Semiconductor device and method for manufacturing the same

By introducing single crystal regions with different aluminum concentrations and passivation treatment in HEMT, the problem of large on-resistance of HEMT is solved, and lower on-resistance and higher performance are achieved.

CN112204752BActive Publication Date: 2024-11-19INNOSCIENCE (ZHUHAI) TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080002864.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-07
Publication Date
2024-11-19
Estimated Expiration
2040-08-07

AI Technical Summary

Technical Problem

High electron mobility transistor (HEMT) has a large on-resistance during operation, which affects its performance.

Method used

By introducing a single crystal region with different aluminum (Al) concentrations in the semiconductor device to form a structure with low on-resistance, the specific method includes forming a first nitride semiconductor layer and a second nitride semiconductor layer on the substrate and in the first Passivation treatment is performed on the nitride semiconductor layer to reduce the aluminum concentration, and regions 20a1 and regions 20b are formed, with the aluminum concentration of regions 20a1 being less than regions 20b, and a heterojunction is formed between the barrier layer and the channel layer to reduce resistance .

Benefits of technology

Significantly reduces the on-resistance of HEMT and improves its performance, which is manifested in reducing the resistance between source and drain, reducing the inherent on-resistance of HEMT (Ron), making its performance better than traditional silicon-based Power chip.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112204752B_ABST
    Figure CN112204752B_ABST
Patent Text Reader

Abstract

The present disclosure relates to a semiconductor device and a method for manufacturing the same. The semiconductor device includes: a substrate; a first nitride semiconductor layer, the first nitride semiconductor layer is located on the substrate; and a second nitride semiconductor layer, the second nitride semiconductor layer is located on the first nitride semiconductor layer. The second nitride semiconductor layer has a first region and a second region, and the second nitride semiconductor layer has a single crystal. The semiconductor device includes an electrode, the electrode is in contact with the first region. The first concentration of aluminum Al in the first region is less than the second concentration of Al in the second region, and the single crystal in the first region replaces the crystal structure of the first nitride semiconductor layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to semiconductor devices, and more particularly to high electron mobility transistors (HEMTs) and methods of manufacturing the same. Background Art

[0002] A high electron mobility transistor (HEMT) includes two layers (e.g., a channel layer and a barrier layer) with different band gaps for forming a heterojunction. The polarization of the heterojunction forms a two-dimensional electron gas (2DEG) region in the channel layer adjacent to the interface between the channel layer and the barrier, which enables the HEMT to operate or work at a relatively high frequency bandwidth and a relatively large voltage level.

[0003] However, it is found that when the HEMT is operating, the on-resistance is relatively large, which may have an adverse effect on its performance. Summary of the invention

[0004] According to some embodiments of the present disclosure, a semiconductor device is provided, the semiconductor device comprising: a substrate; a first nitride semiconductor layer, the first nitride semiconductor layer being located on the substrate; and a second nitride semiconductor layer, the second nitride semiconductor layer being located on the first nitride semiconductor layer. The second nitride semiconductor layer has a first region and a second region, and the second nitride semiconductor layer has a single crystal. The semiconductor device comprises an electrode in contact with the first region, wherein a first concentration of aluminum (Al) in the first region is less than a second concentration of aluminum (Al) in the second region, and the single crystal in the first region takes over the crystal structure of the first nitride semiconductor layer.

[0005] According to some embodiments of the present disclosure, a semiconductor device is provided, the semiconductor device comprising: a substrate; a first nitride semiconductor layer, the first nitride semiconductor layer being located above the substrate; and a second nitride semiconductor layer, the second nitride semiconductor layer being located on the first nitride semiconductor layer. The second nitride semiconductor layer has a first region and a second region, and the second nitride semiconductor layer has a single crystal. The semiconductor device comprises an electrode in contact with the first region, wherein a first concentration of aluminum (Al) in the first region is different from a second concentration of aluminum (Al) in the second region, and the first region lacks a polycrystalline structure.

[0006] According to some embodiments of the present disclosure, a method for manufacturing a semiconductor device is provided. The method includes providing a semiconductor structure having a substrate, a channel layer, and a barrier layer. The method includes providing a passivation layer on the barrier layer, the passivation layer exposing a first region of the barrier layer and covering a second region of the barrier layer. The method further includes soaking the first region of the barrier layer in a first solution, so that a first concentration of aluminum (Al) in the first region is different from a second concentration of aluminum (Al) in the second region. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] When read together with the accompanying drawings, various aspects of the present disclosure can be easily understood from the following detailed description. It should be noted that various features may not be drawn to scale. In fact, the dimensions of various features may be arbitrarily increased or reduced for clarity of discussion.

[0008] Figure 1A shows a cross-sectional view of a semiconductor device according to some embodiments of the present disclosure;

[0009] Figure 1B The results of transmission electron microscopy (TEM) were shown along the Figure 1A A schematic view of a line scan result obtained by arrow x1 shown;

[0010] Figure 1C The TEM shows Figure 1A A schematic view of a line scan result obtained by arrow x2 shown;

[0011] Figure 2 Shows how Figure 1A A cross-sectional view of a temporary structure of a semiconductor device is shown;

[0012] Figure 3A Shows how Figure 2 An enlarged top view of the structure in the dashed rectangle A shown;

[0013] Figure 3B Shows how Figure 2 A schematic view of the lattice arrangement in the dashed rectangle B shown;

[0014] Figure 3C Shows along Figure 2 A cross-sectional view of the structure shown by dashed line C;

[0015] Figure 3D Shows how Figure 2 An enlarged view of the structure in dashed circle D is shown;

[0016] Figure 3E Shows how Figure 2A schematic view of the lattice arrangement in the dashed rectangle E shown;

[0017] Figure 4A , 4B , 4C, 4D, 4E, 4F, 4G, 4H, and 4I illustrate operations for manufacturing a semiconductor device according to some embodiments of the present disclosure;

[0018] Figure 5A , 5B , 5C, 5D, 5E, 5F, 5G, 5H, 5I, and 5J illustrate operations for manufacturing a semiconductor device according to some other embodiments of the present disclosure;

[0019] Fig. 6A Shows how Figure 5G A schematic view of the polycrystalline structure in the dashed rectangle F shown;

[0020] Figure 6B Shows how Figure 5G Schematic view of the polycrystalline structure in the dashed rectangle G shown. DETAILED DESCRIPTION

[0021] The embodiments of the present disclosure will be discussed in detail below. However, it should be understood that the present disclosure provides many applicable concepts that can be embodied under various specific environments. It should be understood that the following disclosure provides many different embodiments or examples for implementing the different features of the provided theme. The specific examples of components and arrangements are described below. Of course, these are only examples and are not intended to be restrictive.

[0022] The following embodiments or examples shown in the accompanying drawings are described using specific language. However, it should be understood that the specific embodiments discussed are merely illustrative and do not limit the scope of the present disclosure. In addition, it should be understood by those of ordinary skill in the art that any changes and / or modifications to the disclosed embodiments and any further applications of the principles disclosed herein are within the scope of the present disclosure.

[0023] In addition, the present disclosure may repeat reference numerals and / or letters in various examples. This repetition is for the purpose of simplicity and clarity and does not in itself indicate the relationship between the various embodiments and / or configurations discussed.

[0024] Gallium nitride (GaN) is expected to become a key material for the next generation of power semiconductor devices. GaN has the following properties: higher breakdown strength, faster switching speed, higher thermal conductivity and lower on-resistance (R on). Power devices containing this bandgap semiconductor material can significantly outperform traditional silicon-based power chips (e.g., MOSFETs). As such, GaN-based power devices will play a key role in the power conversion product market, which includes battery chargers, smartphones, computers, servers, automotive electronics, lighting systems, and photovoltaic power generation.

[0025] To achieve high-performance GaN HEMTs, it is best to reduce the resistance (called R) when the HEMT is turned on. on ). The intrinsic R on Including channel resistance (R ch , 2DEG under the gate), access region (R ac , 2DEG between gate to source and gate to drain) and source / drain contacts (R c , between the ohmic metal and the source / drain). In order to reduce the resistance between the source / drain (R ch +R ac ), increasing the Al% of the barrier layer AlGaN to the GaN 2DEG channel is an effective method; however, it will also increase R c , while higher Al% AlGaN has a higher bandgap, which will hinder the transmission of carriers. Therefore, it is necessary to c Low R on .

[0026] Figure 1A A cross-sectional view of a semiconductor device according to some embodiments of the present disclosure is shown. HEMT 100 may include a substrate 10, a seed layer 12, a buffer layer 14, an electron blocking layer (EBL) 16, a channel layer 18, a barrier layer 20, passivation layers 22 and 24, a semiconductor gate 26, and a gate conductor 28 disposed on the semiconductor gate 26. The semiconductor gate 26 and the gate conductor 28 may form a gate of the HEMT 100. The HEMT 100 further includes electrodes 30 and 32 in contact with the barrier layer 20. The HEMT 100 further includes an electrode 34 in contact with the gate conductor 28. The electrodes 30 and 32 may form source / drain electrodes of the HEMT 100.

[0027] The substrate 10 may include, for example, but not limited to, silicon (Si), doped Si, silicon carbide (SiC), silicon germanium (SiGe), gallium arsenide (GaAs), or other semiconductor materials. The substrate 10 may include, for example, but not limited to, sapphire, silicon on insulator (SOI), or other suitable materials. In some embodiments, the substrate 10 may include a silicon material. In some embodiments, the substrate 10 may be a silicon substrate.

[0028] The seed layer 12 is disposed on the substrate 10. The seed layer 12 helps to compensate for the mismatch of the lattice structure between the substrate 10 and the electron blocking layer 16. In some embodiments, the seed layer 12 includes a plurality of layers. In some embodiments, the seed layer 12 includes the same material formed at different temperatures. In some embodiments, the seed layer 12 includes a stepwise change in the lattice structure. In some embodiments, the seed layer 12 includes a continuous change in the lattice structure. In some embodiments, the seed layer 12 is formed by epitaxially growing the seed layer on the substrate 10.

[0029] The seed layer 12 may be doped with carbon. In some embodiments, the concentration of the carbon dopant is about 2×10 17 atoms / cm 3 To about 1×10 20 atoms / cm 3 In some embodiments, the seed layer 12 may be doped using an ion implantation process. In some embodiments, the seed layer 12 may be doped using an in-situ doping process. In some embodiments, the seed layer 12 may be formed using molecular oriented chemical vapor deposition (MOCVD), molecular beam epitaxy (MBE), hydride vapor phase epitaxy (HVPE), atomic layer deposition (ALD), physical vapor deposition (PVD), or another suitable formation process. In some embodiments, the in-situ doping process includes introducing a carbon dopant during the formation of the seed layer 12. In some embodiments, the source of the carbon dopant includes a hydrocarbon (C x H y )(such as CH4, C7H7, C 16 H 10 ) or another suitable hydrocarbon. In some embodiments, the source of the carbon dopant comprises CBr4, CCl4, or another suitable carbon source.

[0030] like Figure 1A As shown, HEMT 100 includes a buffer layer 14 formed on seed layer 12. Buffer layer 14 may include GaN, AlGaN, or aluminum nitride (AlN), and provides an interface from a non-GaN substrate to a GaN-based active structure. Buffer layer 14 reduces defect concentration in the active device layers.

[0031] The electron blocking layer 16 may be disposed on the buffer layer 14. In some embodiments, the electron blocking layer 16 may include a III-V group layer. The electron blocking layer 16 may include, for example but not limited to, a group III nitride, for example, a compound Al y Ga (1-y) N, where y≦1. The band gap of the electron blocking layer 16 may be greater than the band gap of the channel layer 18 .

[0032] The channel layer 18 may be disposed on the electron blocking layer 16. In some embodiments, the channel layer 18 may include a III-V group layer. The channel layer 18 may include, for example but not limited to, a group III nitride, for example, a compound Al y Ga (1-y) N, where y≤1. In some embodiments, the channel layer 18 may include GaN. Since the channel layer 18 contains nitride, the channel layer 18 may also be referred to as a nitride semiconductor layer.

[0033] The barrier layer 20 may be disposed on the channel layer 18. In some embodiments, the barrier layer 20 may include a III-V layer. The barrier layer 20 may include, for example but not limited to, a III-V nitride, for example, a compound Al y Ga (1-y) N, where y≤1. The band gap of the barrier layer 20 may be greater than the band gap of the channel layer 18. In some embodiments, the material of the barrier layer 20 may include AlGaN. In some embodiments, the material of the barrier layer 20 may include undoped AlGaN. Since the barrier layer 20 contains nitride, the barrier layer 20 may also be referred to as a nitride semiconductor layer.

[0034] A heterojunction may be formed between the barrier layer 20 and the channel 18. The polarization of the heterojunction of different nitrides forms a two-dimensional electron gas (2DEG) region in the channel layer 18. The 2DEG region is usually formed in a layer with a lower bandgap (eg, GaN).

[0035] refer to Figure 1A The barrier layer 20 includes regions (region / area) 20a1, 20a2, and 20b. The region 20a1 may be disposed between the electrode 30 and the channel layer 18. The region 20a2 may be disposed between the electrode 32 and the channel layer 18. The region 20a1 may contact the electrode 30. The region 20a2 may contact the electrode 32.

[0036] The region 20a1 includes a width 20w1 near the interface between the region 20a1 and the electrode 30. The electrode 30 includes a width 30w near the interface between the region 20a1 and the electrode 30.

[0037] In some embodiments, width 20w1 may be substantially the same as width 30w. In some embodiments, width 20w1 may be greater than width 30w. In some embodiments, width 20w1 may be less than width 30w. Region 20a2 may include a structure / size similar to that of region 20a1. Electrode 32 may include a structure / size similar to that of electrode 30.

[0038] In some embodiments, the concentration of the element in region 20a1 is different from the concentration of the element in region 20b. In some embodiments, the concentration of the element in region 20a1 is less than the concentration of the element in region 20b. In some embodiments, the concentration of the conductor element in region 20a1 is different from the concentration of the conductive element in region 20b. In some embodiments, the concentration of the conductor element in region 20a1 is less than the concentration of the conductive element in region 20b. In some embodiments, the concentration of the conductive element in region 20a1 is different from the concentration of the conductive element in region 20b. In some embodiments, the concentration of the conductive element in region 20a1 is less than the concentration of the conductive element in region 20b. In some embodiments, the concentration of the group III element in region 20a1 is different from the concentration of the group III element in region 20b. In some embodiments, the concentration of the group III element in region 20a1 is less than the concentration of the group III element in region 20b.

[0039] In some embodiments, the concentration of aluminum (Al) in region 20a1 is different from the concentration of Al in region 20b. In some embodiments, the concentration of Al in region 20a1 is less than the concentration of Al in region 20b. In some embodiments, region 20a1 contains less aluminum than region 20b. In some embodiments, the amount of Al in region 20a1 is less than the amount of Al in region 20b.

[0040] In some embodiments, the concentration of Al in the region 20a1 may be less than 30%. In some embodiments, the concentration of Al in the region 20a1 may be less than 20%. In some embodiments, the concentration of Al in the region 20a1 may be less than 10%.

[0041] In some embodiments, the concentration of Al in region 20a1 may be 40% lower than the concentration of Al in region 20b. In some embodiments, the concentration of Al in region 20a1 may be 50% lower than the concentration of Al in region 20b. In some embodiments, the concentration of Al in region 20a1 may be 60% lower than the concentration of Al in region 20b. In some embodiments, the concentration of Al in region 20a1 may be 70% lower than the concentration of Al in region 20b. In some embodiments, the concentration of Al in region 20a1 may be 80% lower than the concentration of Al in region 20b.

[0042] The concentration of Al in region 20b may be non-uniform across top surface 20s1 to bottom surface 20s2. In some embodiments, the concentration of Al in region 20b may be distributed in a gradient from top surface 20s1 to bottom surface 20s2. In some embodiments, the concentration of Al in region 20b near top surface 20s1 may be higher than the concentration of Al near bottom surface 20s2. Figure 1B To demonstrate the transmission electron microscopy (TEM) Figure 1A The line scan result obtained by the arrow x1 is shown.

[0043] The concentration of Al in the region 20a1 may be non-uniform across the top surface 20s1 to the bottom surface 20s2 of the region 20a1. In some embodiments, the concentration of Al in the region 20a1 may be distributed in a gradient from the top surface 20s1 to the bottom surface 20s2. In some embodiments, the concentration of Al near the bottom surface 20s2 may be higher than the concentration of Al near the top surface 20s1. Figure 1C To demonstrate the transmission electron microscopy (TEM) Figure 1A The line scan result obtained by the arrow x2 is shown.

[0044] The region 20a2 may include a concentration of Al similar to that of the region 20a1. The region 20a2 may include a distribution of Al similar to that of the region 20a1.

[0045] The regions 20a1 and 20a2 containing a lower Al concentration can reduce the on-resistance (R on ). The regions 20a1 and 20a2 containing a lower Al concentration may be beneficial to the performance of the HEMT 100.

[0046] Inherent R of HEMT 100 on The resistance R of the channel ch (i.e., 2DEG under the semiconductor gate 26), the resistance R ac (i.e., the 2DEG between the semiconductor gate 26 and the source / drain regions contacted by the ohmic contacts 30 and 32, respectively) and the resistance R of the source / drain contacts c (ie, between the ohmic contacts 30 / 32 and the barrier layer 20). The regions 20a1 and 20a2 containing a lower Al concentration can reduce the resistance R c , and thus reduce the R on A typical HEMT may contain about 10 -5 Ω-cm 2 The resistance R c The HEMT 100 including the regions 20a1 and 20a2 may include about 10 -8 Ω-cm 2 The resistance R c , the resistance is 1000 times lower than that of a typical HEMT.

[0047] Passivation layer 22 may include, for example but not limited to, oxides and / or nitrides, such as silicon nitride (SiN) and / or silicon oxide (SiO2). In some embodiments, passivation layer 22 may include silicon nitride and / or silicon oxide formed by a non-plasma film formation process. Passivation layer 24 may include a material similar to that of passivation layer 22. In some embodiments, passivation layer 24 may include the same material as that of passivation layer 22. In some embodiments, passivation layer 24 may include a material different from that of passivation layer 22.

[0048] Electrode 30 may be in contact with barrier layer 20. Electrode 32 may be in contact with barrier layer 20. Ohmic contact may be formed between electrode 30 and barrier layer 20. Ohmic contact may be formed between electrode 32 and barrier layer 20. Electrodes 30 and 32 each include a portion embedded in passivation layer 22. Electrodes 30 and 32 each include a portion embedded in passivation layer 24. In some embodiments, electrodes 30 and 32 may include, for example, but not limited to, titanium (Ti), aluminum (Al), nickel (Ni), gold (Au), palladium (Pd), or any combination or alloy thereof.

[0049] The semiconductor gate 26 may be disposed on the barrier layer 20. The semiconductor gate 26 may be in contact with the barrier layer 20. In some embodiments, the semiconductor gate 26 may include a III-V group layer. The semiconductor gate 26 may include, for example but not limited to, a III-V group nitride, for example, a compound Al y Ga (1-y) N, where y≤1. In some embodiments, the material of the semiconductor gate 26 may include a p-type doped III-V family layer. In some embodiments, the material of the semiconductor gate 26 may include a p-type doped GaN.

[0050] The gate conductor 28 may be in contact with the semiconductor gate 26. The gate conductor 28 may be in contact with the electrode 34. The gate conductor 28 may be covered by the passivation layer 22. The gate conductor 28 may be surrounded by the passivation layer 22. In some embodiments, the gate conductor 28 may include, for example but not limited to, titanium (Ti), tantalum (Ta), tungsten (W), aluminum (Al), cobalt (Co), copper (Cu), nickel (Ni), platinum (Pt), lead (Pb), molybdenum (Mo) and compounds thereof (such as but not limited to titanium nitride (TiN), tantalum nitride (TaN), other conductive nitrides or conductive oxides), metal alloys (such as aluminum-copper alloy (Al-Cu)) or other suitable materials.

[0051] Electrode 34 may be in contact with gate conductor 28. Electrode 34 may include a portion embedded within passivation layer 22. Electrode 34 may include a portion surrounded by passivation layer 22. In some embodiments, electrode 34 may include a material similar to that of electrodes 30 and 32.

[0052] Figure 1B The results of transmission electron microscopy (TEM) were shown along the Figure 1A Schematic view of the line scan result obtained by arrow x1 shown. Figure 1B The shown image can be obtained by an energy dispersive X-ray analyzer (EDX) of TEM.

[0053] refer to Figure 1B The concentration (ie, atomic fraction) of Al in the region 20b may be distributed in a gradient from the top surface 20s1 to the bottom surface 20s2. The concentration of Al in the region 20b gradually decreases from the top surface 20s1 to the bottom surface 20s2.

[0054] Figure 1C The TEM shows Figure 1A Schematic view of the line scan result obtained by arrow x2 shown. Figure 1C The image shown can be obtained by EDX of TEM.

[0055] refer to Figure 1C The concentration (ie, atomic fraction) of Al in the region 20a1 may be distributed in a gradient from the top surface 20s1 to the bottom surface 20s2. The concentration of Al in the region 20b gradually increases from the top surface 20s1 to the bottom surface 20s2.

[0056] Figure 2 Shows how Figure 1A A cross-sectional view of a temporary structure of a semiconductor device is shown. Figure 2 A semiconductor structure 80 is shown. The semiconductor structure 80 may be Figure 1A A portion of a HEMT 100 is shown.

[0057] The structure of the semiconductor structure 80 is Figure 1A The structure of the HEMT 100 shown is similar, except that the semiconductor structure 80 does not include the passivation layer 24 and the electrodes 30, 32, and 34. The semiconductor structure 80 may be obtained after forming the regions 20a1 and 20a2 in the barrier layer 20 and before forming the electrodes 30 and 32.

[0058] Will be based on Figure 2 and Figures 3A-3E Details regarding the structural characteristics of regions 20a1, 20b, and 20a2 are discussed. Figure 2 , an interface 18i1 exists between the channel layer 18 and the barrier layer 20, and an interface 20i1 exists between the region 20a1 and the region 20b.

[0059] exist Figure 3A An enlarged top view of the dashed rectangle A is shown in FIG. Figure 3B A schematic view of a dashed rectangle B is shown in FIG. Figure 3CAn enlarged cross-sectional view along the dashed line C is shown in FIG. Figure 3D An enlarged view of the dotted circle D is shown in FIG. Figure 3E A schematic view of the dashed rectangle E is shown in FIG. Figures 3A-3E Details regarding the structural characteristics surrounding interface 18i1 will be discussed. Figures 3A-3E Details regarding the structural characteristics around the interface 20i1 are discussed.

[0060] Figure 3A An enlarged top view of a portion of a semiconductor structure according to some embodiments of the present disclosure is shown. Figure 3A Shown is included in Figure 2 A top view of a portion of the semiconductor structure 80 within the dashed rectangle A is shown. Figure 3A , the top surface 20s1 of the region 20a1 may be relatively rough, and the top surface 20s3 of the region 20b may be relatively smooth. An interface 20i1 exists between the region 20a1 and the region 20b.

[0061] The region 20a1 may include a nanostructure. The nanostructure of the region 20a1 may be formed during the manufacture of the semiconductor structure 80, for example, by a wet etching process. The region 20a1 may include a nanostructure near the top surface 20s1. The region 20a1 may include a nanostructure near the bottom surface 20s2 (see Figure 1A ). In some embodiments, region 20a1 may include nanostructures across top surface 20s1 and bottom surface 20s2.

[0062] In some embodiments, the region 20a1 may include a diamond-shaped structure. In some embodiments, the region 20a1 may include a diamond-shaped structure near the top surface 20s1. In some embodiments, the region 20a1 may include a rectangular structure. In some embodiments, the region 20a1 may include a rectangular structure near the top surface 20s1.

[0063] In some embodiments, the region 20a1 may include a pyramidal structure. In some embodiments, the region 20a1 may include a pyramidal structure near the top surface 20s1. In some embodiments, the region 20a1 may include a hexagonal pyramid. In some embodiments, the region 20a1 may include a hexagonal pyramid near the top surface 20s1.

[0064] Figure 3B Shows how Figure 2 Schematic view of the lattice arrangement in the dashed rectangle B shown. Figure 3B A schematic view of the lattice arrangement of a portion of the semiconductor structure 80 near the interface 20i1 is shown.

[0065] Figure 3BA plurality of crystals 20 c are shown in a regular arrangement. To simplify the illustration, the crystals 20 c are depicted as circular. However, it is contemplated that the crystals 20 c of the barrier layer 20 may have different crystal shapes depending on the material configuration of the barrier layer 20 .

[0066] The region 20a1 may include a single crystal. The region 20b may include a single crystal. The barrier layer 20 may include a single crystal near the interface 20i1. The region 20a1 may lack a polycrystalline structure. The region 20a1 may lack a polycrystalline structure near the interface 20i1. The region 20b may lack a polycrystalline structure near the interface 20i1. Similarly, the region 20a2 may include a single crystal. The region 20a2 may lack a polycrystalline structure near the interface between the region 20a2 and the region 20b.

[0067] Figure 3C A cross-sectional view of a portion of a semiconductor structure according to some embodiments of the present disclosure is shown. Figure 3C Shown along Figure 2 A cross-sectional view of a portion of semiconductor structure 80 is shown along dashed line C.

[0068] refer to Figure 3C , the region 20a2 (and the region 20a1) may include a pyramidal structure 20p. In some embodiments, the region 20a2 (and the region 20a1) may include a mountain-shaped structure. In some embodiments, the region 20a2 (and the region 20a1) may include a triangular structure. The pyramidal structure 20p may be formed during the manufacture of the semiconductor structure 80, for example, by a wet etching process.

[0069] Figure 3D An enlarged view of a portion of a semiconductor structure according to some embodiments of the present disclosure is shown. Figure 3D Shown is included in Figure 2 An enlarged view of a portion of semiconductor structure 80 within dashed circle D is shown.

[0070] refer to Figure 3D , region 20a2 (as well as region 20a1) may contain voids or holes 20h. Voids or holes 20h may be formed during the manufacture of semiconductor structure 80, for example, by a wet etching process. In some embodiments, the sizes of the voids or holes contained in regions 20a1 and 20a2 may be uniform. In some embodiments, the voids or holes contained in regions 20a1 and 20a2 may have different sizes.

[0071] In some embodiments, the shape of the voids or holes 20h can be regular. In some embodiments, the shape of the voids or holes 20h can be irregular.

[0072] The shape of the void or hole 20h may be a triangle. The shape of the void or hole 20h may be a quadrilateral. The shape of the void or hole 20h may be a pentagon. The shape of the void or hole 20h may be a hexagon. The shape of the void or hole 20h may be a heptagon. The shape of the void or hole 20h may be an octagon. The shape of the void or hole 20h may be a nonagon. The shape of the void or hole 20h may be a decagon. The shape of the void or hole 20h may be a polygon.

[0073] Figure 3E Shows how Figure 2 Schematic view of the lattice arrangement in the dashed rectangle E shown. Figure 3E A schematic view of a portion of a semiconductor structure 80 near the interface 18i1 is shown.

[0074] Figure 3E A plurality of crystals 20 c are shown in a regular arrangement. To simplify the illustration, the crystals 20 c are depicted as circular. However, it is contemplated that the crystals 20 c of the barrier layer 20 may have different crystal shapes depending on the material configuration of the channel layer 18 and the barrier layer 20 .

[0075] refer to Figure 3E , the channel layer 18 may include a single crystal. The barrier layer 20 may include a single crystal. The region 20a1 may include a single crystal. The channel layer 18 may include a single crystal near the interface 18i1. The barrier layer 20 may include a single crystal near the interface 18i1.

[0076] The single crystal in the barrier layer 20 may take over the crystal structure of the channel layer 18. The single crystal in the region 20a1 may take over the crystal structure of the channel layer 18. The term "take over" as used in the present disclosure may refer to the crystal structure of one layer following the crystal structure of another layer. The term "take over" as used in the present disclosure may refer to the crystal structure of one layer being the same as the crystal structure of another layer.

[0077] The barrier layer 20 may lack a polycrystalline structure. The barrier layer 20 may lack a polycrystalline structure near the interface 18i1. The region 20a1 may lack a polycrystalline structure. The region 20a1 may lack a polycrystalline structure near the interface 18i1.

[0078] The channel layer 18 may lack a polycrystalline structure. The channel layer 18 may lack a polycrystalline structure near the interface 18i1. Similarly, the region 20b may lack a polycrystalline structure near the interface between the channel layer 18 and the barrier layer 20. The region 20a2 may lack a polycrystalline structure near the interface between the channel layer 18 and the barrier layer 20.

[0079] Figure 4A , 4B4C, 4D, 4E, 4F, 4G, 4H and 4I show operations for manufacturing a semiconductor device according to some embodiments of the present disclosure. Figure 4A , 4B , 4C, 4D, 4E, 4F, 4G, 4H and 4I to produce Figure 1A HEMT 100 shown.

[0080] refer to Figure 4A , providing a substrate 10. In some embodiments, the substrate 10 may include a silicon material or sapphire. Next, a seed layer 12 is formed on the substrate 10, a buffer layer 14 is formed on the seed layer 12, and an electron blocking layer 16 is formed on the buffer layer 14. A channel layer 18 is formed on the electron blocking layer 16, and then a barrier layer 20 is formed on the channel layer 18. Next, a semiconductor gate material layer 26' is formed on the barrier layer 20.

[0081] The substrate 10 may include Figure 1A The seed layer 12 may include materials according to the HEMT 100 discussed above. Figure 1A The buffer layer 14 may include materials according to Figure 1A The electron blocking layer 16 may include materials according to Figure 1A The materials of HEMT 100 are discussed.

[0082] In some embodiments, the material of the channel layer 18 may include GaN, the material of the barrier layer 20 may include AlGaN, and the material of the semiconductor gate material layer 26' may include GaN. In some embodiments, the channel layer 18, the barrier layer 20 and / or the semiconductor gate material layer 26' may be formed by chemical vapor deposition (CVD), physical vapor deposition (PVD), epitaxial growth or other suitable deposition processes.

[0083] refer to Figure 4B , a gate conductor material layer 28' is formed on the semiconductor gate material layer 26', and a hard mask layer 40 is formed on the gate conductor material layer 28'. In some embodiments, one or more layers of materials may be deposited by PVD, CVD and / or other suitable processes to form the gate conductor material layer 28'. In some embodiments, the gate conductor material layer 28' may be formed by sputtering or evaporating a metal material on the semiconductor gate material layer 26'.

[0084] refer to Figure 4C, a patterning process may be performed on the hard mask layer 40 and the gate conductor material layer 28' to form the gate conductor 28. A patterned hard mask 40' may be first formed over the gate conductor material layer 28', and then the portion of the gate conductor material layer 28' not covered by the patterned hard mask 40' may be removed. In some embodiments, the gate conductor material layer 28' may be patterned by dry etching. In some embodiments, the gate conductor material layer 28' may be patterned by wet etching. The etching process performed on the gate conductor material layer 28' may stop on the top surface of the semiconductor gate material layer 26'. The etching process performed on the gate conductor material layer 28' may continue until the top surface of the semiconductor gate material layer 26' is exposed.

[0085] refer to Figure 4D Spacers 42a and 42b are formed adjacent to the patterned hard mask 40' and the gate conductor 28. Next, portions of the semiconductor gate material layer 26' not covered by the spacers 42a and 42b and the gate conductor 28 are removed to form a semiconductor gate 26.

[0086] In some embodiments, the semiconductor gate material layer 26' can be patterned by dry etching. In some embodiments, the semiconductor gate material layer 26' can be patterned by wet etching. The etching process performed on the semiconductor gate material layer 26' can stop on the top surface of the barrier layer 20. The etching process performed on the semiconductor gate material layer 26' can continue until the top surface of the barrier layer 20 is exposed.

[0087] refer to Figure 4E , spacers 42a and 42b are removed, and patterned hard mask 40' is also removed. Next, passivation layer 22 is disposed to cover barrier layer 20, semiconductor gate 26, and gate conductor 28. In some embodiments, passivation layer 22 may be conformally formed over barrier layer 20, semiconductor gate 26, and gate conductor 28. In some embodiments, passivation layer 22 may include, for example but not limited to, oxide and / or nitride, such as silicon nitride (SiN) and / or silicon oxide (SiO2). In some embodiments, passivation layer 22 may include silicon nitride and / or silicon oxide formed by a non-plasma film formation process.

[0088] refer to Figure 4F , openings 22h1 and 22h2 may be formed on the passivation layer 22. The opening 22h1 exposes a portion of the barrier layer 20. The opening 22h1 exposes the upper surface of the region 20a1 of the barrier layer 20. The opening 22h2 exposes a portion of the barrier layer 20. The opening 22h2 exposes the upper surface of the region 20a2 of the barrier layer 20.

[0089] The barrier layer 20 may include a compound Al y Ga(1-y) N, where y≤1.

[0090] An etching technique, such as but not limited to a wet immersion technique, may be applied to the regions 20a1 and 20a2. The etchant applied to the regions 20a1 and 20a2 may include a hydroxide, which has a greater etching rate on aluminum nitride (AlN) than gallium nitride (GaN). After the etching operation, relatively more aluminum is removed relative to other elements (e.g., gallium and nitrogen). In other words, after the etching operation, the concentration of aluminum (Al) in the regions 20a1 and 20a2 is reduced.

[0091] The etchant that can be used in the operation discussed can include, for example, but not limited to, hydroxide, sodium hydroxide (NaOH), potassium hydroxide (KOH), AZ400K photoresist developer, or one or more other suitable solutions. The etchant that can be used in the operation discussed can include a relatively high selectivity between aluminum and other elements (such as gallium or nitrogen).

[0092] According to experimental results, the AlN etching rate of sodium hydroxide (NaOH) at a temperature of 75°C is 50 nanometers per minute, while it hardly etches gallium nitride (GaN). According to experimental results, the AlN etching rate of potassium hydroxide (KOH) is 2265 nanometers per minute, while it hardly etches gallium nitride (GaN). According to experimental results, the AlN etching rate of AZ400K photoresist developer is about 6 to 1000 nanometers per minute, while it hardly etches gallium nitride (GaN).

[0093] After the etching operation, the region 20 a 1 and the region 20 a 2 may have a lower Al concentration than other portions of the barrier layer 20 .

[0094] refer to Figure 1A , can be compared with reference Figure 4F The one or more operations described and illustrated may be performed in a similar manner to etching the regions 20a1 and 20a2 of the HEMT 100. Therefore, the regions 20a1 and 20a2 of the HEMT 100 may have a relatively low Al concentration, which may reduce the on-resistance (R on ) to improve its performance.

[0095] refer to Figure 4F, after the aluminum is removed, the crystal structure within the region 20a1 and the region 20a2 remains the same. In other words, the removal of the aluminum does not change the crystal structure of the barrier layer 20 within the region 20a1 and the region 20a2. For example, the crystal direction of the region 20a1 can still be the same as the crystal direction of the channel layer 18. For example, the crystal direction of the region 20a1 can still be the same as the crystal direction of the barrier layer 20. For example, the crystal direction of the region 20a2 can still be the same as the crystal direction of the channel layer 18. For example, the crystal direction of the region 20a2 can still be the same as the crystal direction of the barrier layer 20. The same crystal direction across the regions 20a1, 20a2, the barrier layer 20, and the channel layer 18 can be beneficial to the yield of the HEMT to be produced. The same crystal direction across the regions 20a1, 20a2, the barrier layer 20, and the channel layer 18 can be beneficial to the reliability of the HEMT to be produced.

[0096] In some embodiments, the region 20a1 and the region 20a2 may be treated by a dry ashing technique to reduce the Al concentration in the region 20a1 and the region 20a2. For example, O2, N2, H2, or one or more other suitable elements, gases, or plasmas may be used alone or in combination to reduce the Al concentration in the region 20a1 and the region 20a2. For example, the region 20a1 and the region 20a2 may be treated by dry ashing with a plasma of one of O2, N2, or H2. For example, the region 20a1 and the region 20a2 may be treated by dry ashing using a plasma of any combination of O2, N2, and H2.

[0097] In some other embodiments, residues may exist in regions 20a1 and 20a2 after the dry ashing operation ( Figure 4F In some other embodiments, residues may exist within the barrier layer 20 after the dry ashing operation ( Figure 4F In some other embodiments, residues may exist in the passivation layer 22 and the channel layer 18 after the dry ashing operation ( Figure 4F not shown).

[0098] The region 20a1 and the region 20a2 may be treated with a dry ashing technique and a wet soaking technique. For example, the region 20a1 and the region 20a2 may be treated with a wet soaking technique first, and then a dry ashing technique may be employed, or vice versa.

[0099] refer to Figure 4G , conductors 30a and 32a may be formed. Conductor 30a may be formed in opening 22h1 and in contact with region 20a1. Conductor 32a may be formed in opening 22h2 and in contact with region 20a2. A portion of conductor 30a may be surrounded by passivation layer 22. A portion of conductor 32a may be surrounded by passivation layer 22.

[0100] In some embodiments, conductors 30a and 32a may be formed using techniques such as, but not limited to, welding, soldering, crimping, deposition, or electroplating. In some embodiments, conductors 30a and 32a may include, for example, but not limited to, titanium (Ti), aluminum (Al), nickel (Ni), gold (Au), palladium (Pd), or any combination or alloy thereof.

[0101] refer to Figure 4H , forming a passivation layer 24. The passivation layer 24 is disposed above the conductors 30a and 32a and the passivation layer 22 and covers the conductors and the passivation layer. The passivation layer 24 may include, for example but not limited to, oxides and / or nitrides, such as silicon nitride (SiN) and / or silicon oxide (SiO2). In some embodiments, the passivation layer 24 may include silicon nitride and / or silicon oxide formed by a non-plasma film formation process. The passivation layer 24 may include a material similar to that of the passivation layer 22. In some embodiments, the passivation layer 24 may include a material that is the same as that of the passivation layer 22. In some embodiments, the passivation layer 24 may include a material different from that of the passivation layer 22.

[0102] refer to Fig. 4I , conductors 30b and 32b and electrode 34 may be formed. Conductor 30b is formed above and in contact with conductor 30a. Conductors 30a and 30b form electrode 30. Conductor 32b is formed above and in contact with conductor 32a. Conductors 32a and 32b form electrode 32. Electrodes 30, 32, and 34 are exposed by passivation layer 24. Electrodes 30, 32, and 34 are not covered by passivation layer 24.

[0103] In execution according to Figure 4A , 4B After the operations described in 4C, 4D, 4E, 4F, 4G, 4H and 4I, HEMT 100 can be obtained.

[0104] Figure 5A , 5B 5C, 5D, 5E, 5F, 5G, 5H, 5I and 5J illustrate operations for manufacturing a semiconductor device according to some other embodiments of the present disclosure. Figure 5A , 5B , 5C, 5D, 5E, 5F, 5G, 5H, 5I and 5J to produce Figure 5J HEMT 100' shown.

[0105] refer to Figure 5A, providing a substrate 10. In some embodiments, the substrate 10 may include a silicon material or sapphire. Next, a seed layer 12 is formed on the substrate 10, a buffer layer 14 is formed on the seed layer 12, and an electron blocking layer 16 is formed on the buffer layer 14. A channel layer 18 is formed on the electron blocking layer 16, and then a barrier layer 20 is formed on the channel layer 18. Next, a semiconductor gate material layer 26' is formed on the barrier layer 20.

[0106] In some embodiments, the material of the channel layer 18 may include GaN, the material of the barrier layer 20 may include AlGaN, and the material of the semiconductor gate material layer 26' may include GaN. In some embodiments, the channel layer 18, the barrier layer 20 and / or the semiconductor gate material layer 26' may be formed by chemical vapor deposition (CVD), physical vapor deposition (PVD), epitaxial growth or other suitable deposition processes.

[0107] refer to Figure 5B , a gate conductor material layer 28' is formed on the semiconductor gate material layer 26', and a hard mask layer 40 is formed on the gate conductor material layer 28'. In some embodiments, one or more layers of materials may be deposited by PVD, CVD and / or other suitable processes to form the gate conductor material layer 28'. In some embodiments, the gate conductor material layer 28' may be formed by sputtering or evaporating a metal material on the semiconductor gate material layer 26'.

[0108] refer to Figure 5C , a patterning process may be performed on the hard mask layer 40 and the gate conductor material layer 28 ′ to form the gate conductor 28 . Figure 5C The operations shown are similar to Figure 4C The operations shown are similar and therefore the details will not be repeated here.

[0109] refer to Figure 5D , spacers 42a and 42b are formed adjacent to patterned hard mask 40' and gate conductor 28. Next, semiconductor gate 26 is formed. Figure 5D The operations shown are similar to Figure 4D The operations shown are similar and therefore the details will not be repeated here.

[0110] refer to Figure 5E , spacers 42a and 42b are removed, and patterned hard mask 40' is also removed. Next, passivation layer 22 is disposed to cover barrier layer 20, semiconductor gate 26, and gate conductor 28. Figure 5E The operations shown are similar to Figure 4E The operations shown are similar and therefore the details will not be repeated here.

[0111] refer to Fig. 5F, forming openings 20h1 and 20h2. The opening 20h1 may penetrate the passivation layer 22 and the barrier layer 20. The opening 20h2 may penetrate the passivation layer 22 and the barrier layer 20. The opening 20h1 exposes a portion of the channel layer 18. The opening 20h1 exposes a surface of the channel layer 18. The opening 20h2 exposes a portion of the channel layer 18. The opening 20h2 exposes a surface of the channel layer 18. The openings 20h1 and 20h2 may be formed by, for example, a wet etching or dry etching technique.

[0112] refer to Figure 5G , the openings 20h1 and 20h2 may be filled with a material different from the barrier layer 20. In some embodiments, the openings 20h1 and 20h2 may be filled with a heterogeneous alloy, AlGaN with a low aluminum content, or n-type GaN. In some embodiments, the heterogeneous alloy, AlGaN with a low aluminum content, or n-type GaN may be formed by, for example, chemical vapor deposition (CVD), physical vapor deposition (PVD), epitaxial growth, or other suitable deposition processes. Figure 5G The process performed in may also be referred to as selective area growth (SAG).

[0113] The regions 20a1' and 20a2' may be formed after the openings 20h1 and 20h2 are filled. Figure 5G The regions 20a1' and 20a2' are formed by Figure 4F The regions 20a1 and 20a2 are formed by different processes, and thus the regions 20a1' and 20a2' may include microstructures different from those of the regions 20a1 and 20a2. Figure 5G Enlarged views of the dashed rectangles F and G are shown in the following paragraphs. Fig. 6A and 6B Displayed in.

[0114] In execution Figure 5G After the process shown, the crystal structure within the regions 20a1' and 20a2' will be different from the barrier layer 20. The crystal orientation of the region 20a1' will be different from the crystal orientation of the channel layer 18. The crystal orientation of the region 20a2' will be different from the crystal orientation of the channel layer 18. The crystal orientation of the region 20a2' will be different from the crystal orientation of the barrier layer 20. The different crystal orientations across the regions 20a1', 20a2', the barrier layer 20, and the channel layer 18 may adversely affect the yield of the resulting HEMT. The different crystal orientations across the regions 20a1', 20a2', the barrier layer 20, and the channel layer 18 may adversely affect the reliability of the resulting HEMT.

[0115] refer to Figure 5H, conductors 30a and 32a may be formed. Conductor 30a may be formed to contact region 20a1'. Conductor 32a may be formed to contact region 20a2'. A portion of conductor 30a may be surrounded by passivation layer 22. A portion of conductor 32a may be surrounded by passivation layer 22.

[0116] In some embodiments, conductors 30a and 32a may be formed using techniques such as, but not limited to, welding, soldering, crimping, deposition, or electroplating. In some embodiments, conductors 30a and 32a may include, for example, but not limited to, titanium (Ti), aluminum (Al), nickel (Ni), gold (Au), palladium (Pd), or any combination or alloy thereof.

[0117] refer to Fig.5I , forming a passivation layer 24. The passivation layer 24 is disposed over the conductors 30a and 32a and the passivation layer 22 and covers the conductors and the passivation layer. Fig.5I The operations shown are similar to Figure 4H The operations shown are similar and therefore the details will not be repeated here.

[0118] refer to Figure 5J , conductors 30b and 32b and electrode 34 may be formed. Conductor 30b is formed above and in contact with conductor 30a. Conductors 30a and 30b form electrode 30. Conductor 32b is formed above and in contact with conductor 32a. Conductors 32a and 32b form electrode 32. Electrodes 30, 32, and 34 are exposed by passivation layer 24. Electrodes 30, 32, and 34 are not covered by passivation layer 24.

[0119] In execution according to Figure 5A , 5B After the operations described in 5C, 5D, 5E, 5F, 5G, 5H, 5I and 5J, the HEMT 100' can be obtained.

[0120] Fig. 6A A schematic view of a portion of a semiconductor device according to some embodiments of the present disclosure is shown. Fig. 6A Shows Figure 5G An enlarged view of the dashed rectangle F.

[0121] Fig. 6A Crystals near the interface between the region 20a1', the channel layer 18, and the barrier layer 20 of the HEMT 100' are shown. The barrier layer 20 includes a plurality of crystals 20c1. The channel layer 18 includes a plurality of crystals 18c1. The region 20a1' includes a plurality of crystals 20c2. In some embodiments, the crystals 20c1 of the barrier layer 20 form separate crystallites. In some embodiments, the crystals 20c2 of the region 20a1' form separate crystallites. In some embodiments, the crystals 18c1 of the channel layer 18 form separate crystallites.

[0122] Fig. 6A The structure shown corresponds to a polycrystalline structure comprising individual crystallites consisting of crystals 20c1, 20c2, and 18c1. In some embodiments, crystal 20c2 does not succeed to the crystal structure of crystal 18c1. In some embodiments, crystal 20c2 does not succeed to the crystal structure of crystal 20c1. In some embodiments, crystal 20c1 does not succeed to the crystal structure of crystal 18c1.

[0123] Figure 6B A schematic view of a portion of a semiconductor device according to some embodiments of the present disclosure is shown. Figure 6B Shows Figure 5G Magnified view of the dashed rectangle G.

[0124] Figure 6B Crystals near the interface between the region 20a2', the channel layer 18, and the barrier layer 20 of the HEMT 100' are shown. The barrier layer 20 includes a plurality of crystals 20c1. The channel layer 18 includes a plurality of crystals 18c1. The region 20a2' includes a plurality of crystals 20c2. In some embodiments, the crystals 20c1 of the barrier layer 20 form separate crystallites. In some embodiments, the crystals 20c2 of the region 20a2' form separate crystallites. In some embodiments, the crystals 18c1 of the channel layer 18 form separate crystallites.

[0125] Figure 6B The structure shown corresponds to a polycrystalline structure comprising individual crystallites consisting of crystals 20c1, 20c2, and 18c1. In some embodiments, crystal 20c2 does not succeed to the crystal structure of crystal 18c1. In some embodiments, crystal 20c2 does not succeed to the crystal structure of crystal 20c1. In some embodiments, crystal 20c1 does not succeed to the crystal structure of crystal 18c1.

[0126] As used herein, spatially relative terms such as "under", "below", "lower", "above", "upper", "lower", "left side", "right side" and the like may be used herein for ease of description to describe the relationship of one element or feature to another or more elements or features as shown in the accompanying drawings. In addition to the orientation depicted in the accompanying drawings, spatially relative terms are also intended to cover different orientations of the device when in use or when running. The device may be oriented in other ways (rotated 90 degrees or in other orientations), and the spatially relative descriptors used herein may also be interpreted in a corresponding manner. It should be understood that when an element is referred to as being "connected to" or "coupled to" another element, it may be directly connected to or coupled to the other element, or there may be intermediate elements.

[0127] As used herein, the terms "approximately", "substantially", "substantially" and "about" are used to describe and explain small changes. When used in conjunction with an event or situation, the term can refer to an instance where the situation event occurs precisely and an instance where the event or situation is close to occurring. As used herein with respect to a given value or range, the term "approximately" generally means within ±10%, ±5%, ±1% or ±0.5% of a given value or range. The range can be expressed as one endpoint to another endpoint or between two endpoints herein. All ranges disclosed herein include endpoints unless otherwise specified. The term "substantially coplanar" can refer to a position difference of two surfaces positioned along the same plane within a few microns (μm), such as a position difference positioned along the same plane within 10 μm, within 5 μm, within 1 μm or within 0.5 μm. When a numerical value or characteristic is referred to as being "substantially" the same, the term can refer to a value within ±10%, ±5%, ±1% or ±0.5% of the average value of the value.

[0128] The foregoing summarizes the features of several embodiments and detailed aspects of the present disclosure. The embodiments described in the present disclosure can be easily used as a basis for designing or modifying other processes and structures to facilitate the implementation of the same or similar purposes and / or to achieve the same or similar advantages of the embodiments introduced herein. Such equivalent constructions do not depart from the spirit and scope of the present disclosure, and various changes, substitutions and modifications may be made without departing from the spirit and scope of the present disclosure.

Claims

1. A semiconductor device comprising: substrate; A first nitride semiconductor layer, wherein the first nitride semiconductor layer is located on the substrate; the first nitride semiconductor layer is gallium nitride GaN; a second nitride semiconductor layer, the second nitride semiconductor layer being located on the first nitride semiconductor layer and having a band gap greater than that of the first nitride semiconductor layer, the second nitride semiconductor layer having a first region and a second region, and the second nitride semiconductor layer having a single crystal structure, and the second nitride semiconductor layer being aluminum gallium nitride AlGaN; as well as An electrode, the electrode is in contact with the first region, the first region is disposed between the electrode and the first nitride semiconductor layer, and the electrode is a source electrode and a drain electrode; Wherein a first concentration of an element in the first region is lower than a second concentration of the element in the second region, and wherein the single crystal structure in the first region succeeds to a crystal structure in the first nitride semiconductor layer, the element is aluminum Al. 2 . The semiconductor device according to claim 1 , wherein the first region of the second nitride semiconductor layer lacks a polycrystalline structure. 3 . The semiconductor device according to claim 1 , wherein a first interface between the first region and the second region lacks a polycrystalline structure. 4 . The semiconductor device according to claim 1 , wherein a second interface between the first region and the first nitride semiconductor layer lacks a polycrystalline structure. The semiconductor device according to claim 1 , wherein the amount of the element in the first region is uneven. The semiconductor device according to claim 1 , wherein the first concentration of the element in the first region is gradient. 7 . The semiconductor device according to claim 1 , wherein a first amount of the element in the first region adjacent to the electrode is greater than a second amount of the element in the first region adjacent to the first nitride semiconductor layer. 8 . The semiconductor device according to claim 1 , wherein the first region of the second nitride semiconductor layer includes a relatively rough surface. 9 . The semiconductor device according to claim 1 , wherein the second region of the second nitride semiconductor layer includes a relatively smooth surface. 10 . The semiconductor device according to claim 1 , wherein the first region of the second nitride semiconductor layer includes a pyramid-shaped structure as viewed from a cross-sectional view.

11. A semiconductor device comprising: substrate; a first nitride semiconductor layer disposed above the substrate; The first nitride semiconductor layer is gallium nitride GaN; a second nitride semiconductor layer, the second nitride semiconductor layer being located on the first nitride semiconductor layer and having a first region and a second region; a band gap of the second nitride semiconductor layer being greater than a band gap of the first nitride semiconductor layer, and the second nitride semiconductor layer being aluminum gallium nitride AlGaN; as well as a first electrode, the first electrode is in contact with the first region, the first region includes a single crystal, and is disposed between the first electrode and the first nitride semiconductor layer; the first electrode is a source electrode and a drain electrode; The first region includes an element distributed with a gradient along a direction from the first electrode toward the first nitride semiconductor layer; the second region includes an element distributed with a gradient along a direction toward the first nitride semiconductor layer; a first concentration of the element in the first region is less than a second concentration of the element in the second region, and wherein a single crystal structure in the first region replaces a crystal structure in the first nitride semiconductor layer, and the element is aluminum Al. 12 . The semiconductor device according to claim 11 , wherein the element of the first region gradually increases along the direction from the first electrode toward the first nitride semiconductor layer. 13 . The semiconductor device according to claim 11 , wherein the second region includes an element that gradually decreases in a direction toward the first nitride semiconductor layer. The semiconductor device according to claim 11 , wherein the element is conductive. 15 . The semiconductor device according to claim 11 , wherein a first concentration of the element in the first region is less than 30%.

16. A method for manufacturing a semiconductor device, the method comprising: Providing a semiconductor structure having a substrate, a channel layer, and a barrier layer; The barrier layer has a single crystal structure, and the band gap of the barrier layer is greater than the band gap of the channel layer; The channel layer is gallium nitride GaN, and the barrier layer is gallium aluminum nitride AlGaN; providing a passivation layer on the barrier layer, the passivation layer exposing a first region of the barrier layer and covering a second region of the barrier layer; as well as soaking the first region of the barrier layer with a first solution, so that a first concentration of an element in the first region is less than a second concentration of the element in the second region, and the single crystal structure in the first region replaces the crystal structure in the channel layer, and the element is aluminum Al; Before providing a passivation layer on the barrier layer, forming an electrode on the barrier layer, the electrode being in contact with the first region, the first region being disposed between the electrode and the channel layer; The electrodes are a source electrode and a drain electrode.

17. The method of claim 16, wherein the first solution comprises one of: sodium hydroxide, potassium hydroxide, and AZ4000K photoresist developer. The method of claim 16 , wherein the first concentration of the element of the first region is less than 30%.