Semiconductor structure and method for forming the same

By forming an initial work function layer on a semiconductor structure substrate and performing a cyclic etching process, the problem of improving transistor performance in the existing technology is solved, the diversity of work function layers with different thicknesses can be formed on the same substrate, and the efficiency is improved. Overall performance of semiconductor structures.

CN112242299BActive Publication Date: 2024-10-22SEMICON MFG INT (SHANGHAI) CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910649261.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-07-18
Publication Date
2024-10-22
Estimated Expiration
2039-07-18

AI Technical Summary

Technical Problem

The transistor performance of existing semiconductor structures has not yet been improved, especially when the size of the device is reduced, it is difficult to meet different functional requirements.

Method used

Use the dielectric layer to form the first area and the second area on the substrate, form an initial work function layer at the bottom of the dielectric layer, and perform multiple etching cycles through the oxide etching and main etching processes to remove the initial work function layer. , combined with hydrophilic treatment and deionized water cleaning, to ensure the complete removal of the work function layer and form work function layers of different thicknesses.

Benefits of technology

It effectively improves the performance of the semiconductor structure, avoids the problem of incomplete removal of the work function layer, meets the diversity needs of forming work function layers of different thicknesses on the same substrate, and improves device performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112242299B_ABST
    Figure CN112242299B_ABST
Patent Text Reader

Abstract

A semiconductor structure and a method for forming the same, the method comprising: providing a substrate, the substrate comprising a first region and a second region, the substrate having a dielectric layer, the dielectric layer on the first region having a first gate opening, and the dielectric layer on the second region having a second gate opening; forming one or more initial work function layers at the bottom of the first gate opening and the bottom of the second gate opening; etching the initial work function layer in the first gate opening by at least one cyclic etching step, and forming a work function layer in the second gate opening, each cyclic etching step comprising: etching the initial work function layer by an oxide etching process; after the oxide etching process, etching the initial work function layer by a main etching process, and removing a layer of the exposed initial work function layer. The performance of the semiconductor structure formed is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor manufacturing, and in particular to a semiconductor structure and a forming method thereof. Background Art

[0002] In the field of integrated circuit manufacturing, as the size of transistors continues to shrink, the physical limits of devices have an increasingly greater impact on device preparation, and it becomes more difficult to scale down the characteristic dimensions of devices. The difficulty in the field of transistor and circuit manufacturing has also increased significantly.

[0003] In order to meet the requirements, transistors with different functions need to be formed on the same substrate. In the prior art, a work function layer is used to adjust the performance of transistors formed by a post-metal gate process to meet the requirements of transistors with different functions.

[0004] However, the performance of existing transistors still needs to be improved. Summary of the invention

[0005] The technical problem solved by the present invention is to provide a semiconductor structure and a method for forming the same, so as to improve the performance of the semiconductor structure.

[0006] In order to solve the above technical problems, the technical solution of the present invention provides a method for forming a semiconductor structure, including: providing a substrate, the substrate including a first area and a second area, the substrate having a dielectric layer, the dielectric layer on the first area having a first gate opening, and the dielectric layer on the second area having a second gate opening; forming one or more initial work function layers at the bottom of the first gate opening and the bottom of the second gate opening; etching the initial work function layer in the first gate opening by at least one cyclic etching step, and forming a work function layer in the second gate opening, each of the cyclic etching steps comprising: etching the initial work function layer by an oxide etching process; after the oxide etching process, etching the initial work function layer by a main etching process to remove a layer of exposed initial work function layer.

[0007] Optionally, the material of the initial work function layer includes titanium nitride, titanium aluminide or tantalum nitride.

[0008] Optionally, the oxide etching process includes a first wet etching process.

[0009] Optionally, the etching solution of the first wet etching process includes a hydrogen fluoride solution; the volume ratio of the hydrogen fluoride to water is 1:200.

[0010] Optionally, the main etching process includes a second wet etching process.

[0011] Optionally, the etching solution of the second wet etching process includes a hydrogen peroxide solution, a mixed solution of ammonia water and hydrogen peroxide, or a mixed solution of hydrogen chloride and hydrogen peroxide, and the temperature of the hydrogen peroxide solution is 50° C. to 80° C.

[0012] Optionally, each of the cyclic etching steps further includes: before adopting the oxide etching process, performing a first surface treatment on the initial work function layer in the first gate opening.

[0013] Optionally, the first surface treatment process includes a hydrophilic treatment process; and the solution used in the hydrophilic treatment process includes an isopropyl alcohol solution.

[0014] Optionally, each of the cyclic etching steps further includes: before adopting the main etching process and after the oxide etching process, performing a second surface treatment on the initial work function layer in the first gate opening.

[0015] Optionally, the second surface treatment process includes a hydrophilic treatment process; and the solution used in the hydrophilic treatment process includes an isopropyl alcohol solution.

[0016] Optionally, each of the cyclic etching steps further includes: after etching the initial work function layer using the main etching process, cleaning the first gate opening using deionized water.

[0017] Optionally, when the initial work function layer is a multi-layer layer, the number of cycles of the cyclic etching step is less than or equal to the number of layers of the initial work function layer.

[0018] Optionally, after the work function layer is formed in the second gate opening, the method further includes: drying the substrate; the drying process includes electric hot plate heating drying, wind heat drying, hydrothermal drying or chemical reagent dehydration treatment, and the reagent for the chemical reagent dehydration treatment includes an isopropyl alcohol solution at 50°C to 75°C.

[0019] Optionally, before forming one or more initial work function layers at the bottom of the first gate opening and the second gate opening, the method further includes: forming a stop layer at the bottom of the first gate opening and the second gate opening.

[0020] Optionally, the material of the stop layer includes tantalum nitride or a high dielectric constant material, the dielectric constant of the high dielectric constant material is greater than 3.9, and the high dielectric constant material includes hafnium oxide, aluminum oxide or zirconium oxide.

[0021] Optionally, the substrate includes: a base, a first fin located on the base in the first region, and a second fin located on the base in the second region; the dielectric layer is located on the first fin, the second fin and the base; the first gate opening is located on the first fin; and the second gate opening is located on the second fin.

[0022] Optionally, after forming a work function layer in the second gate opening, a gate layer is formed in the first gate opening and in the second gate opening.

[0023] Correspondingly, the technical solution of the present invention also provides a semiconductor structure formed by any of the above methods.

[0024] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0025] In the method for forming a semiconductor structure of the technical solution of the present invention, after one or more initial work function layers are formed at the bottom of the first gate opening and the second gate opening, the initial work function layer is first etched using an oxide etching process, and then the initial work function layer is etched using a main etching process; the oxide etching process can remove the oxidized portion of the surface of the initial work function layer, so that the subsequent main etching process can completely remove the initial work function layer, avoiding the situation where the initial work function layer is not completely removed and affects the performance of the semiconductor device, thereby improving the performance of the semiconductor structure.

[0026] Furthermore, multiple cyclic etching steps are used to remove the multiple initial work function layers, thereby avoiding the situation where the initial work function layers are not completely removed and affect the performance of the semiconductor device. The diversity of forming work function layers of different thicknesses on the same substrate is met, thereby improving the performance of the semiconductor structure.

[0027] Furthermore, before the oxide etching process is used, the initial work function layer in the first gate opening is subjected to a hydrophilic treatment process, so that the contact area between the solution of the oxide etching process and the initial work function layer is increased, thereby increasing the etching rate of the initial work function layer.

[0028] Furthermore, before the main etching process is adopted, the initial work function layer in the first gate opening is subjected to a hydrophilic treatment process, so that the contact area between the solution of the oxide etching process and the initial work function layer is increased, thereby increasing the etching rate of the initial work function layer.

[0029] Furthermore, after the initial work function layer is etched using the main etching process, the first gate opening is cleaned with deionized water. The deionized water treatment can remove a large amount of reaction byproducts in the first gate opening, and the etching efficiency can be improved when the oxide etching process and the main etching process are subsequently cycled. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figures 1 to 4 is a schematic cross-sectional structural diagram of a semiconductor structure forming process according to an embodiment;

[0031] Figures 5 to 14 A schematic cross-sectional view of a semiconductor structure forming process according to an embodiment of the invention. DETAILED DESCRIPTION

[0032] As described in the background art, the performance of existing transistors still needs to be improved. Now, an analysis and description will be given in conjunction with specific embodiments.

[0033] Figures 1 to 4 It is a schematic cross-sectional structure diagram of a semiconductor structure forming process according to an embodiment.

[0034] Please refer to Figure 1 , providing a substrate 100, wherein the substrate 100 has a fin, the substrate 100 includes a first region A, a second region B and a third region C, the first region A has an initial first gate opening 111 on the fin, the second region B has an initial second gate opening 112 on the fin, the third region C has an initial third gate opening 113 on the fin, and the sidewalls of the initial first gate opening 111, the initial second gate opening 112 and the initial third gate opening 113 have sidewalls 102.

[0035] Please refer to Figure 2 A dielectric layer 104 (K is greater than 3.9) is formed on the inner walls of the initial first gate opening 111, the initial second gate opening 112 and the initial third gate opening 113; a stop layer 105 is formed on the surface of the dielectric layer 104; a first work function layer 106 is formed on the surface of the stop layer 105, the initial first gate opening 111 forms an initial first opening 121, the initial second gate opening 112 forms an initial second opening 122, and the initial third gate opening 113 forms an initial third opening 123.

[0036] Please refer to Figure 3 , remove the first work function layer 106 on the inner wall of the initial third opening 123; after removing the first work function layer 106 on the inner wall of the initial third opening 123, form a second work function layer 107 on the inner wall of the initial first opening 121, the inner wall of the initial second opening 122 and the inner wall of the initial third opening 123, the initial first opening 121 forms a first opening 131, the initial second opening 122 forms a second opening 132, and the initial third opening 123 forms a third opening 133.

[0037] Please refer to Figure 4, remove the second work function layer 107 and the first work function layer 106 on the inner wall of the second opening 132; after removing the second work function layer 107 and the first work function layer 106 on the inner wall of the second opening 132, form the third work function layer 108 on the inner wall of the first opening 131, the inner wall of the second opening 132 and the inner wall of the third opening 133, the first opening 131 forms a first gate opening 141, the second opening 132 forms a second gate opening 142, and the third opening 133 forms a third gate opening 143.

[0038] During the formation of the semiconductor structure, the first region A needs to form a work function layer of a first thickness, the second region B needs to form a work function layer of a second thickness, and the third region C needs to form a work function layer of a third thickness, the first thickness is greater than the second thickness, and the second thickness is greater than the third thickness. Since the depth-to-width ratio of the initial first gate opening 111, the initial second gate opening 112, and the initial third gate opening 113 is relatively large, in order to accurately control the thickness of the different work function layers, the work function layers are formed in batches after calculation, and the deposition is repeated in the first region A, and the unnecessary work function layer thickness of the second region B and the third region C is etched, and the deposition and etching process steps are repeated to finally form the required work function layers of the first thickness, the second thickness, and the third thickness.

[0039] However, in the process of repeating the deposition process and the etching process, the material of the work function layer is easily oxidized to form oxides. If the material of the work function layer is titanium nitride, the first work function layer 106 is actually a mixture of titanium nitride and titanium oxynitride, the second work function layer 107 is actually a mixture of titanium nitride and titanium oxynitride, and the third work function layer 108 is actually a mixture of titanium nitride and titanium oxynitride. When the first work function layer 106 of the inner wall of the initial third opening 123 is removed by a wet etching process, and when the second work function layer 106 of the inner wall of the second opening 132 is removed by a wet etching process, 07 and the first work function layer 106, since the titanium nitride and titanium oxynitride have different etching rates, the surface etching rate of the first work function layer 106 and the second work function layer 107 is slower, and the bottom etching rate of the first work function layer 106 and the second work function layer 107 is faster, resulting in that the parameters of the wet etching process are difficult to control. If the etching conditions are not enough, the first work function layer 106 or the second work function layer 107 will have residues, affecting the subsequent process; if the etching conditions are too large, the stop layer 105 and the dielectric layer 104 will be damaged, affecting the performance of the subsequently formed device.

[0040] On the other hand, since the depth-to-width ratio of the initial first gate opening 111, the initial second gate opening 112, and the initial third gate opening 113 is relatively large, the circulation fluidity of the etching solution is poor, and the reaction by-products generated during the wet etching process cannot be removed in time. The residual reaction by-products will also affect the performance of the subsequently formed devices.

[0041] In order to solve the above problems, the technical solution of the present invention provides a semiconductor structure and a method for forming the same, by first etching the initial work function layer using an oxide etching process, and then etching the initial work function layer using a main etching process; the oxide etching process can remove the oxidized portion of the surface of the initial work function layer, so that the subsequent main etching process can completely remove the initial work function layer, avoiding the situation where the initial work function layer is not completely removed and affects the performance of the semiconductor device, thereby improving the performance of the semiconductor structure.

[0042] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0043] Figures 5 to 14 It is a schematic cross-sectional structure diagram of a semiconductor structure forming process according to an embodiment of the present invention.

[0044] Please refer to Figure 5 and Figure 6 , Figure 5 yes Figure 6 Schematic diagram of the cross-section structure along the section line AA'. Figure 6 yes Figure 5 A schematic cross-sectional structure diagram along the section line BB' direction provides a substrate.

[0045] The substrate comprises a first region I and a second region II. A dielectric layer 201 is provided on the substrate. The dielectric layer 201 on the first region I has a first gate opening 211 therein, and the dielectric layer 201 on the second region II has a second gate opening 212 therein.

[0046] In this embodiment, the substrate includes: a base 200, a first fin (not labeled) located on the first region I of the base 200, and a second fin (not labeled) located on the second region II of the base 200; the dielectric layer 201 is located on the first fin, the second fin and the base 200.

[0047] In this embodiment, the first gate opening 211 is located on the first fin; and the second gate opening 212 is located on the second fin.

[0048] The material of the substrate 200 includes silicon. In other embodiments, the material of the substrate includes germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium.

[0049] The material of the dielectric layer 201 includes silicon oxide or silicon nitride. In this embodiment, the material of the dielectric layer 201 includes silicon oxide.

[0050] In this embodiment, the sidewalls of the first gate opening 211 and the second gate opening 212 further have sidewalls 202 .

[0051] The material of the spacer 202 includes silicon nitride or silicon oxide. In this embodiment, the material of the spacer 202 includes silicon nitride.

[0052] Next, one or more initial work function layers are formed at the bottom of the first gate opening 211 and the bottom of the second gate opening 212 .

[0053] In this embodiment, an initial work function layer is formed at the bottom of the first gate opening 211 and the bottom of the second gate opening 212 .

[0054] In other embodiments, a plurality of initial work function layers are formed at the bottom of the first gate opening and the bottom of the second gate opening.

[0055] Before forming one or more initial work function layers at the bottom of the first gate opening 211 and the second gate opening 212 , the method further includes: forming a stop layer 203 at the bottom of the first gate opening 211 and the second gate opening 212 .

[0056] Please refer to Figure 7 and Figure 8 , Figure 7 yes Figure 8 Schematic diagram of the cross-sectional structure along the section line CC'. Figure 8 yes Figure 7 The schematic cross-sectional structure diagram along the section line DD′ direction shows that a stop layer 203 is formed at the bottom of the first gate opening 211 and the second gate opening 212 ; and an initial work function layer 204 is formed on the stop layer 203 .

[0057] The stop layer 203 is used as an etching stop layer for subsequently removing the initial work function layer 204 in the first gate opening 211. When the initial work function layer 204 is subsequently removed by a wet etching process, the material of the stop layer 203 has a greater etching selectivity than the material of the initial work function layer 204, so the stop layer 203 can be used as an etching stop layer for the initial work function layer 204.

[0058] The initial work function layer 204 provides a material layer for subsequently forming a work function layer at the bottom of the first gate opening 211 and the second gate opening 212 .

[0059] The material of the initial work function layer 204 includes titanium nitride, titanium aluminide or tantalum nitride. In this embodiment, the material of the initial work function layer 204 includes titanium nitride.

[0060] The process of forming the initial work function layer 204 includes a chemical vapor deposition process, a physical vapor deposition process or an atomic layer deposition process.

[0061] In this embodiment, the process of forming the initial work function layer 204 includes an atomic layer deposition process. The atomic layer deposition process can form an initial work function layer 204 with uniform thickness and dense structure.

[0062] In this embodiment, the thickness of the initial work function layer 204 ranges from 7 angstroms to 15 angstroms.

[0063] If the thickness of the single-layer initial work function layer 204 is less than 7 angstroms, the thickness of the single-layer initial work function layer 204 is uneven; if the thickness of the single-layer initial work function layer 204 is greater than 15 angstroms, the thickness of the single-layer initial work function layer 204 is relatively thick. When multiple layers of initial work function layers need to be superimposed, the thickness of the multiple layers of initial work function layers is too thick. When work function layers of different thicknesses are finally formed, the thickness accuracy of the work function layers is difficult to control.

[0064] The material of the stop layer 203 includes tantalum nitride or a high dielectric constant material. The tantalum nitride or the high dielectric constant material can be used as a stop layer for the initial work function layer of the titanium nitride and titanium aluminide materials.

[0065] In this embodiment, the material of the stop layer 203 includes tantalum nitride.

[0066] In other embodiments, when the material of the initial work function layer 204 includes tantalum nitride, the material of the stop layer 203 includes a high dielectric constant material, and the high dielectric constant material includes hafnium oxide, aluminum oxide, or zirconium oxide.

[0067] The process of forming the stop layer 203 includes a chemical vapor deposition process, a physical vapor deposition process or an atomic layer deposition process.

[0068] In this embodiment, the process of forming the stop layer 203 includes a chemical vapor deposition process. The chemical vapor deposition process can quickly form the stop layer 203 with uniform thickness.

[0069] In this embodiment, before forming the stop layer 203 at the bottom of the first gate opening 211 and the second gate opening 212 , a gate dielectric layer (not shown) is further formed at the bottom of the first gate opening 211 and the second gate opening 212 .

[0070] The material of the gate dielectric layer includes a high-k (greater than 3.9) dielectric material, and the high-k (greater than 3.9) dielectric material includes hafnium oxide, aluminum oxide or zirconium oxide.

[0071] The process of forming the gate dielectric layer includes a chemical vapor deposition process, a physical vapor deposition process or an atomic layer deposition process.

[0072] Next, at least one cyclic etching step is used to etch the initial work function layer in the first gate opening 211 , and a work function layer is formed in the second gate opening 212 .

[0073] In this embodiment, a single cyclic etching step is used to etch the initial work function layer 204 in the first gate opening 211 , and a work function layer 206 is formed in the second gate opening 212 .

[0074] In other embodiments, multiple cyclic etching steps are used to etch the initial work function layer in the first gate opening. When the initial work function layer is multi-layer, the number of cycles of the cyclic etching step is less than or equal to the number of layers of the initial work function layer.

[0075] The main steps of each cyclic etching include: etching the initial work function layer using an oxide etching process; after the oxide etching process, etching the initial work function layer using a main etching process to remove a layer of the exposed initial work function layer. For specific cyclic etching steps, please refer to Figures 9 to 13 .

[0076] Please refer to Fig. 9 , a protection layer 205 is formed on the surface of the substrate, and the protection layer 205 exposes the first gate opening 211 .

[0077] The protection layer 205 is used to protect an initial functional work function layer subsequently formed in the second gate opening 212 from being etched by the cyclic etching process.

[0078] In this embodiment, the material of the protection layer 205 includes photoresist.

[0079] Please continue to refer to Fig. 9 After forming the protection layer 205 , a first surface treatment is performed on the initial work function layer 204 in the first gate opening 211 .

[0080] In this embodiment, the first surface treatment process includes a hydrophilic treatment process.

[0081] The hydrophilic treatment process reduces the surface tension of the initial work function layer 204 in the first gate opening 211, thereby improving the hydrophilicity of the surface of the initial work function layer 204, thereby increasing the contact area between the surface of the initial work function layer 204 and the etching solution of the oxide etching process, thereby improving the etching efficiency of the oxide etching process.

[0082] In this embodiment, the solution used in the hydrophilic treatment process includes an isopropanol solution. The mass concentration of the isopropanol solution ranges from 10% to 100%. If the mass concentration of the isopropanol solution is too low, the hydrophilic treatment effect on the surface of the initial work function layer 204 is not significant.

[0083] The isopropyl alcohol solution interface has a smaller surface tension, and the etching solution interface of the oxide etching process has a larger surface tension. After the isopropyl alcohol solution infiltrates the surface of the initial work function layer 204, the surface tension of the initial work function layer 204 and the surface tension of the etching solution interface of the oxide etching process can be balanced, thereby having a better hydrophilic effect.

[0084] In other embodiments, the solution used in the hydrophilic treatment process includes: an ethanol solution or a propanol solution; the mass concentration range of the ethanol solution is 10% to 100%; the mass concentration range of the propanol solution is 10% to 100%.

[0085] In this embodiment, the treatment time of the first surface treatment process ranges from 10 seconds to 25 seconds.

[0086] If the processing time of the first surface treatment process is less than 10 seconds, the surface hydrophilicity of the initial work function layer 204 in the first gate opening 211 is not sufficiently improved; if the processing time of the first surface treatment process is greater than 25 seconds, it will lead to reduced production efficiency and waste of production capacity.

[0087] Please refer to Fig.10 After performing a first surface treatment on the initial work function layer 204 in the first gate opening 211 , an oxide etching process is used to etch the initial work function layer 204 in the first gate opening 211 .

[0088] The oxide etching process is used to remove the oxidized initial work function layer 204. The oxide layer on the surface of the initial work function layer 204 is first removed, and then the main etching process is used to remove the initial work function layer 204, so that the initial work function layer 204 can be completely removed.

[0089] In this embodiment, the oxide etching process includes a first wet etching process.

[0090] The first wet etching process is isotropic and can quickly and efficiently remove the oxide layer on the surface of the initial work function layer 204 at the bottom and sidewalls of the first gate opening 211 .

[0091] In this embodiment, the etching solution of the first wet etching process includes a hydrogen fluoride solution; the volume ratio of the hydrogen fluoride to water is 1:200.

[0092] The oxide of the initial work function layer 204 is an alkaline oxide, and the hydrogen fluoride solution is an acidic solution, so that the hydrogen fluoride solution can react quickly with the oxide of the initial work function layer 204, so that the oxide layer on the surface of the initial work function layer 204 can be quickly removed, and the etching effect of the hydrogen fluoride solution is well controlled.

[0093] In other embodiments, the etching solution of the first wet etching process includes a mixed solution of ammonia and hydrogen peroxide at 50°C to 70°C, a mixed solution of hydrogen chloride and hydrogen peroxide at 50°C to 70°C, or a mixed solution of phosphoric acid and hydrogen peroxide at 50°C to 70°C.

[0094] In this embodiment, the reaction time of the first wet etching process is 10 seconds to 60 seconds.

[0095] If the reaction time of the first wet etching process is less than 10 seconds, the oxide of the initial work function layer 204 is not removed cleanly, affecting the subsequent main etching process; if the reaction time of the first wet etching process is greater than 60 seconds, the production efficiency will be reduced and the production capacity will be affected.

[0096] Please refer to Fig.11 After the oxide etching process, a second surface treatment is performed on the initial work function layer 204 in the first gate opening 211 .

[0097] In this embodiment, the second surface treatment process includes a hydrophilic treatment process.

[0098] The hydrophilic treatment process reduces the surface tension of the initial work function layer 204 from which the oxide layer is removed in the first gate opening 211, thereby improving the hydrophilicity of the surface of the initial work function layer 204, thereby increasing the contact area between the surface of the initial work function layer 204 and the etching solution of the main etching process, thereby improving the etching efficiency of the main etching process.

[0099] In this embodiment, the solution used in the hydrophilic treatment process includes an isopropanol solution, and the mass concentration of the isopropanol solution ranges from 10% to 100%.

[0100] If the mass concentration of the isopropyl alcohol solution is too low, the hydrophilic treatment effect on the surface of the initial work function layer 204 is not significant.

[0101] The isopropyl alcohol solution interface has a smaller surface tension, and the etching solution interface of the main etching process has a larger surface tension. After the isopropyl alcohol solution infiltrates the surface of the initial work function layer 204, the surface tension of the initial work function layer 204 and the surface tension of the etching solution interface of the main etching process can be balanced, thereby having a better hydrophilic effect.

[0102] In other embodiments, the solution used in the hydrophilic treatment process includes: an ethanol solution or a propanol solution; the mass concentration range of the ethanol solution is 10% to 100%; the mass concentration range of the propanol solution is 10% to 100%.

[0103] In this embodiment, the treatment time of the second surface treatment process ranges from 10 seconds to 25 seconds.

[0104] If the processing time of the first surface treatment process is less than 10 seconds, the surface hydrophilicity of the initial work function layer 204 in the first gate opening 211 is not sufficiently improved; if the processing time of the first surface treatment process is greater than 25 seconds, it will lead to reduced production efficiency and waste of production capacity.

[0105] Please refer to Fig.12 and Fig.13 , Fig.12 yes Fig.13 Schematic diagram of the cross-sectional structure along the section line EE'. Fig.13 yes Fig.12 The schematic cross-sectional structure diagram along the section line FF′ shows that after the second surface treatment is performed on the initial work function layer 204 in the first gate opening 211 , the initial work function layer 204 is etched by a main etching process to remove a layer of the exposed initial work function layer 204 .

[0106] The main etching process is used to remove the initial work function layer 204 .

[0107] In this embodiment, the main etching process includes a second wet etching process.

[0108] The second wet etching process is isotropic and can quickly and efficiently remove the initial work function layer 204 at the bottom and sidewalls of the first gate opening 211 .

[0109] The etching solution of the second wet etching process includes a hydrogen peroxide solution, a mixed solution of ammonia water and hydrogen peroxide, or a mixed solution of hydrogen chloride and hydrogen peroxide.

[0110] In this embodiment, the etching solution of the second wet etching process includes a hydrogen peroxide solution; the temperature of the hydrogen peroxide solution is 50° C. to 80° C.

[0111] In this embodiment, the reaction time of the second wet etching process is 15 seconds to 30 seconds.

[0112] If the reaction time of the second wet etching process is less than 15 seconds, the initial work function layer 204 is not removed cleanly, which will affect the performance of the device; if the reaction time of the second wet etching process is greater than 30 seconds, it will cause over-etching, thereby damaging the fins and causing waste of production capacity.

[0113] After the initial work function layer 204 is etched using the main etching process, the first gate opening 211 is cleaned using deionized water.

[0114] The first gate opening 211 is cleaned with the deionized water. The deionized water treatment can remove a large amount of reaction byproducts in the first gate opening 211 , and can improve etching efficiency when the oxide etching process and the main etching process are subsequently circulated.

[0115] At this point, the initial work function layer 204 is first etched using an oxide etching process and then etched using a main etching process. The initial work function layer 204 has been completely removed, avoiding the situation where the initial work function layer is not completely removed and affects the performance of the semiconductor device, thereby improving the performance of the semiconductor structure.

[0116] In other embodiments, when multiple cyclic etching steps are used to etch the initial work function layer in the first gate opening, the cyclic etching steps are repeated. Figures 7 to 10 steps.

[0117] When the initial work function layer is a multi-layer layer, the number of cycles of the cyclic etching step is less than or equal to the number of layers of the initial work function layer.

[0118] After etching the initial work function layer 204 in the first gate opening 211 and forming the work function layer 206 in the second gate opening 212 through the one or more cyclic etching processes, the process further includes: drying the substrate; the drying process includes electric hot plate heating drying, wind heat drying, hydrothermal drying or chemical reagent dehydration treatment, and the reagent for the chemical reagent dehydration treatment includes an isopropyl alcohol solution at 50°C to 75°C.

[0119] In this embodiment, the process of drying the substrate includes a chemical reagent dehydration treatment, and the reagent of the chemical reagent dehydration treatment includes an isopropyl alcohol solution at a temperature of 50° C. to 75° C.

[0120] The isopropyl alcohol is a colorless transparent liquid with a low surface tension, so the isopropyl alcohol can be used to dehydrate the substrate to achieve the purpose of drying, which is convenient for subsequent processes.

[0121] After removing the initial work function layer 204 exposed in the first gate opening 211 , the protection layer 205 is removed to expose the second gate opening 212 .

[0122] In this embodiment, the process of removing the protection layer 205 includes an ashing process.

[0123] Please refer to Fig.14 After the work function layer 206 is formed in the second gate opening 212 , a gate layer 207 is formed in the first gate opening 211 and the second gate opening 212 .

[0124] The gate layer 207 and the spacer 201 form a gate structure.

[0125] The method for forming the gate layer 207 includes: forming a gate material layer (not shown) in the first gate opening 211 , in the second gate opening 212 and on the surface of the substrate; flattening the gate material layer until the dielectric layer 201 is exposed, and forming the gate layer 207 in the first gate opening 211 and in the second gate opening 212 .

[0126] The material of the gate layer includes polysilicon or metal. In this embodiment, the material of the gate layer includes metal; the metal includes one or more combinations of tantalum, tungsten, tantalum nitride or titanium nitride.

[0127] In this embodiment, the process of forming the gate material layer includes a deposition process, which includes a physical vapor deposition process, a chemical vapor deposition process, or an atomic layer deposition process.

[0128] Thus, in the semiconductor structure formed, the gate structure on the first region I and the gate structure on the second region II have different work function layers, thereby forming semiconductor structures with different functions on the same substrate.

[0129] Correspondingly, an embodiment of the present invention further provides a semiconductor structure formed by the above method.

[0130] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A method for forming a semiconductor structure, It is characterized in that include: Providing a substrate, the substrate comprising a first region and a second region, the substrate having a dielectric layer, the dielectric layer in the first region having a first gate opening, and the dielectric layer in the second region having a second gate opening; Forming one or more initial work function layers at the bottom of the first gate opening and the bottom of the second gate opening; The initial work function layer in the first gate opening is etched by at least one cyclic etching step to form a work function layer in the second gate opening, wherein each cyclic etching step comprises: performing a first surface treatment on the initial work function layer in the first gate opening; After the first surface treatment, etching the initial work function layer using an oxide etching process; After the oxide etching process, performing a second surface treatment on the initial work function layer in the first gate opening; After the second surface treatment, the initial work function layer is etched using a main etching process to remove a layer of the exposed initial work function layer.

2. The method for forming a semiconductor structure according to claim 1, It is characterized in that The material of the initial work function layer includes titanium nitride, titanium aluminide or tantalum nitride.

3. The method for forming a semiconductor structure according to claim 1, It is characterized in that The oxide etching process includes a first wet etching process.

4. The method for forming a semiconductor structure according to claim 3, It is characterized in that The etching solution of the first wet etching process includes a hydrogen fluoride solution; the volume ratio of the hydrogen fluoride to water is 1:

200.

5. The method for forming a semiconductor structure according to claim 1, It is characterized in that The main etching process includes a second wet etching process.

6. The method for forming a semiconductor structure according to claim 5, It is characterized in that The etching solution of the second wet etching process includes a hydrogen peroxide solution, a mixed solution of ammonia and hydrogen peroxide, or a mixed solution of hydrogen chloride and hydrogen peroxide. The temperature of the hydrogen peroxide solution is 50° C. to 80° C.

7. The method for forming a semiconductor structure according to claim 1, It is characterized in that The first surface treatment process includes a hydrophilic treatment process; and the solution used in the hydrophilic treatment process includes an isopropyl alcohol solution.

8. The method for forming a semiconductor structure according to claim 1, It is characterized in that The second surface treatment process includes a hydrophilic treatment process; and the solution used in the hydrophilic treatment process includes an isopropyl alcohol solution.

9. The method for forming a semiconductor structure according to claim 1, It is characterized in that Each of the cyclic etching steps further includes: after etching the initial work function layer using a main etching process, cleaning the first gate opening using deionized water.

10. The method for forming a semiconductor structure according to claim 1, It is characterized in that When the initial work function layer is a multi-layer layer, the number of cycles of the cyclic etching step is less than or equal to the number of layers of the initial work function layer.

11. The method for forming a semiconductor structure according to claim 1, It is characterized in that After the work function layer is formed in the second gate opening, the method further includes: drying the substrate; the drying process includes electric hot plate heating drying, wind heat drying, hydrothermal drying or chemical reagent dehydration treatment, and the reagent for the chemical reagent dehydration treatment includes an isopropyl alcohol solution at 50°C to 75°C.

12. The method for forming a semiconductor structure according to claim 1, It is characterized in that Before forming one or more initial work function layers at the bottom of the first gate opening and the second gate opening, the method further includes: forming a stop layer at the bottom of the first gate opening and the second gate opening.

13. The method for forming a semiconductor structure according to claim 12, It is characterized in that The material of the stop layer includes tantalum nitride or a high dielectric constant material, the dielectric constant of the high dielectric constant material is greater than 3.9, and the high dielectric constant material includes hafnium oxide, aluminum oxide or zirconium oxide.

14. The method for forming a semiconductor structure according to claim 1, It is characterized in that The substrate comprises: a base, a first fin located on the base in the first region, and a second fin located on the base in the second region; the dielectric layer is located on the first fin, the second fin and the base; the first gate opening is located on the first fin; and the second gate opening is located on the second fin.

15. The method for forming a semiconductor structure according to claim 1, It is characterized in that After forming a work function layer in the second gate opening, a gate layer is formed in the first gate opening and in the second gate opening.

16. A semiconductor structure formed by the method according to any one of claims 1 to 15.