High-efficiency pre-sintering process for low-loss magnetic core and its pressing die

Through the efficient pre-burning process of low-loss magnetic cores and innovative pressing molds, the problem of magnetic core adhesion during the sintering process is solved, and fast, stable magnetic core molding and efficient production are achieved.

CN112259357BActive Publication Date: 2024-10-25HAINING XINGHUO ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011130994.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-21
Publication Date
2024-10-25
Estimated Expiration
2040-10-21

AI Technical Summary

Technical Problem

During the sintering process, the contact surfaces of the magnetic core stacks are prone to adhesion, resulting in material waste and low production efficiency.

Method used

An efficient pre-sintering process for low-loss magnetic cores is adopted, including pressing the magnetic core raw material into a block blank, preparing an isolation liquid and soaking the blank, followed by a rapid pre-sintering process in a sintering furnace, using an innovative pressing mold to spring and drive The cooperation of parts ensures stable separation and molding of the mold.

Benefits of technology

It achieves rapid pre-sintering of the magnetic core, avoids adhesion, improves production stability and efficiency, and reduces material waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112259357B_ABST
    Figure CN112259357B_ABST
Patent Text Reader

Abstract

The present invention provides an efficient pre-burning process for a low-loss magnetic core and a pressing mold thereof, belonging to the field of mechanical technology. It solves the problem of poor stability in the prior art. The efficient pre-burning process for the low-loss magnetic core comprises the following steps: A. pressing; B. preparing an isolation liquid; C. coating; D. rapid pre-burning. The pressing mold for the low-loss magnetic core comprises a frame, an upper mold body and a lower mold body, characterized in that it also comprises a bottom plate, a guide rod, a spring and a driving member, wherein the guide rod is vertically fixed to the bottom plate, the guide rod is passed through the lower mold body and the upper mold body and the lower mold body is against the upper part of the bottom plate, the upper mold body is located directly above the lower mold body, the spring is sleeved on the guide rod and the two ends of the spring act on the lower mold body and the upper mold body respectively, and under the elastic force of the spring, the upper mold body has a tendency to move up and detach from the lower mold body, and the driving member can push the upper mold body to move down and make the upper mold body after moving down buckle on the lower mold body. The efficient pre-burning process for the low-loss magnetic core has high stability and high operating efficiency of the pressing mold.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of mechanical technology and relates to a high-efficiency pre-sintering process of a low-loss magnetic core and a pressing die thereof. Background Art

[0002] With the integration and miniaturization of electronic products, transformers are getting smaller and smaller, and the corresponding magnetic core products are also getting smaller and smaller. During the sintering process, the magnetic cores are stacked in the sintering furnace. In order to prevent adhesion between the contact surfaces of the stacked magnetic cores during the sintering process, a layer of corundum sand is usually sprinkled between the magnetic cores, and then the surface of the magnetic core is ground off after sintering, resulting in material waste. Summary of the invention

[0003] The first object of the present invention is to provide an efficient pre-burning process for preforming a fast and stable low-loss magnetic core in view of the above-mentioned problems existing in the prior art.

[0004] A second object of the present invention is to provide a pressing die used in the above process.

[0005] The first object of the present invention can be achieved by the following technical solutions:

[0006] A high-efficiency pre-burning process for a low-loss magnetic core, characterized in that the process comprises the following steps:

[0007] A. Pressing: Put the powdered magnetic core raw material into a pressing mold, and press the magnetic core raw material into a block-shaped magnetic core blank through the pressing mold;

[0008] B. Preparation of isolation liquid: put aluminum nitride powder with a particle size of 400-600 mesh and boron nitride powder with a particle size of 400-600 mesh into a 3%-5% SiO2 solution and stir and mix to obtain an isolation liquid, wherein the mass ratio of aluminum nitride powder, boron nitride powder and SiO2 solution is 1:1:50;

[0009] C. Coating: Soak the core blank in the isolation liquid for 3-10 minutes;

[0010] D. Rapid pre-sintering: Place the soaked magnetic core blank into a sintering furnace and pre-sinter it at 100-130°C for 10-15 minutes.

[0011] The efficient pre-sintering process of the low-loss magnetic core can quickly sinter the magnetic core blank into shape by pressing, and the subsequent heat treatment can make it fully formed.

[0012] In this pre-sintering process, an isolation liquid with relatively good isolation performance is creatively used. After the core blank is completely immersed in the isolation liquid, good isolation performance can be formed, and the core blank will not stick in the sintering furnace after pre-sintering treatment.

[0013] The second object of the present invention can be achieved by the following technical solutions:

[0014] A pressing mold for a low-loss magnetic core comprises a frame, an upper mold body and a lower mold body, and is characterized in that it also comprises a base plate, a guide rod, a spring and a driving member, wherein the guide rod is vertically fixed to the base plate, the guide rod is passed through the lower mold body and the upper mold body and the lower mold body is against the upper part of the base plate, the upper mold body is located directly above the lower mold body, the spring is sleeved on the guide rod and the two ends of the spring act on the lower mold body and the upper mold body respectively, and under the elastic force of the spring, the upper mold body has a tendency to move upward and separate from the lower mold body, and the driving member can push the upper mold body downward and make the upper mold body after moving downward snap onto the lower mold body.

[0015] The pressing die creatively separates the upper die from the lower die under the elastic force of the spring, and in this state, the magnetic core material can be stably placed in the lower die. After the driving member drives the lower die to move downward, the magnetic core material is stably formed between the upper die and the lower die.

[0016] It can be seen that during the molding process, the guiding effect of the guide rod can ensure that the lower mold body moves downward stably, and the lower mold body can be stably buckled on the upper mold body.

[0017] In the above-mentioned pressing mold for the low-loss magnetic core, the upper mold body is cylindrical, and the center of the lower mold body has a protruding base, and the base matches the inner cavity of the upper mold body.

[0018] Since the base protrudes from the lower mold body, the arrangement of the base can facilitate the separation of the magnetic core blank from the lower mold body.

[0019] In the above-mentioned pressing die for the low-loss magnetic core, the edge of the base has a smoothed introduction portion.

[0020] In the above-mentioned pressing die for the low-loss magnetic core, the introduction portion is a chamfer at the edge of the base.

[0021] The setting of the introduction part can avoid jamming between the upper mold body and the lower mold body. Of course, according to actual conditions, it is also feasible to have the introduction part with rounded corners.

[0022] In the above-mentioned pressing die of the low-loss magnetic core, the side of the upper mold body has a protruding convex edge, the upper end of the above-mentioned guide rod is inserted into the convex edge, and the two ends of the above-mentioned spring act on the convex edge and the lower mold body respectively.

[0023] The arrangement of the convex edge can provide sufficient space for the guide rod.

[0024] In the above-mentioned pressing die for the low-loss magnetic core, the convex edge and the upper mold body are an integrated structure.

[0025] In the above-mentioned pressing die for the low-loss magnetic core, the driving member is a cylinder, and the piston rod of the cylinder abuts against the upper part of the upper die body.

[0026] In the above-mentioned pressing die for the low-loss magnetic core, the guide rod and the spring form a connecting unit, the number of the connecting units is two and the two connecting units are symmetrically distributed on both sides of the lower die body.

[0027] The two symmetrically arranged connecting units can enable the upper mold body to translate stably relative to the lower mold body.

[0028] Compared with the prior art, the high-efficiency pre-burning process of the low-loss magnetic core can be quickly pre-burned and formed with high stability.

[0029] At the same time, the pressing mold of the low-loss magnetic core can achieve pressing and forming only by the action of the driving part. It has a high degree of automation, low loss and high efficiency, and has high practical value. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram of the structure of a pressing die for a low-loss magnetic core.

[0031] In the figure, 1, frame; 2, upper mold body; 2a, convex edge; 3, lower mold body; 3a, base; 3a1, introduction part; 4, bottom plate; 5, guide rod; 6, spring; 7, driving member. DETAILED DESCRIPTION Embodiment 1

[0032] The efficient pre-burning process of this low-loss magnetic core includes the following steps:

[0033] A. Pressing: Put the powdered magnetic core raw material into a pressing mold, and press the magnetic core raw material into a block-shaped magnetic core blank through the pressing mold;

[0034] B. Preparation of isolation liquid: Aluminum nitride powder with a particle size of 400 mesh and boron nitride powder with a particle size of 400 mesh are added into a 3% SiO2 solution and stirred to obtain an isolation liquid, wherein the mass ratio of aluminum nitride powder, boron nitride powder and SiO2 solution is 1:1:50;

[0035] C. Coating: Soak the core blank in the isolation liquid for 3 minutes;

[0036] D. Rapid pre-sintering: Place the soaked magnetic core blank into a sintering furnace and pre-sinter it at 100°C for 10 minutes.

[0037] like Figure 1As shown, the pressing mold of the low-loss magnetic core includes a frame 1, an upper mold body 2 and a lower mold body 3, and also includes a base plate 4, a guide rod 5, a spring 6 and a driving member 7. The guide rod 5 is vertically fixed to the base plate 4, and the guide rod 5 is passed through the lower mold body 3 and the upper mold body 2, and the lower mold body 3 is against the upper part of the base plate 4. The upper mold body 2 is located directly above the lower mold body 3. The spring 6 is sleeved on the guide rod 5 and the two ends of the spring 6 act on the lower mold body 3 and the upper mold body 2 respectively. Under the elastic force of the spring 6, the upper mold body 2 has a tendency to move up and separate from the lower mold body 3, and the driving member 7 can push the upper mold body 2 to move down and make the upper mold body 2 after moving down snap onto the lower mold body 3.

[0038] The upper mold body 2 is cylindrical, and the center of the lower mold body 3 has a protruding base 3a, which matches the inner cavity of the upper mold body 2.

[0039] The base 3a has a smoothed introduction portion 3a1 at its edge.

[0040] The introduction portion 3a1 is a chamfer at the edge of the base 3a.

[0041] The upper mold body 2 has a protruding convex edge 2a on its side, the upper end of the guide rod 5 is passed through the convex edge 2a, and the two ends of the spring 6 act on the convex edge 2a and the lower mold body 3 respectively.

[0042] The convex edge 2a and the upper mold body 2 are an integrated structure.

[0043] The driving member 7 is a cylinder, and the piston rod of the cylinder is against the upper part of the upper mold body 2.

[0044] The guide rod 5 and the spring 6 form a connecting unit. The number of the connecting units is two and the two connecting units are symmetrically distributed on both sides of the lower mold body 3 .

[0045] The efficient pre-sintering process of the low-loss magnetic core can quickly sinter the magnetic core blank into shape by pressing, and the subsequent heat treatment can make it fully formed.

[0046] In this pre-sintering process, an isolation liquid with relatively good isolation performance is creatively used. After the core blank is completely immersed in the isolation liquid, good isolation performance can be formed, and the core blank will not stick in the sintering furnace after pre-sintering treatment.

[0047] The pressing die creatively separates the upper die from the lower die under the elastic force of the spring, and in this state, the magnetic core material can be stably placed in the lower die. After the driving member drives the lower die to move downward, the magnetic core material is stably formed between the upper die and the lower die.

[0048] It can be seen that during the molding process, the guiding effect of the guide rod can ensure that the lower mold body moves downward stably, and the lower mold body can be stably buckled on the upper mold body. Embodiment 2

[0049] The efficient pre-burning process of this low-loss magnetic core includes the following steps:

[0050] A. Pressing: Put the powdered magnetic core raw material into a pressing mold, and press the magnetic core raw material into a block-shaped magnetic core blank through the pressing mold;

[0051] B. Preparation of isolation liquid: Aluminum nitride powder with a particle size of 600 mesh and boron nitride powder with a particle size of 600 mesh are added into a 5% SiO2 solution and stirred to obtain an isolation liquid, wherein the mass ratio of aluminum nitride powder, boron nitride powder and SiO2 solution is 1:1:50;

[0052] C. Coating: Soak the core blank in the isolation liquid for 10 minutes;

[0053] D. Rapid pre-sintering: Place the soaked magnetic core blank into a sintering furnace and pre-sinter it at 130°C for 15 minutes.

[0054] like Figure 1 As shown, the pressing mold of the low-loss magnetic core includes a frame 1, an upper mold body 2 and a lower mold body 3, and also includes a base plate 4, a guide rod 5, a spring 6 and a driving member 7. The guide rod 5 is vertically fixed to the base plate 4, and the guide rod 5 is passed through the lower mold body 3 and the upper mold body 2, and the lower mold body 3 is against the upper part of the base plate 4. The upper mold body 2 is located directly above the lower mold body 3. The spring 6 is sleeved on the guide rod 5 and the two ends of the spring 6 act on the lower mold body 3 and the upper mold body 2 respectively. Under the elastic force of the spring 6, the upper mold body 2 has a tendency to move up and separate from the lower mold body 3, and the driving member 7 can push the upper mold body 2 to move down and make the upper mold body 2 after moving down snap onto the lower mold body 3.

[0055] The upper mold body 2 is cylindrical, and the center of the lower mold body 3 has a protruding base 3a, which matches the inner cavity of the upper mold body 2.

[0056] The base 3a has a smoothed introduction portion 3a1 at its edge.

[0057] The introduction portion 3a1 is a chamfer at the edge of the base 3a.

[0058] The upper mold body 2 has a protruding convex edge 2a on its side, the upper end of the guide rod 5 is passed through the convex edge 2a, and the two ends of the spring 6 act on the convex edge 2a and the lower mold body 3 respectively.

[0059] The convex edge 2a and the upper mold body 2 are an integrated structure.

[0060] The driving member 7 is a cylinder, and the piston rod of the cylinder is against the upper part of the upper mold body 2.

[0061] The guide rod 5 and the spring 6 form a connecting unit. The number of the connecting units is two and the two connecting units are symmetrically distributed on both sides of the lower mold body 3 .

[0062] The efficient pre-sintering process of the low-loss magnetic core can quickly sinter the magnetic core blank into shape by pressing, and the subsequent heat treatment can make it fully formed.

[0063] In this pre-sintering process, an isolation liquid with relatively good isolation performance is creatively used. After the core blank is completely immersed in the isolation liquid, good isolation performance can be formed, and the core blank will not stick in the sintering furnace after pre-sintering treatment.

[0064] The pressing die creatively separates the upper die from the lower die under the elastic force of the spring, and in this state, the magnetic core material can be stably placed in the lower die. After the driving member drives the lower die to move downward, the magnetic core material is stably formed between the upper die and the lower die.

[0065] It can be seen that during the molding process, the guiding effect of the guide rod can ensure that the lower mold body moves downward stably, and the lower mold body can be stably buckled on the upper mold body. Embodiment 3

[0066] The efficient pre-burning process of this low-loss magnetic core includes the following steps:

[0067] A. Pressing: Put the powdered magnetic core raw material into a pressing mold, and press the magnetic core raw material into a block-shaped magnetic core blank through the pressing mold;

[0068] B. Preparation of isolation liquid: Aluminum nitride powder with a particle size of 500 mesh and boron nitride powder with a particle size of 460 mesh are added into a 4% SiO2 solution and stirred to obtain an isolation liquid, wherein the mass ratio of aluminum nitride powder, boron nitride powder and SiO2 solution is 1:1:50;

[0069] C. Coating: Soak the core blank in the isolation liquid for 8 minutes;

[0070] D. Rapid pre-sintering: Place the soaked magnetic core blank into a sintering furnace and pre-sinter it at 120°C for 13 minutes.

[0071] like Figure 1As shown, the pressing mold of the low-loss magnetic core includes a frame 1, an upper mold body 2 and a lower mold body 3, and also includes a base plate 4, a guide rod 5, a spring 6 and a driving member 7. The guide rod 5 is vertically fixed to the base plate 4, and the guide rod 5 is passed through the lower mold body 3 and the upper mold body 2, and the lower mold body 3 is against the upper part of the base plate 4. The upper mold body 2 is located directly above the lower mold body 3. The spring 6 is sleeved on the guide rod 5 and the two ends of the spring 6 act on the lower mold body 3 and the upper mold body 2 respectively. Under the elastic force of the spring 6, the upper mold body 2 has a tendency to move up and separate from the lower mold body 3, and the driving member 7 can push the upper mold body 2 to move down and make the upper mold body 2 after moving down snap onto the lower mold body 3.

[0072] The upper mold body 2 is cylindrical, and the center of the lower mold body 3 has a protruding base 3a, which matches the inner cavity of the upper mold body 2.

[0073] The base 3a has a smoothed introduction portion 3a1 at its edge.

[0074] The introduction portion 3a1 is a chamfer at the edge of the base 3a.

[0075] The upper mold body 2 has a protruding convex edge 2a on its side, the upper end of the guide rod 5 is passed through the convex edge 2a, and the two ends of the spring 6 act on the convex edge 2a and the lower mold body 3 respectively.

[0076] The convex edge 2a and the upper mold body 2 are an integrated structure.

[0077] The driving member 7 is a cylinder, and the piston rod of the cylinder is against the upper part of the upper mold body 2.

[0078] The guide rod 5 and the spring 6 form a connecting unit. The number of the connecting units is two and the two connecting units are symmetrically distributed on both sides of the lower mold body 3 .

[0079] The efficient pre-sintering process of the low-loss magnetic core can quickly sinter the magnetic core blank into shape by pressing, and the subsequent heat treatment can make it fully formed.

[0080] In this pre-sintering process, an isolation liquid with relatively good isolation performance is creatively used. After the core blank is completely immersed in the isolation liquid, good isolation performance can be formed, and the core blank will not stick in the sintering furnace after pre-sintering treatment.

[0081] The pressing die creatively separates the upper die from the lower die under the elastic force of the spring, and in this state, the magnetic core material can be stably placed in the lower die. After the driving member drives the lower die to move downward, the magnetic core material is stably formed between the upper die and the lower die.

[0082] It can be seen that during the molding process, the guiding effect of the guide rod can ensure that the lower mold body moves downward stably, and the lower mold body can be stably buckled on the upper mold body.

Claims

1. An efficient pre-burning process for a low-loss magnetic core, characterized in that: This process includes the following steps: A. Pressing: Put the powdered magnetic core raw material into a pressing mold, and press the magnetic core raw material into a block-shaped magnetic core blank through the pressing mold; The pressing mold includes a frame, an upper mold body and a lower mold body, and also includes a bottom plate, a guide rod, a spring and a driving member. The guide rod is vertically fixed to the bottom plate, the guide rod is passed through the lower mold body and the upper mold body, and the lower mold body is against the upper part of the bottom plate, the upper mold body is located directly above the lower mold body, the spring is sleeved on the guide rod, and the two ends of the spring act on the lower mold body and the upper mold body respectively. Under the elastic force of the spring, the upper mold body has a tendency to move up and separate from the lower mold body, and the driving member can push the upper mold body to move down and make the upper mold body after moving down buckle on the lower mold body; B. Preparation of isolation liquid: Add aluminum nitride powder with a particle size of 400-600 mesh and boron nitride powder with a particle size of 400-600 mesh into a 3%-5% SiO2 solution and stir to obtain an isolation liquid, wherein the mass ratio of aluminum nitride powder, boron nitride powder and SiO2 solution is 1:1:50; C. Coating: Soak the core blank in the isolation liquid for 3-10 minutes; D. Rapid pre-sintering: Place the soaked magnetic core blank into a sintering furnace and pre-sinter it at 100-130°C for 10-15 minutes.

2. The high-efficiency pre-burning process of the low-loss magnetic core according to claim 1, characterized in that: The upper mold body is cylindrical, and the center of the lower mold body has a protruding base, which matches the inner cavity of the upper mold body.

3. The high-efficiency pre-burning process of the low-loss magnetic core according to claim 2, characterized in that: The base has a smoothed introduction portion at its edge.

4. The high-efficiency pre-burning process of the low-loss magnetic core according to claim 3, characterized in that: The introduction portion is a chamfer at the edge of the base.

5. The high-efficiency pre-burning process of the low-loss magnetic core according to claim 4, characterized in that: The side of the upper mold body has a protruding convex edge, the upper end of the guide rod is penetrated through the convex edge, and the two ends of the spring act on the convex edge and the lower mold body respectively.

6. The high-efficiency pre-burning process of the low-loss magnetic core according to claim 5, characterized in that: The convex edge and the upper mold body are an integrated structure.

7. The high-efficiency pre-burning process of the low-loss magnetic core according to claim 6, characterized in that: The driving member is a cylinder, and the piston rod of the cylinder is against the upper part of the upper mold body.

8. The high-efficiency pre-burning process of the low-loss magnetic core according to claim 7, characterized in that: The guide rod and the spring form a connecting unit, the number of the connecting units is two and the two connecting units are symmetrically distributed on both sides of the lower mold body.