Laminated ceramic electronic component and method for producing the same
By forming a specific side edge structure on the inner electrode side of the laminated ceramic capacitor, the specific bending conditions are met, and the problem of insufficient moisture resistance in the prior art is solved, and a high reliability and small large capacitance is realized.
Patent Information
- Application Number
- CN202010668165.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-04-23
- Filing Date
- 2020-07-13
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-07-13
AI Technical Summary
The conventional laminated ceramic capacitors are difficult to improve moisture resistance after the side edges become thinner, resulting in insufficient reliability.
By forming a side edge portion of a specific structure on the side surface of the internal electrode, the corner portion is ensured to meet the conditions of a≥1 μm and 0.1≤a/b≤0.4, and the corner portion is bent, thereby suppressing moisture resistance deterioration and short circuit.
It realizes sufficient moisture resistance and high reliability when the side edge portion is thinned, ensuring moisture resistance and short circuit prevention of stacked ceramic electronic components.
Smart Images

Figure CN112242245B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a laminated ceramic electronic component such as a laminated ceramic capacitor and a method for manufacturing the same. Background Art
[0002] In recent years, as electronic devices have become smaller and more powerful, there has been a growing desire for smaller and larger capacitors for use in electronic devices. To meet this expectation, it is effective to enlarge the internal electrodes of the multilayer ceramic capacitors. To enlarge the internal electrodes, it is necessary to thin the side edges that ensure insulation around the internal electrodes.
[0003] Patent Document 1 discloses a technique of later adding side margins from the viewpoint of achieving a thinner side margin. In this technique, a ceramic protective layer (side margin) is provided on the side surface of a green sheet in a state where internal electrodes are exposed on the side surface.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2012-209539 Summary of the invention
[0007] Technical problem to be solved by the invention
[0008] However, in the technology described in Patent Document 1, when the side edge portion is thinned, sufficient moisture resistance cannot be obtained, and it is difficult to improve reliability.
[0009] In view of the above circumstances, an object of the present invention is to provide a multilayer ceramic electronic component capable of improving reliability and a method for manufacturing the same.
[0010] Technical solutions for solving technical problems
[0011] In order to achieve the above object, one embodiment of the present invention provides a multilayer ceramic electronic component including a functional portion, a cover portion, and a side edge portion.
[0012] The functional portion includes internal electrodes stacked in a first direction.
[0013] The covering portion covers the functional portion from the first direction.
[0014] The side edge portion covers the functional portion from a second direction perpendicular to the first direction.
[0015] The functional portion has, in a cross section perpendicular to the third direction which divides the functional portion into two equal parts, a first straight line portion adjacent to the covering portion and extending in the second direction; a second straight line portion adjacent to the side edge portion and extending in the first direction; and a corner portion connected to the first straight line portion and the second straight line portion.
[0016] In the above-mentioned corner portion, when the distance along the first direction between a first imaginary line formed by extending the above-mentioned first straight line portion in the above-mentioned second direction and the endpoint on the above-mentioned first imaginary line side of the above-mentioned second straight line portion is set to a, and the distance along the second direction between a second imaginary line formed by extending the above-mentioned second straight line portion in the above-mentioned first direction and the endpoint on the above-mentioned second imaginary line side of the above-mentioned first straight line portion is set to b, the above-mentioned corner portion is bent in a manner that satisfies the conditions of a≥1μm and 0.1≤a / b≤0.4.
[0017] In this structure, the functional portion has a corner portion that is bent in a manner of a ≥ 1 μm and 0.1 ≤ a / b ≤ 0.4. By making the corner portion satisfy the conditions of a ≥ 1 μm and a / b ≥ 0.1, the distance from the surface of the laminated ceramic electronic component to the end of the outermost internal electrode can be fully ensured, and the moisture resistance degradation can be suppressed. Moreover, by making the corner portion satisfy the condition of a / b ≤ 0.4, the outermost internal electrode can be prevented from bending sharply. Thus, the short circuit between adjacent internal electrodes in the first direction can be suppressed. Therefore, according to the above structure, the moisture resistance degradation and short circuit failure can be suppressed, and a laminated ceramic electronic component with high reliability can be obtained.
[0018] The side edge portion may have a thickness of 10 μm or more and 15 μm or less.
[0019] The side edge portion may have a thickness of 12 μm or less.
[0020] Thus, even when the thickness of the side edge portion is extremely thin, sufficient moisture resistance can be ensured, so that a compact, high-capacitance, and highly reliable laminated ceramic electronic component can be obtained.
[0021] The corner portion may be curved inward in the first direction as it moves from the end point on the second imaginary line side of the first straight line portion toward the end point on the first imaginary line side of the second straight line portion.
[0022] Specifically, the functional portion may have the four corner portions in the cross section.
[0023] Another method of manufacturing a laminated ceramic electronic component of the present invention includes the following steps: a step of manufacturing a laminated sheet by laminating a third ceramic sheet without an internal electrode in the first direction on the first direction outer surface of a laminated body formed by alternately laminating a first ceramic sheet and a second ceramic sheet in the first direction, wherein the first ceramic sheet and the second ceramic sheet are respectively formed with a plurality of internal electrodes.
[0024] A step of pressure-bonding the laminated sheets from the first direction.
[0025] A process for making a stacked chip by cutting the stacked sheet, wherein the stacked chip comprises: a functional portion having internal electrodes stacked in the first direction; a covering portion covering the functional portion from the first direction; and a side surface on which the internal electrodes are exposed and facing a second direction orthogonal to the first direction.
[0026] A step of forming side edge portions on the side surfaces.
[0027] A step of forming a fired functional portion by firing the stacked chip having the side edge portion formed thereon.
[0028] The fired functional portion has, in a cross section perpendicular to the third direction which divides the fired functional portion into two equal parts, a first straight line portion adjacent to the covering portion and extending in the second direction; a second straight line portion adjacent to the side edge portion and extending in the first direction; and a corner portion connected to the first straight line portion and the second straight line portion.
[0029] In the above-mentioned corner portion, when the distance along the first direction between a first imaginary line formed by extending the above-mentioned first straight line portion in the above-mentioned second direction and the endpoint on the above-mentioned first imaginary line side of the above-mentioned second straight line portion is set to a, and the distance along the second direction between a second imaginary line formed by extending the above-mentioned second straight line portion in the above-mentioned first direction and the endpoint on the above-mentioned second imaginary line side of the above-mentioned first straight line portion is set to b, the above-mentioned corner portion is bent in a manner that satisfies the conditions of a≥1μm and 0.1≤a / b≤0.4.
[0030] Furthermore, in the first ceramic sheet and the second ceramic sheet, the plurality of internal electrodes are arranged at intervals from each other in the second direction with the non-electrode forming region interposed therebetween.
[0031] In the process of crimping from the first direction, the following are formed on the laminated sheet: a functional area where the plurality of internal electrodes are stacked in the first direction; and a cut-off area where the non-electrode forming area is stacked, which is configured to be adjacent to the functional area in the second direction, and the thickness in the first direction gradually decreases as it moves away from the functional area in the second direction.
[0032] In the step of cutting the laminated sheet, the cut-out region is cut out.
[0033] In the region of the functional region adjacent to the cutout region, the internal electrode is bent inward in the first direction by crimping. Thus, a corner portion bent so as to satisfy the above-mentioned conditions can be formed.
[0034] Effects of the Invention
[0035] As described above, according to the present invention, a multilayer ceramic electronic component capable of improving reliability and a method for manufacturing the same can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a perspective view of a multilayer ceramic capacitor according to one embodiment of the present invention.
[0037] Figure 2 1 is a cross-sectional view taken along line AA′ of the multilayer ceramic capacitor.
[0038] Figure 3 BB' is a cross-sectional view of the multilayer ceramic capacitor.
[0039] Figure 4 : is a flowchart showing a method for manufacturing the above-mentioned multilayer ceramic capacitor.
[0040] Figure 5 It is a top view showing the manufacturing process of the above-mentioned laminated ceramic capacitor.
[0041] Figure 6 It is a perspective view showing the manufacturing process of the above-mentioned multilayer ceramic capacitor.
[0042] Figure 7 It is a cross-sectional view showing the manufacturing process of the above-mentioned laminated ceramic capacitor.
[0043] Figure 8 It is a perspective view showing the manufacturing process of the above-mentioned multilayer ceramic capacitor.
[0044] Fig. 9 It is a perspective view showing the manufacturing process of the above-mentioned multilayer ceramic capacitor.
[0045] Fig.10 Yes Figure 3 An enlarged cross-sectional view of a portion of the
[0046] Fig.11 In the drawings, (A) is a diagram schematically showing a cross section of the multilayer ceramic capacitor taken along line BB′, and (B) is a diagram schematically showing the same cross section of a multilayer ceramic capacitor according to a comparative example of the embodiment.
[0047] Fig.12 It is a cross-sectional view showing the manufacturing process of the above-mentioned laminated ceramic capacitor.
[0048] Description of Reference Numerals
[0049] 10……Multilayer ceramic capacitors (Multilayer ceramic electronic components)
[0050] 12, 13...Internal electrodes
[0051] 17...Side edge
[0052] 18: Capacitor forming part (functional part)
[0053] 19……Covering
[0054] 181……First straight line
[0055] 182...Second straight line
[0056] 183……corner part DETAILED DESCRIPTION
[0057] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings.
[0058] In the drawings, an X-axis, a Y-axis, and a Z-axis orthogonal to each other are appropriately shown. The X-axis, the Y-axis, and the Z-axis are common to all the drawings.
[0059] 1. Structure of the Multilayer Ceramic Capacitor 10
[0060] Figures 1 to 3 FIG. 1 is a diagram showing a multilayer ceramic capacitor 10 according to an embodiment of the present invention. Figure 1 It is a perspective view of the multilayer ceramic capacitor 10 . Figure 2 The multilayer ceramic capacitor 10 is Figure 1 Cross-sectional view along line A-A'. Figure 3 The multilayer ceramic capacitor 10 is Figure 1 Cross-sectional view of line BB'.
[0061] The multilayer ceramic capacitor 10 includes a ceramic body 11, a first external electrode 14, and a second external electrode 15. Typically, the ceramic body 11 has two main surfaces facing the Z-axis direction, two end surfaces facing the X-axis direction, and two side surfaces facing the Y-axis direction. For example, the edge 11d connecting the surfaces of the ceramic body 11 has rounded corners. The dimensions (length) in the X-axis direction, the dimensions (width) in the Y-axis direction, and the dimensions (height) in the Z-axis direction of the multilayer ceramic capacitor 10 are, for example, 0.25 mm in length, 0.125 mm in width, and 0.125 mm in height, or 0.4 mm in length, 0.2 mm in width, and 0.2 mm in height, or 0.6 mm in length, 0.3 mm in width, and 0.3 mm in height, or 1.0 mm in length, 0.5 mm in width, and 0.5 mm in height, or 1.6 mm in length, 0.8 mm in width, and 0.8 mm in height. In addition, the dimension of the multilayer ceramic capacitor 10 in the X-axis direction is the dimension of the largest portion in the X-axis direction, the dimension of the multilayer ceramic capacitor 10 in the Y-axis direction is the dimension of the largest portion in the Y-axis direction, and the dimension of the multilayer ceramic capacitor 10 in the Z-axis direction is the dimension of the largest portion in the Z-axis direction. In addition, each dimension includes a tolerance of up to 10% of each dimension on the positive side and the negative side.
[0062] The external electrodes 14 and 15 cover the end faces of the ceramic body 11 and are opposed to each other in the X-axis direction across the ceramic body 11. The external electrodes 14 and 15 extend from the end faces of the ceramic body 11 to the main face and the side faces. Thus, the cross-sections of the external electrodes 14 and 15 parallel to the XZ plane and the cross-sections parallel to the XY plane are both formed into a U shape. In addition, the shapes of the external electrodes 14 and 15 are not limited to Figure 1 Shape shown.
[0063] The external electrodes 14 and 15 are formed of a good electrical conductor. Examples of the good electrical conductor forming the external electrodes 14 and 15 include metals or alloys mainly composed of copper (Cu), nickel (Ni), tin (Sn), palladium (Pd), platinum (Pt), silver (Ag), gold (Au), etc.
[0064] The ceramic body 11 has a laminate 16 and side edge portions 17. The laminate 16 has two end surfaces 16a facing the X-axis direction, two side surfaces 16b facing the Y-axis direction, and two main surfaces 16c facing the Z-axis direction.
[0065] The side edge portion 17 covers the two side surfaces 16b of the stack 16 respectively, and covers the capacitor forming portion 18 from the Y-axis direction. The thickness dimension of the side edge portion 17 in the Y-axis direction can be, for example, less than 15 μm, and more preferably less than 12 μm. Thus, the miniaturization and high capacitance of the stacked ceramic capacitor 10 can be achieved. In addition, the thickness dimension of the side edge portion 17 in the Y-axis direction can be, for example, more than 10 μm. Thus, the moisture resistance of the stacked ceramic capacitor 10 can be ensured. In addition, the thickness dimension of the side edge portion 17 in the Y-axis direction is the maximum dimension in the Y-axis direction from the side of the ceramic body 11 facing the Y-axis direction to the side 16b of the stack 16.
[0066] The laminate 16 includes a capacitance forming portion 18 and a covering portion 19 covering the capacitance forming portion 18 in the Z-axis direction. The capacitance forming portion 18 includes a first internal electrode 12 and a second internal electrode 13 stacked in the Z-axis direction with ceramic layers interposed therebetween. The capacitance forming portion 18 constitutes a functional portion of the present embodiment.
[0067] The internal electrodes 12 and 13 are each formed into a sheet extending along the XY plane. The first internal electrode 12 extends to one end face 16a along the X-axis direction and is connected to the first external electrode 14. The second internal electrode 13 extends to the other end face 16a along the X-axis direction and is connected to the second external electrode 15. Thus, when a voltage is applied between the first external electrode 14 and the second external electrode 15, a voltage is applied to the ceramic layer between the first internal electrode 12 and the second internal electrode 13, and a charge corresponding to the voltage can be stored in the capacitor forming portion 18.
[0068] The internal electrodes 12 and 13 are formed of a good electrical conductor. Typical examples of good electrical conductors forming the internal electrodes 12 and 13 include nickel (Ni), and other metals or alloys mainly composed of copper (Cu), palladium (Pd), platinum (Pt), silver (Ag), gold (Au), etc.
[0069] In the ceramic body 11, a dielectric ceramic with a high dielectric constant is used to increase the capacitance of each ceramic layer between the internal electrodes 12 and 13. Examples of the dielectric ceramic with a high dielectric constant include barium titanate (BaTiO 3 ) is a material with a perovskite structure containing barium (Ba) and titanium (Ti).
[0070] In addition, the ceramic layer can also be made of strontium titanate (SrTiO 3 ) type, calcium titanate (CaTiO 3 ) type, magnesium titanate (MgTiO 3 ) type, calcium zirconate (CaZrO 3 ) type, calcium zirconium titanate (Ca(Zr,Ti)O 3 ) type, barium zirconate (BaZrO3 ) type, titanium oxide (TiO 2 ) category, etc.
[0071] Cover 19 and side edge 17 are made of insulating ceramics, but may also include, for example, dielectric ceramics used in capacitor forming portion 18. This can suppress internal stress that may be generated between cover 19 and side edge 17 and capacitor forming portion 18.
[0072] The internal electrodes 12 and 13 are formed over the entire width of the capacitance forming portion 18 in the Y-axis direction, and the peripheral portions 12b and 13b in the Y-axis direction are arranged on both side surfaces 16b of the stacked body 16. In the present embodiment, the peripheral portions 12b and 13b of the internal electrodes 12 and 13 have a shape that is bent inward in the Z-axis direction. The peripheral portions 12b and 13b of the internal electrodes 12 and 13 have a tendency to bend more inward in the Z-axis direction as they are arranged outward in the Z-axis direction. The details of this curved shape will be described later.
[0073] Furthermore, “inward in the Z-axis direction” refers to a direction closer to an imaginary plane that bisects the multilayer ceramic capacitor 10 in the Z-axis direction, and “outward in the Z-axis direction” refers to a direction farther from the imaginary plane.
[0074] The multilayer ceramic capacitor 10 having the peripheral edge portions 12 b and 13 b of the curved internal electrodes 12 and 13 can be manufactured by, for example, the following manufacturing method.
[0075] 2. Method for Manufacturing Multilayer Ceramic Capacitor 10
[0076] Figure 4 1 is a flowchart showing a method for manufacturing the multilayer ceramic capacitor 10 . Figures 5 to 9 FIG. 1 is a diagram schematically showing a manufacturing process of a laminated ceramic capacitor 10. Figure 4 , with appropriate reference to Figures 5 to 9 , a method for manufacturing the multilayer ceramic capacitor 10 will be described.
[0077] 2.1 Step S01: Laminating ceramic sheets
[0078] In step S01 , the first ceramic sheet 101 and the second ceramic sheet 102 for forming the capacitance forming portion 18 and the third ceramic sheet 103 for forming the cover portion 19 are prepared and stacked.
[0079] Ceramic sheets 101, 102, 103 are formed as unfired dielectric green sheets mainly composed of dielectric ceramics. Ceramic sheets 101, 102, 103 are formed into sheets using, for example, a roll coater or a doctor blade. The thickness of ceramic sheets 101, 102, 103 can be adjusted appropriately.
[0080] Figure 5 1 is a plan view of the ceramic sheets 101 and 102. At this stage, the ceramic sheets 101 and 102 are constituted as large sheets that have not been separated into individual pieces. Figure 5 , the cutting lines Lx1, Lx2, Ly1, and Ly2 are shown when each of the multilayer ceramic capacitors 10 is singulated. The cutting lines Lx1 and Lx2 are parallel to the X axis, and the cutting lines Ly1 and Ly2 are parallel to the Y axis. In addition, the middle line Lc is an imaginary line extending from a position that divides the adjacent cutting lines Lx1 and Lx2 into two equal parts.
[0081] like Figure 5 As shown, an unfired first internal electrode 112 corresponding to the first internal electrode 12 is formed on the first ceramic sheet 101, and an unfired second internal electrode 113 corresponding to the second internal electrode 13 is formed on the second ceramic sheet 102. Figure 5 Although not shown in the figure, no internal electrode is formed on the third ceramic sheet 103 corresponding to the cover portion 19 .
[0082] Internal electrodes 112 and 113 can be formed by applying any conductive paste to ceramic sheets 101 and 102. The method for applying the conductive paste can be arbitrarily selected from known techniques. For example, screen printing or gravure printing can be used for applying the conductive paste.
[0083] In the first ceramic sheet 101, the first column of internal electrodes 112 extending across the cutting line Ly1 and arranged in the X-axis direction and the second column of internal electrodes 112 extending across the cutting line Ly2 and arranged in the X-axis direction are arranged alternately in the Y-axis direction. In the first column, the internal electrodes 112 adjacent in the X-axis direction are opposed to each other across the cutting line Ly2. In the second column, the internal electrodes 112 adjacent in the X-axis direction are opposed to each other across the cutting line Ly1. That is, in the first and second columns adjacent in the Y-axis direction, the internal electrodes 112 are arranged one chip apart in the X-axis direction. The first internal electrodes 112 are arranged across the center line Lc in the Y-axis direction. The outer edges of the first internal electrodes 112 in the Y-axis direction extend along the cutting lines Lx1 and Lx2.
[0084] The internal electrode 113 on the second ceramic sheet 102 is also constructed in the same manner as the internal electrode 112. In the second ceramic sheet 102, the internal electrode 113 of the column corresponding to the first column of the first ceramic sheet 101 extends across the cutting line Ly2, and the internal electrode 113 of the column corresponding to the second column of the first ceramic sheet 101 extends across the cutting line Ly1. In other words, the internal electrode 113 is formed in a manner that is offset from the internal electrode 112 by one chip in the X-axis direction and the Y-axis direction. The second internal electrodes 113 are arranged in the Y-axis direction with the center line Lc between them. The outer edges of the second internal electrodes 113 in the Y-axis direction extend along the cutting lines Lx1 and Lx2.
[0085] In the first ceramic sheet 101, the non-electrode forming region N1 to which the internal electrode 112 is not applied is formed in a lattice shape on the middle line Lc and the cutting line Ly2. Similarly, in the second ceramic sheet 102, the non-electrode forming region N2 to which the internal electrode 113 is not applied is formed in a lattice shape on the middle line Lc and the cutting line Ly1. That is, on the middle line Lc between the cutting lines Lx1 and Lx2, the non-electrode forming regions N1 and N2 overlap.
[0086] These ceramic sheets 101, 102, 103 are as follows Figure 6 Specifically, the first ceramic sheet 101 and the second ceramic sheet 102 are alternately stacked, and the third ceramic sheet 103 is stacked on the upper and lower surfaces of the stacked body of the ceramic sheets 101 and 102 in the Z-axis direction. Figure 6 In the example shown, four third ceramic sheets 103 are stacked, but the number of third ceramic sheets 103 can be changed as appropriate.
[0087] 2.2 Step S02: Crimping
[0088] In step S02 , the laminated sheets 104 are pressed together in the Z-axis direction.
[0089] Figure 7 It is a schematic cross-sectional view of the laminated sheet 104 viewed from the X-axis direction for explaining the pressure-bonding process of step S02 .
[0090] In the pressure bonding process of this step, a pair of pressure plates S1 are opposed to each other in the Z-axis direction with the laminated sheet 104 interposed therebetween, and the pressure plates S1 are pressed against the laminated sheet 104 to thereby pressure bond the laminated sheet 104. The pressure plates S1 are pressed by, for example, hydrostatic pressure or uniaxial pressure.
[0091] In addition, an elastic sheet S2 is disposed between the pressurizing plate S1 and the laminated sheet 104. The elastic sheet S2 is made of a sheet-shaped elastic body, and is formed of, for example, polyethylene terephthalate (PET) resin. The elastic sheet S2 presses the laminated sheet 104 through the pressurizing plate S1.
[0092] In the laminated sheet 104, a capacitor forming region (functional region) 105 on which the internal electrodes 112 and 113 are stacked, and a cut-out region 106 on which the non-electrode forming regions N1 and N2 are stacked are formed. The capacitor forming region 105 corresponds to the capacitor forming portion 18 and the covering portion 19 covering the upper and lower portions thereof. The cut-out region 106 is a region adjacent to the capacitor forming region 105 in the Y-axis direction and on which the internal electrodes 112 and 113 are not stacked. That is, the cut-out region 106 is a region sandwiched by the cutting lines Lx1 and Lx2, and is cut out in the cutting process described later.
[0093] By providing the elastic sheet S2 and pressurizing the laminated sheet 104, as described below, the cutout region 106 having a shape sunken inward in the Z-axis direction can be formed.
[0094] like Fig.12 As shown, the elastic sheet S2 is formed into a region S21 having a crimped capacitor forming region 105 and a region S22 crimped to a cut-off region 106, and the region S22 is thicker in the Z-axis direction than the region S21. The surface of the region S22 opposite to the laminated sheet 104 protrudes in the Z-axis direction from the surface of the region S21 opposite to the laminated sheet 104. The cross-section on the YZ plane of the protruding portion of the region S22 is configured to be roughly rectangular. For example, a height difference is formed between the region S22 and the region S21. The difference (size) in thickness in the Z-axis direction between the region S22 and the region S21 is set to z. The region S22 is configured in a manner opposite to the center of the cut-off region 106 in the Y-axis direction. The size of the region S22 in the Y-axis direction is set to y. In the capacitor forming region 105, ceramic sheets 101 and 102 with internal electrodes 112 and 113 are stacked without gaps. Thus, the capacitance forming region 105 is extended as a whole on the XY plane and is compressed substantially uniformly by the compression bonding process. As a result, a substantially flat surface is formed on the capacitance forming region 105 .
[0095] On the other hand, a gap corresponding to the non-electrode forming regions N1 and N2 is formed in the cutout region 106 before pressurization. In addition, the green sheet is softer and easier to stretch than the internal electrodes 112 and 113. Therefore, by pressurization, the green sheet extending from the capacitor forming region 105 enters the gap.
[0096] In addition, the elastic sheet S2 is configured with a region S22 that is thicker than the region S21 in a manner opposite to the central portion of the cut-out region 106 in the Y-axis direction, and a greater load can be applied to the thinner cut-out region 106 through elastic deformation. Thus, in the cut-out region 106, the raw sheet extending from the capacitor forming region 105 and the raw sheet stacked before pressurization extend in the XY plane and are crimped in the Z-axis direction. Therefore, in the cut-out region 106, the thickness between the internal electrodes 12 and 13 gradually becomes thinner as the cutting lines Lx1 and Lx2 on the side of the capacitor forming region 105 go to the middle line Lc. In other words, the cut-out region 106 is configured so that the thickness in the Z-axis direction gradually decreases as it leaves the capacitor forming region 105 in the Y-axis direction. As a result, the cut-out region 106 is formed in a manner that is significantly sunk inward in the Z-axis direction near the middle line Lc.
[0097] As the cut-out region 106 sinks, the peripheral portions 112b and 113b of the internal electrodes 112 and 113 adjacent to the cut-out region 106 also bend inwardly in the Z-axis direction. In more detail, the peripheral portions 112b and 113b are bent by the force inwardly in the Z-axis direction received by the elastic sheet S2 invading the cut-out region 106. In addition, the peripheral portions 112b and 113b can also be subjected to the force inwardly in the Z-axis direction through the stack of ceramic sheets 103 extending from the central portion side of the capacitor forming region 105. As a result, curved peripheral portions 112b and 113b are formed in the internal electrodes 112 and 113. The more the internal electrodes 112 and 113 are located on the outside in the Z-axis direction, the more easily they are subjected to the force inwardly in the Z-axis direction, and therefore, they are bent more severely than on the inside in the Z-axis direction.
[0098] 2.3 Step S03: Cutting
[0099] In step S03, the laminated sheet 104 crimped in step S02 is cut along the cutting lines Lx1, Lx2, Ly1, and Ly2 to produce Figure 8 The unfired laminated chip 116 is shown. The laminated chip 116 corresponds to the fired laminated body 16. In the cutting of the laminated sheet 104 in this step, for example, a press cutter or a rotary blade can be used.
[0100] In addition, Figures 8-9 In FIG. 1 , the region outside the peripheral portions 112 b and 113 b on the main surface facing the Z-axis direction is described as being substantially flat. However, in reality, this region is curved inward in the Z-axis direction similarly to the peripheral portions 112 b and 113 b.
[0101] When the cutting lines Lx1 and Lx2 are cut by a press cutter, the width of the cutter is relatively narrow, so the cutter can be cut by making the cutter contact with the cut lines Lx1 and Lx2. Thus, by cutting the laminated sheet 104 along the cut lines Lx1 and Lx2 and removing the cut-off area 106 between the cut lines Lx1 and Lx2, each laminated chip 116 can be formed.
[0102] When the rotary blade cuts along the dicing lines Lx1 and Lx2, the blade is relatively wide, so the blade is brought into contact with the entire cutout region 106 including the dicing lines Lx1 and Lx2. Thus, the cutout region 106 is cut out by the rotary blade, and each stacked chip 116 can be formed.
[0103] like Figure 8 As shown, in the stacked chip 116, the side surface 116b is formed as a cut surface corresponding to the cutting lines Lx1 and Lx2. The peripheral portions 112b and 113b of the internal electrodes 112 and 113 are exposed from the side surface 116b. The peripheral portions 112b and 113b are bent inward in the Z-axis direction as they approach the side surface 116b. On the other hand, in the stacked chip 116, the end surface 116a is formed as a cut surface corresponding to the cutting lines Ly1 and Ly2. One of the internal electrodes 112 and 113 is exposed from the end surface 116a.
[0104] In more detail, the stacked chip 116 includes: an unfired capacitor forming portion 118 corresponding to the capacitor forming portion 18; and an unfired covering portion 119 corresponding to the covering portion 19. In the capacitor forming portion 118, the internal electrodes 112 and 113 are alternately stacked between the green sheets corresponding to the ceramic layers. Regarding the capacitor forming portion 118, the peripheral portions 112b and 113b of the internal electrodes 112 and 113 are curved, so that in the cross section of the capacitor forming portion 118 viewed from the X-axis direction, it is formed of a rectangular shape with rounded corners.
[0105] 2.4 Step S04: Side edge formation
[0106] In step S04, an unfired side edge portion 117 is formed on the side surface 116b where the internal electrodes 112 and 113 of the laminated chip 116 obtained in step S03 are exposed. Fig. 9 An unfired ceramic body 111 is shown.
[0107] The side edge portion 117 includes an unfired ceramic material, specifically, is formed of a ceramic sheet or a ceramic slurry. The side edge portion 117 can be formed, for example, by attaching a ceramic sheet to the side surface 116b of the stacked chip 116. In addition, the side edge portion 117 can also be formed by applying a ceramic paste to the side surface 116b of the stacked chip 116, for example, by coating or dipping.
[0108] 2.5 Step S05: Firing
[0109] In step S05, the unfired ceramic body 111 obtained in step S04 is fired. The firing temperature in step S05 can be determined based on the sintering temperature of the ceramic body 111. In addition, firing can be performed in a reducing atmosphere or a low oxygen partial pressure atmosphere, for example.
[0110] 2.6 Step S06: Drum grinding
[0111] In step S06, the fired ceramic body 111 is subjected to roller grinding. The roller grinding is performed by, for example, sealing a plurality of ceramic bodies 111 in a roller grinding container and rotating or vibrating the roller grinding container. Alternatively, a grinding medium or liquid may be sealed in the roller grinding container together with the plurality of ceramic bodies 111. Thus, the edge portions 11d connecting the surfaces of the ceramic body 111 are chamfered to produce a Figures 1 to 3 The ceramic body 11 is shown.
[0112] In addition, the barrel polishing of step S06 may be performed on the ceramic body 111 before firing. In other words, the barrel polishing of step S06 may be performed before the firing process of step S05.
[0113] 2.7 Step S07: Forming external electrodes
[0114] In step S07, external electrodes 14 and 15 are formed at both ends of the ceramic body 11 obtained in step S06 in the X-axis direction. The method for forming the external electrodes 14 and 15 in step S07 can be arbitrarily selected from known methods. Figures 1 to 3 A stacked ceramic capacitor 10 is shown.
[0115] In addition, a part of the process in the above-mentioned step S07 may be performed before step S05. For example, before step S05, unfired electrode materials may be applied to both end surfaces of the unfired ceramic body 111 in the X-axis direction, and in step S05, the unfired electrode materials may be fired at the same time as the unfired ceramic body 111 is fired to form the base layer of the external electrodes 14 and 15. In addition, unfired electrode materials may be applied to the ceramic body 111 that has been subjected to the binder removal process, and they may be fired at the same time.
[0116] In the above manner, the laminated ceramic capacitor 10 is manufactured. In this manufacturing method, the side edge portion 17 is added to the side surface 16b of the laminated body 16 where the internal electrodes 12 and 13 are exposed, so that the positions of the ends of the plurality of internal electrodes 12 and 13 in the ceramic body 11 in the Y-axis direction are aligned in the Z-axis direction with a deviation within 0.5 μm.
[0117] Furthermore, the fired internal electrodes 12 and 13 have curved peripheral portions 12b and 13b corresponding to the peripheral portions 112b and 113b. The peripheral portions 12b and 13b provide the capacitance forming portion 18 with a cross-sectional shape as described below.
[0118] 3. Detailed Structure of Capacitor Forming Section 18
[0119] The capacitor forming portion 18 is configured as a rectangular shape with rounded corners in a cross section (a cross section along line BB') perpendicular to the X-axis direction where the capacitor forming portion 18 is divided into two equal parts in the X-axis direction. Hereinafter, the cross section along line BB' is referred to as a "BB' cross section".
[0120] like Figure 3 As shown, the capacitor forming portion 18 has, in the above cross section, two first straight portions 181 adjacent to the covering portion 19 and extending in the Y-axis direction; two second straight portions 182 adjacent to the side edge portion 17 and extending in the Z-axis direction; and four corner portions 183 connected to the first straight portion 181 and the second straight portion 182. The two first straight portions 181 are opposite to each other in the Z-axis direction, and the two second straight portions 182 are opposite to each other in the Y-axis direction.
[0121] In the BB' cross section, the capacitor forming portion 18 is substantially line-symmetrical with respect to the Y-axis direction and the Z-axis direction. Figure 3 An enlarged cross-sectional view of Fig.10 , the structure of a corner portion 183 and the first straight portion 181 and the second straight portion 182 connected thereto are described in detail.
[0122] like Fig.10 As shown, the first straight portion 181 is a straight portion extending in the Y-axis direction and is composed of the outermost internal electrodes 12 and 13 in the Z-axis direction. In addition, the first straight portion 181 only needs to be substantially a straight line, and for example, it can also meander or bend in the Z-axis direction within a very small range within 1% of the height dimension of the ceramic body 11 in the Z-axis direction.
[0123] The outermost internal electrodes 12 and 13 are referred to as the outermost internal electrode E. The outermost internal electrode E includes: a flat portion E1 constituting the first straight portion 181; and a peripheral portion E2 located at the Y-axis peripheral edge of the flat portion E1 and curved inward from the flat portion E1 in the Z-axis direction. In addition, the flat portion E1 only needs to be substantially flat, and for example, may have projections and depressions in the Z-axis direction within a very small range within 1% of the height dimension of the ceramic body 11 in the Z-axis direction.
[0124] The end point P1 of the first straight portion 181 is located at the boundary between the flat portion E1 and the peripheral portion E2 .
[0125] The second straight line portion 182 is a straight line portion extending in the Z-axis direction and is formed by the side surface 16b of the stacked body 16. In addition, the second straight line portion 182 only needs to be substantially a straight line, and for example, it can meander or bend in the Y-axis direction within a very small range within 0.5% of the width dimension of the ceramic body 11 in the Y-axis direction.
[0126] The end point P2 of the second straight portion 182 is formed by a front end portion Ea2 of the peripheral edge portion E2 of the outermost internal electrode E in the Y-axis direction.
[0127] The corner portion 183 is a curved portion connecting the end point P1 of the first straight portion 181 and the end point P2 of the second straight portion 182. The corner portion 183 is formed by the peripheral edge portion E2 of the outermost internal electrode E. The corner portion 183 curves inward in the Z-axis direction as it moves from the end point P1 of the first straight portion 181 to the end point P2 of the second straight portion 182.
[0128] Furthermore, “inward in the Z-axis direction” refers to a direction closer to an imaginary plane that bisects the multilayer ceramic capacitor 10 in the Z-axis direction, and “outward in the Z-axis direction” refers to a direction farther from the imaginary plane.
[0129] The shape of corner 183 is defined by the following values of a and a / b. a is a value corresponding to the height dimension of corner 183 along the Z axis, and b is a value corresponding to the length dimension of corner 183 along the Y axis. Thus, a preferred shape of corner 183 can be specified.
[0130] More specifically, a is set to be the distance along the Z-axis direction between the first imaginary line L1 extended from the first straight portion 181 and the end point P2 on the first imaginary line L1 side of the second straight portion 182. The value of a can be controlled by the number of stacked ceramic sheets 101 and 102 or the thickness of the ceramic sheets 101 and 102. Alternatively, the value of a can also be controlled by the elastic modulus of the elastic sheet S2 or the load of the pressurizing plate S1 in the above-mentioned pressure bonding process of step S02.
[0131] b is defined as the distance along the Y-axis direction between the second imaginary line L2 formed by extending the second straight portion 182 and the end point P1 on the second imaginary line L2 side of the first straight portion 181. The value of b can be controlled by the number of stacked ceramic sheets 101 and 102 or the thickness of the ceramic sheets 101 and 102, and can also be controlled by the elastic modulus of the elastic sheet S2 or the load of the pressure plate S1 in the crimping process of step S02. In addition, for example, referring to Fig.12When the dimension y of the region S22 where the elastic sheet S2 is thickened in the region opposite to the cut-out region 106 is increased in the Y-axis direction, the b value can be increased; when the dimension y of the region S22 where the elastic sheet S2 is thickened is decreased in the Y-axis direction, the b value can be decreased. The dimension y is 15% or more and 95% or less of the dimension yw in the Y-axis direction of the cut-out region 106 and can be adjusted appropriately. In addition, when the thickness z of the region S22 where the elastic sheet S2 is thickened in the region opposite to the cut-out region 106 is increased in the Z-axis direction, the a value can be increased; when the thickness z of the region S22 where the elastic sheet S2 is thickened is decreased in the Z-axis direction, the a value can be decreased. The dimension z is 5% or more and 40% or less of the thickness of the laminated sheet 104 in the Z-axis direction before crimping and can be adjusted appropriately. In addition, when the ratio of the dimension z to the dimension y of the elastic sheet S2 is obtained, the a / b value can be increased when z / y is increased, and the a / b value can be decreased when z / y is decreased.
[0132] Corner portion 183 is curved so as to satisfy the conditions of a≧1 μm and 0.1≦a / b≦0.4.
[0133] Among the above conditions, by making the corner portion 183 satisfy a ≥ 1 μm and a / b ≥ 0.1, the peripheral edge portion E2 of the outermost internal electrode E can be sufficiently curved, and the moisture resistance can be improved as described below.
[0134] Fig.11 (A) is a diagram schematically showing a BB′ cross section of the ceramic body 11 of the present embodiment, in which a region occupied by the capacitance forming portion 18 is surrounded by a dotted line. Fig.11 (B) is a diagram schematically showing a BB′ cross section of the ceramic body 21 of a comparative example of the present embodiment, in which a region occupied by the capacitance forming portion 28 is surrounded by a dotted line.
[0135] In the ceramic bodies 11 and 21, typically, the edge portions 11d and 21d are chamfered from the viewpoint of preventing chipping, etc. Therefore, the edge portions 11d and 21d of the ceramic bodies 11 and 21 are formed to be rounded.
[0136] exist Fig.11 In the ceramic body 21 of the comparative example (B), the Y-axis direction peripheral portion of the internal electrode of the capacitor forming portion 28 has no rounded corners, so the cross-sectional shape of the capacitor forming portion 28 is substantially rectangular. In other words, the capacitor forming portion 28 includes a first straight portion 281 extending in the Y-axis direction, a second straight portion 282 extending in the Z-axis direction, and a corner portion 283 bent substantially at a right angle.
[0137] As a result, in the ceramic body 21, the distance from the rounded edge 21d on the surface to the corner 283 formed by the end of the outermost internal electrode is likely to be reduced. Therefore, in particular, when the side edge 27 is formed thin in the Y-axis direction, the distance between the edge 21d and the outermost internal electrode is reduced. Therefore, moisture easily enters from the vicinity of the edge 21d, and moisture resistance is reduced.
[0138] On the other hand, Fig.11 In the ceramic body 11 of the present embodiment (A), the capacitor forming portion 18 includes a corner portion 183 bent in a manner satisfying a ≥ 1 μm and a / b ≥ 0.1. Thus, the distance from the ridge portion 11 d of the ceramic body 11 to the peripheral edge portion E2 of the outermost internal electrode E can be sufficiently ensured. Therefore, the reduction in moisture resistance due to the thinning of the side edge portion 17 can be suppressed.
[0139] In addition, refer to Fig.10 By making the corner 183 satisfy a≥1μm, the distance from the main surface 16c to the front end Ea2 of the outermost internal electrode E can be sufficiently ensured. In the present embodiment, the side edge portion 17 is added later, so the boundary portion between the laminate 16 and the side edge portion 17 easily becomes a path for moisture to enter. On the other hand, in the present embodiment, the distance in the Z-axis direction from the boundary portion between the main surface 16c and the side edge portion 17 to the front end Ea2 can be increased according to the value of a. Therefore, by making the corner 183 satisfy a≥1μm, the above distance can be sufficiently ensured, and the moisture resistance to moisture entering from the main surface 16c side can also be improved.
[0140] In addition, by making the corner 183 satisfy the condition of a / b≤0.4, the peripheral portion E2 of the outermost internal electrode E can be prevented from being bent too sharply in the Z-axis direction. As described above, the peripheral portions 12b and 13b of the internal electrodes 12 and 13 tend to bend more sharply inward in the Z-axis direction as they are arranged on the outer side in the Z-axis direction. Therefore, when the outermost internal electrode E is bent sharply, there is a possibility that the peripheral portion E2 contacts with the adjacent peripheral portions 12b and 13b in the Z-axis direction and short-circuits. By making the corner 183 satisfy the condition of a / b≤0.4, the bending of the peripheral portion E2 can be appropriately alleviated, and a short circuit caused by the contact between the internal electrodes 12 and 13 can be prevented.
[0141] As described above, according to the multilayer ceramic capacitor 10 of the present embodiment, it is possible to improve moisture resistance and suppress short circuits between the internal electrodes 12 and 13 , thereby improving reliability.
[0142] Hereinafter, this embodiment will be further described by way of examples.
[0143] 4. Examples
[0144] As examples and comparative examples of this embodiment, samples of multilayer ceramic capacitors having capacitor-forming portions with various cross-sectional shapes were prepared, and the reliability was studied. In these samples, the dimension in the X-axis direction was 1.0 mm, and the dimensions in the Y-axis direction and the Z-axis direction were 0.5 mm. In addition, the thickness dimension in the Y-axis direction of the side edge portion was 10 μm.
[0145] Table 1 shows the values of a and b of the corners of the above-mentioned capacitor forming portion measured in the samples of the comparative examples of each embodiment volume of the stacked ceramic capacitor, and the value of a / b calculated based on these values. In addition, the values shown in Table 1 are the average values of 1000 samples in the comparative examples of each embodiment volume. Regarding the values of a and b of the corners, the capacitor forming portion of each sample is divided into two equal parts in the X-axis direction and the cross section along the BB' line is exposed by grinding, and the values are confirmed by scanning electron microscope (SEM) at 3000 to 30000 times.
[0146] Table 1
[0147]
[0148] a is a value corresponding to the height dimension of the corner along the Z-axis direction. Fig.10 As shown in FIG. 1 , a is set to be the distance along the Z-axis direction between the first imaginary line (L1) extended from the first straight line portion (181) and the end point (P2) on the first imaginary line (L1) side of the second straight line portion (182). The value of a is adjusted so as to become the value shown in Table 1 by adjusting the dimension z of the region S22 where the elastic sheet S22 is thickened.
[0149] b is a value corresponding to the length dimension of the corner along the Y-axis direction. Fig.10 As shown in FIG. 1 , b is set to be the distance along the Y-axis direction between the second imaginary line (L2) formed by extending the second straight line portion (182) and the end point (P1) on the second imaginary line (L2) side of the first straight line portion (181). The value of b is adjusted so as to obtain the value in Table 1 by adjusting the dimension y of the region S22 where the elastic sheet S2 is thickened.
[0150] As shown in Table 1, the corners of the samples of Examples 1 to 4 all satisfy the conditions of a ≥ 1 μm and 0.1 ≤ a / b ≤ 0.4.
[0151] On the other hand, in the sample of Comparative Example 1, a was 0.2 μm and a / b was 0.01, which did not satisfy the conditions of a ≥ 1 μm and a / b ≥ 0.1.
[0152] In addition, in the sample of Comparative Example 2, although a was 1 μm, a / b was 0.03, which did not satisfy the condition of a / b ≥ 0.1.
[0153] The a / b of the samples of Comparative Examples 3 to 8 were all 0.50 or more, and did not satisfy the condition of a / b ≤ 0.4.
[0154] The moisture resistance degradation rate was studied for 1,000 samples of each of Examples 1 to 4 and Comparative Examples 1 to 8. The moisture resistance degradation rate was calculated based on the ratio of the number of samples with an insulation resistance of less than 1 MΩ after applying a voltage twice the rated voltage for 100 hours at a temperature of 85°C and a humidity of 85%.
[0155] In Examples 1 to 4 and Comparative Examples 3 to 8, which satisfied the conditions of a ≥ 1 μm and a / b ≥ 0.1 at the corners, the moisture resistance degradation rate was 0.0%, and it was confirmed that all of them had sufficient moisture resistance.
[0156] On the other hand, in Comparative Example 1 in which a was 0.2 μm and a / b was 0.01, the moisture resistance degradation rate was confirmed to be 0.5%, and the moisture resistance was inferior to that of the Examples.
[0157] In Comparative Example 2 in which a was 1.0 μm and a / b was 0.03, the moisture resistance degradation rate was also confirmed to be 0.1%, and the moisture resistance was slightly inferior to that of the Examples.
[0158] Next, the short circuit failure rate of each sample was evaluated. The short circuit failure rate was evaluated using an LCR meter under the conditions of applying an Osc (Oscillation level) of 0.5 V and a frequency of 1 kHz. For each sample, 100 randomly selected samples were evaluated, and the ratio of the number of samples that short-circuited among the 100 samples was taken as the short circuit failure rate.
[0159] As a result, the short circuit failure rate was 0% in Examples 1 to 4 and Comparative Examples 1 and 2 satisfying a / b≤0.4. Therefore, in Examples 1 to 4 satisfying the above conditions, it was confirmed that the peripheral edge of the internal electrode was less sharply bent as it came into contact with the adjacent internal electrode, and short circuits could be prevented.
[0160] On the other hand, in Comparative Examples 3 to 8 where a / b is greater than 0.4, the short circuit failure rate is all above 1%. In particular, there is a tendency that the short circuit failure rate increases as a / b increases. Based on this result, it is confirmed that short circuits can be reliably suppressed by suppressing a / b to less than 0.4.
[0161] Through the above, it was confirmed that in Examples 1 to 4, the corners satisfying the conditions of a ≥ 1 μm and 0.1 ≤ a / b ≤ 0.4 are all structures with high moisture resistance and high reliability in suppressing short circuits. In addition, in the sample with a dimension of 0.2 mm in the X-axis direction and 0.125 mm in the Y-axis and Z-axis directions of the stacked ceramic capacitor, and the sample with a dimension of 1.6 mm in the X-axis direction and 0.8 mm in the Y-axis and Z-axis directions of the stacked ceramic capacitor, it was confirmed that when the corners satisfy the conditions of a ≥ 1 μm and 0.1 ≤ a / b ≤ 0.4, all of them are structures with high moisture resistance and high reliability in suppressing short circuits.
[0162] 5. Other Implementation Methods
[0163] As mentioned above, although embodiment of this invention was demonstrated, this invention is not limited to the said embodiment, It is a matter of course that various changes can be made within the range which does not deviate from the summary of this invention.
[0164] In the above embodiment, the multilayer ceramic capacitor 10 is described as an example of a multilayer ceramic electronic component, but the present invention can be applied to all multilayer ceramic electronic components having a ceramic body with stacked internal electrodes. Examples of such multilayer ceramic electronic components include chip varistors, chip thermistors, and stacked inductors.
Claims
1. A laminated ceramic electronic component, characterized in that: include: a functional portion having internal electrodes stacked in a first direction; a covering portion covering the functional portion from the first direction; and covering the side edge of the functional portion from a second direction orthogonal to the first direction, The functional portion has, in a cross section perpendicular to the third direction where the functional portion is bisected in a third direction perpendicular to the first direction and the second direction, a first straight line portion adjacent to the covering portion and extending in the second direction; and a second straight line portion adjacent to the side edge portion and extending in the first direction; and a corner portion connected to the first straight line portion and the second straight line portion, In the corner portion, when a distance along the first direction between a first imaginary line formed by extending the first straight line portion in the second direction and an end point on the first imaginary line side of the second straight line portion is set as a, and a distance along the second direction between a second imaginary line formed by extending the second straight line portion in the first direction and an end point on the second imaginary line side of the first straight line portion is set as b, the corner portion is bent in a manner satisfying the conditions of 2μm≤a≤20μm, 20μm≤b≤50μm, and 0.1≤a / b≤0.4, The internal electrode is formed over the entire width of the functional portion in the second direction, and the peripheral edge portion thereof stops at the side surface of the functional portion covered by the side edge portion. The outermost internal electrode includes: a flat first flat portion constituting the first straight portion; and a first peripheral portion located at the periphery of the first flat portion in the second direction and bent inward from the first flat portion in the first direction. The internal electrode other than the outermost internal electrode includes: a second flat portion parallel to the first straight portion; and a second peripheral portion located at the periphery of the second flat portion in the second direction and bent from the second flat portion inward in the first direction, The first peripheral edge portion and the second peripheral edge portion have a tendency to bend more toward the inside of the first direction as they are arranged outside the first direction. The inner side in the first direction is a direction close to an imaginary plane that bisects the multilayer ceramic electronic component in the first direction, and the outer side in the first direction is a direction away from the imaginary plane.
2. The multilayer ceramic electronic component according to claim 1, wherein: The thickness of the side edge portion is not less than 10 μm and not more than 15 μm.
3. The multilayer ceramic electronic component according to claim 2, wherein: The side edge portion has a thickness of 12 μm or less.
4. The multilayer ceramic electronic component according to any one of claims 1 to 3, wherein: The corner portion is bent inward in the first direction as it goes from the end point on the second imaginary line side of the first straight line portion to the end point on the first imaginary line side of the second straight line portion.
5. The multilayer ceramic electronic component according to any one of claims 1 to 3, wherein: The functional portion has four corners in the cross section.
6. A method for manufacturing a laminated ceramic electronic component, characterized in that: include: A step of manufacturing a laminated sheet by laminating a third ceramic sheet without an internal electrode in the first direction on an outer surface of a laminated body formed by alternately laminating first ceramic sheets and second ceramic sheets in the first direction, wherein the first ceramic sheets and the second ceramic sheets are respectively formed with a plurality of internal electrodes; The step of pressing the laminated sheets from the first direction; A step of manufacturing a laminated chip by cutting the laminated sheet that has been crimped, wherein the laminated chip has: a functional portion having internal electrodes laminated in the first direction; a covering portion covering the functional portion from the first direction; and a side surface where the internal electrodes are exposed and facing a second direction orthogonal to the first direction; A step of forming a side edge portion on the side surface; and a step of forming a fired functional portion by firing the stacked chip having the side edge portion formed thereon, The fired functional portion has, in a cross section perpendicular to the third direction where the fired functional portion is bisected in a third direction perpendicular to the first direction and the second direction, a first straight portion adjacent to the covering portion and extending in the second direction; a second straight portion adjacent to the side edge portion and extending in the first direction; and a corner portion connected to the first straight portion and the second straight portion, In the corner portion, when the distance along the first direction between a first imaginary line formed by extending the first straight line portion in the second direction and the end point of the second straight line portion on the first imaginary line side is set to a, and the distance along the second direction between a second imaginary line formed by extending the second straight line portion in the first direction and the end point of the first straight line portion on the second imaginary line side is set to b, the corner portion is bent in a manner that satisfies the conditions of a≥1μm and 0.1≤a / b≤0.
4.
7. The method for manufacturing a laminated ceramic electronic component according to claim 6, wherein: In the first ceramic sheet and the second ceramic sheet, the plurality of internal electrodes are arranged at intervals from each other in the second direction with the non-electrode forming region interposed therebetween. In the step of crimping from the first direction, the laminated sheet is formed with: a functional region on which the plurality of internal electrodes are stacked in the first direction; and a cut-away region on which the non-electrode forming region is stacked, the cut-away region being adjacent to the functional region in the second direction and having a thickness in the first direction gradually decreasing as the cut-away region moves away from the functional region in the second direction, In the process of cutting the laminated sheet, the cut-off area is cut off.
Citation Information
Patent Citations
Manufacturing method of laminated ceramic electronic component
JP2012209539A
Multilayer ceramic electronic component and multilayer ceramic capacitor
CN102810397A
Monolithic ceramic capacitor
CN104576053A
Multilayer capacitor and manufacturing method for same
CN105655127A
Multilayer capacitor and method for producing the same
CN105914038A