Anodized aluminum as a hard mask for plasma etching

By using a self-assembled anodized aluminum hard mask in the fluorine-based plasma etching process, the problem of insufficient selectivity of the hard mask in the existing technology is solved, high aspect ratio etching and memory density are improved, and the aluminum oxide is avoided. Difficulties in deposition and cleaning.

CN112262458BActive Publication Date: 2024-10-01LAM RES CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980038751.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-06-12
Filing Date
2019-05-17
Publication Date
2024-10-01
Estimated Expiration
2039-05-17

AI Technical Summary

Technical Problem

In the fluorine-based plasma etching process, it is difficult for existing hard mask materials to achieve sufficient etching selectivity and depth, which limits the memory density and formation of channel holes in 3D NAND integrated circuits, and aluminum oxide is deposited as a hard mask material. and difficult cleaning issues.

Method used

Self-assembled anodized aluminum oxide (AAO) is used as the hard mask material, and a hole structure with high aspect ratio characteristics is formed by electrochemical conversion of the aluminum seed layer, and an aluminum-based hard mask is used in the fluorine-based etching process to achieve high etching Selectivity.

Benefits of technology

It achieves the etching of high aspect ratio features in the fluorine-based plasma etching process, improves the memory density and channel hole formation depth of 3D NAND integrated circuits, avoids the difficulties of aluminum oxide deposition and cleaning, and provides higher etching options. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112262458B_ABST
    Figure CN112262458B_ABST
Patent Text Reader

Abstract

An aluminum seed layer is deposited over the wafer. A layer of photoresist material is deposited on the aluminum seed layer. The photoresist material is patterned and developed to expose portions of the aluminum seed layer through openings in the photoresist material. An electrochemical conversion process is performed on the wafer to electrochemically convert portions of the aluminum seed layer exposed through the openings in the photoresist material into anodized aluminum oxide (AAO). The AAO includes a hole pattern extending through the AAO to expose an area of ​​the top surface of the wafer below the aluminum seed layer. The photoresist material is removed from the wafer. The wafer is exposed to a plasma to etch holes into the wafer at areas of the top surface of the wafer exposed by the hole pattern in the AAO.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the fabrication of semiconductor devices. Background Art

[0002] Plasma etching processes are commonly used in the manufacture of semiconductor devices. In a plasma etching process, a semiconductor wafer including a semiconductor device being manufactured is exposed to a plasma that interacts with at least one material on the semiconductor wafer to remove the at least one material. The plasma can be generated using a specific reactive gas that will cause components of the plasma to interact with the material to be removed from the semiconductor wafer without significantly interacting with other materials on the wafer that will not be removed. In addition, in some plasma etching processes, a bias voltage can be applied to the semiconductor wafer to achieve anisotropic etching of features on the semiconductor wafer by attracting charged components of the plasma toward the semiconductor wafer in a more vertical direction. It is in this context that the present disclosure emerges. Summary of the invention

[0003] In an example embodiment, a method for performing a plasma etching process is disclosed. The method includes depositing an aluminum seed layer on a top surface of a wafer. The method also includes depositing a layer of photoresist material on the aluminum seed layer. The method also includes patterning and developing the photoresist material layer to expose one or more portions of the aluminum seed layer through openings in the photoresist material. The method also includes performing an electrochemical conversion process on the wafer to electrochemically convert the one or more portions of the aluminum seed layer exposed through the openings in the photoresist material into anodized aluminum oxide. The anodized aluminum oxide includes a hole pattern extending through the anodized aluminum oxide to expose an area of ​​the top surface of the wafer below the aluminum seed layer. The method also includes removing the photoresist material from the wafer. The method also includes exposing the wafer to a plasma to etch holes into the wafer at the area of ​​the top surface of the wafer exposed by the hole pattern in the anodized aluminum oxide.

[0004] In an exemplary embodiment, a method for performing a plasma etching process is disclosed. The method includes depositing an aluminum seed layer on a top surface of a wafer. The method also includes depositing a mask material layer on the aluminum seed layer. The method also includes depositing a photoresist material layer on the mask material layer. The method also includes patterning and developing the photoresist material layer to expose one or more portions of the mask material. The method also includes removing the one or more portions of the mask material to expose corresponding portions of the aluminum seed layer. The method also includes performing an electrochemical conversion process on the wafer to electrochemically convert the exposed corresponding portions of the aluminum seed layer into anodized aluminum oxide. The anodized aluminum oxide includes a hole pattern extending through the anodized aluminum oxide to expose an area of ​​the top surface of the wafer below the aluminum seed layer. The method also includes exposing the wafer to a plasma to etch holes into the wafer at the area of ​​the top surface of the wafer exposed by the hole pattern in the anodized aluminum oxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0005] Figure 1A A vertical cross section through a section of a semiconductor wafer is shown.

[0006] Figure 1B Shown through Figure 1A A vertical cross-section of the section of the wafer wherein the patterned and developed hard mask material is deposited on the top surface of the wafer.

[0007] Figure 1C shows the hole after it has been etched to a partial depth through Figure 1B A vertical cross-section of said section of the wafer is shown.

[0008] Figure 1D The breakthrough is shown after further etching and when the hard mask material is completely removed. Figure 1C A vertical cross-section of said section of the wafer is shown.

[0009] Figure 2A A flow chart of a method for performing a plasma etching process including forming and using anodized aluminum oxide (AAO) as a hard mask is shown according to some embodiments.

[0010] Figure 2B A more detailed flow chart of operations for electrochemically converting an exposed portion of an aluminum seed layer to AAO is shown, according to some embodiments.

[0011] Figure 3A A vertical cross section through a segment of a wafer after deposition of an aluminum seed layer is shown, according to some embodiments.

[0012] Figure 3B According to some embodiments, after depositing a layer of photoresist material, Figure 3A A vertical cross-section of said section of the wafer is shown.

[0013] Figure 3C According to some embodiments, after patterning and developing the photoresist material layer, Figure 3B A vertical cross-section of said section of the wafer is shown.

[0014] Figure 3D FIG. 1 shows a schematic diagram of a process for electrochemically converting an exposed portion of an aluminum seed layer to AAO to expose / expose a region of a top surface of an underlying processing material layer during operation according to some embodiments. Figure 3C A vertical cross-section of said section of the wafer is shown.

[0015] Figure 3E FIG. 1 shows a method of electrochemically converting the exposed portion of the aluminum seed layer to AAO to expose / expose an area of ​​the top surface of the underlying in-process material layer after the operation is completed according to some embodiments. Figure 3D A top view of the section of the wafer is shown.

[0016] Figure 3F FIG. 1 shows a schematic diagram of a process for removing photoresist material from an aluminum seed layer after removing the photoresist material from the aluminum seed layer according to some embodiments. Figure 3D A vertical cross-section of said section of the wafer is shown.

[0017] Figure 3G FIG. 1 shows a method of etching a hole through an underlying in-process material layer in an area exposed through a hole in the AAO according to some embodiments. Figure 3F A vertical cross-section of said section of the wafer is shown.

[0018] Figure 3H FIG. 1 shows a method of forming a dense aluminum oxide film after oxidizing the portion of the aluminum seed layer that has not been converted into AAO to form a dense aluminum oxide film according to some embodiments. Figure 3F A vertical cross-section of said section of the wafer is shown.

[0019] Fig. 3I FIG. 1 shows a method of etching a hole through an underlying in-process material layer in an area exposed through a hole in the AAO according to some embodiments. Figure 3H A vertical cross-section of said section of the wafer is shown.

[0020] Figure 3J FIG. 1 shows a flow chart of a process for removing the aluminum seed layer, AAO, and aluminum oxide (if present) from the material layer under processing according to some embodiments. Figure 3GOr a vertical cross section of the segment of the wafer shown in 3I.

[0021] Figure 4 A flow chart of a method for performing a plasma etching process including forming and using AAO as a hard mask and including using an electrochemically compatible mask material is shown according to some embodiments.

[0022] Figure 5A After depositing a layer of electrochemically compatible mask material, a Figure 3A A vertical cross-section of said section of the wafer is shown.

[0023] Figure 5B After depositing a layer of photoresist material, a Figure 5A A vertical cross-section of said section of the wafer is shown.

[0024] Figure 5C After patterning and developing the photoresist material layer, a Figure 5B A vertical cross-section of said section of the wafer is shown.

[0025] Figure 5D FIG. 1 shows a method of removing a portion of the electrochemically compatible mask material in a specified area after removing the portion of the electrochemically compatible mask material in a specified area according to some embodiments. Figure 5C A vertical cross-section of the section of the wafer is shown where a pattern of holes will be etched through the underlying layer of material being processed in the specified area.

[0026] Figure 5E FIG. 1 shows a process for electrochemically converting an exposed portion of an aluminum seed layer in a specified region to AAO to expose / expose a region of a top surface of an underlying processing material layer, according to some embodiments. Figure 5D A vertical cross-section of said section of the wafer is shown.

[0027] Fig. 5F FIG. 1 shows a method of electrochemically converting an exposed portion of an aluminum seed layer in a specified region to AAO to expose / expose a region of a top surface of an underlying processing material layer after the operation is completed according to some embodiments. Figure 5E A top view of the section of the wafer is shown. DETAILED DESCRIPTION

[0028] In the following description, many specific details are set forth in order to provide an understanding of the embodiments of the present disclosure. However, it will be apparent to those skilled in the art that embodiments of the present disclosure may be practiced without some or all of these specific details. In other cases, well-known processing operations are not described in detail to avoid unnecessarily obscuring the present disclosure.

[0029] Figure 1A A vertical cross section through a section of a semiconductor wafer 100 (hereinafter referred to as a "wafer") is shown. Wafer 100 includes one or more layers of material 103 in process extending downward from the top surface of wafer 100 to a depth 104 within wafer 100. Below depth 104, wafer 100 includes an underlying section 101, which includes underlying wafer materials, structures, and substrates. In various embodiments, wafer 100 may vary in form, shape, and / or size. For example, in some embodiments, wafer 100 referred to herein may correspond to a semiconductor wafer having a diameter of 200 mm (millimeter), a semiconductor wafer having a diameter of 300 mm, or a semiconductor wafer having a diameter of 450 mm. In addition, in some embodiments, wafer 100 referred to herein may have a non-circular shape, such as a rectangular substrate for a flat panel display, etc., as well as other shapes.

[0030] In some embodiments, one or more of the material layers 103 being processed may include a stack of materials. For example, in the case of 3D NAND integrated circuit manufacturing, the material layer 103 being processed may include an ONON stack (oxide / nitride stack) and / or an OPOP stack (oxide / polysilicon stack). The ONON stack is a vertical stack of alternating oxide films and nitride films. The OPOP stack is a vertical stack of alternating oxide films and polysilicon films. Depending on the memory density of the 3D NAND integrated circuit, each of the ONON stack and the OPOP stack may contain up to 60 or more film layers. The 3D NAND integrated circuit also includes a channel formed to extend vertically through the entire ONON stack or OPOP stack. The channel is partially formed by etching down through the channel hole of the ONON stack or OPOP stack. At full depth, the aspect ratio of the channel hole (i.e., the ratio of the hole depth to the hole width (hole depth: hole width)) can be as high as 40:1 or greater. One challenge in manufacturing 3D NAND integrated circuits is to etch the channel hole to the maximum depth.

[0031] Figure 1B Shown through Figure 1AFIG. 1 is a vertical cross-section of a segment of a wafer 100 in which a patterned and developed hard mask material 105 is deposited on the top surface of the wafer 100, i.e., on the exposed top surface of the processing material layer 103. The hard mask material 105 is patterned and developed to expose an area 106 of the top surface of the processing material layer 103 where a hole is to be etched, such as an area 106 where a channel hole for 3D NAND integrated circuit fabrication is to be etched. During the plasma etching process for forming the hole at the area 106, the hard mask material 105 is intended to protect other areas of the processing material layer 103 covered by the hard mask material 105.

[0032] When plasma etching holes on region 106, material within the processing material layer 103 at region 106 will be removed at a first etch rate, and hard mask material 105 will be removed at a second etch rate. The selectivity of the plasma etching process is the ratio of the first etch rate to the second etch rate, i.e., the ratio of the etch rate through the processing material layer 103 to the etch rate of the hard mask material 105. The selectivity should be high enough so that a target etch depth can be achieved at region 106 before the hard mask material 105 is removed to the extent that the hard mask material 105 can no longer provide protection to the underlying processing material layer 103.

[0033] like Figure 1B As shown, hard mask material 105 is deposited with an initial thickness 107A. Figure 1C After the hole has been etched to a partial depth 109A at region 106, Figure 1B A vertical cross section of a segment of wafer 100 . Figure 1C It is also shown that when the hole reaches the partial depth 109A, the hard mask material 105 has been reduced to a thickness 107B. Figure 1D After further etching and when the hard mask material 105 is completely removed, the Figure 1C A vertical cross section of a segment of a wafer 100. Figure 1D As shown, the hole is etched only to a partial depth 109B at region 106. However, the hole is specified to be etched through the entire depth 104 of the material layer 103 being processed at region 106. Figures 1A-1D In the example of FIG. 1 , the hard mask material 105 may not provide sufficient selectivity to completely etch the holes at the region 106 .

[0034] In the 3D NAND integrated circuit manufacturing process, a fluorine-based plasma etching process is used to form a channel hole with a very high aspect ratio through the ONON and / or OPOP stack. Some carbon-containing hard mask materials have been used in fluorine-based plasma etching processes to form channel holes, such as carbon-based hard mask materials and / or doped carbon-based hard mask materials and / or metal carbide hard mask materials. These carbon-containing hard mask materials will form carbon fluoride (CF4) in the presence of a fluorine-based plasma etching process. And, because carbon fluoride is volatile at room temperature, during the fluorine-based plasma etching process, carbon fluoride will be lost and the carbon-containing hard mask material will be removed accordingly. As the ONON and / or OPOP stack is formed to have a greater total vertical thickness, the etching depth required to form the channel hole through the ONON and / or OPOP stack becomes greater, and the etching selectivity using the carbon-containing hard mask material becomes too low to achieve the full etching depth in the presence of a fluorine-based plasma etching process. Furthermore, even highly selective hard mask materials of tungsten carbide can form volatile tungsten fluoride (WF6), resulting in insufficient etch selectivity, which can limit the number and overall vertical thickness of ONON and / or OPOP stacks.

[0035] In a fluorine-based plasma etching process, a carbon-containing hard mask material with an initial thickness of 2.5 microns provides a total etching depth of about 5 to 6 microns through the ONON stack. Therefore, in order to scale the thickness of the ONON stack from 5 to 6 microns to about 10 microns, the initial thickness of the carbon-containing hard mask material will need to be increased from 2.5 microns to more than 5 microns. However, this is not possible because the current maximum achievable initial thickness of the carbon-containing hard mask material is about 2.5 microns. Therefore, the use of a carbon-containing hard mask material in a fluorine-based plasma etching process to manufacture 3D NAND integrated circuits limits the total etch depth that can be achieved for forming channel holes, thereby limiting the total vertical thickness of the ONON and / or OPOP stacks, thereby limiting the achievable memory density.

[0036] In order to maximize the etch selectivity in fluorine-based plasma etching processes, it is of interest to use hard mask materials that do not form volatile fluoride byproducts. One material that can survive fluorine-based etchants is aluminum oxide (Al2O3). In fluorine-based plasma etching processes, aluminum oxide hard masks have high etching selectivity to silicon (Si), polycrystalline silicon (polySi), silicon oxide (SiO) and silicon nitride (SiN). Similarly, exposing aluminum oxide to fluorine-based etching processes will result in the formation of aluminum fluoride (AlF3), which is non-volatile and will persist and remain in place as a hard mask material. However, there are some challenges with using aluminum oxide as a hard mask material.

[0037] For example, one challenge of using aluminum oxide as a hard mask material is that it is difficult to deposit an aluminum oxide layer on a wafer without causing aluminum oxide to be deposited on other structures and components in the processing chamber. For example, when an aluminum oxide film is deposited on a wafer using a plasma chemical vapor deposition (PCVD) process, the aluminum oxide will also be deposited on chamber structures and components when exposed to the PCVD process. Since the dry cleaning method used to clean the processing chamber is fluorine-based, the dry cleaning method will cause the aluminum oxide to be converted to aluminum fluoride, which is non-volatile and difficult to clean itself. Therefore, it should be understood that it is problematic to deposit aluminum oxide directly on a wafer using a PCVD process due to concerns about cleaning aluminum oxide and aluminum fluoride from the processing chamber. Similarly, when an aluminum oxide film is grown on a wafer using an atomic layer deposition (ALD) process, aluminum oxide will also grow on chamber structures and components exposed to the ALD process. Therefore, as with the PCVD process, it should be appreciated that an ALD process that deposits aluminum oxide directly on a wafer is also problematic due to concerns about cleaning aluminum oxide and aluminum fluoride from the processing chamber. Another challenge of using aluminum oxide as a hard mask material is the difficulty in forming openings in the aluminum oxide through which the underlying material can be etched. More specifically, because aluminum oxide is inert to most etchants, it is difficult to etch openings through the aluminum oxide hard mask material at areas where the underlying in-process material layer is to be subsequently etched.

[0038] Disclosed herein is a method for using aluminum oxide as a hard mask material in a plasma etching process, more specifically in a fluorine-based plasma etching process. The method disclosed herein provides the use of aluminum oxide as a hard mask material while avoiding the challenges of the above-mentioned process chamber cleaning and hard mask opening. Specifically, the method disclosed herein includes forming a self-assembled anodic aluminum oxide (AAO) hard mask for etching high aspect ratio features into an underlying material layer in the process. The self-assembled AAO hard mask is formed by applying a positive voltage to an aluminum seed layer that is simultaneously exposed to an electrochemical solution. A patterned mask is formed above the aluminum seed layer so that the electrochemical solution contacts only the portion of the aluminum seed layer to be converted into the AAO hard mask. When the AAO hard mask is formed, holes are inherently formed in the AAO hard mask. The holes in the AAO hard mask extend through the AAO hard mask to expose the top surface of the underlying material layer in the process, and the high aspect ratio features will be etched into the material layer in the process. Like aluminum oxide, the AAO hard mask is inert to many etchant materials including fluorine. Thus, the AAO hard mask provides a high selectivity for etching high aspect ratio features using a fluorine-based plasma etching process. Likewise, in certain embodiments, the portion of the aluminum seed layer that is not converted to AAO can be in-situ oxidized (e.g., by a thermal oxidation process) to form a dense aluminum oxide film, which is used as a solid (i.e., non-perforated) high selectivity hard mask for etching high aspect ratio features using a fluorine-based plasma etching process.

[0039] Figure 2A A flow chart of a method for performing a plasma etching process according to some embodiments is shown, the method including forming and using AAO as a hard mask. The method includes operation 201 for providing a wafer 100 having one or more processing material layers 103 through which etch holes are formed. Figure 1A As described, a processing material layer 103 is formed on an underlying section 101 of a wafer 100, the underlying section 101 including underlying wafer materials, structures, and substrates. In some embodiments, such as in 3D NAND integrated circuit manufacturing, the processing material layer 103 includes an ONON stack and / or an OPOP stack. However, in various embodiments, the processing material layer 103 may substantially include any material or combination of materials through which holes are etched using a plasma-based etching process. The method continues with operation 203, in which an aluminum seed layer 301 is deposited above the top surface of the wafer 100, that is, above the top surface of the processing material layer 103 through which holes are etched. It should be understood that the aluminum seed layer deposited in operation 203 is aluminum metal (Al).

[0040] Figure 3A A vertical cross-section of a segment of wafer 100 is shown after completing operation 203 to deposit an aluminum seed layer 301 , according to some embodiments. Figure 3A An aluminum seed layer 301 is shown deposited on the material layer 103 being processed. In various embodiments, the aluminum seed layer 301 can have a thickness 303 ranging from about 100 nanometers to about 50 micrometers. In some embodiments, the thickness 303 of the aluminum seed layer 301 is about 2500 nanometers. It should be understood that the thickness 303 of the aluminum seed layer 301 can depend on the depth to be etched into the process material layer 103. In other words, because the thickness 303 of the aluminum seed layer 301 is associated with the thickness of the AAO hard mask to be formed later in the method, the desired thickness 303 of the aluminum seed layer 301 can depend on the etch selectivity provided by the AAO hard mask and the depth to be etched into the material layer 103 being processed. In some embodiments, it is meaningful to form the thickness 303 of the aluminum seed layer 301 as small as possible to reduce the overall aspect ratio of the features to be etched through the holes in the AAO hard mask formed by the aluminum seed layer 301 into the underlying material layer 103 being processed. In some embodiments, the aluminum seed layer 301 is deposited on the wafer 100 using a sputtering process. It should be understood that the aluminum seed layer 301 can be deposited on the wafer 100 in a tool / chamber separate from the plasma etch processing chamber.

[0041] The method continues with operation 205 by depositing a layer of photoresist material 305 on a top surface of the aluminum seed layer 301 . Figure 3B 205 to deposit a layer of photoresist material 305 after completing operation 205 according to some embodiments. Figure 3A 1. A vertical cross section of a segment of the wafer 100 shown. In operation 207, the photoresist material 305 is patterned and developed to expose / demonstrate portions of the aluminum seed layer 301 in a prescribed area 309 where a hole pattern is to be etched through the underlying in-process material layer 103. It should be understood that the photoresist material 305 remains on portions of the aluminum seed layer 301 that are not in the prescribed area 309 where a hole pattern is to be etched through the underlying in-process material layer 103. For example, in 3D NAND integrated circuit manufacturing, during the memory hole etching process, the photoresist material 305 can be patterned and developed to protect the peripheral area around the memory array so that the peripheral area around the memory array can be opened in a later manufacturing operation to form the desired gap and stair structure. Therefore, in this example, the photoresist material 305 can be patterned and developed to protect areas of the wafer 100 that are not the prescribed area 309 where the memory hole etching is to be performed. Figure 3C After completing operation 207 to pattern and develop the photoresist material layer 305, the Figure 3B A vertical cross section of a segment of wafer 100 is shown. Figure 3C In the example of FIG. 2 , the patterning and development of the photoresist material 305 in operation 207 exposes / exposes the top surface of the aluminum seed layer 301 in a specified area 309 where a hole pattern will be etched through the underlying processing material layer 103. In various embodiments, the photoresist material 305 can be a positive photoresist material or a negative photoresist material 305. For example, in various embodiments, the photoresist material 305 can be a positive photoresist (e.g., Shepley 1813), or a negative photoresist material (e.g., SU8), etc.

[0042] From operation 207, the method continues to operation 209, which electrochemically converts the exposed portion of the aluminum seed layer 301 into anodized aluminum oxide (AAO) 307. The AAO 307 includes a pattern of holes extending through the AAO 307 to expose a region 308 of the top surface of the underlying processing material layer 103. Figure 3D FIG. 2 shows a schematic diagram of a process for electrochemically converting an exposed portion of the aluminum seed layer 301 in a defined region 309 to AAO 307 to expose a region 308 of a top surface of an underlying in-process material layer 103 during operation 209, according to some embodiments. Figure 3C A vertical cross-section of a segment of wafer 100 is shown. Figure 3E 307 to expose / expose an area 308 of the top surface of the underlying in-process material layer 103, after completing operation 209 of electrochemically converting the exposed portion of the aluminum seed layer 301 in the specified area 309 to AAO 307, according to some embodiments. Figure 3C A top view of a section of wafer 100 is shown.

[0043] Figure 2B A more detailed flow chart of operation 209 for electrochemically converting an exposed portion of the aluminum seed layer to AAO 307 is shown in accordance with some embodiments. Operation 209 includes operation 209A for establishing an electrical connection between a power source 311 and a portion of the aluminum seed layer 301 that is exposed through an opening in the photoresist material 305 in the prescribed area 309. Operation 209 also includes operation 209B for applying an electrochemical solution 310 to the portion of the aluminum seed layer 301 that is exposed through the opening in the photoresist material 305 in the prescribed area 309. Operation 209 also includes operation 209C for operating the power source 311 to apply a positive voltage to the portion of the aluminum seed layer 301 that is exposed through the opening in the photoresist material 305 and to which the electrochemical solution 310 is applied in operation 209B to convert the portion of the aluminum seed layer 301 that is exposed through the opening in the photoresist material 305 to AAO 307. In operation 209C, the aluminum seed layer 301 functions as a physically continuous conductive layer such that current can flow through the aluminum seed layer 301 throughout the wafer 100. In some embodiments, the aluminum seed layer 301 can be contacted at multiple locations around the periphery of the wafer 100 to provide a substantially uniform current distribution through the aluminum seed layer 301 throughout the wafer 100. In some embodiments, a ring electrode can be used to contact the aluminum seed layer 301 around the periphery of the wafer 100 to provide a substantially uniform current distribution through the aluminum seed layer 301 throughout the wafer 100. In this manner, operation 209A can include establishing a physically continuous electrical connection between the power source 311 and the aluminum seed layer 301 around the entire periphery of the wafer 100.

[0044] During operation 209, AAO 307 is generated by removing oxygen-containing anions (O 2- and / or OH - ) migrates inwardly into the aluminum seed layer 301 and grows at the interface between the aluminum metal (of the aluminum seed layer 301) and the AAO 307. In addition, as the AAO 307 grows inwardly into the aluminum seed layer 301 from the electrochemical solution 310, the aluminum cations (Al 3+) is released from the aluminum seed layer 301 into the electrochemical solution 310. Therefore, during the conversion of the aluminum seed layer 301 to AAO 307, in the presence of a sufficiently high electric field provided by a positive voltage applied to the aluminum seed layer 301, the Al 3+ Cations and oxygen-containing anions (O 2- and / or OH - ) all move in AAO307.

[0045] In various embodiments, the electrochemical solution 310 includes one or more acidic electrolytes, such as phosphoric acid (H3PO4), sulfuric acid (H2SO4), oxalic acid (H2C2O4), selenic acid (H2SeO4), chromic acid (H2CrO4), malonic acid (C3H4O4), tartaric acid (C4H6O6), citric acid (C6H8O7), malic acid (C4H6O5), etc. The composition of the electrochemical solution is provided in "Porous Anodic Aluminum Oxide: Anodization and Templated Synthesis of Functional Nanostructures," by Woo Lee and Sang-Joon Park, Chemical Reviews 2014, 114, pages 7487-7556, American Chemical Society Publications, June 13, 2014 (hereinafter referred to as "Lee"). In addition, Lee provides an example of a process for forming AAO from an aluminum metal layer that can be used to perform operation 209.

[0046] In the process of converting the aluminum seed layer 301 into the AAO 307 , the reactions shown in reaction formulas 1 and 2 occur at the interface between the aluminum metal (in the aluminum seed layer 301 ) and the AAO 307 formed from the aluminum seed layer 301 .

[0047] Reaction 1.

[0048]

[0049] Reaction 2.

[0050]

[0051] In the process of converting the aluminum seed layer 301 into the AAO 307 , the reactions shown in reaction formulas 3 to 7 may occur at the interface between the electrochemical solution 310 and the AAO 307 formed from the aluminum seed layer 301 .

[0052] Reaction 3.

[0053]

[0054] Reaction 4.

[0055]

[0056] Reaction 5.

[0057]

[0058] Reaction 6.

[0059]

[0060] Reaction 7.

[0061]

[0062] The photoresist material 305 is used to prevent the electrochemical solution 310 from contacting the aluminum seed layer 301 at locations on the wafer 100 that are not within the specified area 309 where the AAO 307 is to be formed. Figure 2A and 2B In the method, the photoresist material 305 is chemically stable when exposed to the electrochemical solution 310. For example, if the electrochemical solution 310 is acidic or basic, the photoresist material 305 is chemically stable in the presence of the acidity or basicity of the electrochemical solution 310. Similarly, in Figure 2A and 2B In the method, the photoresist material 305 is selected to prevent ion exchange between the electrochemical solution 310 and the aluminum seed layer 301 below the photoresist material 305 through the photoresist material 305. Figure 2A and 2B In the method, the photoresist material 305 is capable of blocking the transfer of both electrons and ions between the electrochemical solution 310 and the aluminum seed layer 301 below the photoresist material 305. Therefore, although the current flows through the portions of the aluminum seed layer 301 below the photoresist material 305, these portions of the aluminum seed layer 301 below the photoresist material 305 will not be converted into AAO 307 because they cannot be contacted by the electrochemical solution 310 and cannot exchange electrons and / or ions with the electrochemical solution 310. In this way, AAO 307 is formed in a self-assembled manner in the prescribed area 309 where the aluminum seed layer 301 is exposed to the electrochemical solution 310 through the opening in the photoresist material 305.

[0063] It should be understood that operations 209A, 209B, and 209C may be performed in any order, sequentially, or simultaneously, so as to meet the following two conditions for the formation of AAO 307: 1) the portion of the aluminum seed layer 301 exposed through the opening in the photoresist material 305 is in contact with the electrochemical solution 310; and 2) a positive voltage is applied to the portion of the aluminum seed layer 301 exposed through the opening in the photoresist material 305. When these two conditions for the formation of AAO 307 are met, the portion of the aluminum seed layer 301 exposed through the opening in the photoresist material 305 is converted into AAO 307. In other words, the process of electrochemically forming AAO 307 has two required conditions: 1) electrical contact between the power supply 311 and the aluminum seed layer 301, so that current can be applied to the aluminum seed layer 301 in the specified area 309, where AAO 307 will be formed, and 2) direct contact between the electrochemical solution 310 and the aluminum seed layer 301 will be formed in the specified area 309 where AAO 307 will be formed, so as to achieve ion exchange between the aluminum seed layer 301 and the electrochemical solution 310 in the specified area 309.

[0064] When a positive voltage is applied to the aluminum seed layer 301, the portion of the aluminum seed layer 301 exposed to the electrochemical solution 310 in the prescribed area 309 will oxidize to form AAO 307 having a physical structure including hexagonal pores. In various embodiments, the positive voltage applied to the aluminum seed layer 301 in operation 209C can be in a range extending from about 5 volts (V) to about 500 V. Moreover, in some embodiments, the positive voltage can be applied to the aluminum seed layer 301 in an inclined manner (i.e., an increasing manner and / or a decreasing manner) during the formation of the AAO 307. In some embodiments, the application of the positive voltage to the aluminum seed layer 301 in an inclined manner can be defined / controlled to adjust the profile of the AAO 307 pores. Lee provides an example of a voltage that can be used in performing operation 209C.

[0065] The hexagonal pattern of holes in AAO 307 is a result of the manner in which grain boundaries are formed within AAO 307. Thus, the holes are self-aligned to form the hexagonal pattern of holes in AAO 307. It should be understood that operation 209 may include controlling various parameters, such as the composition and / or temperature and / or pressure and / or flow rate of electrochemical solution 310, as well as controlling the temperature of aluminum seed layer 301 and the voltage applied to aluminum seed layer 301, to control the physical properties of AAO 307. The formation of AAO 307 may be controlled so that the holes in the hexagonal pattern of holes extend completely through AAO 307 to expose / expose area 308 on the top surface of the underlying process material layer 103. The characteristics of the hexagonal pattern of holes in AAO 307, namely the hole size (diameter) and the hole spacing (P) (center-to-center spacing), depend on the voltage applied to the aluminum seed layer 301 and the composition of the electrochemical solution 310 in operation 209C. Thus, the pore size and pore spacing (P) in AAO 307 can be adjusted by controlling the voltage applied to the aluminum seed layer 301 and the composition of the electrochemical solution 310 in operation 209C. In some embodiments, AAO 207 can be formed to have a pore size in a range extending from about 10 nanometers to about 100 nanometers. In some embodiments, AAO 207 can be formed to have a pore size in a range extending from about 80 nanometers to about 100 nanometers. In some embodiments, AAO 207 can be formed to have a pore spacing (P) in a range extending from about 150 nanometers to about 200 nanometers (see Figure 3E ).

[0066] It should be understood that AAO 307 is resistant to fluorine-based etchants. As with conventional aluminum oxide, exposure of AAO 307 to a fluorine-based etching process results in the formation of aluminum fluoride, which is not volatile and will persist and remain in place as a hard mask material. Therefore, in a fluorine-based plasma etching process, AAO 307 can be used as a hard mask with high etch selectivity to silicon (Si), polycrystalline silicon (polySi), silicon oxide (SiO), and silicon nitride (SiN). By using AAO 307 as a hard mask, the hexagonal pattern of holes in AAO 307 defines the geometry and spacing of the holes that will be etched into the underlying material layer 103 being processed.

[0067] Starting from operation 209, Figure 2A The method proceeds to operation 211 to remove the photoresist material 305 from the aluminum seed layer 301. Operation 211 may be performed using a stripping process suitable for the photoresist material 305. Figure 3F FIG. 2 shows a schematic diagram of a process for removing the photoresist material 305 from the aluminum seed layer 301 after completing operation 211 according to some embodiments. Figure 3DA vertical cross-section of the segment of wafer 100 is shown.

[0068] Like aluminum oxide and AAO, aluminum is also resistant to etching by fluorine-based etchant materials. Therefore, in some embodiments, after removing the photoresist material 305 in operation 211, the aluminum seed layer 301 can be left intact, i.e., like aluminum, during a subsequent plasma etching process. In these embodiments, the method proceeds from operation 211 to operation 215, where holes 313 are etched through the underlying process material layer 103 at the areas 308 exposed through the holes in the AAO 307. Figure 3G 307, after completing operation 215 to etch holes through the underlying in-process material layer 103 in the areas exposed by the holes in the AAO 307, according to some embodiments. Figure 3F A vertical cross-section of the segment of wafer 100 is shown.

[0069] In some embodiments, after removing the photoresist material 305 in operation 211, the method can proceed to operation 213, where the portion of the aluminum seed layer 301 that has not been converted to AAO 307 is oxidized to form an aluminum oxide film (dense film) 301A, and then a subsequent plasma etching process is performed. In some embodiments, operation 213 includes performing a thermal oxidation process on the portion of the aluminum seed layer 301 that has not been converted to AAO 307. It should be understood that the aluminum oxide film 301A formed in operation 213 is a solid film that does not have holes like AAO 307. By performing operation 213 to oxidize the portion of the aluminum seed layer 301 that has not been converted to AAO 307, the heterogeneity of the hard mask is reduced. Therefore, as opposed to a hard mask (in the form of AAO 307) that is a heterogeneous combination of aluminum and aluminum oxide, the aluminum oxide hard mask can be considered to define the process of etching holes 313 through the underlying processing material layer 103 in operation 215.

[0070] Figure 3H FIG. 2 shows a method of forming a dense aluminum oxide film (dense film) 301A by oxidizing the portion of the aluminum seed layer 301 that has not been converted into AAO 307 to form a dense aluminum oxide film (dense film) 301A according to some embodiments. Figure 3F A vertical cross-section of the section of wafer 100 is shown. After operation 213, the method proceeds to operation 215 to etch holes 313 through the underlying in-process material layer 103 at the areas 308 exposed through the holes in AAO 307, according to some embodiments. Fig. 3I 307 after completing operation 215 to etch holes 313 through the underlying in-process material layer 103 in the area exposed through the holes in the AAO 307. Figure 3HA vertical cross-section of the segment of wafer 100 is shown.

[0071] In some embodiments, the plasma etching process performed in operation 215 can be performed in an anisotropic manner to etch holes 313 with high aspect ratios. Even in the presence of fluorine-based etchant materials, the aluminum-based hard mask (which includes AAO 307 and a portion of aluminum and / or dense film aluminum oxide) can provide an etching selectivity of up to 50:1 or more. This high etching selectivity of the aluminum-based hard mask enables deeper etching through the underlying material layer 103 in the process because the aluminum-based hard mask will remain unchanged for a longer etching time. Moreover, the high etching selectivity of the aluminum-based hard mask allows a thinner aluminum-based hard mask compared to a carbon-based hard mask. The reduced thickness of the aluminum-based hard mask helps to reduce the overall aspect ratio within the region 308 where the hole 313 is etched at the end of the etching process. And, because the aluminum-based hard mask reduces the overall aspect ratio of the hole 313 at the end of the etching process, the time required to complete the etching process can be reduced. As previously described, the thickness 303 of the aluminum seed layer 301 is related to the thickness of the aluminum-based hard mask. In some embodiments, the thickness of the aluminum-based hard mask is in a range extending from about 100 nanometers to about 50 micrometers. In some embodiments, the thickness of the aluminum-based hard mask is about 2500 nanometers.

[0072] After completing operation 215 to etch the hole 313 through the underlying in-process material layer 103, the method proceeds to operation 217 to remove the aluminum seed layer 301, AAO 307, and aluminum oxide 301A (if present) from the underlying in-process material layer 103. Operation 217 may include performing a wet cleaning process (using an acidic cleaning solution). The wet cleaning process may be performed in a wet cleaning chamber separate from the processing chamber in which the plasma-based etching process is performed. The wet cleaning process may remove the aluminum seed layer 301, AAO 307, and aluminum oxide 301A (if present) without corroding silicon, silicon oxide, and silicon nitride that may be present on the wafer 100. Figure 3J FIG. 2 shows a process of removing the aluminum seed layer 301, the AAO 307, and the aluminum oxide 301A (if present) from the material layer 103 under processing after operation 217 is completed. Figure 3G Or a vertical cross section of the segment of the wafer 100 shown in 3I.

[0073] In some embodiments, if there is chemical incompatibility between the photoresist material 305 and the electrochemical solution 310, an electrochemically compatible mask material 501 may be deposited on the aluminum seed layer 301 prior to depositing the photoresist material 305. The photoresist material 305 is then patterned and developed to serve as a mask to pattern the electrochemically compatible mask material 501, thereby exposing the prescribed areas 309 of the aluminum seed layer 301 where the AAO 307 is to be formed. Then, in various embodiments, the photoresist material 305 may be allowed to remain or may be removed when the electrochemical solution 310 is applied to the wafer 100 in operation 209. The electrochemically compatible mask material 501 is chemically compatible with the electrochemical solution 310 and is capable of preventing electron and / or ion exchange between the electrochemical solution 310 and the aluminum seed layer 301 during operation 209, thereby forming the AAO 307 in the prescribed areas 309.

[0074] Figure 4 A flow chart of a method for performing a plasma etching process including forming and using AAO as a hard mask and including using an electrochemically compatible mask material 501 is shown according to some embodiments. Figure 4 Operations 201 and 203 are related to Figure 2A Same as described. Figure 4 In the method of , after operation 203 , the method proceeds to operation 401 to deposit a layer of electrochemically compatible mask material 501 on the top surface of the aluminum seed layer 301 . Figure 5A After completing operation 401 to deposit a layer of electrochemically compatible mask material 501, a Figure 3A 1. A vertical cross section of the section of wafer 100 is shown. Electrochemically compatible mask material 501 is electrically insulating and substantially inert to the acid in electrochemical solution 310. In some exemplary embodiments, electrochemically compatible mask material 501 is formed as a thin layer of silicon dioxide (SiO2) having a thickness of about 30 nanometers to about 40 nanometers. However, it should be understood that in other embodiments, electrochemically compatible mask material 501 can be formed of a material other than silicon dioxide having an appropriate thickness to electrically insulate aluminum seed layer 301 from electrochemical solution 310.

[0075] Starting from operation 401 , the method continues with operation 403 to deposit a layer of photoresist material 305 on a top surface of the electrochemically compatible mask material 501 . Figure 5B After completing operation 403 to deposit a photoresist material layer 305, the Figure 5A1 is a vertical cross-section of the section of wafer 100 shown. In operation 405, photoresist material 305 is patterned and developed to expose / expose portions of electrochemically compatible mask material 501 that overlie prescribed areas 309 where a hole pattern is to be etched through the underlying in-process material layer 103. It should be understood that photoresist material 305 remains on portions of electrochemically compatible mask material 501 that do not overlie prescribed areas 309 where a hole pattern is to be etched through the underlying in-process material layer 103. Figure 5C After completing operation 405 to pattern and develop the photoresist material layer 305, the Figure 5B The vertical cross section of the section of wafer 100 is shown. Figure 5C In the example of FIG. 4 , patterning and developing the photoresist material 305 in operation 405 uncovers / exposes portions of the electrochemically compatible mask material 501 covering a defined area 309 where a hole pattern is to be etched through the underlying processing material layer 103 .

[0076] The method proceeds to operation 407 to remove the portion of the electrochemically compatible mask material 501 exposed through the opening formed in the photoresist material layer 305 in operation 405. In operation 407, the portion of the electrochemically compatible mask material 501 is removed to expose the aluminum seed layer 301 in the specified area 309 where the hole pattern will be etched through the underlying processing material layer 103. Figure 5D 5. After completing operation 407 to remove the portion of electrochemically compatible mask material 501 in the specified area 309, according to some embodiments, Figure 5C A vertical cross-section of the section of the wafer is shown, in which a pattern of holes will be etched through the underlying layer of material being processed 103 in a defined area 309 .

[0077] In some embodiments, after operation 407, the method may optionally proceed to operation 409 to remove the photoresist material 305 from the electrochemically compatible mask material 501 throughout the wafer 100. Starting from operation 409, as described with respect to Figure 2A and 2B As depicted, the method proceeds to operation 209 to electrochemically convert the exposed portion of the aluminum seed layer 301 to AAO 307. However, in some embodiments, the photoresist material 305 may be allowed to remain in place on the electrochemically compatible mask material 501. In these embodiments, the method proceeds from operation 407 to operation 209.

[0078] Figure 5EFIG. 2 shows a schematic diagram of a process for electrochemically converting an exposed portion of the aluminum seed layer 301 in a defined region 309 to AAO 307 to expose a region 308 of a top surface of an underlying in-process material layer 103 during operation 209, according to some embodiments. Figure 5D A vertical cross-section of a segment of wafer 100 is shown. Fig. 5F 307 to expose / expose an area 308 of the top surface of the underlying in-process material layer 103, after completing operation 209 of electrochemically converting the exposed portion of the aluminum seed layer 301 in the specified area 309 to AAO 307, according to some embodiments. Figure 5E 1. A top view of a section of the wafer 100 is shown. After operation 209, the method proceeds to operation 411 to remove any remaining photoresist material 305 (if still present) and electrochemically compatible mask material 501 from the wafer 100, i.e., from the aluminum seed layer 301. Then, as with respect to Figure 2A As described, the method continues with operation 213 (optional), operation 215, and operation 217.

[0079] It should be understood that the method disclosed herein using AAO as a hard mask in a plasma-based etching process provides high etching selectivity to enable etching of high aspect ratio features, such as those encountered in etching memory holes through ONON and / or OPOP stacks in 3D NAND integrated circuit manufacturing. Compared with carbon-based hard mask materials such as carbon or metal carbides, AAO hard masks have much higher etching selectivity. Moreover, as disclosed herein, AAO hard masks can be formed on wafers using electrochemical processes to avoid chamber cleaning issues associated with PCVD and / or ALD aluminum oxide deposition on wafers. In addition, since the self-aligned hexagonal pattern of holes appearing in the AAO hard mask defines an opening in the AAO hard mask through which the underlying processing layer is etched, there is no need to perform a separate lithography-based process to create an opening in the AAO hard mask. The formation and removal of the AAO hard mask can be accomplished using a wet processing method.

[0080] According to the methods disclosed herein, a hard mask formed by combining AAO with aluminum and / or aluminum oxide provides higher etching selectivity (up to 50 to 1 or more) in a fluorine-based plasma etching process compared to a carbon-based hard mask that can provide an etching selectivity of up to 5 to 1. Moreover, according to the methods disclosed herein, an electrochemical process enables the formation of an AAO hard mask in a self-aligned manner, wherein holes exist within the AAO hard mask. Therefore, it is not necessary to perform photolithographic patterning of the individual holes within the AAO hard mask as required when using other non-AAO hard mask materials. More specifically, photolithography is used to expose a specified area where the AAO hard mask will be formed, but there is no need to subsequently form openings through the AAO material, i.e., individual holes, because the openings through the AAO material are inherently formed when the AAO material is formed. Therefore, it should be understood that the use of an AAO hard mask as disclosed herein alleviates photolithographic challenges, particularly when etching closely spaced small-diameter holes such as in the manufacture of 3D NAND integrated circuits.

[0081] For the purpose of illustration and description, the foregoing description of the embodiment has been provided. It is not intended to be exhaustive or limit the present disclosure. The individual elements or features of a particular embodiment are generally not limited to that particular embodiment, but are interchangeable where applicable, and can also be used in the selected embodiment even if not specifically shown or described. Also can be changed in many ways. Such modification should not be considered as departing from the present disclosure, and all such modifications are intended to be included in the scope of the present disclosure.

[0082] Although the above disclosure has been described in detail for the purpose of clear understanding, it will be apparent that certain changes and modifications may be made within the scope of the embodiments disclosed herein. Therefore, the embodiments herein are to be considered illustrative rather than restrictive, and the disclosure is not limited to the details given herein, but may be modified within the scope and equivalent range of the described embodiments.

Claims

1. A method for performing a plasma etching process, comprising: depositing an aluminum seed layer on a top surface of the wafer; depositing a layer of photoresist material on the aluminum seed crystal layer; patterning and developing the layer of photoresist material to expose one or more portions of the aluminum seed layer through openings in the photoresist material; performing an electrochemical conversion process on the wafer to electrochemically convert the one or more portions of the aluminum seed layer exposed through the openings in the photoresist material into anodized aluminum oxide, wherein the anodized aluminum oxide includes a pattern of holes extending through the anodized aluminum oxide to expose an area of ​​the top surface of the wafer underlying the aluminum seed layer; removing the photoresist material from the wafer; as well as The wafer is exposed to a plasma to etch holes into the wafer at the areas of the top surface of the wafer exposed by the pattern of holes in the anodized aluminum.

2. A method according to claim 1, wherein the electrochemical conversion process includes establishing an electrical connection between a power source and the aluminum seed layer, and wherein the electrochemical conversion process includes applying an electrochemical solution to the one or more portions of the aluminum seed layer exposed through the openings in the photoresist material, wherein the electrochemical conversion process includes operating the power source to apply a positive voltage to the aluminum seed layer so as to convert the one or more portions of the aluminum seed layer exposed to the electrochemical solution through the openings in the photoresist material into anodized aluminum.

3. The method according to claim 2, wherein: The electrochemical solution includes an acidic component.

4. The method according to claim 3, wherein the acidic component is one or more of phosphoric acid, sulfuric acid, oxalic acid, selenic acid, chromic acid, malonic acid, tartaric acid, citric acid and malic acid.

5. The method according to claim 2, wherein: The positive voltage is within a range extending from 5 volts to 500 volts.

6. The method of claim 2, wherein establishing the electrical connection between the power source and the aluminum seed layer comprises electrically connecting the power source to the aluminum seed layer at multiple locations around the periphery of the wafer to achieve uniform current distribution through the aluminum seed layer.

7. The method of claim 2, wherein establishing the electrical connection between the power source and the aluminum seed layer comprises establishing a physically continuous electrical connection between the power source and the aluminum seed layer around the entire periphery of the wafer.

8. The method according to claim 2, further comprising: The composition of the electrochemical solution and the positive voltage applied to the aluminum seed layer are controlled to control physical characteristics of the pore pattern in the anodized aluminum oxide, wherein the physical characteristics of the pore pattern include pore diameter and pore spacing.

9. The method according to claim 8, wherein: The pore diameters range from 10 nanometers to 100 nanometers.

10. The method according to claim 8, wherein: The inter-aperture spacing is in the range extending from 150 nanometers to 200 nanometers.

11. The method according to claim 1, wherein: The aluminum seed layer is deposited to have a thickness in a range extending from 100 nanometers to 50 micrometers.

12. The method according to claim 1, wherein: The aluminum seed layer provides a physically continuous conductive layer during the electrochemical conversion process.

13. The method of claim 2, wherein the photoresist material is chemically stable when exposed to the electrochemical solution.

14. The method according to claim 2, wherein: The photoresist material is configured to prevent ion exchange through the photoresist material between the electrochemical solution and portions of the aluminum seed layer covered by the photoresist material.

15. The method according to claim 1, further comprising: After etching the holes into the wafer, the anodized aluminum oxide and the aluminum seed layer are removed from the wafer.

16. The method of claim 1, further comprising: Prior to exposing the wafer to the plasma, a remaining portion of the aluminum seed layer is oxidized into a dense aluminum oxide film, the remaining portion of the aluminum seed layer corresponding to areas of the aluminum seed layer that are not converted to anodized aluminum oxide. 17 . The method of claim 16 , wherein oxidizing the remaining portion of the aluminum seed layer comprises performing a thermal oxidation process.

18. A method for performing a plasma etching process, comprising: depositing an aluminum seed layer on a top surface of the wafer; depositing a mask material layer on the aluminum seed crystal layer; depositing a photoresist material layer on the mask material layer; patterning and developing the layer of photoresist material to expose one or more portions of the mask material; removing the one or more portions of the mask material to expose corresponding portions of the aluminum seed layer; performing an electrochemical conversion process on the wafer to electrochemically convert the exposed corresponding portions of the aluminum seed layer into anodized aluminum oxide, wherein the anodized aluminum oxide includes a pattern of holes extending through the anodized aluminum oxide to expose an area of ​​the top surface of the wafer underlying the aluminum seed layer; as well as The wafer is exposed to a plasma to etch holes into the wafer at the areas of the top surface of the wafer exposed by the pattern of holes in the anodized aluminum.

19. The method according to claim 18, further comprising: The photoresist material is removed from the wafer after removing the one or more portions of the mask material and before performing the electrochemical conversion process on the wafer.

20. The method of claim 19, further comprising: The mask material is removed from the wafer after performing the electrochemical conversion process on the wafer and before exposing the wafer to the plasma to etch holes into the wafer.