Cleanable filter media

By using synthetic organic polymer fiber nonwoven fabrics and forming an embossed pattern filter media, the existing filter media is solved, and efficient and robust filtration performance and energy efficiency are achieved.

CN112316559BActive Publication Date: 2024-11-26JOHNS MANVILLE CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010749874.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-31
Filing Date
2020-07-30
Publication Date
2024-11-26
Estimated Expiration
2040-07-30

AI Technical Summary

Technical Problem

Existing filter media is prone to clogging during use, resulting in an increase in pressure drop, requiring frequent replacement or cleaning, and the number of cleaning cycles is limited, which affects filtration efficiency and energy efficiency.

Method used

The non-woven fabric of synthetic organic polymer fibers is used as the filter medium, and is consolidated by thermoplastic adhesives and mechanical means to form an embossed patterned non-woven fabric to ensure that the media maintains good filtration performance during multiple cleaning cycles.

Benefits of technology

The number of cleaning cycles of the filter media is extended, the filtration efficiency and energy efficiency are improved, the cost of replacement and cleaning is reduced, and the robustness and dust capacity of the filter are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112316559B_ABST
    Figure CN112316559B_ABST
Patent Text Reader

Abstract

The present invention relates to a cleanable filter medium. The present invention relates to a cleanable 3D filter medium, a method for manufacturing the filter and the use of the filter. The filter medium according to the present invention comprises at least one fabric layer, which is a non-woven fabric of synthetic organic polymer fibers. The non-woven fabric has an embossed pattern, wherein the non-woven fabric has a thickness D in the non-embossed area and a thickness d in the embossed area, and the ratio d / D is a compression factor CF, and the compression factor CF is in the range of 0.2≤CF≤0.5. The filter medium according to the present invention can be cleaned and used in filter systems for air / gas and liquid filtration, in particular for the motor vehicle industry, air conditioning systems, cabin filters, pollen filters, clean room filters, household filters, etc., as well as as oil filters and hydraulic filters, thereby removing solids from air / gas and liquids.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a cleanable 3D filter medium, a method for manufacturing the filter and the use of the filter. Background Art

[0002] Filters have been used for a long time in various applications. For example, air filters are used in the automotive industry, air conditioning systems, cabin filters, pollen filters, clean room filters, household filters, etc. In addition, filters have also been used for filtering liquid media for many years. Examples of these include oil filters and hydraulic filters.

[0003] Filter media are described, for example, in EP-A-0878226, EP-A-1134013, DE-A-2000139245 and EP-A-0980700.

[0004] Depending on the field of application, the filter can be adjusted to achieve satisfactory filtration efficiency and service life. Removing solids from liquid and / or gaseous fluids is the most common field of filtration. Usually, liquid and / or gas feeds containing such solid particles cannot pass through the lattice structure of the filter, and the filter medium will become blocked as the use time increases. Blockage will cause a pressure drop, which means that an increased pressure is required to pass the same volume through the filter, resulting in higher energy consumption. Therefore, it is necessary to replace the filter with a new filter or to clean the filter by removing the filter material from the filter. All these activities are time-consuming and expensive measures, leading to the need for improved cleanable filter media. Such cleanable filter media are usually cleaned by simply reversing the flow direction of the filtered fluid, and a pulse-pressurized filtered fluid is usually used to remove the filtered solids from the filter.

[0005] The present inventors have discovered that it is possible to provide a cleanable filter media that is robust enough to withstand multiple cleaning cycles while maintaining good filtration properties, such as filtration efficiency, dust holding capacity, and energy efficiency. Summary of the invention

[0006] It is therefore an object of the present invention to provide a filter medium comprising:

[0007] a) at least one textile layer (layer 1), said textile layer being a non-woven fabric of synthetic organic polymer fibers,

[0008] a1) The nonwoven fabric has a thickness of 50 to 400 g / m 2 The weight per unit area,

[0009] a2) the fibers of the nonwoven fabric have a fineness in the range of 0.5 to 15 dtex,

[0010] a3) the nonwoven fabric is consolidated by thermoplastic adhesives and / or mechanical means, provided that the nonwoven fabric is not consolidated by needling and / or hydro-jet needling,

[0011] a4) the nonwoven fabric has an embossed pattern, the nonwoven fabric has a thickness of at least 50 L / m 2 Seconds, preferably 100L / m 2 Seconds and 2000L / m 2 Air permeability between seconds,

[0012] a5) the nonwoven fabric has an embossed pattern, and the surface area of ​​the embossed pattern of the nonwoven fabric is 7% to 30% of the total surface area of ​​the nonwoven fabric,

[0013] a6) Each individual embossed pattern surface area of ​​the nonwoven fabric is 0.4 to 5.6 mm 2 The surface area of

[0014] a7) The nonwoven fabric has a thickness D in the non-embossed area and a thickness d in the embossed area, and the ratio d / D is a compression factor CF, and the compression factor CF is in the range of 0.2≤CF≤0.5. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 Graph showing the residual pressure drop according to the VDI 3926 test procedure for three filter media made according to the invention (FI180036, FI180040 and FI180044) and one prior art media for comparison (778 / 250 standard).

[0016] Figure 2a One embodiment of forming an embossing pattern on a filter medium by a structured roller according to the present invention is shown.

[0017] Figure 2b Another embodiment of forming an embossing pattern on a filter medium by a structured roller according to the present invention is shown.

[0018] Figure 3 Exemplary embossing patterns are shown. DETAILED DESCRIPTION

[0019] Non-woven fabric (layer 1)

[0020] The textile layer used according to the invention is a nonwoven of synthetic organic polymer fibers which is preferably pleated.

[0021] The nonwoven fabric can be made of various synthetic organic polymer fibers from different polymers or different polymer classes. Moreover, the nonwoven fabric itself can also be made in a multi-layered manner. Here, the individual layers within the nonwoven fabric can differ in terms of the various selected synthetic polymer fibers and / or have various fiber diameters, but such parameters are within the ranges given for the nonwoven fabric.

[0022] The nonwoven fabric is a wet-laid nonwoven fabric, a dry-laid nonwoven fabric or a spunbond nonwoven fabric, which is consolidated by thermoplastic adhesives and / or mechanical means, provided that the nonwoven fabric is not consolidated by needling and / or spunlacing. The nonwoven fabric is preferably consolidated only by thermoplastic adhesives. The nonwoven fabric is preferably a short fiber nonwoven fabric and / or a spunbond nonwoven fabric. Spunbond nonwoven fabrics are usually referred to as spunbonds and are produced by random deposition of fresh melt-spun filaments. The filaments are continuous synthetic fibers consisting of a melt-spinnable polymer material.

[0023] Suitable synthetic organic polymer materials are, for example, thermoplastics, preferably polyamides, such as polyhexamethylene-diadipamide, polycaprolactam, aromatic polyamides or partially aromatic polyamides ("aramids"), aliphatic polyamides, such as nylon, partially aromatic polyesters or fully aromatic polyesters, aliphatic polyesters, polycarbonate (PC), polyphenylene sulfide (PPS), polyphenylene oxide (PPO), polystyrene (PS), polyvinylcarbazole (PVK), polyacetal (POM), polyarylether, polyarylethersulfone, polyethersulfone, polymers with ether and keto groups, such as polyetherketone (PEK) and polyetheretherketone (PEEK), polyolefins, such as polyethylene or polypropylene, or polybenzimidazoles. Particular preference is given to polyesters, polyolefins, for example polyethylene or polypropylene, or aromatic polyamides or partially aromatic polyamides ("aramids"), aliphatic polyamides, for example nylon.

[0024] The spunbond nonwoven fabric is preferably composed of melt-spinnable polyester. In principle, the polyester material can be any known type suitable for fiber manufacturing. Such polyester is mainly composed of components derived from aliphatic or aromatic dicarboxylic acids and aliphatic diols. Commonly used aromatic dicarboxylic acid components are divalent residues of benzene dicarboxylic acids, especially terephthalic acid and isophthalic acid; commonly used diols have 2 to 4 carbon atoms, of which ethylene glycol is particularly suitable. Spunbond fabrics composed of at least 85 mol % of polyethylene terephthalate are particularly advantageous. Then, the remaining 15 mol % are formed by dicarboxylic acid parts and diol parts, which act as so-called modifiers and enable those skilled in the art to specifically affect the physical and chemical properties of the filaments produced. Examples of such dicarboxylic acid units are residues of isophthalic acid or residues of aliphatic dicarboxylic acids such as glutaric acid, adipic acid and sebacic acid; examples of modifying glycol residues are those composed of long chain glycols (such as propylene glycol or butanediol), diethylene glycol or triethylene glycol or, if present in small amounts, polyethylene glycols having a molecular weight of about 500 to 2000.

[0025] Particular preference is given to polyesters which comprise at least 95 mol % of polyethylene terephthalate (PET), in particular those which consist of unmodified PET.

[0026] The polyester contained in the spunbond nonwoven fabric preferably has a molecular weight corresponding to an intrinsic viscosity (IV) of 0.6 to 1.4, the intrinsic viscosity being measured at 25° C. in a solution of 1 g of the polymer in 100 mL of dichloroacetic acid.

[0027] In one embodiment of the invention, the nonwoven fabric, in particular the spunbonded nonwoven fabric, is consolidated by a meltable adhesive to form a melt-bonded nonwoven fabric, i.e., the consolidation is carried out by a thermoplastic adhesive, which is preferably present in the form of fibers. Therefore, the melt-bonded nonwoven fabric comprises carrier fibers and hot-melt adhesive fibers. The carrier fibers and the hot-melt adhesive fibers can be derived from any thermoplastic fiber-forming polymer, and in addition, the carrier fibers can also be derived from non-melting fiber-forming polymers. For example, such melt-bonded spunbond fabrics are fundamentally described in EP-A 0,446,822 and EP-A 0,590,629.

[0028] Examples of polymers that can be used as a source of carrier fibers are polyacrylonitrile, polyolefins such as polyethylene or polypropylene, predominantly aliphatic polyamides such as nylon 6,6, predominantly aromatic polyamides (aramids) such as polyhydroquinone terephthalate or copolymers containing a certain amount of aromatic meta-diamine moieties to improve solubility, or polyisophthalate, predominantly aromatic polyesters such as poly(parabens), or preferably predominantly aliphatic polyesters such as polyethylene terephthalate.

[0029] While ensuring that the proportion of hot-melt adhesive fibers is sufficient to bond the carrier fibers to the hot-melt adhesive fibers, the relative proportion of the two fiber types can be selected within a wide range, so that the nonwoven fabric has a strength sufficient for the intended application while ensuring the necessary air permeability. In the nonwoven fabric, the proportion of hot melt derived from the hot-melt fibers is generally less than 50% by weight (based on the weight of the nonwoven fabric).

[0030] Modified polyesters having a melting point 10 to 50° C., preferably 30 to 50° C. lower than the raw material of the nonwoven fabric are particularly suitable as hot melt adhesives. Examples of such hot melt adhesives are polypropylene terephthalate (polypropylene), polybutylene terephthalate or polyethylene terephthalate modified by condensation of long-chain diols and / or isophthalic acid or aliphatic dicarboxylic acids.

[0031] The hot-melt adhesive is preferably introduced into the nonwoven in the form of fibers.

[0032] The carrier fiber and the hot-melt adhesive fiber are preferably composed of a class of polymers. This means that all fibers used are selected from a class of materials, so that after the nonwoven is used, these fibers can be easily recovered. For example, if the carrier fiber is composed of polyester, the selected hot-melt adhesive fiber will be a mixture of polyester or polyesters equally, for example, with PET as the core and with a polyethylene terephthalate copolymer with a low melting point as the bicomponent fiber form of the sheath. However, in addition, the bicomponent fiber composed of different polymers is also feasible. These examples are the bicomponent fibers (core / sheath) of polyester and polyamide.

[0033] The filament fineness of the carrier fiber and the hot-melt adhesive fiber may be selected within the range.

[0034] The filaments or staple fibers constituting the nonwoven fabric may have a substantially circular cross section, or may also have other shapes, such as dumbbell-shaped, kidney-shaped, triangular, trilobal or multilobal cross sections. Hollow fibers and bicomponent or multicomponent fibers may also be used. In addition, hot melt adhesive fibers may also be used in the form of bicomponent or multicomponent fibers.

[0035] The fibers forming the nonwoven can also be modified by conventional additives, for example by antistatic agents such as carbon black or additives which allow electrostatic charges. In addition, the fibers can contain antimicrobial materials.

[0036] The unit weight of non-woven fabric is between 50 and 400 g / m 2 Between, preferably 80 and 300g / m 2 Between, especially 100 and 250g / m 2The weight per unit area is determined in accordance with DIN EN ISO 29073-1 (1992-08).

[0037] In another embodiment of the invention, the nonwoven is pre-consolidated by mechanical means such as heated rolls or calenders, but with the proviso that the nonwoven is not consolidated by needling and / or hydraulic entanglement (hydroentanglement).

[0038] For the purpose of pre-consolidation, a nonwoven containing a meltable binder, which contains binder fibers in addition to carrier fibers, is thermally pre-consolidated in a manner known per se by means of hot rollers, by means of a calender or in an oven. The fibers may also have a bicomponent structure (e.g. core / sheath), wherein the sheath is the binder polymer.

[0039] The nonwoven fabric consolidated by thermoplastic adhesives and / or mechanical means such as calenders may also contain chemical adhesives, such chemical adhesives harden by curing reaction, usually such chemical adhesives are acrylic adhesives and / or styrene adhesives and / or starch adhesives and / or phenolic adhesives and / or latex adhesives. If present, such chemical adhesives are present in an amount of 0.1% to 30% by weight (based on the total weight of the nonwoven fabric).

[0040] The individual denier of the synthetic organic polymer fibers forming the nonwoven is 0.5 to 15 dtex, preferably 1 to 10 dtex. The denier is usually set during the production of the fibers. The denier of the fibers can be determined according to DIN EN ISO 1973: 1995-12 (vibrometer method).

[0041] Preferably, if the nonwoven fabric is made of synthetic organic polymer staple fibers, such staple fibers have a length between 5 and 100 mm, preferably between 10 and 80 mm.

[0042] The nonwoven fabric in the filter according to the present invention has a 50 L / m 2 Seconds, preferably 100L / m 2 Seconds and 2000L / m 2 seconds, more preferably 150L / m 2 Seconds to 1000L / m 2 Air permeability in the range of 100 Å to 100 Å seconds, as measured in accordance with DIN EN ISO 9237:1995-12. According to the invention, the nonwoven fabric in the filter has an embossing pattern with a compression factor.

[0043] As mentioned above, the nonwoven itself can also consist of multiple layers. Here, the individual layers within the nonwoven can differ in terms of the various selected synthetic polymer fibers and / or have various fiber diameters, but such parameters are within the ranges given for the nonwoven. Thus, in the case of a nonwoven with a multi-layer arrangement, there are at least 2 layers and at most 10 layers, preferably 2 to 4 layers. Preferably, the fiber fineness increases in one direction of the thickness of the nonwoven, so that a fineness gradient is formed within the aforementioned fineness range.

[0044] The nonwoven fabric, in particular the spunbonded nonwoven fabric, in the filter medium according to the present invention has a thickness D of 0.4-0.95 mm, preferably 0.45-0.8 mm in the non-embossed area. The aforementioned thickness D also includes nonwoven fabrics having a multi-layer structure.

[0045] The nonwoven fabric, in particular the spunbonded nonwoven fabric in the filter medium according to the present invention, has a thickness D in the non-embossed area and a thickness d in the embossed area, and the ratio d / D is a compression factor CF, and the compression factor CF is in the range of 0.2≤CF≤0.5, preferably, the compression factor CF is in the range of 0.25≤CF≤0.4. The thickness D and d are determined by observing the cross-section of the embossed area and the non-embossed area by the REM microscopic optical method.

[0046] The nonwoven fabric, in particular the spunbonded nonwoven fabric, in the filter medium according to the invention has an embossed pattern surface area of ​​7% to 30% of the total surface area of ​​the nonwoven fabric.

[0047] According to the present invention, each individual embossing pattern surface area of ​​the nonwoven fabric has a surface area of ​​0.4 to 5.6 mm 2 surface area.

[0048] Generally, the shape of the individual embossing patterns is not limited, but, for practical reasons, the individual embossing patterns are angular shapes and / or circular and / or oval with a length-to-width ratio of 1:1 to 1:8.

[0049] The embossing pattern is made by one or more embossing rolls having the desired pattern on the surface of the rolls. Typically, the embossing rolls are heated to a temperature typically between 80 and 250°C.

[0050] The embossing pattern is produced by one or more embossing rollers which press the nonwoven with a line pressure of at least 13 daN / cm. Suitable embossing rollers are provided in the calender arrangement.

[0051] According to the invention, the mechanism for producing a nonwoven fabric with an embossed pattern can be realized by a calender arrangement of at least two rollers, wherein two opposing rollers are pressed against each other with a line pressure of at least 13 daN / cm, one roller of the calender having a smooth surface and the other roller of the calender having a structured surface corresponding to the desired embossed pattern. Typically, the two opposing rollers are heated to a temperature between 80 and 250°C.

[0052] The areas of the structured roller protruding from the surface of the roller compress the nonwoven fabric to a thickness d, while the non-protruding areas of the roller compress the nonwoven fabric to a thickness D, resulting in a ratio d / D with a compression factor CF in the range of 0.2≤CF≤0.5, preferably in the range of 0.25≤CF≤0.4. This embodiment consists of Figure 2a shown.

[0053] In one embodiment of the invention, the area of ​​the structured roll that protrudes from the surface of the roll preferably has a flank angle of 18 to 30 degrees, which introduces the embossing pattern while the mechanical properties of the nonwoven remain robust so that the filter media can be cleaned during a cleaning cycle. This embodiment consists of Figure 2b Shown.

[0054] The nonwoven fabric according to the present invention, in particular the spunbond nonwoven fabric, has an embossed pattern surface area of ​​7% to 30% of the total surface area of ​​the nonwoven fabric, providing a larger filtration active area than a nonwoven fabric without such an embossed pattern surface area.

[0055] The embossed pattern may be produced by embossing the pattern in one x-direction or in both x and y-directions.The embossed pattern may be distributed statistically or in an ordered pattern. Figure 3 Exemplary embossing patterns are shown.

[0056] As explained, the aforementioned embossing pattern present in the nonwoven fabric of the present invention can be produced by means of calender rolls, which provide the aforementioned embossing pattern.

[0057] For a given volumetric gas / air flow rate, the embossing present in the nonwoven filter media provides a more effective filter media surface and reduces the local flow velocity inside the filter media. As a result, filter efficiency is increased and dust holding capacity is improved.

[0058] The filter medium according to the invention is a so-called cleanable filter medium which can be cleaned by merely reversing the flow direction of the filtered fluid, typically using a pulse pressurized filtered fluid to remove filtered solids from the filter. Surprisingly, the filter medium according to the invention exhibits an excellent cleaning performance.

[0059] The cleaning cycle removes the majority of the filtered material in the filter media primarily from the surface of the filter media. However, it is not possible to completely remove the filtered material. In particular, filter media with a large dust holding capacity suffer from the filtered material not being completely removed from the body / volume of the filter media. This results in a gradual increase in pressure drop at the beginning of each cleaning cycle, limiting the number of such cleaning cycles. The filter media of the present invention greatly increases the number of possible cleaning cycles.

[0060] exist Figure 1 In Figure 1, the residual pressure drop according to the VDI 3926 test procedure is shown for three filter media (FI180036, FI180040 and FI180044) made according to the invention and for one prior art medium (778 / 250 standard) for comparison. Table 1 contains more information about the aforementioned filter media. It can be seen that the media of the invention already exhibit a reduced pressure drop in the first 30 cleaning cycles. Even after 10,000 cleaning cycles ("aging", not shown), the improved performance of the filter media of the invention continues.

[0061] Use ISO 12103-1A2 fine test dust (concentration 5g / m 3 ) to test the filter media. The air-to-cloth ratio is 120m 3 / (m2h). The first 30 cycles and the last 30 cycles were cleaned after a pressure drop of 10 mbar. Aging was performed with cleaning after every 5 seconds (10,000 cycles). Cleaning was performed with compressed air (tank pressure: 5 bar) and a valve opening time of 60 ms.

[0062] Table 1

[0063]

[0064] FI180036, FI180040 and FI180044 are spunbond nonwoven fabrics using core-sheath fibers. The core polymer is PET (polyethylene terephthalate) and the sheath is a modified PET having a lower melting point than the core PET.

[0065] FI180036, FI180040 and FI180044 are thermally bonded spunbond nonwovens that are not needle punched and do not contain chemical binders.

[0066] The reference is a thermally bonded spunbond nonwoven.

[0067] Filter Media Manufacturing

[0068] The nonwoven layer according to the invention is produced by known methods available to the skilled person. Suitable methods are shown, for example, in the Handbook of Nonwovens, CRC Press, 2007. The formation of nonwovens, such as spunbond nonwovens, is also common knowledge to the skilled person.

[0069] The nonwoven fabric can be formed in-line or provided as a coil. In the in-line process, the nonwoven fabric can be pre-consolidated. Pre-consolidation is performed by using hot rollers or calenders known to those skilled in the art. The nonwoven fabric formed in-line or provided as a coil is fed into an embossing calender to provide the embossing pattern according to the present invention. The embossing of nonwoven materials is also known per se, however, the specific embossing of the present invention provides the benefits of the present invention.

[0070] As previously described, the embossed pattern is produced using a calender heated roll at ambient pressure; however, the process can be performed with or without heat and / or pressure. The embossed pattern can be a continuous pattern across the media ( Figure 3 ), or may be discrete marks such as rectangles, circles, other regular polygons, indentations, or repeating patterns of non-traditional shapes ( Figure 3 ).

[0071] The filter media according to the invention are used in filter systems for air / gas and liquid filtration, in particular in the motor vehicle industry, air conditioning systems, cabin filters, pollen filters, clean room filters, household filters, etc., and as oil filters and hydraulic filters, in order to remove solids from air / gas and liquids.

[0072] Therefore, the object of the present invention is also to provide a filter system and a filter cartridge comprising a filter medium according to the invention.

[0073] Filter media according to the present invention may be formed into any number of filter configurations.

[0074] Further areas of application of the filter according to the invention are mounting panels and sound absorbing panels.

Claims

1. A filter medium comprising: a) at least one textile layer, said textile layer being a nonwoven fabric of synthetic organic polymer fibers, a1) The nonwoven fabric has a thickness of 50 to 400 g / m 2 The weight per unit area, a2) the fibers of the nonwoven fabric have a fineness in the range of 0.5 to 15 dtex, a3) the nonwoven is consolidated by a thermoplastic hot melt adhesive polyester or a mixture of hot melt adhesive polyester fibers, provided that the nonwoven is not consolidated by needle punching and / or hydroentanglement, a4) the nonwoven fabric has an embossed pattern, the nonwoven fabric has a surface area of ​​at least 50 L / m 2 Air permeability in seconds, a5) the nonwoven fabric has an embossed pattern, and the surface area of ​​the embossed pattern of the nonwoven fabric is greater than 7% and less than 30% of the total surface area of ​​the nonwoven fabric, a6) Each individual embossed pattern of the nonwoven fabric has a surface area of ​​0.4 to 5.6 mm 2 The surface area of a7) the nonwoven fabric has a thickness D in the non-embossed area and a thickness d in the embossed area, and the ratio d / D is a compression factor CF, and the compression factor CF is in the range of 0.2 ≤ CF < 0.

5.

2. The filter medium of claim 1, wherein: The hot melt adhesive polyester fibers are in the form of bicomponent fibers.

3. The filter medium of claim 2, wherein the hot melt adhesive polyester fiber is a bicomponent fiber having a first polyester material forming a core and a second sheath polyester material having a melting point 30 to 50°C lower than the melting point of the core PET material.

4. The filter medium according to claim 1, wherein the nonwoven fabric has a unit area weight of 80 to 300 g / m 2 between.

5. The filter medium according to claim 1, wherein the nonwoven fabric has a unit area weight of 100 to 250 g / m 2 between. 6 . The filter medium according to claim 1 , wherein the individual deniers of the synthetic organic polymer fibers forming the nonwoven fabric are between 1 and 10 dtex.

7. The filter medium of claim 1, wherein the nonwoven fabric in the filter has a flow rate of 100 L / m 2 Seconds and 2000 L / m 2 Air permeability in the range between 10 and 20 seconds.

8. The filter medium of claim 1, wherein the nonwoven fabric in the filter has a flow rate of 150 L / m 2 Seconds to 1000 L / m 2 Air permeability in the range of seconds. 9 . The filter medium according to claim 1 , wherein the nonwoven fabric in the filter medium has a thickness D of 0.4 to 0.95 mm in the non-embossed area.

10. The filter medium of claim 9, wherein the nonwoven fabric is a spunbond nonwoven fabric.

11. The filter medium of claim 1, wherein the compressibility factor is in the range of 0.25 ≤ CF ≤ 0.

4. 12 . The filter medium of claim 1 , wherein the nonwoven fabric in the filter medium having an embossed pattern surface area of ​​7% or more and less than 30% of the total surface area of ​​the nonwoven fabric is a spunbond nonwoven fabric.

13. The filter medium of claim 1, wherein each of the individual embossed pattern surface areas of the nonwoven fabric has a surface area of ​​0.4 to 5.6 mm 2 surface area.

14. A method of making a filter medium comprising the steps of: (i) providing a nonwoven fabric of synthetic organic polymer fibers, the nonwoven fabric having a thickness of 50 to 400 g / m 2 The fibers of the nonwoven fabric have a density within the range of 0.5 to 15 dtex, (ii) the nonwoven fabric is consolidated by a thermoplastic hot melt adhesive polyester or a mixture of hot melt adhesive polyester fibers, provided that the nonwoven fabric is not consolidated by needle punching and / or hydroentanglement, (iii) applying an embossing pattern to the nonwoven fabric, wherein the surface area of ​​the embossing pattern of the nonwoven fabric is 7% or more and less than 30% of the total surface area of ​​the nonwoven fabric, and each individual embossing pattern surface area of ​​the nonwoven fabric has a surface area of ​​0.4 to 5.6 mm 2 The embossed pattern nonwoven fabric has a surface area of ​​at least 50 L / m 2 Air permeability in seconds, The nonwoven fabric has a thickness D of 0.4 to 0.95 mm in the non-embossed area and a thickness d in the embossed area, and the ratio d / D is a compression factor CF, and the compression factor CF is in the range of 0.2 ≤ CF < 0.5, wherein the embossing pattern is applied by one or more embossing rollers which press the nonwoven fabric with a linear pressure of at least 13 daN / cm, The embossing pattern is applied by an arrangement of at least two roller calenders, wherein two opposing rollers are pressed against each other with a line pressure of at least 13 daN / cm, one roller of the calender having a smooth surface and the other roller of the calender having a structured surface corresponding to the desired embossing pattern, the area of ​​the roller having the structured surface protruding from the surface of the roller having a side angle of 8 to 30 degrees.

15. The method according to claim 14, wherein the embossed pattern nonwoven fabric has a 2 Seconds and 2000L / m 2 Air permeability between seconds.

16. The method of claim 14, wherein the thickness D is 0.45 to 0.8 mm.

17. Use of the filter medium of claim 1 in gas and liquid filtration.

18. A filter module comprising a housing and at least one filter medium according to claim 1.