A method for preparing a long-life neutral zinc-iron flow battery
By using specific solutions and separator materials in the negative electrode electrolyte of neutral zinc iron flow batteries, the deposition and desorption process of zinc is improved, and the problems of low energy density and fast capacity decline of the flow batteries are solved, achieving low cost , high performance and long-life battery performance.
Patent Information
- Application Number
- CN202010903160.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-01
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-09-01
AI Technical Summary
The existing zinc-bromo, zinc-iron, iron-chromium and all-vana flow battery systems have problems such as low energy density, high cost, easy corrosion and fast capacity decline, which limits the large-scale configuration and application of flow batteries.
By using deionized water and ferricyanide solutions prepared in the negative electrode electrolyte of neutral zinc iron flow batteries, combined with the use of metal cation exchange membrane and zinc salt, the deposition and decomposition of zinc on the electrode is improved. The process is attached to improve the redox reversibility of Zn/Zn2+ electric pairs and stabilizes the battery cycle process.
The flow battery with low cost, high performance and ultra-long cycle life is achieved, reducing the corrosion and cost of the battery, and significantly improving the battery capacity retention rate and Coulomb efficiency.
Smart Images

Figure HDA0002660454630000011 
Figure HDA0002660454630000021 
Figure HDA0002660454630000031
Abstract
Description
Technical Field
[0001] The invention relates to the field of redox neutral zinc-iron liquid flow batteries, in particular to a method for preparing a long-life neutral zinc-iron liquid flow battery. Background Art
[0002] With the increasing exhaustion of traditional fossil fuels and the serious environmental pollution they bring, it is imperative to find new energy sources and develop new energy technologies. At present, electric energy is mainly provided by thermal, wind, hydro and solar power generation methods. However, thermal power generation brings serious environmental pollution, and renewable energy sources such as wind, hydro and solar power have the characteristics of intermittent and discontinuous, which cannot meet the demand for direct electricity. In order to solve this problem, it is necessary to develop efficient and cheap energy storage devices. As a large-scale energy storage device, flow batteries can fully meet the needs of power grids and life, and have the advantages of flexible design, long cycle life, fast response, independent adjustment of storage capacity and output power, and are expected to be widely used in the field of power grid energy storage. However, in recent years, system research based on zinc-bromine, zinc-iron, iron-chromium and all-vanadium flow batteries has faced problems such as low energy density, high cost, easy corrosion and fast capacity decay. On the one hand, these problems greatly limit the large-scale configuration of flow batteries and need to be solved urgently; on the other hand, this has also accelerated the development and exploration of new systems for flow batteries. Metal zinc has a high theoretical capacity (820mAh g -1 ), low electrode potential (-0.762V vs standard hydrogen electrode), large reserves, non-toxicity, and high safety, it has always been considered an ideal anode material for liquid flow batteries. However, its large-scale application is also restricted by problems such as low coulombic efficiency and poor cycle life caused by dendrite growth during battery cycling. Inhibiting dendrite growth during the cycle and improving the cycle stability of zinc negative electrode are currently urgent problems to be solved. There are currently four common methods to solve this problem: electrolyte modification, metal zinc anode modification, electric field regulation, and ion transport control. Summary of the invention
[0003] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a long-life neutral zinc-iron liquid flow battery, in which the negative electrode of the battery is modified by the electrolyte to improve the Zn / Zn 2+ The redox reversibility of the electrode also stabilizes the deposition and desorption process of zinc on the electrode, and can be applied to the neutral zinc-iron liquid flow battery system to obtain ultra-long cycle life and good performance. This method can be used to obtain a low-cost, high-performance, long-cycle-life liquid flow battery, achieving the purpose of reducing costs, reducing corrosion, and increasing battery cycle life.
[0004] The technical solution of the present invention is as follows:
[0005] A method for preparing a long-life neutral zinc-iron flow battery comprises the following steps:
[0006] (1) Preparation of positive electrode electrolyte: Prepare a solution of halide and ferrocyanide using deionized water;
[0007] (2) Preparation of negative electrode electrolyte: a series of halide solutions with different concentrations were prepared using deionized water;
[0008] (3) Battery assembly: Immerse the ion exchange membrane in an alkaline solution and keep it at a constant temperature of 50 to 100° C. for 1 to 3 hours to obtain a metal cation exchange membrane; cut and polish the zinc sheet to serve as the negative electrode reaction active material of the battery;
[0009] (4) Assemble the key materials obtained in steps (1), (2) and (3) into a neutral zinc-iron liquid flow battery.
[0010] In the method for preparing a long-life neutral zinc-iron flow battery, the concentration of the ferrocyanide aqueous solution prepared in step (1) is 0.1 mol L -1 ~1mol L -1 , the concentration of halide aqueous solution is 0.1 mol L -1 ~4.5mol L -1 The volume ratio of ferrocyanide aqueous solution to halide aqueous solution is 1:0.5~5.
[0011] The preparation method of the long-life neutral zinc-iron liquid flow battery, in step (1), the ferrocyanide is K3Fe(CN)6, K4Fe(CN)6 or Na3Fe(CN)6, and the halide is NaBr, KBr, CaBr2, MgBr2, NaCl, KCl, MgCl2, CaCl2, NaI, KI or AgI.
[0012] In the method for preparing a long-life neutral zinc-iron flow battery, the concentration of the halide aqueous solution prepared in step (2) is 0.1 mol L -1 ~4.5mol L -1 .
[0013] In the preparation method of the long-life neutral zinc-iron liquid flow battery, in step (2), the halide is NaBr, KBr, CaBr2, MgBr2, NaCl, KCl, MgCl2, CaCl2, NaI, KI or AgI.
[0014] The preparation method of the long-life neutral zinc-iron flow battery is as follows: on the basis of step (2), before charging and discharging the battery, a zinc salt is added to the negative electrode electrolyte as a supplement, the zinc salt is Zn(NO3)2, ZnCl2, ZnSO4, ZnBr2 or Zn(CH3COO)2, and the concentration of the supplemented zinc salt aqueous solution is 0.1 mol L-1 ~1mol L -1 The volume ratio of the zinc salt aqueous solution to the negative electrode electrolyte is 1:1~10.
[0015] In the method for preparing the long-life neutral zinc-iron liquid flow battery, in step (3), the alkaline solution is a 0.5-2 mol / L KOH aqueous solution or a NaOH aqueous solution.
[0016] The preparation method of the long-life neutral zinc-iron liquid flow battery, the neutral zinc-iron liquid flow battery is tested as follows:
[0017] (1) Battery discharge test: The neutral zinc-iron flow battery is subjected to the first cycle discharge test, and the obtained negative electrode electrolyte is taken out for testing;
[0018] (2) Cyclic voltammetry test: Select a working electrode, a counter electrode and a reference electrode, and perform a cyclic voltammetry test on the negative electrode electrolyte obtained in step (1);
[0019] (3) Battery cycle test: The battery test system is used to perform long cycle, rate, and polarization tests on neutral zinc-iron flow batteries.
[0020] The design concept of the present invention is:
[0021] The present invention improves the reaction energy barrier in the process of zinc deposition in the negative electrode of the battery by modifying the electrolyte; during the charging process, zinc deposition in the electrolyte can be carried out in a more stable process, reducing the growth of zinc dendrites and extending the cycle life of the battery; at the same time, ferrocyanide in the positive electrode storage tank is converted. In addition, the negative electrode electrolyte cyclic voltammetry test study shows that the electrolyte can also improve Zn / Zn 2+ The redox reversibility of the electrode couple also helps to improve the cycle life of neutral zinc-iron flow batteries.
[0022] Compared with the prior art, the present invention has the following significant advantages:
[0023] 1. The present invention uses metal cation salt as supporting electrolyte in the negative electrode electrolyte of neutral zinc-iron flow battery, and at the same time, makes halogen ions and zinc ions generated by discharge to carry out complex coordination, thereby improving Zn / Zn 2+ The redox reversibility of the electrode couple regulates the deposition and desorption process of metallic zinc on the electrode and stabilizes the negative electrode electrolyte, thereby solving the problem of rapid capacity decay of neutral zinc-iron liquid flow batteries and greatly improving the battery's capacity retention rate.
[0024] 2. The positive and negative active materials of the neutral zinc-iron flow battery of the present invention are [Fe(CN)6] 3- / [Fe(CN)6] 4- and Zn / Zn 2+Metallic zinc has a large specific capacity, is non-toxic and safe, while iron reserves are abundant and low in cost, and can meet large-scale application needs. This energy storage device has good application prospects in the field of large-scale energy storage.
[0025] 3. The electrolyte designed by the present invention for use in the negative electrode of a neutral zinc-based liquid flow battery has the characteristics of industrial practicability such as low price, readily available raw materials, simple process, and convenient operation. In addition, the battery using the electrolyte has the advantages of ultra-low cost, ultra-long cycle, and high efficiency, which will help promote the commercial development of liquid flow batteries.
[0026] In summary, the present invention uses ferrocyanide and zinc foil as positive and negative active materials, and uses metal salts as negative electrode supporting electrolytes to assemble a neutral zinc-iron flow battery. During the discharge process, the metal zinc loses electrons and enters the solution to form a complex with halogen ions. Through cyclic voltammetry analysis, it was found that halogen ions can increase the Zn / Zn 2+ In addition to the redox reversibility of the electrolyte, the existence of a stable complex state was also confirmed by consulting the literature. Finally, the neutral zinc-iron flow battery was assembled with this electrolyte for long-term cycle testing. -2 The battery can stably cycle for more than 1340 cycles at the current density, maintaining a coulombic efficiency of 100% and a capacity retention rate of more than 80%. -2 At the current density, the performance of 100% coulombic efficiency, 75.40% energy efficiency and 75.53% voltage efficiency can also be obtained. In addition, the raw materials used in the electrolyte used in this method have abundant reserves, low prices, no corrosive substances, and are environmentally friendly. It is an electrolyte that is expected to be widely used in neutral zinc-based flow batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 .Comparison of cyclic voltammetry at different halide concentrations at the negative electrode.
[0028] Figure 2 Neutral zinc-iron flow battery at 30 mA cm -2 Efficiency and capacity retention rate within 1340 cycles at current density.
[0029] Figure 3 Neutral zinc-iron flow battery at 80 mA cm -2 Efficiency plot at current density.
[0030] Figure 4 Neutral zinc-iron flow battery at 30 mA cm -2 Capacity and energy of the battery after more than 300 cycles at different current densities. DETAILED DESCRIPTION
[0031] In the specific implementation process, the preparation method of the long-life neutral zinc-iron liquid flow battery of the present invention includes the following process and testing steps:
[0032] (1) Preparation of positive electrode electrolyte (ferrocyanide solution): Use deionized water to prepare a certain concentration of ferrocyanide solution (such as K3Fe(CN)6, K4Fe(CN)6, Na3Fe(CN)6, etc.) and halide solution (such as NaBr, KBr, CaBr2, MgBr2, NaCl, KCl, MgCl2, CaCl2, NaI, KI, AgI, etc.).
[0033] (2) Preparation of negative electrode electrolyte: Use deionized water to prepare a series of halide solutions (such as NaBr, KBr, CaBr2, MgBr2, NaCl, KCl, MgCl2, CaCl2, NaI, KI, AgI, etc.) with different concentrations.
[0034] (3) Battery assembly: Immerse a certain amount of ion exchange membrane in a certain concentration of KOH (or NaOH) aqueous solution (0.1-5 mol / L), and cook at a constant temperature of 50-100°C for 1-3 hours to obtain a potassium (or sodium) ion diaphragm. Cut a zinc sheet of a certain size and polish it until there is no passivation layer and contaminants on the surface. Rinse it with deionized water and use it as the negative electrode reaction active material of the battery.
[0035] The positive electrode storage tank is filled with positive electrode electrolyte, and the positive electrode storage tank is connected to the positive electrode inlet and outlet of the battery through a peristaltic pump through a pipeline; the negative electrode storage tank is filled with negative electrode electrolyte, and the negative electrode storage tank is connected to the negative electrode inlet and outlet of the battery through a magnetic pump through a pipeline. The key materials obtained in steps (1), (2), and (3) are assembled into a single battery for testing. The liquid flow battery generally includes an end plate, a sealing gasket, a current collector, a porous carbon felt electrode, and a diaphragm.
[0036] (4) Battery discharge test: The battery obtained in step (3) was charged at 10 mA cm -2 The first discharge test is carried out at the current density, and the obtained negative electrode electrolyte is taken out for testing;
[0037] (5) Cyclic voltammetry test: The negative electrode electrolyte obtained in step (4) was subjected to a cyclic voltammetry test. The scan rate was 10 to 50 mV / s, the working electrode was a glassy carbon electrode, the counter electrode was a platinum mesh electrode, and the reference electrode was a calomel electrode;
[0038] (6) Battery cycle test: Based on steps (1), (2) and (3), a certain concentration of negative electrode electrolyte is selected. In order to allow the complexation reaction to fully occur, before charging and discharging the battery, a certain concentration (0.1-1 mol / L) of zinc salt (such as: Zn(NO3)2, ZnCl2, ZnSO4, ZnBr2, Zn(CH3COO)2, etc.) is added to the negative electrode electrolyte to complete part of the complexation reaction in advance. The key materials obtained in the above steps are assembled into a battery, and the battery long cycle, rate, polarization and other tests are performed using a battery testing system.
[0039] Below, the present invention is further described in conjunction with examples:
[0040] Example 1
[0041] In this embodiment, the preparation method of the long-life neutral zinc-iron flow battery includes the following process and testing steps:
[0042] (1) Preparation of electrolyte:
[0043] Prepare 0.1 mol L -1 15 mL of K3[Fe(CN)6] aqueous solution was used as the positive electrolyte, and the positive supporting electrolyte was 3 mol L -1 10 mL of KBr aqueous solution was placed in the positive electrode storage tank. The negative electrode electrolyte was 1, 2, 3, 4, 4.5 mol L -1 Take 60 mL of KBr aqueous solution and place it in each negative electrode storage tank.
[0044] (2) Diaphragm material processing and battery assembly
[0045] Place the metal cation exchange membrane in a 1 mol / L KOH alkaline aqueous solution at 80°C for 1 hour, take it out, wash it, and soak it in deionized water for later use. Take a zinc sheet with a thickness of 6 μm and cut it to a size of 3×4.5 cm 2 The zinc sheet is polished clean and used as the negative electrode reaction active material of the battery. A group of single cells are assembled and equipped with the electrolyte involved in the present invention. A cyclic voltammetry test is performed after the first cycle of discharge using the Xinwei test system.
[0046] like Figure 1 As shown in the figure, at a scan rate of 50 mV / s, as the bromide ion concentration at the negative electrode of the battery increases, the Zn / Zn 2+ The redox reversibility of the electrode pair is improved. This phenomenon shows that bromide ions have a great influence on the redox reversibility of Zn / Zn 2+ The redox reversibility of the electrode pair is improved, and this effect becomes more obvious as the concentration of bromide ions increases. Improving the redox reversibility of the active material in the flow battery helps to increase the cycle life of the battery.
[0047] Example 2
[0048] In this embodiment, the preparation method of the long-life neutral zinc-iron flow battery includes the following process and testing steps:
[0049] (1) Preparation of electrolyte:
[0050] Prepare 0.1 mol L -1 15 mL of K3[Fe(CN)6] aqueous solution was used as the positive electrolyte, and the positive supporting electrolyte was 3.0 mol L -1 30mL of KBr aqueous solution was placed in the positive electrode storage tank. The negative electrode electrolyte was 0.3 mol L -1 20 mL of ZnBr2 aqueous solution, 3.6 mol L -1 40 mL of KBr aqueous solution were placed in the negative electrode storage tank.
[0051] (2) Diaphragm material processing and battery assembly
[0052] Place the metal cation exchange membrane in a 1 mol / L KOH alkaline aqueous solution at 80°C for 1 hour, take it out, wash it, and soak it in deionized water for later use. Take a zinc sheet with a thickness of 4 μm and cut it into a size of 3×4.5 cm 2 The zinc sheet was polished clean and used as the negative electrode active material of the battery. A single cell was assembled and equipped with the electrolyte involved in the present invention. The battery long cycle test was carried out using the Xinwei test system. The charge and discharge current density was 30 mA cm -2 .
[0053] In this embodiment, the obtained neutral zinc-iron flow battery system has good battery performance, very high coulombic efficiency, long cycle life and very good cycle stability. Figure 2 As shown, the new neutral zinc-iron flow battery 30mA cm -2 Capacity retention and efficiency diagram under current density. The battery can be stably cycled for more than 1340 cycles, with the coulombic efficiency maintained at 100% and the capacity retention rate above 80%.
[0054] Example 3
[0055] In this embodiment, the preparation method of the long-life neutral zinc-iron flow battery includes the following process and testing steps:
[0056] (1) Preparation of electrolyte:
[0057] Prepare 0.1 mol L -1 15 mL of K3[Fe(CN)6] aqueous solution was used as the positive electrolyte, and the positive supporting electrolyte was 3.0 mol L -130mL of KBr aqueous solution was placed in the positive electrode storage tank. The negative electrode electrolyte was 0.3 mol L -1 15 mL of ZnBr2 aqueous solution, 3.6 mol L -1 45 mL of KBr aqueous solution were placed in the negative electrode storage tank.
[0058] (2) Diaphragm material processing and battery assembly
[0059] Place the metal cation exchange membrane in a 1 mol / L KOH alkaline aqueous solution at 80°C for 1 hour, take it out, wash it, and soak it in deionized water for later use. Take a zinc sheet with a thickness of 8 μm and cut it into a size of 3×4.5 cm 2 The zinc sheet was polished clean and used as the negative electrode active material of the battery. A single cell was assembled and equipped with the electrolyte involved in the present invention. The battery long cycle test was carried out using the Xinwei test system. The charge and discharge current density was 80 mA cm -2 .
[0060] In this embodiment, the obtained neutral zinc-iron flow battery system has good battery performance, very high coulombic efficiency, long cycle life and very good cycle stability. Figure 3 As shown, the new neutral zinc-iron flow battery of the present invention can achieve a high current density at 80 mA cm -2 Efficiency diagram under current density. After 300 stable cycles, the coulombic efficiency is maintained at 100%, and the energy efficiency and voltage efficiency are both above 75%.
[0061] Example 4
[0062] In this embodiment, the preparation method of the long-life neutral zinc-iron flow battery includes the following process and testing steps:
[0063] (1) Preparation of electrolyte:
[0064] Prepare 0.5 mol L -1 10 mL of K3Fe(CN)6 aqueous solution was used as the positive electrolyte, and the positive supporting electrolyte was 1.5 mol L -1 10 mL of KBr aqueous solution was placed in the positive electrode storage tank. The negative electrode electrolyte was 0.3 mol L -1 10 mL of ZnBr2 aqueous solution, 1.5 mol L -1 50mL of KBr aqueous solution were placed in the negative electrode storage tank.
[0065] (2) Diaphragm material processing and battery assembly
[0066] Place the metal cation exchange membrane in a 1 mol / L KOH alkaline aqueous solution at 100°C for 1 hour, take it out, wash it, and soak it in deionized water for later use. Take a zinc sheet with a thickness of 10 μm and cut it into a size of 3×4.5 cm 2 The zinc sheet was polished clean and used as the negative electrode active material of the battery. A single cell was assembled and equipped with the electrolyte involved in the present invention. The battery long cycle test was carried out using the Xinwei test system. The charge and discharge current density was 30 mA cm -2 .
[0067] In this embodiment, the obtained neutral zinc-iron flow battery system has good battery performance, such as Figure 4 As shown, after more than 300 cycles, there is no obvious attenuation in the capacity and energy of the battery, which indicates that the negative electrode electrolyte can also operate stably under high capacity conditions.
[0068] The results of the examples show that the present invention not only stabilizes the Zn / Zn 2+ The deposition and desorption process of the electrode also increases the Zn / Zn 2+ The redox reversibility of the electrode couple greatly extends the cycle life of the neutral zinc-iron flow battery.
Claims
1. A method for preparing a long-life neutral zinc-iron flow battery, characterized in that: The following steps are involved: (1) Preparation of positive electrode electrolyte: prepare halide and ferrocyanide solutions using deionized water; (2) Preparation of negative electrode electrolyte: prepare halide solution using deionized water; (3) Battery assembly: Immerse the ion exchange membrane in an alkaline solution and keep it at a constant temperature of 50-100 °C for 1-3 h to obtain a metal cation exchange membrane; cut and polish the zinc sheet to serve as the negative electrode reaction active material of the battery; (4) Assembling the key materials obtained in steps (1), (2) and (3) into a neutral zinc-iron liquid flow battery; The concentration of the ferricyanide aqueous solution prepared in step (1) is 0.1 mol L -1 ~1 mol L -1 , the concentration of halide aqueous solution is 1.5 mol L -1 ~4.5 mol L -1 , the volume ratio of ferrocyanide aqueous solution to halide aqueous solution is 1:0.5~5; The ferrocyanide is K3Fe(CN)6, and the halides in the positive and negative electrolytes are NaBr, KBr, CaBr2, and MgBr2; The concentration of the halide aqueous solution prepared in step (2) is 1 mol L -1 ~4.5 mol L -1 ; Based on step (2), before charging and discharging the battery, a zinc salt is added to the negative electrode electrolyte as a supplement, and the zinc salt is Zn(NO3)2, ZnCl2, ZnSO4, ZnBr2 or Zn(CH3COO)2. The concentration of the supplemented zinc salt aqueous solution is 0.1 mol L -1 ~1 molL -1 , the volume ratio of zinc salt aqueous solution to negative electrode electrolyte is 1:1~10; In step (3), the alkaline solution is a 0.5-2 mol / L KOH aqueous solution or a NaOH aqueous solution.
2. The method for preparing a long-life neutral zinc-iron flow battery according to claim 1, characterized in that: The neutral zinc-iron flow battery was tested as follows: (1) Battery discharge test: The neutral zinc-iron liquid flow battery is subjected to the first cycle discharge test, and the obtained negative electrode electrolyte is taken out for testing; (2) Cyclic voltammetry test: Select a working electrode, a counter electrode and a reference electrode, and perform a cyclic voltammetry test on the negative electrode electrolyte obtained in step (1); (3) Battery cycle test: The battery testing system is used to perform long cycle, rate and polarization tests on neutral zinc-iron liquid flow batteries.