "ABN-E") with 210 parts by mass of toluene was added dropwise to the reaction container over 4 hours while the temperature was kept at 105°C.
[0469] After the dropwise addition was completed, the mixture was reacted at 105° C. for 6 hours to obtain a solution of an acrylic urethane resin having a weight average molecular weight of 105,000.
[0470] Production Example 2 (Preparation of Adhesive Sheet)
[0471] In the preparation of the following pressure-sensitive adhesive sheet, the details of the pressure-sensitive adhesive resin, additives, thermally expandable particles, substrate, and release material used to form each layer are as follows.
[0472] <Adhesive resin>
[0473] Acrylic copolymer (i): an acrylic copolymer having a Mw of 600,000 and having structural units derived from raw material monomers composed of 2-ethylhexyl acrylate (2EHA) / 2-hydroxyethyl acrylate (HEA) = 80.0 / 20.0 (mass ratio).
[0474] Acrylic copolymer (ii): an acrylic copolymer having a Mw of 600,000 and having structural units derived from raw material monomers consisting of n-butyl acrylate (BA) / methyl methacrylate (MMA) / 2-hydroxyethyl acrylate (HEA) / acrylic acid = 86.0 / 8.0 / 5.0 / 1.0 (mass ratio).
[0475] <Additives>
[0476] Isocyanate crosslinking agent (i): manufactured by Tosoh Corporation, product name: "Coronate L", solid content concentration: 75% by mass.
[0477] <Thermal expansion particles>
[0478] Thermally expandable particles (i): manufactured by Kureha Corporation, product name "S2640", expansion starting temperature (t) = 208°C, average particle size (D 50 )=24μm, 90% particle size (D 90 )=49μm.
[0479] <Peeling Material>
[0480] Heavy release film: manufactured by Lintec Corporation, product name “SP-PET382150”, a material in which a release agent layer formed of a silicone release agent is provided on one surface of a polyethylene terephthalate (PET) film, thickness: 38 μm.
[0481] Light release film: manufactured by Lintec Corporation, product name “SP-PET381031”, a material having a release agent layer formed of a silicone-based release agent provided on one surface of a PET film, thickness: 38 μm.
[0482] (1) Formation of the first adhesive layer (X1)
[0483] 5.0 parts by mass (solid content ratio) of the above-mentioned isocyanate crosslinking agent (i) was added to 100 parts by mass of the solid content of the above-mentioned acrylic copolymer (i) as the adhesive resin, and the mixture was diluted with toluene and stirred until uniform to prepare an adhesive composition having a solid content concentration (active ingredient concentration) of 25% by mass.
[0484] Then, the adhesive composition was applied to the surface of the release agent layer of the heavy release film to form a coating film, and the coating film was dried at 100° C. for 60 seconds to form a first adhesive layer (X1) as a non-swelling adhesive layer having a thickness of 5 μm.
[0485] The shear storage modulus G'(23) of the first adhesive layer (X1) at 23°C is 2.5×10 5 Pa.
[0486] (2) Formation of the Second Adhesive Layer (X2)
[0487] 0.8 parts by mass (solid content ratio) of the above-mentioned isocyanate crosslinking agent (i) was added to 100 parts by mass of the solid content of the above-mentioned acrylic copolymer (ii) as an adhesive resin, and the mixture was diluted with toluene and stirred until uniform to prepare an adhesive composition having a solid content concentration (active ingredient concentration) of 25% by mass.
[0488] Then, the pressure-sensitive adhesive composition was applied onto the surface of the release agent layer of the light release film to form a coating film, and the coating film was dried at 100° C. for 60 seconds to form a second pressure-sensitive adhesive layer (X2) having a thickness of 10 μm.
[0489] The shear storage modulus G'(23) of the second adhesive layer (X2) at 23°C is 9.0×10 3 Pa.
[0490] The adhesive strength of the second pressure-sensitive adhesive layer (X2) measured by the above method was 1.0 N / 25 mm.
[0491] It should be noted that since the probe tack values of the second adhesive layer (X2) and the first adhesive layer (X1) were clearly 50 mN / 5 mmφ or more, the measurement of the probe tack values was omitted.
[0492] (3) Preparation of substrate (Y)
[0493] 6.3 parts by mass (solid content ratio) of an isocyanate crosslinking agent (i), 1.4 parts by mass (solid content ratio) of dioctyl bis(2-ethylhexanoate)tin as a catalyst, and the above-mentioned heat-expandable particles (i) were added to 100 parts by mass of the solid content of the acrylic urethane resin obtained in Preparation 1, and the mixture was diluted with toluene and stirred until uniform, thereby preparing a resin composition having a solid content concentration (active ingredient concentration) of 30% by mass.
[0494] The content of the heat-expandable particles (i) was 20% by mass relative to the total amount (100% by mass) of the effective components in the obtained resin composition.
[0495] Then, the resin composition was applied on the surface of a 50 μm thick polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name "COSMOSHINE A4100", probe viscosity value: 0 mN / 5 mmφ) as a non-expandable substrate to form a coating film, and the coating film was dried at 100° C. for 120 seconds to form an expandable substrate layer (Y1) with a thickness of 50 μm.
[0496] Here, the PET film corresponds to the non-expandable base material layer (Y2).
[0497] It should be noted that, as a sample for measuring the physical properties of the expandable substrate layer (Y1), the resin composition was applied to the surface of the release agent layer of the above-mentioned light release film to form a coating film, and the coating film was dried at 100°C for 120 seconds to similarly form an expandable substrate layer (Y1) with a thickness of 50 μm.
[0498] Then, the storage modulus and probe viscosity value of the expandable base material layer (Y1) at each temperature were measured based on the above-mentioned measurement method. The measurement results are as follows.
[0499] Storage modulus at 23°C E'(23) = 2.0 × 10 8 Pa
[0500] Storage modulus at 208°C E'(208) = 5.0 × 10 5 Pa
[0501] ·Probe viscosity value = 0mN / 5mmφ
[0502] The storage modulus and probe tack value of the PET film, ie, the non-expandable base layer (Y2), at various temperatures were measured. The measurement results are as follows.
[0503] Storage modulus at 23°C E'(23) = 1.0 × 10 3 MPa
[0504] Storage modulus at 208°C E'(208) = 0.8 × 10 2 MPa
[0505] ·Probe viscosity value = 0mN / 5mmφ
[0506] (4) Stacking of layers
[0507] The non-expandable substrate layer (Y2) of the substrate (Y1) prepared in the above (1-3) is bonded to the second adhesive layer (X2) formed in the above (2), and the heat-expandable substrate layer (Y1) is bonded to the first adhesive layer (X1) formed in the above (1).
[0508] Then, a PSA sheet was prepared by laminating heavy release film / first PSA layer (X1) / expandable substrate layer (Y1) / non-expandable substrate layer (Y2) / second PSA layer (X2) / light release film in this order.
[0509] It should be noted that the peeling force (F) of the produced PSA sheet was measured according to the above method as follows: 0 ) and (F 1 ).
[0510] As a result, the peeling force (F0 )=0.23N / 25mm, peeling force (F 1 )=0mN / 25mm, peel force (F 1 ) and peeling force (F 0 ) ratio [(F 1 ) / (F 0 )] is 0.
[0511] <Peel force(F 0 ) determination>
[0512] The produced pressure-sensitive adhesive sheet was left to stand in an environment of 23° C. and 50% RH (relative humidity) for 24 hours, and then the heavy release film of the pressure-sensitive adhesive sheet was removed, and the exposed first pressure-sensitive adhesive layer ( X1 ) was attached to a silicon wafer.
[0513] Next, the end of the silicon wafer to which the adhesive sheet was attached was fixed to the lower chuck of a universal tensile testing machine (manufactured by Orientec Corporation, product name “TENSILON UTM-4-100”), and the adhesive sheet was fixed to the upper chuck.
[0514] Then, the peeling force measured at the interface P between the silicon wafer and the first adhesive layer (X1) of the adhesive sheet was peeled at a tensile speed of 300 mm / min by a 180° peeling method in accordance with JIS Z0237:2000 in the same environment as above was referred to as the "peeling force (F 0 )”.
[0515] <Peel force(F 1 ) determination>
[0516] The heavy release film of the produced pressure-sensitive adhesive sheet was removed, and the exposed first pressure-sensitive adhesive layer (X1) was attached to a silicon wafer and heated at 240° C. for 3 minutes to expand the heat-expandable particles in the expandable base layer (Y1).
[0517] Then, compared with the above peeling force (F 0 ) is measured in the same manner as described above, and the peeling force measured at the interface P between the silicon wafer and the first adhesive layer (X1) of the adhesive sheet when peeling is performed under the above conditions is referred to as the "peeling force (F 1 )”.
[0518] It should be noted that in the peeling force (F 1 ), when the adhesive sheet (I) is to be fixed by the upper chuck of the universal tensile tester, if the adhesive sheet (I) is completely separated from the silicon wafer and cannot be fixed, the measurement is terminated and the peeling force (F 1 ) is regarded as “0mN / 25mm”.
[0519] Manufacturing Example 3 (Production of Transfer Tape)
[0520] An acrylic copolymer obtained by reacting butyl acrylate / 2-hydroxyethyl acrylate = 85 / 15 (mass ratio) and an energy-ray-curable acrylic copolymer having a weight average molecular weight (Mw) of 600,000 was obtained by reacting 80 mol % of methacryloyloxyethyl isocyanate (MOI) relative to the 2-hydroxyethyl acrylate, and the energy-ray-curable acrylic copolymer was used as the adhesive resin.
[0521] With respect to 100 parts by mass of the solid content of the energy-ray-curable acrylic copolymer, 3 parts by mass of 1-hydroxycyclophenyl ketone (manufactured by BASF, product name "Irgacure 184") as a photopolymerization initiator and 0.45 parts by mass of a toluene diisocyanate crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L") as a crosslinking agent were mixed in a solvent to obtain an adhesive composition.
[0522] Next, the adhesive composition was applied to the release-treated surface of the light release film (i) to form a coating film, and the coating film was dried to form an adhesive layer having a thickness of 10 μm.
[0523] Then, one surface of a polyester-based polyurethane elastomer sheet (manufactured by Sheedom Co., Ltd., product name "Higress DUS202", thickness 50 μm) as a substrate film was bonded to the exposed surface of the pressure-sensitive adhesive layer.
[0524] As described above, a transfer tape in which the base film, the adhesive layer, and the light release film were laminated in this order was obtained.
[0525] Example 1
[0526] <Step (1)>
[0527] The pressure-sensitive adhesive sheet prepared in Production Example 2 was cut into a square size of 230 mm×230 mm.
[0528] The heavy release film of the cut adhesive sheet was peeled off using a back grinding tape laminating machine (manufactured by Lintec Co., Ltd., device name "RAD-3510F / 12"), and the exposed adhesive surface of the first adhesive layer (X1) was pasted on a hard support (material: silicon, thickness: 725 μm, Young's modulus: 30 GPa). Then, the light release film was also peeled off, and the circuit surface of a semiconductor wafer (disk-shaped with a diameter of 200 mm and a thickness of 725 μm) having a circuit surface formed on the other side surface was pasted on the exposed adhesive surface of the second adhesive layer (X2).
[0529] Then, invisible laser irradiation was performed from the back side of the semiconductor wafer opposite to the circuit surface using an invisible laser irradiation device (manufactured by Tokyo Seimitsu Co., Ltd., device name "ML300PlusWH"), thereby forming a modified region inside the semiconductor wafer.
[0530] <Step (2)>
[0531] The back side of the semiconductor wafer without circuits was ground using a polishing grinder (manufactured by Tokyo Seimitsu Co., Ltd., device name "PG3000RM") while being exposed to ultrapure water, thereby dividing the semiconductor wafer and singulating the chips to obtain a plurality of semiconductor chips with a thickness of 20 μm.
[0532] <Step (3)>
[0533] The temperature in the system including the hard support, the adhesive sheet and the plurality of semiconductor chips was raised to 240° C. which was equal to or higher than the expansion starting temperature (208° C.) of the heat-expandable particles (i), and a heat treatment was performed for 3 minutes.
[0534] After the heat treatment, the hard support and the first adhesive layer (X1) can be easily separated at one time. At this time, the plurality of semiconductor chips remain attached to the second adhesive layer (X2), and no separation occurs between the layers constituting the adhesive sheet.
[0535] Furthermore, after separation from the rigid support, no part of the first adhesive layer (X1) was confirmed to remain on the surface of the rigid support, and no contamination was observed. Therefore, it is considered that there is no need to perform a new cleaning step on the surface of the rigid support.
[0536] <Step (4)>
[0537] The transfer tape obtained in Production Example 3 was cut into a square size of 210 mm×210 mm. At this time, the transfer tape was cut so that each side of the cut transfer tape was parallel to or perpendicular to the MD direction of the base film (Y2).
[0538] Next, the light release film is peeled off from the transfer tape, and the surface of the exposed adhesive layer is bonded to the back surfaces of the plurality of semiconductor chips separated from the hard support in step (3).
[0539] It should be noted that, at this time, the plurality of semiconductor chips are attached in such a manner that a group is located in the center of the transfer tape, and the dicing line when the semiconductor wafer is singulated is parallel or perpendicular to each side of the transfer tape. Furthermore, the plurality of semiconductor chips are peeled off from the adhesive surface of the second adhesive layer (X2) to remove the adhesive sheet.
[0540] <Step (5)>
[0541] The transfer tape with a plurality of semiconductor chips attached thereto is placed in a film expansion device capable of bidirectional stretching. The film expansion device has mutually orthogonal X-axis directions (positive direction is +X-axis direction, negative direction is -X-axis direction) and Y-axis directions (positive direction is +Y-axis direction, negative direction is -Y-axis direction), and has a holding mechanism for stretching in each direction (i.e., +X-axis direction, -X-axis direction, +Y-axis direction, -Y-axis direction).
[0542] Among them, the MD direction of the transfer tape is set in the expansion device to be consistent with the X-axis or Y-axis direction, the edges of the transfer tape are held by a holding mechanism, and then the transfer tape is stretched under the following conditions, thereby increasing the spacing between multiple semiconductor chips pasted on the transfer tape.
[0543] Number of retaining mechanisms: 5 on each side
[0544] ·Stretching speed: 5mm / sec
[0545] Stretching distance: Each side is stretched 60mm.
[0546] <Step (6)>
[0547] The transfer tape was irradiated with ultraviolet light (light intensity: 500 mJ / cm) from the base film side using an ultraviolet irradiation device (manufactured by Lintec Co., Ltd., product name "RAD-2000"). 2 , Illuminance: 220mW / cm 2 , irradiation speed: 15mm / s), so that the adhesive force of the adhesive layer of the transfer tape is reduced. Then, the semiconductor chip is picked up.
[0548] It should be noted that among the plurality of semiconductor chips obtained, no chip having an edge chip or the like was confirmed.
Claims
1. A method for producing a semiconductor chip, which is a method for producing a semiconductor chip from a semiconductor wafer using an adhesive sheet, wherein the adhesive sheet has a substrate (Y) and has a first adhesive layer (X1) and a second adhesive layer (X2) on both sides of the substrate (Y), respectively, wherein the substrate (Y) has at least an expandable substrate layer (Y1) containing expandable particles and a non-expandable substrate layer (Y2), The PSA sheet can generate irregularities on the adhesive surface of the first PSA layer (X1) due to the expansion of the expandable particles. The method for manufacturing the semiconductor chip comprises the following steps (1) to (3): Step (1): a step of attaching the adhesive surface of the first adhesive layer (X1) to a hard support and attaching the adhesive surface of the second adhesive layer (X2) to a surface of a semiconductor wafer; Step (2): a step of dividing the semiconductor wafer to obtain a plurality of semiconductor chips; Step (3): a step of expanding the expandable particles and separating the semiconductor chips at the interface P between the rigid support and the first adhesive layer (X1) while maintaining the plurality of semiconductor chips attached to the second adhesive layer (X2). The expandable substrate layer (Y1) and the non-expandable substrate layer (Y2) constituting the substrate (Y) are both non-adhesive layers. The pressure-sensitive adhesive sheet includes a first pressure-sensitive adhesive layer (X1) on the expandable substrate layer (Y1) side of the substrate (Y) and a second pressure-sensitive adhesive layer (X2) on the non-expandable substrate layer (Y2) side of the substrate (Y).
2. A method for producing a semiconductor chip, which is a method for producing a semiconductor chip from a semiconductor wafer using an adhesive sheet, wherein the adhesive sheet has a substrate (Y) and has a first adhesive layer (X1) and a second adhesive layer (X2) on both sides of the substrate (Y), respectively, wherein the substrate (Y) has at least an expandable substrate layer (Y1) containing expandable particles and a non-expandable substrate layer (Y2), The PSA sheet can generate irregularities on the adhesive surface of the first PSA layer (X1) due to the expansion of the expandable particles. The method for manufacturing the semiconductor chip comprises the following steps (1) to (3): Step (1): a step of attaching the adhesive surface of the first adhesive layer (X1) to a hard support and attaching the adhesive surface of the second adhesive layer (X2) to a surface of a semiconductor wafer; Step (2): a step of dividing the semiconductor wafer into a plurality of semiconductor chips; Step (3): a step of expanding the expandable particles and separating the semiconductor chips at the interface P between the rigid support and the first adhesive layer (X1) while maintaining the plurality of semiconductor chips attached to the second adhesive layer (X2). The expandable substrate layer (Y1) and the non-expandable substrate layer (Y2) constituting the substrate (Y) are both non-adhesive layers. The substrate (Y) comprises the expandable substrate layer (Y1), a non-expandable substrate layer (Y2-1) provided on the first adhesive layer (X1) side of the expandable substrate layer (Y1), and a non-expandable substrate layer (Y2-2) provided on the second adhesive layer (X2) side of the expandable substrate layer (Y1), The storage modulus E' of the non-expandable base layer (Y2-1) when the expandable particles expand is lower than the storage modulus E' of the non-expandable base layer (Y2-2) when the expandable particles expand.
3. The method for manufacturing a semiconductor chip according to claim 1, wherein: The non-expandable substrate layer (Y2) is located at a position farther from the first adhesive layer (X1) than the expandable substrate layer (Y1), and the non-expandable substrate layer (Y2) is not present between the expandable substrate layer (Y1) and the first adhesive layer (X1). The storage modulus E' of the non-expandable base layer (Y2) when the expandable particles expand is greater than the storage modulus E' of the expandable base layer (Y1) when the expandable particles expand.
4. The method for manufacturing a semiconductor chip according to claim 1 or 2, wherein: In step (3), when the expandable particles are expanded, separation does not occur between the layers constituting the pressure-sensitive adhesive sheet.
5. The method for manufacturing a semiconductor chip according to claim 1 or 2, further comprising the following step (4): Step (4): After separation from the rigid support in step (3), the back surfaces of the plurality of semiconductor chips opposite to the circuit surfaces are attached to a transfer tape, and then the adhesive sheet is removed from the semiconductor chips, wherein the transfer tape has a base film and has an adhesive layer and / or a bonding agent layer.
6. The method for manufacturing a semiconductor chip according to claim 1 or 2, wherein: The expandable particles are heat-expandable particles having an expansion starting temperature (t) of 60 to 270°C.
7. The method for manufacturing a semiconductor chip according to claim 6, wherein: The expansion of the heat-expandable particles is performed by heating the heat-expandable particles at a temperature between "expansion starting temperature (t) + 10° C." and "expansion starting temperature (t) + 60° C.".
8. The method for manufacturing a semiconductor chip according to claim 6, wherein: The expandable substrate layer (Y1) is a heat-expandable substrate layer (Y1-1) containing the heat-expandable particles, and the heat-expandable substrate layer (Y1-1) has a storage modulus E'(23) at 23°C of 1.0×10 6 Pa or above.
9. The method for manufacturing a semiconductor chip according to claim 1 or 2, wherein: The volume change rate (%) of the non-expandable base material layer (Y2) is less than 2 volume %.
10. The method for manufacturing a semiconductor chip according to claim 1 or 2, wherein: Step (2) is a step of grinding the back surface of the semiconductor wafer having the reformed region, which is opposite to the circuit surface and on which no circuit is formed, to divide the semiconductor wafer into a plurality of semiconductor chips.
Citation Information
Patent Citations
Energy-beam curable thermal-releasable pressure-sensitive adhesive sheet and method for producing cut pieces using the same
CN1471565A
Method for processing adherend using adhesive sheet
JP2003292916A