Organic film-forming composition, pattern forming method, and polymer

By using high carbon density indenofluorene structure polymers and a multi-layer resist process, the problem of difficulty in flattening organic films on high-level substrates is solved, high etching resistance and distortion resistance are achieved, and the accuracy of photolithography is improved. and efficiency.

CN112213919BActive Publication Date: 2024-09-27SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010660845.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-12
Filing Date
2020-07-10
Publication Date
2024-09-27
Estimated Expiration
2040-07-10

AI Technical Summary

Technical Problem

In the manufacturing of semiconductor components in the existing technology, the organic film used is difficult to form a flat surface on the high-level substrate, which leads to the deterioration of focus latitude and pattern shape during photolithography, and insufficient etching resistance and distortion resistance, making it difficult to meet the requirements of micro-fining after the 20nm generation. needs.

Method used

It uses an indenofluorene structure with high carbon density and a thermosetting polymer to form an organic film with high etching resistance and distortion resistance through thermal cross-linking reaction. It combines the spin coating method and the multi-layer resist process to use silicon-containing The resist lower film and the photoresist upper film achieve high-precision transfer of patterns.

Benefits of technology

It achieves the formation of a flat organic film on a high-level substrate, improves etching resistance and distortion resistance, enhances the focus latitude and pattern accuracy of photolithography, and meets the requirements for miniaturization after the 20nm generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112213919B_ABST
    Figure CN112213919B_ABST
Patent Text Reader

Abstract

The present invention relates to an organic film-forming composition, a pattern forming method, and a polymer. The problem to be solved by the present invention is to provide an organic film-forming composition that can exhibit high etching resistance and excellent twist resistance by using a polymer containing an indeno[1,2-b]fluorene structure with a high carbon content and having thermosetting properties; to provide a pattern forming method using such an organic film-forming composition; and to provide a polymer for such an organic film-forming composition. The solution to this problem is an organic film-forming composition containing: a polymer having a partial structure represented by the following general formula (1A) as a repeating unit and an organic solvent. [Chemical formula 1] #imgabs0# In the general formula (1A), AR1 and AR2 are benzene rings or naphthalene rings which may have substituents, R is a hydrogen atom or a monovalent organic group having an unsaturated bond and having 2 to 10 carbon atoms, R' is a single bond or W1, and W1 is a divalent organic group having 6 to 80 carbon atoms and having one or more aromatic rings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composition for forming an organic film, a pattern forming method using the composition, and a polymer contained in the composition. Background Art

[0002] In recent years, with the high integration and high speed of semiconductor devices, there is a demand for finer pattern rules. In photolithography using light exposure, which is currently used as a general technology, various technical developments are being carried out to implement finer and higher-precision pattern processing using the light source used.

[0003] As for the light source for photolithography used in the formation of resist patterns, light exposure using g-rays (436nm) or i-rays (365nm) of mercury lamps as light sources is widely used in parts with low integration. On the other hand, photolithography using shorter wavelengths of KrF excimer lasers (248nm) and ArF excimer lasers (193nm) has also been put into practical use in parts with high integration and miniaturization. In the most advanced generation that requires even more miniaturization, photolithography using extreme ultraviolet rays (EUV, 13.5nm) is also approaching practical use.

[0004] As described above, if the thinning of the resist pattern progresses, it is known that the ratio of the pattern height to the pattern line width (aspect ratio) will increase in the single-layer resist method used as a representative resist pattern forming method, and the pattern collapses due to the surface tension of the developer during development. Therefore, in order to form a pattern with a high aspect ratio on a high-height substrate, a multilayer resist method in which a pattern is formed by laminating films having different dry etching characteristics is known to be excellent, and the following methods have been developed: a two-layer resist method combining a photoresist layer obtained from a silicon-containing photosensitive polymer and a lower layer obtained from an organic polymer having carbon, hydrogen and oxygen as main constituent elements, such as a novolac polymer (Patent Document 1, etc.); a three-layer resist method combining a photoresist layer obtained from an organic photosensitive polymer used in the single-layer resist method, a silicon-containing resist lower film obtained from a silicon polymer or a silicon CVD film, and an organic film obtained from an organic polymer (Patent Document 2, etc.).

[0005] In the three-layer resist method, first, the pattern of the photoresist layer is transferred to the resist lower film containing silicon using a fluorocarbon-based dry etching gas, and then the pattern is used as a mask to dry-etch an organic film containing carbon and hydrogen as main constituent elements, and then the organic film is used as a mask to form a pattern on the substrate to be processed by dry etching. However, in the semiconductor device manufacturing process after the 20nm generation, if the organic film pattern is used as a hard mask and the substrate to be processed is transferred by dry etching, distortion or bending is observed in the organic film pattern.

[0006] The carbon hard mask formed directly above the substrate to be processed is generally an amorphous carbon (hereinafter referred to as CVD-C) film made by CVD method using methane gas, ethane gas, acetylene gas, etc. as raw materials. In this CVD-C film, it is known that the hydrogen atoms in the film can be reduced to a very small amount, and it is very effective for the distortion and bending of the pattern as described above. However, when there is a height difference on the substrate to be processed as the base, it is also known that it is not easy to fill such a height difference evenly in terms of the characteristics of the CVD process. Therefore, if the substrate to be processed with a height difference is filled with a CVD-C film and then patterned on the photoresist, a height difference will be generated on the coating surface of the photoresist due to the influence of the height difference of the substrate to be processed, so the film thickness of the photoresist will become uneven, and as a result, the focus tolerance and pattern shape during photolithography will deteriorate.

[0007] On the other hand, when an organic film as a carbon hard mask is formed directly above a substrate to be processed by spin coating, it is known that there is an advantage that the height difference of a substrate with height difference can be filled evenly. If the substrate is flattened by the organic film material, the thickness variation of the silicon-containing resist lower layer film and resist upper layer film formed thereon is suppressed, the focus latitude of photolithography can be expanded, and a normal pattern can be formed.

[0008] Therefore, an organic film material and a method for forming the organic film are required that can form an organic film having high etching resistance and high flatness on a substrate to be processed by spin coating when the substrate to be processed is dry-etched.

[0009] In the past, as for such organic film materials, it is known that condensation resins obtained by using carbonyl compounds such as ketones or aldehydes and aromatic alcohols as condensing agents for phenolic and naphthol compounds are used as organic film forming materials for multilayer resist methods. For example, bisphenol fluorene novolac resins described in Patent Document 2, bisphenol compounds and novolac resins thereof described in Patent Document 3, novolac resins of adamantane phenol compounds described in Patent Document 4, and bisnaphthol compounds and novolac resins thereof described in Patent Document 5 can be exemplified. Although the resins used in such materials are composed of naphthalene, fluorene, adamantane and the like with high carbon density as the main skeleton, the etching resistance and distortion resistance are still not satisfactory, and further etching improvement is required.

[0010] As for the resin for organic film materials that does not contain heteroatoms such as oxygen in order not to impair etching resistance, the resin having a fluorene structure described in Patent Document 6 can be exemplified. However, since a composition to which a crosslinking agent such as a hydroxymethyl compound is added is used to form a cured film and the cured film is formed thereby, even if the carbon content of the resin is increased, it still contains a crosslinking agent with a low carbon content, which causes a problem of impairing etching resistance.

[0011] As for the compounds or polymers of organic film materials having an indenofluorene structure as a partial structure with a higher carbon density, examples include the monomolecular compound having a naphthol structure described in Patent Document 7, or a phenolic varnish resin using the compound, etc. However, since a structure containing multiple oxygen atoms is used in the repeating unit, there is still room for improvement in etching resistance.

[0012] Prior art documents

[0013] Patent Literature

[0014] [Patent Document 1] Japanese Patent Application Laid-Open No. 6-118651, etc.

[0015] [Patent Document 2] Japanese Patent Application Publication No. 2005-128509

[0016] [Patent Document 3] Japanese Patent Application Publication No. 2006-293298

[0017] [Patent Document 4] Japanese Patent Application Publication No. 2006-285095

[0018] [Patent Document 5] Japanese Patent Application Publication No. 2010-122656

[0019] [Patent Document 6] International Publication No. 2013 / 047106 Pamphlet

[0020] [Patent Document 7] Japanese Patent Application Publication No. 2017-21337 Summary of the invention

[0021] Problem that the invention aims to solve

[0022] The present invention is made in view of the above situation, and its purpose is to provide an organic film forming composition that can exhibit high etching resistance and excellent distortion resistance by using a polymer containing an indenofluorene structure with a high carbon content and having thermosetting properties; to provide a pattern forming method using the composition, and to provide a polymer of such an organic film forming composition.

[0023] Solutions for solving problems

[0024] In order to achieve the above-mentioned problem, the present invention provides an organic film-forming composition comprising:

[0025] A polymer having a partial structure represented by the following general formula (1A) as a repeating unit, and

[0026] Organic solvents.

[0027] [Chemistry 1]

[0028]

[0029] In the above general formula (1A), AR1 and AR2 are benzene rings or naphthalene rings which may have substituents, R is a hydrogen atom or a monovalent organic group having an unsaturated bond and having 2 to 10 carbon atoms, R' is a single bond or W1, and W1 is a divalent organic group having 6 to 80 carbon atoms and having one or more aromatic rings.

[0030] If the organic film formed by the composition of the polymer represented by the general formula (1A) is heated, the coupling reaction of the dehydrogenation of the hydrogens at the benzyl position represented by R or the thermal crosslinking by unsaturated bonds can form an organic film with a high carbon structure of indenofluorene ring with high etching resistance as the main component. Since the film has few heteroatoms such as oxygen atoms in the main structure and a high carbon content, an organic film with high dry etching resistance can be formed. In addition, the repeating unit of the polymer has more than 2 crosslinking groups, so compared with the case of a monomolecular compound with a limited amount of crosslinking groups, a denser organic film can be formed, and an organic film with excellent heat resistance and distortion resistance can be formed. In addition, since a polymer with a molecular weight distribution is used instead of a monomolecular with high crystallinity, the film forming property for substrates of complex structures and various materials is excellent, and since the content of low molecular components that become sublimates is small, the dissipated gas generated during baking can be suppressed.

[0031] The above general formula (1A) is preferably represented by the following general formula (1B).

[0032] [Chemistry 2]

[0033]

[0034] In the aforementioned general formula (1B), AR1, AR2, R and W1 are the same as those described above.

[0035] By using a polymer with an indenofluorene structure introduced into the main chain, the carbon density can be improved and an organic film with excellent etching resistance and distortion resistance can be formed. At the same time, by appropriately selecting the structure of W1, the solvent solubility, filling / flattening characteristics, film forming properties, adhesion to the substrate, etc. can be adjusted according to the required performance.

[0036] In the general formulae (1A) and (1B), R is preferably a hydrogen atom or a structure represented by the following formula (1C).

[0037] [Chemistry 3]

[0038]

[0039] By introducing such R into a polymer as a crosslinking group, an organic film having sufficient thermosetting properties and excellent etching resistance, distortion resistance, and filling / planarization properties can be formed.

[0040] The divalent organic group represented by W1 preferably has at least one of a naphthalene ring, a fluorene ring, and a carbazole ring.

[0041] By using a polymer having a partial structure as described above introduced into W1, an organic film having excellent heat resistance, etching resistance, distortion resistance, and film-forming properties can be formed.

[0042] The polymer preferably has a weight average molecular weight of 1,000 to 5,000.

[0043] When the organic film-forming composition contains a polymer having a weight average molecular weight within such a range, outgassing during baking can be suppressed without impairing solubility in an organic solvent.

[0044] The organic solvent is preferably a mixture of one or more organic solvents having a boiling point of less than 180°C and one or more organic solvents having a boiling point of 180°C or higher.

[0045] When the organic solvent is the mixture, the organic film-forming composition can have high filling / planarizing properties at the same time by providing the polymer with thermal fluidity of the organic film due to the addition of the high-boiling-point solvent.

[0046] The organic film-forming composition preferably further contains one or more of a surfactant and a plasticizer.

[0047] If the organic film-forming composition contains the above-mentioned additives, it can be a composition with better coating properties and filling / planarization characteristics.

[0048] The present invention provides a pattern forming method, comprising the following steps: forming an organic film on a workpiece using the aforementioned organic film forming composition, forming a silicon-containing resist underlayer film on the aforementioned organic film using a silicon-containing resist underlayer film material, forming a resist upper layer film on the aforementioned silicon-containing resist underlayer film using a photoresist composition, forming a circuit pattern on the aforementioned resist upper layer film, using the aforementioned resist upper layer film with the circuit pattern formed thereon as a mask and transferring the pattern to the aforementioned silicon-containing resist underlayer film by etching, using the aforementioned silicon-containing resist underlayer film with the pattern transferred thereon as a mask and transferring the pattern to the aforementioned organic film by etching, and using the aforementioned organic film with the pattern transferred thereon as a mask and forming a pattern on the aforementioned workpiece by etching.

[0049] The pattern forming method using the three-layer resist process can form a fine pattern on the processed substrate with high precision.

[0050] The present invention provides a pattern forming method, comprising the following steps: forming an organic film on a workpiece using the aforementioned organic film forming composition, forming a silicon-containing resist underlayer film on the aforementioned organic film using a silicon-containing resist underlayer film material, forming an organic antireflective film (BARC) on the aforementioned silicon-containing resist underlayer film, forming a resist upper layer film using a photoresist composition on the aforementioned BARC, forming a circuit pattern on the aforementioned resist upper layer film, using the aforementioned resist upper layer film with the circuit pattern formed as a mask and sequentially transferring the pattern of the BARC and the aforementioned silicon-containing resist underlayer film by etching, using the aforementioned silicon-containing resist underlayer film with the pattern transferred as a mask and transferring the pattern of the organic film by etching, and using the aforementioned organic film with the pattern transferred as a mask and etching the aforementioned workpiece to form a pattern on the aforementioned workpiece.

[0051] The pattern forming method using the above-mentioned four-layer resist process can form a fine pattern on the processed substrate with higher precision.

[0052] The present invention provides a pattern forming method, comprising the following steps: using the aforementioned organic film forming composition to form an organic film on a workpiece, forming an inorganic hard mask selected from silicon oxide film, silicon nitride film, and silicon oxide nitride film on the aforementioned organic film, using a photoresist composition to form a resist upper film on the aforementioned inorganic hard mask, forming a circuit pattern on the aforementioned resist upper film, using the aforementioned resist upper film with the circuit pattern formed as a mask and performing pattern transfer to the aforementioned inorganic hard mask by etching, using the aforementioned inorganic hard mask with the pattern formed as a mask and performing pattern transfer to the aforementioned organic film by etching, and using the aforementioned organic film with the pattern formed as a mask and etching the aforementioned workpiece to form a pattern on the aforementioned workpiece.

[0053] The pattern forming method using the three-layer resist process can form a fine pattern on a processed substrate with high precision.

[0054] In addition, the present invention provides a pattern forming method, comprising the following steps: forming an organic film on a workpiece using the aforementioned organic film forming composition, forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film on the aforementioned organic film, forming a BARC on the aforementioned inorganic hard mask, forming a resist upper film on the aforementioned BARC using a photoresist composition, forming a circuit pattern on the aforementioned resist upper film, using the aforementioned resist upper film having the circuit pattern formed thereon as a mask and sequentially transferring the pattern of the BARC and the aforementioned inorganic hard mask by etching, using the aforementioned inorganic hard mask having the pattern formed thereon as a mask and transferring the pattern of the aforementioned organic film by etching, and using the aforementioned organic film having the pattern formed thereon as a mask and etching the aforementioned workpiece to form a pattern on the aforementioned workpiece.

[0055] The pattern forming method using the four-layer resist process can form a fine pattern on a processed substrate with higher precision.

[0056] The inorganic hard mask is preferably formed by a CVD method or an ALD method.

[0057] When the inorganic hard mask is formed by the CVD method or the ALD method, a fine pattern can be formed on the substrate to be processed with higher precision.

[0058] The method of forming the circuit pattern on the resist upper layer film preferably uses optical lithography with a wavelength of 10 nm to 300 nm, direct writing by electron beam, nanoimprinting, or a combination thereof.

[0059] The method for forming a circuit pattern on the resist upper layer film can form a fine pattern on the processed substrate with higher precision if the method is used.

[0060] As the developing method, alkali development or development using an organic solvent is preferably used.

[0061] When alkali development or development using an organic solvent is used as the development method, a fine pattern can be formed on the substrate to be processed with higher precision.

[0062] The object to be processed is preferably a semiconductor device substrate, a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film or a metal oxide nitride film.

[0063] In the present invention, for example, the aforementioned object can be used as the aforementioned object to be processed.

[0064] As the metal, preferably used is silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, cobalt, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, molybdenum, ruthenium, or an alloy thereof.

[0065] These can be used as the aforementioned metal.

[0066] The present invention also provides a polymer having a partial structure represented by the following general formula (1A) as a repeating unit.

[0067] [Chemistry 4]

[0068]

[0069] In the above general formula (1A), AR1 and AR2 are benzene rings or naphthalene rings which may have substituents, R is a hydrogen atom or a monovalent organic group having an unsaturated bond and having 2 to 10 carbon atoms, R' is a single bond or W1, and W1 is a divalent organic group having 6 to 80 carbon atoms and having one or more aromatic rings.

[0070] The polymer represented by the general formula (1A) has thermosetting properties and is composed of a main chain containing an indenofluorene ring structure having a high carbon content. Therefore, an organic film having both high bending resistance and dry etching resistance can be formed.

[0071] The above general formula (1A) is preferably represented by the following general formula (1B).

[0072] [Chemistry 5]

[0073]

[0074] In the aforementioned general formula (1B), AR1, AR2, R and W1 are the same as those described above.

[0075] Since the indenofluorene structure is introduced into the main chain, the carbon density can be improved and an organic film with excellent etching resistance and distortion resistance can be formed. At the same time, due to the structure of W1, solvent solubility, filling / flattening characteristics, film forming properties, adhesion to the substrate, etc. can be adjusted according to the required performance.

[0076] In the general formulae (1A) and (1B), R is preferably a hydrogen atom or a structure represented by the following formula (1C).

[0077] [Chemistry 6]

[0078]

[0079] Such R functions as a thermally crosslinkable group, and the polymer contains one or more crosslinkable groups in the repeating unit, so that a dense cured film can be formed, and thus it is suitable for forming an organic film excellent in etching resistance and warp resistance.

[0080] The divalent organic group represented by W1 preferably has at least one of a naphthalene ring, a fluorene ring, and a carbazole ring.

[0081] By introducing such a condensed carbon ring structure into the main skeleton of the aforementioned polymer, it is possible to improve solvent solubility and film-forming properties without impairing carbon density, and simultaneously impart thermal fluidity without impairing heat resistance.

[0082] Effects of the Invention

[0083] As described above, the polymer of the present invention is composed of an indenofluorene with a high carbon density structure having a thermal crosslinking group in each repeating unit and excellent etching resistance to form a main chain structure. Therefore, due to the high carbon density and the use of thermal curing to form a dense film, it is effective for forming an organic film with excellent etching resistance and distortion resistance. In addition, the organic film forming composition containing the polymer is an effective material when forming an organic film with excellent etching resistance and distortion resistance, and having many characteristics such as heat resistance, filling / planarization characteristics. Therefore, the organic film forming composition of the present invention is extremely effective as an organic film material in a multilayer resist process such as a two-layer resist process, a three-layer resist process using a silicon-containing resist lower film, and a four-layer resist process using a silicon-containing resist lower film and an organic anti-reflection film. In addition, if it is a pattern forming method of the present invention, in a multilayer resist process, a fine pattern can be formed on a processed substrate with high precision. BRIEF DESCRIPTION OF THE DRAWINGS

[0084] Figure 1 This is a process diagram showing an example of the pattern forming method of the present invention.

[0085] Figure 2 The organic film-forming composition of the present invention is applied to a SiO2 having a groove pattern. 2 A cross-sectional view of an example of an organic film formed on a wafer substrate. DETAILED DESCRIPTION

[0086] As described above, there is a demand for the development of an organic film-forming composition containing a thermosetting polymer having an indenofluorene structure with a high carbon content and capable of exhibiting high etching resistance and excellent distortion resistance.

[0087] As a result of repeated and in-depth studies on the above-mentioned issues, the present inventors have discovered that an organic film-forming composition containing a polymer having a partial structure represented by the following general formula (1A) as a repeating unit and an organic solvent can form an organic film having excellent etching resistance and distortion resistance, as well as heat resistance, filling / planarization characteristics, film-forming properties, low sublimation content and other properties, thereby completing the present invention.

[0088] That is, the present invention is a composition for forming an organic film, comprising a polymer having a partial structure represented by the following general formula (1A) as a repeating unit and an organic solvent.

[0089] [Chemistry 7]

[0090]

[0091] In the above general formula (1A), AR1 and AR2 are benzene rings or naphthalene rings which may have substituents, R is a hydrogen atom or a monovalent organic group having an unsaturated bond and having 2 to 10 carbon atoms, R' is a single bond or W1, and W1 is a divalent organic group having 6 to 80 carbon atoms and having one or more aromatic rings.

[0092] Furthermore, the present invention is a polymer comprising the partial structure represented by the above general formula (1A) as a repeating unit.

[0093] Hereinafter, although the embodiment of the present invention will be described, the present invention is not limited thereto.

[0094] [polymer]

[0095] The organic film-forming composition of the present invention contains a polymer including a repeating unit represented by the following general formula (1A) as a partial structure.

[0096] [Chemistry 8]

[0097]

[0098] In the above general formula (1A), AR1 and AR2 are benzene rings or naphthalene rings which may have substituents, R is a hydrogen atom or a monovalent organic group having an unsaturated bond and having 2 to 10 carbon atoms, R' is a single bond or W1, and W1 is a divalent organic group having 6 to 80 carbon atoms and having one or more aromatic rings.

[0099] The partial structure of the main chain consisting of AR1 and AR2 of the polymer in the general formula (1A) can be exemplified as follows. The polymer may also have substituents such as vinyl, ethynyl, ethynylphenyl, allyl, propargyl, aryl, allyloxy, propargyloxy, etc. on their aromatic rings. Among the following, AR1 and AR2 are preferably both benzene rings in terms of the ease of obtaining raw materials.

[0100] [Chemistry 9]

[0101]

[0102] The substituent represented by R in the general formula (1A) may be a hydrogen atom or the following groups: The polymer may have a substituent on its aromatic ring, and examples thereof include a hydroxyl group, a methyl group, a methoxy group, a nitro group, a halogen group, and a trifluoromethyl group.

[0103] [Chemistry 10]

[0104]

[0105] The above general formula (1A) can be represented by the following general formula (1B).

[0106] [Chemistry 11]

[0107]

[0108] The partial structure represented by W1 in the above general formula can be exemplified by the following structures. They may also have a substituent on the aromatic ring, and examples thereof include a hydroxyl group, an alkyl group, a methoxy group, a propargyloxy group, an allyloxy group, a nitro group, a halogen group, a trifluoromethyl group, an acetyl group, a vinyl group, an ethynyl group, an ethynylphenyl group, an allyl group, an aryl group, etc. The hydrogen atom on the nitrogen atom can also be substituted by an alkyl group, an acetyl group, a propargyl group, an allyl group, a vinyl group, an aryl group, etc.

[0109] [Chemistry 12]

[0110]

[0111] [Chemistry 13]

[0112]

[0113] [Chemistry 14]

[0114]

[0115] In the general formulae (1A) and (1B), R is preferably a hydrogen atom or any of the following from the viewpoints of curability and availability of raw materials. Among them, hydrogen, propargyl, and allyl are more preferred from the viewpoints of imparting solvent solubility and availability of raw materials.

[0116] [Chemistry 15]

[0117]

[0118] The divalent organic group represented by W1 in the general formula (1B) preferably has at least one of a naphthalene ring, a fluorene ring, and a carbazole ring. Specific examples thereof include the following.

[0119] [Chemistry 16]

[0120]

[0121] [Chemistry 17]

[0122]

[0123] Furthermore, the Mw (weight average molecular weight) of the polymer is preferably 1,000 to 5,000, and more preferably 1,000 to 4,500.

[0124] If it is such a molecular weight, the solubility of the polymer in organic solvents can be ensured, and the sublimates generated during baking can be suppressed. In addition, the thermal fluidity of the polymer is good, so when the polymer is deployed in the composition, not only can the fine structure formed on the substrate be well buried, but also an organic film with a flat substrate as a whole can be formed.

[0125] [Production method 1 of polymer]

[0126] An example of the method for producing the polymer of the present invention is an electrophilic substitution reaction on the aromatic ring of the indenofluorene ring accompanied by dehydration using a diol having R as a substituent as shown below as a monomer. AR1, AR2, and R in the following formula are the same as those described above.

[0127] [Chemistry 18]

[0128]

[0129] The polymer of the present invention having W1 represented by the general formula (1B) in a partial structure can be synthesized by polycondensation using the following diols and W1 as monomers. AR1, AR2, R, and W1 in the following reaction formula are the same as those described above.

[0130] [Chemistry 19]

[0131]

[0132] At this time, when dimerization is carried out in a state where diols and W1 are mixed, it is generally considered that there are the following two modes. There are cases where diols react with each other (mode 1) and cases where diols react with W1 (mode 2). There is a possibility of reaction with W1 or diols, so if the degree of polymerization increases, it is expected to provide a complex product. Therefore, the present invention uses the structure represented by chemical formula (1B) that takes into account the two possibilities as a general formula.

[0133] [Chemistry 20]

[0134] Mode 1

[0135]

[0136] Mode 2

[0137]

[0138] The polymer having the partial structure represented by the general formula (1A) as a repeating unit can be obtained usually in an organic solvent in the presence of an acid catalyst at room temperature or under cooling or heating as required. The acid catalyst may be an inorganic acid such as hydrochloric acid, hydrobromic acid, sulfuric acid, nitric acid, phosphoric acid, heteropoly acid, etc.; an organic acid such as oxalic acid, trifluoroacetic acid, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, trifluoromethanesulfonic acid, etc.; an Lewis acid such as aluminum trichloride, ethoxyaluminum, isopropoxyaluminum, boron trifluoride, boron trichloride, boron tribromide, tin tetrachloride, tin tetrabromide, dibutyltin dichloride, dimethoxydibutyltin, dibutyltin oxide, titanium tetrachloride, titanium tetrabromide, methoxytitanium (IV), ethoxytitanium (IV), isopropoxytitanium (IV), titanium (IV) oxide, etc.

[0139] The solvent is not particularly limited, and examples thereof include: alcohols such as methanol, ethanol, isopropanol, butanol, ethylene glycol, propylene glycol, diethylene glycol, glycerol, ethylene glycol monomethyl ether, and propylene glycol monomethyl ether; ethers such as diethyl ether, dibutyl ether, diethylene glycol diethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, and 1,4-dioxane; chlorine-based solvents such as dichloromethane, chloroform, dichloroethane, and trichloroethylene; hydrocarbons such as hexane, heptane, benzene, toluene, xylene, and cumene; nitriles such as acetonitrile; ketones such as acetone, methyl ethyl ketone, and isobutyl methyl ketone; esters such as ethyl acetate, n-butyl acetate, and propylene glycol methyl ether acetate; and aprotic polar solvents such as dimethyl sulfoxide, N,N-dimethylformamide, and hexamethylphosphoric acid triamide. These solvents can be used alone or in combination of two or more.

[0140] As for the reaction method, there are methods of using the aforementioned diol compound alone as a monomer or using the diol compound and W1 as monomers, and feeding the acid catalyst as a catalyst all at once; a method of adding the catalyst all at once or in portions after dispersing or dissolving the monomer, or a method of diluting with a solvent and adding dropwise; a method of adding the monomer all at once or in portions after dispersing or dissolving the catalyst, or a method of diluting with a solvent and adding dropwise. After the reaction is completed, in order to remove the catalyst used in the reaction, it can be diluted with an organic solvent, and then separated and washed to recover the target product.

[0141] In addition, in these reactions, copolymerization and condensation can be carried out using compounds that are different from the above-mentioned monomers. Examples of copolymerization and condensation compounds include fluorenols and diol compounds as shown below. The aromatic rings of these compounds may also have substituents such as vinyl, ethynyl, ethynylphenyl, allyl, propargyl, aryl, allyloxy, and propargyloxy. Considering the viewpoint of imparting etching resistance and solvent solubility, it is preferred to have a naphthalene ring, a fluorene structure, and a carbazole structure, which can be added simultaneously or separately when the reaction is carried out using the method shown above and copolymerization and condensation are carried out.

[0142] [Chemistry 21]

[0143]

[0144] [Chemistry 22]

[0145]

[0146] [Chemistry 23]

[0147]

[0148] The organic solvent used in the liquid separation cleaning is not particularly limited as long as it is an organic solvent that can dissolve the target and separate into two layers when mixed with water. Examples thereof include: hydrocarbons such as hexane, heptane, benzene, toluene, and xylene; esters such as ethyl acetate, n-butyl acetate, and propylene glycol methyl ether acetate; ketones such as methyl ethyl ketone, methyl amyl ketone, cyclohexanone, and methyl isobutyl ketone; ethers such as diethyl ether, diisopropyl ether, methyl tert-butyl ether, and ethyl cyclopentyl methyl ether; chlorine-based solvents such as dichloromethane, chloroform, dichloroethane, and trichloroethylene; and mixtures thereof. The cleaning water used at this time can be what is generally called deionized water or ultrapure water. The number of cleaning times may be one or more, but since the corresponding cleaning effect cannot be obtained by cleaning more than 10 times, it is preferably about 1 to 5 times.

[0149] In order to remove the acidic components in the reaction system during the liquid separation and washing, an alkaline aqueous solution may be used for washing. Specific examples of the alkali include alkali metal hydroxides, alkali metal carbonates, alkaline earth metal hydroxides, alkaline earth metal carbonates, ammonia, and organic ammonium.

[0150] In addition, in order to remove metal impurities or alkaline components in the reaction system during liquid separation and cleaning, an acidic aqueous solution can also be used for cleaning. Specifically, the acid includes inorganic acids such as hydrochloric acid, hydrobromic acid, sulfuric acid, nitric acid, phosphoric acid, and heteropoly acids; and organic acids such as oxalic acid, fumaric acid, maleic acid, trifluoroacetic acid, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and trifluoromethanesulfonic acid.

[0151] The liquid separation cleaning using the alkaline aqueous solution and the acidic aqueous solution may be performed alone or in combination. Liquid separation cleaning using the alkaline aqueous solution and the acidic aqueous solution in sequence is more preferred from the viewpoint of removing metal impurities.

[0152] After the aforementioned liquid separation cleaning using alkaline aqueous solution or acidic aqueous solution, cleaning with neutral water may be continued. The cleaning frequency may be performed once or more, preferably about 1 to 5 times. Neutral water may be the aforementioned deionized water, ultrapure water, etc. The cleaning frequency may be performed once or more, but if the frequency is less, the alkaline component or acidic component may not be removed. Since the corresponding cleaning effect may not be obtained even after cleaning for more than 10 times, it is preferably about 1 to 5 times.

[0153] In addition, the reaction product after the liquid separation operation can also be concentrated to dryness or crystallized under reduced pressure or normal pressure, and recovered in the form of powder, but in order to improve the operability when preparing the organic film-forming composition, it can also be made into a solution state of appropriate concentration in advance. The concentration at this time is preferably 0.1 to 50% by mass, and more preferably 0.5 to 30% by mass. If it is such a concentration, the viscosity is not easy to increase, so it can prevent the operability from being damaged. In addition, it is more economical because the amount of solvent is not too large.

[0154] The solvent at this time is not particularly limited as long as it is a solvent that can dissolve the polymer. Specific examples include: ketones such as cyclohexanone and methyl-2-pentyl ketone; alcohols such as 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol, and 1-ethoxy-2-propanol; ethers such as propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether, and diethylene glycol dimethyl ether; esters such as propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl lactate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tert-butyl acetate, tert-butyl propionate, and propylene glycol mono-tert-butyl ether acetate. These can be used alone or in combination of two or more.

[0155] [Production method of polymer 2]

[0156] In addition, another method for obtaining the polymer used in the organic film-forming composition of the present invention can be obtained by using a diol having a hydrogen atom in R as shown below or by using the diol and W1 to obtain an intermediate (Step 1), and then converting the hydrogen atom to R by a substitution reaction (Step 2). In the following formula, AR1, AR2, W1, and R are the same as those described above.

[0157] [Chemistry 24]

[0158] [Step 1]

[0159]

[0160] [Step 2]

[0161]

[0162] [Chemistry 25]

[0163] [Step 1]

[0164]

[0165] [Step 2]

[0166]

[0167] These reactions are not particularly limited as long as they can introduce a desired substituent, and examples thereof include substitution reactions using a halide, toluenesulfonate, or mesylate of R and a base catalyst. X in the following formula represents a halogen, toluenesulfonyl group, or mesylate group.

[0168] [Chemistry 26]

[0169]

[0170] Examples of the base catalyst used in the above-mentioned substitution reaction include inorganic base compounds such as sodium bicarbonate, sodium carbonate, potassium carbonate, calcium carbonate, cesium carbonate, sodium hydroxide, potassium hydroxide, sodium hydride, potassium phosphate, etc.; organic amine compounds such as triethylamine, pyridine, N-methylmorpholine, etc., and they can be used alone or in combination of two or more.

[0171] The solvent used at this time is not particularly limited as long as it is a solvent inactive to the above-mentioned reaction. Examples thereof include: ether solvents such as diethyl ether, tetrahydrofuran, and dioxane; aromatic solvents such as benzene, toluene, and xylene; acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, N-methylpyrrolidone, water, etc., which can be used alone or in combination.

[0172] The reaction method of the polymer and the recovery method of the compound are the same as those of the reaction and recovery methods of the polymer production method 1.

[0173] In the preparation of the polymer used in the composition for forming an organic film obtained by this method, various halides, toluenesulfonates and mesylates can be used alone or in combination according to the required performance. For example, those having a side chain structure that contributes to the improvement of planarization characteristics, a rigid aromatic ring structure that contributes to etching resistance and heat resistance, etc. can be combined in any proportion. Therefore, the composition for forming an organic film using these polymers can achieve both high-level filling / planarization characteristics and etching resistance.

[0174] As described above, the polymer of the present invention can provide an organic film-forming composition that can exhibit high etching resistance and excellent distortion resistance.

[0175] [Organic film-forming composition]

[0176] The present invention provides an organic film-forming composition comprising a polymer having a partial structure represented by general formula (1A) as a repeating unit and an organic solvent. In the organic film-forming composition of the present invention, the polymer of the present invention may be used alone or in combination of two or more.

[0177] <Modifier>

[0178] The organic film-forming composition of the present invention may further contain a compound for blending, other polymers, and other modifiers. The modifier is mixed with the organic film-forming composition of the present invention to improve the film-forming property of spin coating or the filling property of a substrate having a height difference.Examples of such modifiers include phenol, o-cresol, m-cresol, p-cresol, 2,3-dimethylphenol, 2,5-dimethylphenol, 3,4-dimethylphenol, 3,5-dimethylphenol, 2,4-dimethylphenol, 2,6-dimethylphenol, 2,3,5-trimethylphenol, 3,4,5-trimethylphenol, 2-tert-butylphenol, 3-tert-butylphenol, 4-tert-butylphenol, 2-phenylphenol, 3-phenylphenol, 4-phenylphenol, 3,5-diphenylphenol, 2-naphthylphenol, 3-naphthylphenol, 4-naphthylphenol, 4-tritylphenol, resorcinol, 2-methylresorcinol, 4-methylresorcinol, 5-methylresorcinol, catechol, 4-tert-butylcatechol, 2-methoxyphenol, 3-methoxyphenol , 2-propylphenol, 3-propylphenol, 4-propylphenol, 2-isopropylphenol, 3-isopropylphenol, 4-isopropylphenol, 2-methoxy-5-methylphenol, 2-tert-butyl-5-methylphenol, gallol, thymol, isothymol, 4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,2'-dimethyl-4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,2'-diallyl-4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,2'-difluoro-4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,2'-diphenyl-4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,2'-dimethoxy-4,4'-(9H-fluorene-9-ylidene) Bisphenol, 2,3,2',3'-tetrahydro-(1,1')-spirobiindene-6,6'-diol, 3,3,3',3'-tetramethyl-2,3,2',3'-tetrahydro-(1,1')-spirobiindene-6,6'-diol, 3,3,3',3',4,4'-hexamethyl-2,3,2',3'-tetrahydro-(1,1')-spirobiindene-6,6'-diol, 2,3,2',3'-tetrahydro-(1,1')-spirobiindene-5,5'-diol, 5,5'-dimethyl-3,3,3',3'-tetramethyl-2,3,2',3'-tetrahydro-(1,1')-spirobiindene-6,6'-diol, 1-naphthol, 2-naphthol, 2-methyl-1 Novolac resins such as 1,5-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, and 2,6-dihydroxynaphthalene, 3-hydroxynaphthalene-2-carboxylic acid methyl ester, indene, hydroxyindene, benzofuran, hydroxyanthracene, acenaphthene, biphenyl, bisphenol, trisphenol, dicyclopentadiene, tetrahydroindene, 4-vinylcyclohexene, norbornadiene, 5-vinylnorborn-2-ene, α-pinene, β-pinene, and limonene, polyhydroxystyrene, polystyrene, polyvinylnaphthalene, polyvinylanthracene, polyvinylcarbazole, polyindene, polyacenaphthene, polynorbornene, polycyclodecene, polytetracyclododecene, polynortricycloene, poly(meth)acrylate, and copolymers thereof.In addition, naphthol dicyclopentadiene copolymers described in Japanese Patent Application Laid-Open No. 2004-205685, bisphenol fluorene novolac resins described in Japanese Patent Application Laid-Open No. 2005-128509, acenaphthene copolymers described in Japanese Patent Application Laid-Open No. 2005-250434, fullerenes having a phenol group described in Japanese Patent Application Laid-Open No. 2006-227391, bisphenol compounds and novolac resins thereof described in Japanese Patent Application Laid-Open No. 2006-293298, novolac resins of adamantane phenol compounds described in Japanese Patent Application Laid-Open No. 2006-285095, bisnaphthol compounds and novolac resins thereof described in Japanese Patent Application Laid-Open No. 2010-122656, fullerene resin compounds described in Japanese Patent Application Laid-Open No. 2008-158002, etc. may also be blended. The amount of the modifier to be added is preferably 0 to 1,000 parts by mass, more preferably 0 to 500 parts by mass, based on 100 parts by mass of the polymer of the present invention.

[0179] <Organic Solvents>

[0180] The organic solvent that can be used in the organic film-forming composition of the present invention is not particularly limited as long as it is an organic solvent that can dissolve the constituent components contained in the materials such as the aforementioned polymer, acid generator, crosslinking agent, other additives, etc. Specifically, a solvent having a boiling point lower than 180° C. such as the solvents described in paragraphs (0091) to (0092) of Japanese Patent Application Laid-Open No. 2007-199653 can be used. Among them, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, 2-heptanone, cyclopentanone, cyclohexanone, and a mixture of two or more thereof are preferably used.

[0181] Such an organic film-forming composition can be applied by spin coating, and since it contains the polymer of the present invention, it is possible to provide an organic film-forming composition having good dry etching resistance, heat resistance, and high-level filling / planarization properties.

[0182] In the composition for forming an organic film of the present invention, as for the organic solvent, a high boiling point solvent having a boiling point of 180°C or higher (a mixture of a solvent having a boiling point of less than 180°C and a solvent having a boiling point of 180°C or higher) may be added to the solvent having a boiling point of less than 180°C. As for the high boiling point organic solvent, there is no particular limitation on hydrocarbons, alcohols, ketones, esters, ethers, chlorine-based solvents, etc., as long as the high boiling point organic solvent is an organic solvent that can dissolve the polymer of the present invention. Specific examples thereof include 1-octanol, 2-ethylhexanol, 1-nonanol, 1-decanol, 1-undecanol, ethylene glycol, 1,2-propylene glycol, 1,3-butanediol, 2,4-pentanediol, 2-methyl-2,4-pentanediol, 2,5-hexanediol, 2,4-heptanedi ... 1,3-hexanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, glycerol, n-nonyl acetate, ethylene glycol monohexyl ether, ethylene glycol mono-2-ethylhexyl ether, ethylene glycol monophenyl ether, ethylene glycol monobenzyl ether, diethylene glycol monoethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol monoisobutyl ether, diethylene glycol monohexyl ether, diethylene glycol monophenyl ether, diethylene glycol monobenzyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl methyl ether, triethylene glycol dimethyl ether , triethylene glycol monomethyl ether, triethylene glycol n-butyl ether, triethylene glycol butyl methyl ether, triethylene glycol diacetate, tetraethylene glycol dimethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, tripropylene glycol mono-n-propyl ether, tripropylene glycol mono-n-butyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, triacetin, Propylene glycol diacetate, dipropylene glycol monomethyl ether acetate, dipropylene glycol methyl n-propyl ether, dipropylene glycol methyl ether acetate, 1,4-butanediol diacetate, 1,3-butanediol diacetate, 1,6-hexanediol diacetate, triethylene glycol diacetate, γ-butyrolactone, dihexyl malonate, diethyl succinate, dipropyl succinate, dibutyl succinate, dihexyl succinate, dimethyl adipate, diethyl adipate, dibutyl adipate, etc., which can be used alone or in combination.

[0183] The boiling point of the high boiling point solvent is appropriately selected according to the temperature at which the organic film forming composition is heat treated. The boiling point of the added high boiling point solvent is preferably 180°C to 300°C, more preferably 200°C to 300°C. If it is such a boiling point, there is no concern that the solvent volatilizes too quickly during baking (heat treatment) due to the boiling point being too low, so sufficient thermal fluidity can be obtained. In addition, if it is such a boiling point, since the boiling point is high, there will be no situation where the solvent remains in the film after baking without volatilization, so there is no concern that the film properties such as etching resistance are adversely affected.

[0184] In addition, when the high boiling point solvent is used, the amount of the high boiling point solvent is preferably set to 1 to 30 parts by mass relative to 100 parts by mass of the solvent having a boiling point lower than 180° C. If such an amount is used, there is no concern that the amount is too small to provide sufficient thermal fluidity during baking, or that the amount is too large to remain in the organic film and cause deterioration of film properties such as etching resistance.

[0185] According to such an organic film-forming composition, by providing thermal fluidity to the polymer of the present invention by adding a high-boiling-point solvent, it becomes a composition having both high-level filling and planarizing properties.

[0186] <Acid Generator>

[0187] In order to further promote the curing reaction, an acid generator may be added to the organic film-forming composition of the present invention. The acid generator includes an acid generator that generates acid by thermal decomposition and an acid generator that generates acid by light exposure, and any of them may be added. Specifically, the materials described in paragraphs (0061) to (0085) of Japanese Patent Publication No. 2007-199653 may be added, but the present invention is not limited thereto.

[0188] The acid generator may be used alone or in combination of two or more. The amount of the acid generator added is preferably 0.05 to 50 parts by mass, more preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the polymer of the present invention.

[0189] <Surfactant>

[0190] In order to improve the coating property in spin coating, a surfactant may be added to the organic film-forming composition of the present invention. As the surfactant, for example, the surfactants described in (0142) to (0147) of JP-A-2009-269953 may be used.

[0191] <Crosslinking agent>

[0192] In addition, in order to improve the curability and further suppress the mutual mixing with the film formed on the upper layer, a crosslinking agent may be added to the organic film-forming composition of the present invention. As for the crosslinking agent, there is no particular limitation, and various known crosslinking agents can be widely used. For example, melamine crosslinking agents, glycoluril crosslinking agents, benzoguanamine crosslinking agents, urea crosslinking agents, β-hydroxyalkylamide crosslinking agents, isocyanurate crosslinking agents, aziridine crosslinking agents, oxazoline crosslinking agents, and epoxy crosslinking agents can be illustrated.

[0193] Specifically, for melamine-based crosslinking agents, hexamethoxymethylated melamine, hexabutoxymethylated melamine, their alkoxy and / or hydroxyl substitutions, and their partial self-condensation products can be exemplified. Specifically, for glycoluril-based crosslinking agents, tetramethoxymethylated glycoluril, tetrabutoxymethylated glycoluril, their alkoxy and / or hydroxyl substitutions, and their partial self-condensation products can be exemplified. Specifically, for benzoguanamine-based crosslinking agents, tetramethoxymethylated benzoguanamine, tetrabutoxymethylated benzoguanamine, their alkoxy and / or hydroxyl substitutions, and their partial self-condensation products can be exemplified. Specifically, for urea-based crosslinking agents, dimethoxymethylated dimethoxyethylene urea, its alkoxy and / or hydroxyl substitutions, and their partial self-condensation products can be exemplified. Specifically, for β-hydroxyalkylamide-based crosslinking agents, N,N,N',N'-tetrakis(2-hydroxyethyl)adipamide can be exemplified. Specific examples of isocyanurate crosslinking agents include triglycidyl isocyanurate and triallyl isocyanurate. Specific examples of aziridine crosslinking agents include 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane and 2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate]. Specific examples of oxazoline crosslinking agents include 2,2'-isopropylidenebis(4-benzyl-2-oxazoline), 2,2'-isopropylidenebis(4-phenyl-2-oxazoline), 2,2'-methylenebis-4,5-diphenyl-2-oxazoline, 2,2'-methylenebis-4-phenyl-2-oxazoline, 2,2'-methylenebis-4-tert-butyl-2-oxazoline, 2,2'-bis(2-oxazoline), 1,3-phenylenebis(2-oxazoline), 1,4-phenylenebis(2-oxazoline), and 2-isopropenyloxazoline copolymers. Specific examples of epoxy crosslinking agents include diglycidyl ether, ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, poly(glycidyl methacrylate), trimethylolethane triglycidyl ether, trimethylolpropane triglycidyl ether, and pentaerythritol tetraglycidyl ether.

[0194] <Plasticizer>

[0195] In addition, in order to further improve the planarization / burying characteristics, a plasticizer may be added to the organic film-forming composition of the present invention. There is no particular limitation on the plasticizer, and various known plasticizers can be widely used. Examples thereof include low molecular weight compounds such as phthalates, adipic acid esters, phosphates, trimellitic acid esters, and citrates, polyethers, polyesters, and polymers such as polyacetal polymers described in Japanese Patent Application Laid-Open No. 2013-253227.

[0196] <Thermodegradable polymer>

[0197] In addition, in the composition for forming an organic film of the present invention, as an additive for imparting a filling / planarizing property similarly to a plasticizer, it is preferable to use, for example, a liquid additive having a polyethylene glycol or polypropylene glycol structure, or a pyrolyzable polymer having a weight loss rate of 40% by mass or more between 30° C. and 250° C. and a weight average molecular weight of 300 to 200,000. The pyrolyzable polymer preferably contains a repeating unit having an acetal structure represented by the following general formula (DP1) or (DP1a).

[0198] [Chemistry 27]

[0199]

[0200] In the formula, R 6 Y is a hydrogen atom or an optionally substituted saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms. 1 It is a saturated or unsaturated divalent organic group having 2 to 30 carbon atoms.

[0201] [Chemistry 28]

[0202]

[0203] In the formula, R 6a Y is an alkyl group having 1 to 4 carbon atoms. a It is a saturated or unsaturated divalent hydrocarbon group having 4 to 10 carbon atoms, and may have an ether bond. n represents the average number of repeating units, and is 3 to 500.

[0204] The organic film-forming composition of the present invention may be used alone or in combination of two or more thereof. The organic film-forming composition of the present invention may be used as a planarizing material for manufacturing a semiconductor device.

[0205] In addition, the organic film forming composition of the present invention is extremely effective as an organic film material for multilayer resist processes such as a two-layer resist process, a three-layer resist process using a silicon-containing resist underlayer film, and a four-layer resist process using an inorganic hard mask and an organic antireflective film.

[0206] [Method for forming organic film]

[0207] An organic film that is a multilayer resist film used in photolithography or an organic film that functions as a planarizing film for semiconductor manufacturing is formed using the organic film-forming composition.

[0208] The method for forming the aforementioned organic film is to apply the aforementioned organic film-forming composition to the processed substrate by spin coating or the like. By using the spin coating method or the like, good filling characteristics can be obtained. After spin coating, baking (heat treatment) is performed to evaporate the solvent and prevent mixing with the resist upper film and the resist lower film, and to promote the cross-linking reaction. The baking is preferably performed at a temperature of 100°C to 600°C and within a range of 10 to 600 seconds, more preferably at a temperature of 200°C to 500°C and within a range of 10 to 300 seconds. Considering the effects of damage to the device and deformation of the wafer, the upper limit of the heating temperature of the wafer processing in the photolithography is preferably set to below 600°C, more preferably below 500°C.

[0209] In addition, the method for forming the aforementioned organic film can also be carried out by coating the organic film forming composition of the present invention on the processed substrate by spin coating, etc. in the same way as described above, and then calcining and curing the organic film forming composition of the present invention in an environment with an oxygen concentration of not less than 0.1% and not more than 21% to form an organic film.

[0210] By firing the organic film-forming composition of the present invention in such an oxygen atmosphere, a fully cured organic film can be obtained. The baking environment may be in air, but in order to reduce oxygen, N 2 Inert gases such as Ar, He, etc. are preferably used to prevent oxidation of the organic film. In order to prevent oxidation, the oxygen concentration needs to be controlled, preferably below 1000ppm, more preferably below 100ppm. If the organic film is prevented from being oxidized during baking, it is more preferred because there will be no increase in absorption or reduction in etching resistance.

[0211] The above-mentioned method for forming an organic film can obtain a flat organic film regardless of the unevenness of the processed substrate due to its excellent filling / planarization characteristics. Therefore, it is very effective in forming a flat organic film on a processed substrate with a structure having a height of more than 30nm or a height difference.

[0212] The thickness of the organic film such as the resist underlayer film and the planarization film for manufacturing a semiconductor device is appropriately selected and is preferably set to 30 to 20,000 nm, and more preferably set to 50 to 15,000 nm.

[0213] [Pattern Formation Method]

[0214] The present invention provides a pattern forming method for a three-layer resist process using such an organic film forming composition, comprising the following steps: forming an organic film on a workpiece using the organic film forming composition of the present invention, forming a silicon-containing resist underlayer film using a silicon-containing resist underlayer material on the aforementioned organic film, forming a resist upper layer film using a photoresist composition on the aforementioned silicon-containing resist underlayer film, forming a circuit pattern on the aforementioned resist upper layer film, using the aforementioned resist upper layer film with the circuit pattern formed as a mask and transferring the pattern to the aforementioned silicon-containing resist underlayer film by etching, using the aforementioned silicon-containing resist underlayer film with the pattern transferred as a mask and transferring the pattern to the aforementioned organic film by etching, and using the aforementioned organic film with the pattern transferred as a mask and forming a pattern on the aforementioned workpiece by etching.

[0215] The silicon-containing resist underlayer film in the above-mentioned three-layer resist process will show etching resistance caused by oxygen or hydrogen. Therefore, in the above-mentioned three-layer resist process, dry etching of the organic film using the silicon-containing resist underlayer film as a mask is preferably carried out using an etching gas mainly composed of oxygen or hydrogen.

[0216] As for the silicon-containing resist lower film in the above-mentioned three-layer resist process, a polysiloxane-based lower film can also be preferably used. By making the silicon-containing resist lower film have an antireflection effect, reflection can be suppressed. In particular, for 193nm exposure, if a material containing a large number of aromatic groups and having a high etching selectivity with the substrate is used as an organic film, although the k value becomes high and the substrate reflection becomes high, for the silicon-containing resist lower film, by making it have an absorption with an appropriate k value, reflection can be suppressed, and the substrate reflection can be controlled to less than 0.5%. For the silicon-containing resist lower film with an antireflection effect, it is preferred to use a polysiloxane with an anthracene group pendant and cross-linked by acid or heat for 248nm and 157nm exposure, and it is preferred to use a polysiloxane with a phenyl group pendant or a light-absorbing group having a silicon-silicon bond and cross-linked by acid or heat for 193nm exposure.

[0217] An organic antireflective film (BARC) may also be formed on the aforementioned silicon-containing resist underlayer film, and in this case, a pattern may be formed on the aforementioned workpiece using the following steps: forming an organic film on the workpiece using the organic film forming composition of the present invention, forming a silicon-containing resist underlayer film on the aforementioned organic film using a silicon-containing resist underlayer film material, forming a BARC on the aforementioned silicon-containing resist underlayer film, forming a resist upper film using a photoresist composition on the aforementioned BARC, forming a circuit pattern on the aforementioned resist upper film, using the aforementioned resist upper film with the circuit pattern formed thereon as a mask and sequentially transferring the pattern of the BARC and the aforementioned silicon-containing resist underlayer film by etching, using the aforementioned silicon-containing resist underlayer film with the pattern transferred thereon as a mask and transferring the pattern of the aforementioned organic film by etching, and using the aforementioned organic film with the pattern transferred thereon as a mask and etching the aforementioned workpiece to form a pattern on the aforementioned workpiece.

[0218] In addition, an inorganic hard mask can also be formed as an anti-etching agent lower film. In this case, the following steps can be used to form a pattern on the aforementioned processed object; using the organic film forming composition of the present invention to form an organic film on the processed substrate, forming an inorganic hard mask selected from silicon oxide film, silicon nitride film, and silicon oxide nitride film on the aforementioned organic film, using a photoresist composition to form an anti-etching agent upper film on the aforementioned inorganic hard mask, forming a circuit pattern on the aforementioned anti-etching agent upper film, using the aforementioned anti-etching agent upper film with the circuit pattern formed as a mask and transferring the pattern to the aforementioned inorganic hard mask by etching, using the aforementioned inorganic hard mask with the pattern formed as a mask and transferring the pattern to the aforementioned organic film by etching, and using the aforementioned organic film with the pattern formed as a mask and etching the aforementioned processed object to form a pattern on the aforementioned processed object.

[0219] As described above, when an inorganic hard mask is formed on an organic film, a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film (SiON film) can be formed by a CVD method, an ALD method, or the like. The method for forming a silicon nitride film is described, for example, in Japanese Patent Application Publication No. 2002-334869 and International Publication No. 2004 / 066377. The film thickness of the inorganic hard mask is preferably 5 to 200 nm, and more preferably 10 to 100 nm. In addition, as for the inorganic hard mask, it is most preferred to use a SiON film that has a high effect as an anti-reflective film. The substrate temperature when forming the SiON film will reach 300 to 500°C, so the organic film needs to withstand a temperature of 300 to 500°C. The composition for forming an organic film used in the present invention has high heat resistance and can withstand high temperatures of 300 to 500°C, so it can be a combination of an inorganic hard mask formed by a CVD method or an ALD method and an organic film formed by a spin coating method.

[0220] In addition, a four-layer resist process using BARC is also ideal, in which case a pattern can be formed on the aforementioned workpiece using the following steps: forming an organic film on the workpiece using the organic film forming composition of the present invention, forming an inorganic hard mask selected from silicon oxide film, silicon nitride film, and silicon oxide nitride film on the aforementioned organic film, forming a BARC on the aforementioned inorganic hard mask, forming a resist upper film on the aforementioned BARC using a photoresist composition, forming a circuit pattern on the aforementioned resist upper film, using the aforementioned resist upper film with the circuit pattern formed as a mask and sequentially transferring the pattern of the BARC and the aforementioned inorganic hard mask by etching, using the aforementioned inorganic hard mask with the pattern formed as a mask and transferring the pattern of the aforementioned organic film by etching, and using the aforementioned organic film with the pattern formed as a mask and etching the aforementioned workpiece to form a pattern on the aforementioned workpiece.

[0221] As described above, a photoresist film can be formed on an inorganic hard mask as a resist upper film, or a BARC can be formed on the inorganic hard mask by spin coating, and then a resist upper film can be formed thereon. In particular, when a SiON film is used as an inorganic hard mask, the two-layer antireflection film of the SiON film and the BARC can suppress reflection even in high NA immersion exposure with an NA exceeding 1.0. As for another benefit of forming a BARC, there is an effect of reducing the tailing of the photoresist pattern directly above the SiON film.

[0222] The resist upper film in the aforementioned three-layer resist process can be either positive or negative, and can use the same photoresist composition as commonly used. After spin coating the photoresist composition, pre-baking will be implemented, preferably falling within the range of 60 to 180°C and 10 to 300 seconds. Thereafter, exposure is performed according to the common method, and then post-exposure baking (PEB) and development are performed to obtain a resist pattern. In addition, the thickness of the resist upper film is not particularly limited, preferably 30 to 500 nm, more preferably 50 to 400 nm.

[0223] Examples of exposure light include high-energy rays with a wavelength of 300 nm or less, specifically, excimer lasers of 248 nm, 193 nm, and 157 nm, soft X-rays of 3 to 20 nm, electron beams, X-rays, etc. Nanoimprinting or a combination thereof may be used.

[0224] In the pattern forming method of the present invention, the method of forming the circuit pattern on the resist upper layer film preferably uses optical lithography with a wavelength of 10 nm to 300 nm, direct writing by electron beam, nanoimprinting, or a combination thereof.

[0225] In the formation of the circuit pattern, it is preferred to develop the circuit pattern using an alkali developer or an organic solvent.

[0226] Then, etching is performed using the obtained resist pattern as a mask. The etching of the silicon-containing resist lower film and the inorganic hard mask in the three-layer resist process is performed using a fluorocarbon gas and the upper resist pattern as a mask. Thus, the silicon-containing resist lower film pattern and the inorganic hard mask pattern are formed.

[0227] Then, the organic film is etched using the obtained resist underlayer film pattern containing silicon and the inorganic hard mask pattern as masks.

[0228] The etching of the processed substrate or other processed body can also be carried out by a common method. For example, if the processed substrate is SiO 2 If the substrate is a low dielectric constant insulating film of SiN or silicon dioxide, etching is mainly performed with flon gas. If the substrate is p-Si, Al, or W, etching is mainly performed with chlorine or bromine gas. When the substrate is processed with flon gas etching, the silicon-containing resist lower film pattern in the three-layer resist process is stripped at the same time as the substrate processing. When etching the substrate with chlorine or bromine gas, the stripping of the silicon-containing resist lower film pattern is a dry etching stripping that needs to be performed separately with flon gas after the substrate processing.

[0229] The organic film obtained using the organic film-forming composition of the present invention has a characteristic of being excellent in etching resistance when etching these substrates to be processed.

[0230] In the pattern forming method of the present invention, the object to be processed is preferably a semiconductor device substrate, a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film or a metal oxide nitride film.

[0231] In addition, the aforementioned metal is preferably silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, cobalt, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, molybdenum, ruthenium or an alloy thereof.

[0232] In addition, the substrate to be processed is not particularly limited, and Si, α-Si, p-Si, SiO 2 , SiN, SiON, W, TiN, Al and other substrates, or a substrate having a processed layer formed on the substrate. As for the processed layer, Si, SiO 2 , SiON, SiN, p-Si, α-Si, W, W-Si, Al, Cu, Al-Si and other Low-k films and barrier films thereof can be formed to a thickness of 50 to 10,000 nm, more preferably 100 to 5,000 nm. In addition, when forming the processed layer, different materials can be used for the substrate and the processed layer.

[0233] In addition, as for the substrate to be processed, it is preferable to use a substrate to be processed having a structure or a height difference of 30 nm or more.

[0234] An example of a three-layer resist process using Figure 1 To express it specifically, it is as follows.

[0235] In the case of a 3-layer resist process, Figure 1 As shown in (A), after an organic film 3 is formed on a processing layer 2 stacked on a substrate 1 using the organic film-forming composition of the present invention, a resist underlayer film 4 containing silicon is formed, and a resist upperlayer film 5 is formed thereon.

[0236] Then, if Figure 1 As shown in (B), the used portion 6 of the resist upper layer film is exposed, and PEB and development are performed to form a resist pattern 5a ( Figure 1 (C)). Using the obtained resist pattern 5a as a mask, the silicon-containing resist underlayer film 4 is etched using a CF-based gas to form a silicon-containing resist underlayer film pattern 4a ( Figure 1 (D)). After removing the resist pattern 5a, the obtained silicon-containing resist lower film pattern 4a is used as a mask to perform oxygen plasma etching on the organic film 3 to form an organic film pattern 3a ( Figure 1 (E)). After removing the silicon-containing resist lower film pattern 4a, the processed layer 2 is etched using the organic film pattern 3a as a mask to form a pattern 2a ( Figure 1 (F)).

[0237] When an inorganic hard mask is used, the resist lower film 4 containing silicon is the inorganic hard mask, and when BARC is applied, the BARC layer is disposed between the resist lower film 4 containing silicon or the inorganic hard mask and the resist upper film 5. The etching of BARC may be performed continuously before the etching of the resist lower film 4 containing silicon, or the etching of the resist lower film 4 containing silicon may be performed after only the etching of BARC is performed, and then the etching device or the like is changed to perform the etching.

[0238] As described above, according to the pattern forming method of the present invention, a fine pattern can be formed on a processed substrate with high precision in a multilayer resist process.

[0239] [Example]

[0240] Hereinafter, exemplify synthesis example, comparative synthesis example, embodiment and comparative example to more specifically illustrate the present invention, but the present invention is not limited thereto. In addition, with regard to molecular weight and dispersity, obtain weight average molecular weight (Mw), number average molecular weight (Mn) calculated using polystyrene of gel permeation chromatography (GPC) using tetrahydrofuran as eluent, and obtain dispersity (Mw / Mn, also referred to as molecular weight distribution).

[0241] [Synthesis Example: Synthesis of Polymer]

[0242] The following compound group B: (B1) to (B6) and compound group C: (C1) to (C2) were used for the synthesis of polymers (A1) to (A15).

[0243] Compound Group B:

[0244] [Chemistry 29]

[0245]

[0246] Compound Group C:

[0247] [Chemistry 30]

[0248]

[0249] [Synthesis Example 1] Synthesis of polymer (A1)

[0250] 50.0 g of compound (C1) and 300 g of 1,2-dichloroethane were prepared into a suspension at an internal temperature of 70°C under a nitrogen atmosphere. 33.6 g of methanesulfonic acid was slowly added, and after confirming that the heat generation had stopped, the temperature was raised to 70°C and the reaction was carried out for 8 hours. After cooling to room temperature, 500 g of toluene was added, and the organic layer was washed 6 times with 200 g of pure water, and then the organic layer was dried under reduced pressure. 150 g of tetrahydrofuran (THF) was added to the residue to make a uniform solution, and the polymer was reprecipitated with 500 g of methanol. The precipitated polymer was sorted by filtration, washed twice with 300 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A1). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were obtained by GPC, Mw=3820 and Mw / Mn=2.63.

[0251] [Chemistry 31]

[0252]

[0253] [Synthesis Example 2] Synthesis of polymer (A2)

[0254] 10.0 g of the polymer (A1) synthesized in Synthesis Example 1, 0.7 g of tetrabutylammonium iodide, 38.4 g of 25% sodium hydroxide aqueous solution, 50 g of toluene, and 50 g of tetrahydrofuran were prepared into a uniform dispersion at an internal temperature of 50°C under a nitrogen environment. 19.0 g of propargyl bromide was slowly added dropwise, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 100 g of toluene was added and the water layer was removed. The organic layer was then washed twice with 50 g of 3.0% nitric acid aqueous solution and five times with 50 g of pure water, and the organic layer was dried under reduced pressure. 40 g of THF was added to the residue, and the polymer was reprecipitated with 150 g of methanol. The precipitated polymer was sorted by filtration, washed twice with 100 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A2). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, Mw=4470 and Mw / Mn=2.86.

[0255] [Chemistry 32]

[0256]

[0257] [Synthesis Example 3] Synthesis of polymer (A3)

[0258] 10.0 g of the polymer (A1) synthesized in Synthesis Example 1, 0.7 g of tetrabutylammonium iodide, 38.4 g of 25% sodium hydroxide aqueous solution, 50 g of toluene, and 50 g of tetrahydrofuran were prepared into a uniform dispersion at an internal temperature of 50°C under a nitrogen environment. 19.3 g of allyl bromide was slowly added dropwise, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 100 g of toluene was added and the water layer was removed. The organic layer was then washed twice with 50 g of 3.0% nitric acid aqueous solution and five times with 50 g of pure water, and the organic layer was dried under reduced pressure. 40 g of THF was added to the residue, and the polymer was reprecipitated with 150 g of methanol. The precipitated polymer was sorted by filtration, washed twice with 100 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A3). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, Mw=4260 and Mw / Mn=2.74.

[0259] [Chemistry 33]

[0260]

[0261] [Synthesis Example 4] Synthesis of polymer (A4)

[0262] 50.0 g of compound (C2) and 300 g of 1,2-dichloroethane were prepared into a suspension at an internal temperature of 70°C under a nitrogen environment. 28.7 g of methanesulfonic acid was slowly added, and after confirming that the heat generation had stopped, the temperature was raised to 70°C and the reaction was carried out for 8 hours. After cooling to room temperature, 500 g of toluene was added, and the organic layer was washed 6 times with 200 g of pure water, and then the organic layer was dried under reduced pressure. After adding 150 g of THF to the residue to make a uniform solution, the polymer was reprecipitated with 500 g of methanol. The precipitated polymer was sorted by filtration, washed twice with 300 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A4). When the weight average molecular weight (Mw) and dispersity (Mw / Mn) were obtained by GPC, Mw=3980 and Mw / Mn=2.63.

[0263] [Chemistry 34]

[0264]

[0265] [Synthesis Example 5] Synthesis of polymer (A5)

[0266] 36.1 g of compound (B1), 30.0 g of compound (C2), and 400 g of 1,2-dichloroethane were prepared into a suspension at an internal temperature of 70°C under a nitrogen atmosphere. 20.1 g of methanesulfonic acid was slowly added, and after confirming that the heat generation had stopped, the temperature was raised to 70°C and the reaction was carried out for 8 hours. After cooling to room temperature, 600 g of toluene was added, and the organic layer was washed 6 times with 200 g of pure water, and then the organic layer was dried under reduced pressure. 200 g of THF was added to the residue to make a uniform solution, and the polymer was reprecipitated with 600 g of methanol. The precipitated polymer was sorted by filtration, washed twice with 400 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A5). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were obtained by GPC, Mw=2380 and Mw / Mn=2.45.

[0267] [Chemistry 35]

[0268]

[0269] [Synthesis Example 6] Synthesis of polymer (A6)

[0270] 10.0 g of the polymer (A5) synthesized in Synthesis Example 5, 0.3 g of tetrabutylammonium iodide, 16.1 g of a 25% sodium hydroxide aqueous solution, 50 g of toluene, and 50 g of tetrahydrofuran were prepared into a uniform dispersion at an internal temperature of 50°C under a nitrogen environment. 7.2 g of vinyl bromide was slowly added dropwise, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 100 g of toluene was added and the water layer was removed. The organic layer was then washed twice with 50 g of a 3.0% nitric acid aqueous solution and five times with 50 g of pure water, and the organic layer was dried under reduced pressure. 40 g of THF was added to the residue, and the polymer was reprecipitated with 150 g of methanol. The precipitated polymer was sorted by filtration, washed twice with 100 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A6). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, Mw=2960 and Mw / Mn=2.65.

[0271] [Chemistry 36]

[0272]

[0273] [Synthesis Example 7] Synthesis of polymer (A7)

[0274] 22.9 g of compound (B2), 30.0 g of compound (C2), and 400 g of 1,2-dichloroethane were made into a suspension at an internal temperature of 70°C under a nitrogen atmosphere. 17.2 g of methanesulfonic acid was slowly added, and after confirming that the heat generation had stopped, the temperature was raised to 70°C and the reaction was carried out for 8 hours. After cooling to room temperature, 600 g of toluene was added, and the organic layer was washed 6 times with 200 g of pure water, and then the organic layer was dried under reduced pressure. 200 g of THF was added to the residue to make a uniform solution, and the polymer was reprecipitated with 600 g of methanol. The precipitated polymer was sorted by filtration, washed twice with 400 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A7). When the weight average molecular weight (Mw) and dispersity (Mw / Mn) were obtained by GPC, Mw=2450 and Mw / Mn=2.58.

[0275] [Chemistry 37]

[0276]

[0277] [Synthesis Example 8] Synthesis of polymer (A8)

[0278] 23.5 g of compound (B3), 30.0 g of compound (C1), and 400 g of 1,2-dichloroethane were made into a suspension at an internal temperature of 70°C under a nitrogen atmosphere. 20.1 g of methanesulfonic acid was slowly added, and after confirming that the heat generation had stopped, the temperature was raised to 70°C and the reaction was carried out for 8 hours. After cooling to room temperature, 600 g of toluene was added, and the organic layer was washed 6 times with 200 g of pure water, and then the organic layer was dried under reduced pressure. 200 g of THF was added to the residue to make a uniform solution, and the polymer was reprecipitated with 600 g of methanol. The precipitated polymer was sorted by filtration, washed twice with 400 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A8). When the weight average molecular weight (Mw) and dispersity (Mw / Mn) were obtained by GPC, Mw=2150 and Mw / Mn=2.24.

[0279] [Chemistry 38]

[0280]

[0281] [Synthesis Example 9] Synthesis of polymer (A9)

[0282] 10.0 g of the polymer (A8) synthesized in Synthesis Example 8, 0.7 g of tetrabutylammonium iodide, 27.0 g of a 25% aqueous sodium hydroxide solution, 50 g of toluene, and 50 g of tetrahydrofuran were prepared into a uniform dispersion at an internal temperature of 50°C under a nitrogen environment. 22.4 g of 2-butynyl bromide was slowly added dropwise, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 100 g of toluene was added and the water layer was removed. The organic layer was then washed twice with 100 g of a 5.0% aqueous nitric acid solution and five times with 50 g of pure water, and the organic layer was dried under reduced pressure. 40 g of THF was added to the residue, and the polymer was reprecipitated with 150 g of methanol. The precipitated polymer was sorted by filtration, washed twice with 100 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A9). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, Mw=3120 and Mw / Mn=2.61.

[0283] [Chemistry 39]

[0284]

[0285] [Synthesis Example 10] Synthesis of polymer (A10)

[0286] 17.8 g of compound (B4), 21.0 g of compound (C1), 10.5 g of compound (C2), and 400 g of 1,2-dichloroethane were prepared into a suspension at an internal temperature of 70°C under a nitrogen environment. 20.1 g of methanesulfonic acid was slowly added, and after confirming that the heat generation had stopped, the temperature was raised to an internal temperature of 70°C and the reaction was carried out for 8 hours. After cooling to room temperature, 600 g of toluene was added, and the organic layer was washed 6 times with 200 g of pure water, and then the organic layer was dried under reduced pressure. 200 g of THF was added to the residue to make a uniform solution, and the polymer was reprecipitated with 600 g of methanol. The precipitated polymer was sorted by filtration, washed twice with 400 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A10). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, Mw=2720 and Mw / Mn=3.11.

[0287] [Chemistry 40]

[0288]

[0289] [Synthesis Example 11] Synthesis of polymer (A11)

[0290] 29.0 g of compound (B5), 30.0 g of compound (C1), and 400 g of 1,2-dichloroethane were prepared into a suspension at an internal temperature of 70°C under a nitrogen atmosphere. 20.1 g of methanesulfonic acid was slowly added, and after confirming that the heat generation had stopped, the temperature was raised to 70°C and the reaction was carried out for 8 hours. After cooling to room temperature, 600 g of toluene was added, and the organic layer was washed 6 times with 200 g of pure water, and then the organic layer was dried under reduced pressure. 200 g of THF was added to the residue to make a uniform solution, and the polymer was reprecipitated with 600 g of methanol. The precipitated polymer was sorted by filtration, washed twice with 400 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A11). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were obtained by GPC, Mw=2230 and Mw / Mn=2.15.

[0291] [Chemistry 41]

[0292]

[0293] [Synthesis Example 12] Synthesis of polymer (A12)

[0294] 10.0 g of the polymer (A11) synthesized in Synthesis Example 11, 0.4 g of tetrabutylammonium iodide, 12.1 g of a 25% sodium hydroxide aqueous solution, 50 g of toluene, and 50 g of tetrahydrofuran were prepared into a uniform dispersion at an internal temperature of 50°C under a nitrogen environment. 9.2 g of allyl bromide was slowly added dropwise, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 100 g of toluene was added and the water layer was removed. The organic layer was then washed twice with 50 g of a 3.0% nitric acid aqueous solution and five times with 50 g of pure water, and the organic layer was dried under reduced pressure. 40 g of THF was added to the residue, and the polymer was reprecipitated with 150 g of methanol. The precipitated polymer was sorted by filtration, washed twice with 100 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A12). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, Mw=3020 and Mw / Mn=2.43.

[0295] [Chemistry 42]

[0296]

[0297] [Synthesis Example 13] Synthesis of polymer (A13)

[0298] 10.0 g of the polymer (A11) synthesized in Synthesis Example 11, 0.4 g of tetrabutylammonium iodide, 12.1 g of a 25% sodium hydroxide aqueous solution, 50 g of toluene, and 50 g of tetrahydrofuran were prepared into a uniform dispersion at an internal temperature of 50°C under a nitrogen atmosphere. After slowly dropping 1.0 g of butyl bromide, the mixture was reacted at an internal temperature of 50°C for 8 hours, and then slowly dropping 8.1 g of propargyl bromide was reacted at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 100 g of toluene was added and the aqueous layer was removed. The organic layer was then washed twice with 50 g of a 3.0% nitric acid aqueous solution and five times with 50 g of pure water, and the organic layer was dried under reduced pressure. 40 g of THF was added to the residue, and the polymer was reprecipitated with 150 g of methanol. The precipitated polymer was sorted by filtration, washed twice with 100 g of methanol, and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A13). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, Mw=3140 and Mw / Mn=2.57.

[0299] [Chemistry 43]

[0300]

[0301] [Synthesis Example 14] Synthesis of polymer (A14)

[0302] 40.9 g of compound (B6), 20.0 g of compound (C1), and 400 g of 1,2-dichloroethane were made into a suspension at an internal temperature of 70°C under a nitrogen atmosphere. 13.4 g of methanesulfonic acid was slowly added, and after confirming that the heat generation had stopped, the temperature was raised to 70°C and the reaction was carried out for 8 hours. After cooling to room temperature, 600 g of toluene was added, and the organic layer was washed 6 times with 200 g of pure water, and then the organic layer was dried under reduced pressure. 200 g of THF was added to the residue to make a uniform solution, and the polymer was reprecipitated with 600 g of methanol. The precipitated polymer was sorted by filtration, washed twice with 400 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A14). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were obtained by GPC, Mw=2640 and Mw / Mn=2.24.

[0303] [Chemistry 44]

[0304]

[0305] [Synthesis Example 15] Synthesis of polymer (A15)

[0306] 10.0 g of the polymer (A14) synthesized in Synthesis Example 14, 0.4 g of tetrabutylammonium iodide, 15.3 g of 25% sodium hydroxide aqueous solution, 50 g of toluene, and 50 g of tetrahydrofuran were prepared into a uniform dispersion at an internal temperature of 50°C under a nitrogen environment. 11.4 g of propargyl bromide was slowly added dropwise, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 100 g of toluene was added and the water layer was removed. The organic layer was then washed twice with 100 g of 5.0% nitric acid aqueous solution and five times with 50 g of pure water, and the organic layer was dried under reduced pressure. 40 g of THF was added to the residue, and the polymer was reprecipitated with 150 g of methanol. The precipitated polymer was sorted by filtration, washed twice with 100 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A15). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, Mw=3370 and Mw / Mn=2.28.

[0307] [Chemistry 45]

[0308]

[0309] [Comparative Synthesis Example 1] Synthesis of Polymer (R1)

[0310] Under nitrogen environment, 12.8 g of naphthalene and 18.0 g of 9-fluorenone were added, the temperature was raised to 230°C and the reaction was carried out for 8 hours. From the beginning of the reaction, 0.25 ml of methanesulfonic acid was added to the reaction solution 8 times at intervals of 1 hour. After cooling to room temperature, 40 g of toluene was added to the reaction solution, and it was washed with pure water 6 times, and the organic layer was dried under reduced pressure. After adding 100 g of THF (tetrahydrofuran) to the residue to make a uniform solution, crystallization was carried out in 300 g of methanol. The crystals after precipitation were sorted by filtration, and washed twice with 200 g of methanol and recovered. The recovered crystals were vacuum dried at 70°C to obtain (R1). When the weight average molecular weight (Mw) and dispersity (Mw / Mn) were obtained by GPC, Mw=2130 and Mw / Mn=2.61.

[0311] [Chemistry 46]

[0312]

[0313] [Comparative Synthesis Example 2] Synthesis of Compound (R2)

[0314] Under nitrogen atmosphere, 10.0 g of indeno[1,2-b]fluorene-6,12-dione, 40.9 g of 2-naphthol, and 150 mL of 1,2-dichloroethane were added to form a uniform dispersion at 0°C, and then a mixed solution of 16.1 g of methanesulfonic acid and 1.3 g of 3-mercaptopropionic acid was slowly added dropwise, and the reaction was carried out at 60°C for 6 hours. After cooling to room temperature, 300 g of methyl isobutyl ketone and 100 g of pure water were added thereto, and after a brief stirring, the insoluble matter was filtered and the water layer was removed. The organic layer was then washed five times with 100 g of pure water and dried under reduced pressure. 100 g of ethyl acetate was added to the residue to form a uniform solution, and then crystallized in 400 g of methanol. The precipitated crystals were separated by filtration, washed twice with 100 g of methanol, and recovered. The recovered crystals were vacuum dried at 70°C to obtain (R2). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, Mw=860 and Mw / Mn=1.02.

[0315] [Chemistry 47]

[0316]

[0317] [Comparative Synthesis Example 3] Synthesis of Polymer (R3)

[0318] Under a nitrogen environment, 10.0 g of the compound (R2) synthesized in Comparative Synthesis Example 2, 0.5 g of a 37% formaldehyde aqueous solution, and 40 g of 2-methoxy-1-propanol were added, and a uniform solution was prepared at an internal temperature of 80°C. Then, 1.0 g of a 20 wt% p-toluenesulfonic acid PGME solution was slowly added, and the reaction was carried out at an internal temperature of 110°C for 8 hours. After cooling to room temperature, 200 g of methyl isobutyl ketone was added, and the organic layer was washed 5 times with 50 g of pure water, and then the organic layer was dried under reduced pressure. After adding 40 g of THF to the residue to prepare a uniform solution, the polymer was reprecipitated using 100 g of hexane. The precipitated polymer was sorted by filtration, washed twice with 80 g of hexane and recovered. The recovered crystals were vacuum dried at 70°C to obtain (R3). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, Mw=3100 and Mw / Mn=3.23.

[0319] [Chemistry 48]

[0320]

[0321] The structural formula, weight average molecular weight (Mw) and dispersity (Mw / Mn) of the polymers and compounds obtained above are shown in Tables 1 and 2.

[0322] [Table 1]

[0323]

[0324]

[0325]

[0326] [Table 2]

[0327]

[0328]

[0329] [Preparation of organic film-forming compositions (UDL-1 to 17, comparative UDL 1 to 4)]

[0330] The above-mentioned polymers or compounds (A1) to (A15) and (R1) to (R3), a crosslinking agent (XL) as an additive, an acid generator (AG), and (S1) 1,6-diacetoxyhexane: boiling point 260°C and (S2) tripropylene glycol monomethyl ether: boiling point 242°C as a high boiling point solvent were dissolved in a solvent containing propylene glycol monomethyl ether acetate (PGMEA) or cyclohexanone (CyHO) and 0.1% by mass of FC-4430 (manufactured by Sumitomo 3M Co., Ltd.) at the ratios shown in Table 3, and filtered using a 0.1 μm fluororesin filter to prepare organic film-forming compositions (UDL-1 to 17, comparative UDL-1 to 4).

[0331] [Table 3]

[0332]

[0333] The structural formulas of the acid generator (AG) and the cross-linking agent (XL) used in comparative UDL-2 are shown below.

[0334] [Chemistry 49]

[0335]

[0336] [Example 1 Solvent Resistance Measurement]

[0337] The prepared UDL-1 to 17 and comparative UDL-1 to 4 were coated on a silicon substrate, baked at 350°C for 60 seconds in the atmosphere, and the film thickness was measured. PGMEA solvent was dispensed on it, left for 30 seconds and spin dried, and baked at 100°C for 60 seconds to evaporate PGMEA, and the film thickness before and after PGMEA treatment was measured. The residual film rate was calculated using the film thickness after film formation and the film thickness after PGMEA treatment. The results are shown in Table 4.

[0338] [Table 4]

[0339]

[0340] As shown in Table 4, the organic membranes using the polymer of the present invention (Examples 1-1 to 1-17) have a residual membrane rate of more than 99% after PGMEA treatment, and a crosslinking reaction is induced by heat treatment to show sufficient solvent resistance. In contrast, the organic membranes using only the polymer (R1) (Comparative Example UDL-1) do not have a crosslinking site, so the polymer alone cannot show solvent resistance, and an acid generator and a crosslinking agent must be added to show solvent resistance. From these results, it can be seen that the partial structure introduced into the polymer of the present invention functions effectively as a thermal crosslinking group.

[0341] [Example 2 Hardness Measurement]

[0342] The above-mentioned UDL-1 to 17 and comparative UDL-1 to 4 were coated on a silicon substrate and baked at 350°C for 60 seconds in air to form a coating film with a film thickness of 200 nm. These films were subjected to a nanoindentation test using a NANOINDENTER SA2 device manufactured by TOYO Corporation to measure the hardness of the above-mentioned coating films. The results are shown in Table 5.

[0343] [Table 5]

[0344] Organic film forming composition Hardness(Gpa) Example 2-1 UDL-1 0.75 Example 2-2 UDL-2 0.75 Example 2-3 UDL-3 0.76 Embodiment 2-4 UDL-4 0.79 Embodiment 2-5 UDL-5 0.69 Embodiment 2-6 UDL-6 0.70 Embodiment 2-7 UDL-7 0.75 Embodiment 2-8 UDL-8 0.67 Embodiment 2-9 UDL-9 0.68 Embodiment 2-10 UDL-10 0.71 Example 2-11 UDL-11 0.71 Example 2-12 UDL-12 0.70 Example 2-13 UDL-13 0.68 Embodiment 2-14 UDL-14 0.65 Example 2-15 UDL-15 0.68 Example 2-16 UDL-16 0.74 Example 2-17 UDL-17 0.63 Comparative Example 2-1 Compare UDL-1 0.45 Comparative Example 2-2 Compare UDL-2 0.48 Comparative Example 2-3 Compare UDL-3 0.54 Comparative Examples 2-4 Compare UDL-4 0.58

[0345] As shown in Table 5, it can be confirmed that Examples 2-1 to 2-17 have greater hardness than Comparative Examples 2-1 to 2-4, and the polymers of Examples 2-1 to 2-17 can form denser and stronger films than the polymers and compounds used in Comparative Examples 2-1 to 2-4. The cured films of the aforementioned UDL-1 to 17 contain an indenofluorene structure with a high carbon density, and each repeating unit is introduced with a cross-linked structure to form a dense film, resulting in a high hardness. In contrast, although the polymer (R1) used in Comparative Example 2-1 has a high carbon density, the polymer itself is not thermosetting, so the film hardness cannot reach a high value. In addition, although the polymer (R1) uses a cross-linking agent to exhibit solvent resistance, the cross-linking agent causes the carbon density of the polymer to be damaged, so the hardness cannot be greatly improved after the cured film. As shown in Table 5, the compound (R2) used in Comparative Example 2-3 and the polymer (R3) used in Comparative Example 2-4 can form a cured film without adding a crosslinking agent, but the hardness is inferior to the polymer of the present invention.

[0346] [Example 3 Etching Test]

[0347] [Using CF 4 / CHF 3 Etching test with gas]

[0348] The above-mentioned UDL-1 to 17 and comparative UDL-1 to 4 were coated on a silicon substrate and baked in air at 350° C. for 60 seconds to form an organic film with a film thickness of 200 nm. 4 / CHF 3 This is a gas etching test. In this case, a dry etching apparatus TE-8500 manufactured by Tokyo Electron Co., Ltd. was used to determine the difference in film thickness of the polymer film before and after etching. The results are shown in Table 6.

[0349] The etching conditions are as follows.

[0350]

[0351] In Table 6, the comparison UDL-1 is made using CF4 / CHF 3 The film reduction of each of the examples and comparative examples is expressed as a ratio when the film thickness reduction due to the etching with the gas is 100. The smaller the ratio, the better the etching resistance.

[0352] [Use O 2 Etching test with gas]

[0353] The above-mentioned UDL-1 to 17 and comparative UDL-1 to 4 were coated on a silicon substrate and baked in air at 350° C. for 60 seconds to form an organic film with a film thickness of 200 nm. The organic film was subjected to the following conditions: 2 This is a gas etching test. In this case, a dry etching apparatus TE-8500 manufactured by Tokyo Electron Co., Ltd. was used to determine the difference in film thickness of the polymer film before and after etching. The results are shown in Table 6.

[0354] The etching conditions are as follows.

[0355]

[0356]

[0357] and using CF 4 / CHF 3 Similarly, in Table 6, the comparative UDL-1 was subjected to the etching test using O 2 The film reduction of each of the examples and comparative examples is expressed as a ratio when the film thickness reduction due to the etching with the gas is 100. The smaller the ratio, the better the etching resistance.

[0358] [Table 6]

[0359]

[0360] As shown in Table 6, by comparing Examples 3-1 to 3-17 with Comparative Example 3-1, it can be seen that in CF 4 / CHF 3 Gas, O 2In any etching test using a system gas, the reduction in the film after etching is smaller than that of the comparative UDL-1, and a film with excellent etching resistance is formed in all cases. Comparing Comparative Examples 3-1 and 3-2, in Comparative Example 3-2 in which a crosslinking agent is used to form a cured film, the carbon content of the film is reduced due to the addition of the crosslinking agent, resulting in a reduction in etching resistance of about 10%. In addition, when comparing Examples 3-1 to 3-17 using the polymer of the present invention and Comparative Examples 3-1 to 3-4 using the polymer and compound of the comparative synthesis example, as shown by the results of the hardness measurement, the polymer of the present invention has a high carbon density and becomes a dense cured film due to thermal crosslinking, so the reduction in film thickness after etching is suppressed, resulting in excellent etching resistance.

[0361] [Example 4 Pattern Etching Test]

[0362] The above-mentioned UDL-1 to 17 and comparative UDL-1 to 4 were applied to SiO 2 An organic film was formed on a Si wafer substrate with a diameter of 300 mm in the atmosphere, in such a way that the film thickness became 200 nm after baking at 350°C for 60 seconds. A silicon-containing resist lower film material (SOG-1) was coated thereon, and baked at 220°C for 60 seconds to form a silicon-containing resist lower film with a film thickness of 35 nm, and then a resist upper film material (SL resist for ArF) was coated thereon, and baked at 105°C for 60 seconds to form a resist upper film with a film thickness of 100 nm. An immersion protective film (TC-1) was coated on the resist upper film, and baked at 90°C for 60 seconds to form a protective film with a film thickness of 50 nm.

[0363] The resist upper film material (single-layer resist for ArF) is obtained by dissolving 100 parts by mass of a polymer (RP1) represented by the following formula, 6.6 parts by mass of an acid generator (PAG1) represented by the following formula, and 0.8 parts by mass of a basic compound (Amine1) represented by the following formula in 2500 parts by mass of PGMEA containing 0.1% by mass of FC-430 (manufactured by Sumitomo 3M Co., Ltd.), and filtering with a 0.1 μm fluororesin filter.

[0364] [Chemistry 50]

[0365]

[0366] The wet protective film material (TC-1) was prepared by dissolving 100 parts by mass of a protective film polymer (PP1) represented by the following formula in an organic solvent consisting of 2700 parts by mass of diisoamyl ether and 270 parts by mass of 2-methyl-1-butanol, and filtering the solution with a 0.1 μm fluororesin filter.

[0367] [Chemistry 51]

[0368]

[0369] The silicon-containing resist underlayer film material (SOG-1) is obtained by dissolving 100 parts by mass of a polymer (SiP1) represented by the following formula and 1 part by mass of a cross-linking catalyst (CAT1) in 4000 parts by mass of propylene glycol monoethyl ether containing 0.1% by mass of FC-4430 (produced by Sumitomo 3M Co., Ltd.), and filtering the mixture with a fluororesin filter having a pore size of 0.1 μm.

[0370] [Chemistry 52]

[0371]

[0372] Then, exposure was performed using an ArF immersion exposure device (manufactured by Nikon Co., Ltd.; NSR-S610C, NA1.30, σ0.98 / 0.65, 35 degree dipole s-polarized illumination, 6% halftone phase shift mask) while changing the exposure amount, and the pattern was baked (PEB) at 100°C for 60 seconds and developed with a 2.38 mass % tetramethylammonium hydroxide (TMAH) aqueous solution for 30 seconds to obtain a positive line and space pattern with a pitch of 100 nm and a resist line width ranging from 50 nm to 30 nm.

[0373] Then, using an etching apparatus Telius manufactured by Tokyo Electron, dry etching was performed to process the silicon-containing lower layer film using the resist pattern as a mask, process the organic film using the silicon-containing lower layer film as a mask, and process the SiO2 film using the organic film as a mask. 2 Film processing.

[0374] The etching conditions are as follows.

[0375] Transfer conditions for transferring the resist pattern to the SOG film.

[0376]

[0377] Transfer conditions of SOG film to organic film.

[0378]

[0379] Transfer to SiO 2 Membrane transfer conditions.

[0380]

[0381] The pattern cross-section was observed using an electron microscope (S-4700) manufactured by Hitachi, Ltd., and the shapes were compared and summarized in Table 7.

[0382] [Table 7]

[0383]

[0384] As shown in Table 7, the results of Examples 4-1 to 4-17 show that when UDL-1 to 17 were used as the organic film of the three-layer resist for immersion lithography, the resist shape after development was good in the pattern shape evaluation, and the film had an effective effect as an antireflection film. In contrast, since Comparative Example 4-1 used Comparative UDL-1, which had no thermal curing properties and could not obtain solvent resistance, when the silicon-containing resist underlayer film material (SOG-1) was applied, the film dissolved and could not form a pattern.

[0385] In the pattern shape after etching, the resist shape after development, the shape of the organic film after oxygen etching, and the shape of the substrate after etching are all good in Examples 4-1 to 4-17. The pattern size after substrate transfer will also change with the resist line width obtained by exposure. In Comparative Example 4-2, pattern distortion occurred at a line width of about 40nm, and in Comparative Examples 4-3 and 4-4, pattern distortion occurred at a line width of about 35nm. However, Examples 4-1 to 4-17 using the polymer of the present invention will not be distorted even at a line width thinner than the pattern size of 35nm, indicating high distortion resistance. This result is also taught by the fact that the polymer of the present invention has high hardness and forms a dense and high-strength organic film.

[0386] [Evaluation of landfill characteristics in Example 5]

[0387] A SiO substrate with a dense hole pattern of 500 nm in thickness and 160 nm in diameter is formed on the Si substrate. 2 On the uneven substrate, UDL-1 to 17 were coated under the conditions of baking at 350°C for 60 seconds to form an organic film with a film thickness of 80 nm on a flat substrate. The substrate with the organic film formed was cut and observed with a scanning electron microscope (SEM) to see whether the organic film was buried at the bottom of the hole. The results are shown in Table 8.

[0388] [Table 8]

[0389] Organic film forming composition Landfill characteristics Example 5-1 UDL-1 Until the bottom of the hole is well filled Example 5-2 UDL-2 Until the bottom of the hole is well filled Example 5-3 UDL-3 Until the bottom of the hole is well filled Example 5-4 UDL-4 Until the bottom of the hole is well filled Example 5-5 UDL-5 Until the bottom of the hole is well filled Embodiment 5-6 UDL-6 Until the bottom of the hole is well filled Embodiment 5-7 UDL-7 Until the bottom of the hole is well filled Embodiment 5-8 UDL-8 Until the bottom of the hole is well filled Embodiment 5-9 UDL-9 Until the bottom of the hole is well filled Embodiment 5-10 UDL-10 Until the bottom of the hole is well filled Embodiment 5-11 UDL-11 Until the bottom of the hole is well filled Example 5-12 UDL-12 Until the bottom of the hole is well filled Example 5-13 UDL-13 Until the bottom of the hole is well filled Embodiment 5-14 UDL-14 Until the bottom of the hole is well filled Example 5-15 UDL-15 Until the bottom of the hole is well filled Embodiment 5-16 UDL-16 Until the bottom of the hole is well filled Example 5-17 UDL-17 Until the bottom of the hole is well filled

[0390] As shown in Table 8, Examples 5-1 to 5-17 using UDL-1 to UDL-17 of the present invention to form organic films can all be well filled to the bottom of the hole, and sufficient filling characteristics can be expected even when the processed substrate has a height difference, which has effective characteristics for organic film materials used in multilayer processes.

[0391] [Evaluation of Flattening Characteristics of Example 6]

[0392] The organic film-forming compositions (UDL-1, 10, 16, 17, comparative UDL-1, 3, 4) were applied to SiO2 films having a giant isolated groove pattern (groove width 10 μm, groove depth 0.10 μm). 2 The wafer substrate was calcined at 350°C for 60 seconds in the atmosphere, and the height difference of the organic film between the groove part and the non-groove part was observed using an NX10 atomic force microscope (AFM) manufactured by Park Systems. Figure 2 The results are shown in Table 9. In this evaluation, the smaller the height difference, the better the planarization characteristics. In addition, in this evaluation, the groove pattern with a depth of 0.10 μm is usually planarized using an organic film-forming composition with a film thickness of about 0.2 μm, which becomes a more stringent evaluation condition in order to evaluate the quality of the planarization characteristics.

[0393] [Table 9]

[0394] Organic film forming composition Height difference(nm) Example 6-1 UDL-1 80 Example 6-2 UDL-10 75 Example 6-3 UDL-16 70 Example 6-4 UDL-17 70 Comparative Example 6-1 Compare UDL-1 90 Comparative Example 6-2 Compare UDL-3 85 Comparative Example 6-3 Compare UDL-4 90

[0395] As shown in Table 9, it can be confirmed that the organic film-forming composition of the present invention has a smaller height difference between the groove part and the non-groove part of the organic film than Comparative Examples 6-1 to 6-3, and has excellent flattening characteristics. In Comparative Examples 6-1 to 6-3, it is estimated that the density of the film is poor, so the film loss caused by baking becomes larger, and the difference in film thickness between the upper part of the height difference and the lower part of the height difference is more prominent, and the flatness becomes poor. In addition, by comparing Examples 6-3 and 6-4 to which a high boiling point solvent is added and Examples 6-1 and 6-2 to which no high boiling point solvent is added, it can be seen that the flatness is improved by adding a high boiling point solvent.

[0396] [Example 7 Coating Test]

[0397] The organic film-forming compositions (UDL-1 to 17 and comparative UDL-3) were coated on the bare-Si substrate, the substrate treated with hexamethyldisilazane (HMDS), and the substrate treated with SiON shown in Table 10, respectively, and baked at 350°C for 60 seconds in the air to form an organic film with a thickness of 200 nm. The formed organic film was observed using an optical microscope (ECLIPSEL200 manufactured by Nikon Corporation) to see if there was any coating abnormality. The confirmation results are shown in Table 10.

[0398] [Table 10]

[0399]

[0400] As shown in Table 10, Examples 7-1 to 7-17, in which organic films were formed using UDL-1 to UDL-17 of the present invention, had no substrate dependence and could form uniform organic films without coating abnormalities. In Comparative Example 7-1, since a monomolecular compound was used, aggregation was easily caused depending on the substrate, and a large number of pinhole-shaped coating defects, which were considered as shrinkage cavities, were observed. By using an organic film-forming composition containing a polymer of the present invention, a uniform coating film could be formed without substrate dependence.

[0401] As described above, the organic film-forming composition of the present invention has high etching resistance and excellent distortion resistance during etching, and is extremely effective as an organic film for a multilayer resist process, especially a three-layer resist process, for ultrafine and high-precision pattern processing.

[0402] The present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and achieving the same functions and effects as the technical concept described in the claims of the present invention are all included in the technical scope of the present invention.

[0403] Description of Reference Numerals

[0404] 1:Substrate

[0405] 2: Processing layer

[0406] 2a: Pattern formed on substrate

[0407] 3: Organic film

[0408] 3a: Organic film pattern

[0409] 4: Silicon-containing resist lower layer film

[0410] 4a: Silicon-containing resist lower film pattern

[0411] 5: Resist upper film

[0412] 5a: Resist pattern

[0413] 6: Parts used

Claims

1. A composition for forming an organic film, characterized in that it contains: A polymer having a partial structure represented by the following general formula (1A) as a repeating unit, and Organic solvents; In the general formula (1A), AR1 and AR2 are benzene rings or naphthalene rings which may have a substituent, R is a hydrogen atom or a monovalent organic group having an unsaturated bond and having 2 to 10 carbon atoms, R' is a single bond or W1, and W1 is a divalent organic group having 6 to 80 carbon atoms and having one or more aromatic rings.

2. The composition for forming an organic film according to claim 1, wherein The general formula (1A) is represented by the following general formula (1B); In the general formula (1B), AR1, AR2, R and W1 are the same as those described in claim 1.

3. The composition for forming an organic film according to claim 1 or 2, wherein R in the general formula (1A) and (1B) is a hydrogen atom or any one of the structures represented by the following formula (1C); 4. The composition for forming an organic film according to claim 1 or 2, wherein The divalent organic group represented by W1 has at least one of a naphthalene ring, a fluorene ring, and a carbazole ring.

5. The composition for forming an organic film according to claim 1 or 2, wherein The weight average molecular weight of the polymer is 1000-5000.

6. The composition for forming an organic film according to claim 1 or 2, wherein The organic solvent is a mixture of one or more organic solvents having a boiling point lower than 180 degrees and one or more organic solvents having a boiling point higher than 180 degrees.

7. The composition for forming an organic film according to claim 1 or 2, wherein The organic film-forming composition further contains one or more of a surfactant and a plasticizer.

8. A method for forming a pattern, comprising the following steps: An organic film is formed on a workpiece using the organic film-forming composition according to any one of claims 1 to 7, forming a resist underlayer film containing silicon on the organic film using a resist underlayer film material containing silicon, forming a resist upper film on the silicon-containing resist lower film using a photoresist composition, forming a circuit pattern on the resist upper film, The resist upper layer film having the circuit pattern formed thereon is used as a mask and the pattern of the resist lower layer film containing silicon is transferred by etching. The pattern of the organic film is transferred by etching using the silicon-containing resist underlayer film having the transferred pattern as a mask, and The pattern is formed on the object to be processed by etching using the organic film to which the pattern is transferred as a mask.

9. A method for forming a pattern, comprising the following steps: An organic film is formed on a workpiece using the organic film-forming composition according to any one of claims 1 to 7, forming a resist underlayer film containing silicon on the organic film using a resist underlayer film material containing silicon, forming an organic anti-reflective film on the silicon-containing resist underlayer film, A photoresist composition is used on the organic anti-reflective film to form a resist upper film. forming a circuit pattern on the resist upper film, The resist upper layer film having the circuit pattern formed thereon is used as a mask and the organic anti-reflection film and the silicon-containing resist lower layer film are pattern-transferred by etching in sequence. The pattern of the organic film is transferred by etching using the silicon-containing resist underlayer film having the transferred pattern as a mask, and The object to be processed is etched using the organic film to which the pattern is transferred as a mask, thereby forming a pattern on the object to be processed.

10. A pattern forming method, characterized by comprising the following steps: An organic film is formed on a workpiece using the organic film-forming composition according to any one of claims 1 to 7, forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film on the organic film, forming a resist upper film on the inorganic hard mask using a photoresist composition, forming a circuit pattern on the resist upper film, The resist upper layer film having the circuit pattern formed thereon is used as a mask and the inorganic hard mask is pattern-transferred by etching. The inorganic hard mask having the pattern is used as a mask and the pattern is transferred to the organic film by etching, and The object to be processed is etched using the patterned organic film as a mask to form a pattern on the object to be processed.

11. A method for forming a pattern, comprising the following steps: An organic film is formed on a workpiece using the organic film-forming composition according to any one of claims 1 to 7, forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film on the organic film, forming an organic anti-reflection film on the inorganic hard mask, A photoresist composition is used on the organic anti-reflective film to form a resist upper film. forming a circuit pattern on the resist upper film, The resist upper layer film having the circuit pattern formed thereon is used as a mask and the organic anti-reflection film and the inorganic hard mask are sequentially pattern-transferred by etching, The inorganic hard mask having the pattern is used as a mask and the pattern is transferred to the organic film by etching, and The object to be processed is etched using the patterned organic film as a mask to form a pattern on the object to be processed.

12. The pattern forming method according to claim 10 or 11, wherein: The inorganic hard mask is formed by a CVD method or an ALD method.

13. The pattern forming method according to any one of claims 8 to 11, wherein: The method of forming the circuit pattern on the resist upper layer film uses optical lithography with a wavelength of 10 nm to 300 nm, direct writing by electron beam, nanoimprinting, or a combination thereof.

14. The pattern forming method according to any one of claims 8 to 11, wherein: As the developing method, alkali development or development using an organic solvent is used.

15. The pattern forming method according to any one of claims 8 to 11, wherein: The object to be processed is a semiconductor device substrate, a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film or a metal oxide nitride film.

16. The pattern forming method according to claim 15, wherein: The metal used is silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, cobalt, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, molybdenum, ruthenium, or an alloy thereof.

17. A polymer having a partial structure represented by the following general formula (1A) as a repeating unit; In the general formula (1A), AR1 and AR2 are benzene rings or naphthalene rings which may have a substituent, R is a hydrogen atom or a monovalent organic group having an unsaturated bond and having 2 to 10 carbon atoms, R' is a single bond or W1, and W1 is a divalent organic group having 6 to 80 carbon atoms and having one or more aromatic rings.

18. The polymer according to claim 17, wherein The general formula (1A) is represented by the following general formula (1B); In the general formula (1B), AR1, AR2, R and W1 are the same as those described in claim 17.

19. The polymer according to claim 17 or 18, wherein In the general formula (1A) and (1B), R is a hydrogen atom or any one of the structures represented by the following formula (1C); 20. The polymer according to claim 17 or 18, wherein The divalent organic group represented by W1 has at least one of a naphthalene ring, a fluorene ring, and a carbazole ring.