A high-safety composite electric heating film and preparation method thereof
By introducing insulating thermally conductive color changers into the composite electric heating film, the problems of electrode short circuit and uneven heating are solved, its safety and reliability are improved, and real-time status detection is realized, which is suitable for the field of low and high temperature special-shaped heating elements.
Patent Information
- Application Number
- CN202011323831.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-23
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-11-23
AI Technical Summary
During the preparation and use of composite electric heating films, electrodes are easily short-circuited due to external forces, posing safety risks, and the uneven heating is poor, affecting the safety and efficiency of its application.
It adopts a structure including a lower electrode, an insulating heat-conducting color-changing body, an electric heating layer and an upper electrode. The insulating and heat-conducting color-changing body not only acts as a pillar to prevent short circuits, but also has excellent thermal conductivity and temperature-sensitive color-changing functions. Through the embedding of the insulating and heat-conducting color-changing body The device and slurry are cured to form a composite electric heating film to improve its safety and heating uniformity.
It effectively reduces the risk of electrode short circuit, improves the uniformity of heating, and has the function of real-time detection of working status, improving the safety performance and reliability of the electric heating film.
Smart Images

Figure CN112351524B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electric heating materials, and in particular relates to a short-circuit-proof high-safety composite electric heating film and a preparation method thereof. Background Art
[0002] Compared with traditional metal wire heating elements and ceramic heating elements, composite electric heating films not only have the advantages of easy preparation, no precious metals such as chromium and nickel, high electric heat conversion efficiency, energy saving and environmental protection, and low cost, but also due to their excellent flexibility and processability, they are widely used in flexible wearable devices and thin and light heating devices. It is a new type of high-performance heating element.
[0003] Although composite electric heating films have broad application prospects, they are currently limited by the conditions of the preparation process and have the disadvantages of high driving voltage, large resistance deviation, and poor consistency, which can easily cause problems such as electrical breakdown and poor heating uniformity, leading to safety accidents. In view of this, the "sandwich" structure, which is to assemble the electrode, electric heating layer, and electrode layer by layer, can not only easily adjust the membrane resistance, obtain extremely small resistance, and effectively reduce the working voltage, but also because the electrodes are distributed on the surface of the electric heating layer, the current transmission distance can be greatly shortened to achieve the rapid heating function, and because the electrode material is also an excellent thermal conductor, it can speed up the heat transfer from the inside of the electric heating layer and improve its heating unevenness, thus it is expected to solve the above problems.
[0004] During the preparation process of ordinary "sandwich" structure composite electric heating films, the electrodes and the electric heating layer need to be composited so that the electrodes are in close contact with the electric heating layer materials. However, when the mechanical properties of the electric heating layer material are poor or the thickness of the electric heating layer is small, the electric heating layer is easily rolled and thinned due to the action of mechanical force, resulting in direct contact between the electrodes on both sides, causing a short circuit during operation; and during use, when it is squeezed or bent by external force, it may also cause contact between the electrodes on both sides, causing a short circuit inside. Therefore, ordinary "sandwich" structure composite electric heating films have serious safety risks. Summary of the invention
[0005] In view of the above shortcomings of the prior art, one of the purposes of the present invention is to solve the above technical problems and provide a short-circuit-proof composite electric heating film, which includes a lower electrode 1, a plurality of insulating thermally conductive color-changing bodies 2, an electric heating layer 3 and an upper electrode layer 4. Compared with ordinary composite electric heating films, the introduced insulating thermally conductive color-changing bodies can not only play a supporting role to prevent the problem of electrode short circuit caused by external force during the preparation and use of the composite electric heating film, but also because the insulating thermally conductive color-changing body itself has excellent thermal conductivity, it can accelerate the heat conduction inside the composite electric heating film, so that it has better heating uniformity than ordinary composite electric heating films; at the same time, due to the temperature-sensitive color-changing function of the insulating thermally conductive color-changing body itself, it has the function of real-time detection of the working state of the composite electric heating film compared with ordinary electric heating films.
[0006] The technical solution adopted by the present invention to solve its technical problem is:
[0007] A high-safety composite electric heating film comprises a lower electrode layer, a plurality of insulating heat-conducting color-changing bodies, an electric heating layer and an upper electrode layer, wherein the electric heating layer is arranged between the upper electrode layer and the lower electrode layer, any of the insulating heat-conducting color-changing bodies is adhered to the upper surface of the lower electrode layer, and any of the insulating heat-conducting color-changing bodies is embedded in the electric heating layer.
[0008] Preferably, the upper surface of the lower electrode layer is a conductive surface, and is in contact with the insulating thermal conductive color-changing body and the electric heating layer; the lower surface of the upper electrode layer is a conductive surface, and is in contact with the electric heating layer.
[0009] Preferably, any of the insulating thermally conductive color-changing bodies is a protrusion arranged on the upper surface of the lower electrode layer, and there is a gap between adjacent insulating thermally conductive color-changing bodies. Several insulating thermally conductive color-changing bodies form a preset shape, and the preset shape is custom set, including various common shapes, such as cartoon shapes, array shapes, text shapes, creative shapes, etc.
[0010] Preferably, the gap distance between the insulating thermally conductive color-changing bodies is 10-1000 μm.
[0011] Preferably, the insulating thermally conductive color-changing body is evenly distributed on the upper surface of the lower electrode layer in an array, and the array includes common array patterns with a certain spacing, such as cylindrical and / or square column arrays, strip arrays, network arrays, and concentric ring arrays.
[0012] Preferably, the thickness of the insulating thermally conductive color-changing body is 10-150 μm, and the thickness of any two insulating thermally conductive color-changing bodies can be the same or different, which plays a role in supporting the internal structure and promoting heat conduction in all directions.
[0013] Preferably, the thickness of the electric heating layer is 10 to 500 μm, and is not less than the thickness of any of the insulating thermally conductive color-changing bodies; the thickness of the electric heating layer refers to the distance from the end of the electric heating layer in contact with the upper surface of the lower electrode layer to the end of the electric heating layer in contact with the lower surface of the upper electrode layer; the term "not less than" means that the thickness of the electric heating layer may be greater than the thickness of the insulating thermally conductive color-changing body, or may be equal to the thickness of the insulating thermally conductive color-changing body. When the thicknesses are equal, the electric heating layer only fills the gaps in the insulating thermally conductive color-changing body, but does not cover the upper surface of the insulating thermally conductive color-changing body. In this case, the electric heating layer and the insulating thermally conductive color-changing body are both in contact with the lower electrode layer and the upper electrode layer.
[0014] Preferably, the insulating thermally conductive color body is obtained by coating the insulating thermally conductive color body slurry on the upper surface of the lower electrode layer and then curing it, and the electric heating layer is obtained by coating the electric heating layer slurry on the composite surface of the insulating thermally conductive color body and the upper surface of the lower electrode layer and then curing it, wherein the composite surface refers to the uneven upper surface formed by a plurality of insulating thermally conductive color bodies after being cured on the upper surface of the lower electrode layer; that is, when the thickness of the electric heating layer and the insulating thermally conductive color body is the same, the electric heating layer slurry is coated on the gaps of the insulating thermally conductive color body and contacts the upper surface of the lower electrode layer; when the thickness of the electric heating layer is greater than the thickness of the insulating thermally conductive color body, the electric heating layer is coated on the gaps and upper surface of the insulating thermally conductive color body so that it is evenly covered on the upper surfaces of a plurality of insulating thermally conductive color bodies, and filled in the gaps of a plurality of insulating thermally conductive color bodies, and at the same time covers the corresponding upper surface of the lower electrode layer, and the electric heating layer slurry at the gaps contacts the upper surface of the lower electrode layer; the upper electrode layer is arranged in affixed relation to the electric heating layer and is pressed with the electric heating layer by mechanical hot pressing.
[0015] Preferably, the insulating thermally conductive color-changing body slurry is composed of a polymer resin, a solvent, a thermochromic capsule powder and a high thermal conductivity inorganic material powder. The insulating thermally conductive color-changing body slurry is made of the following components in parts by weight: 5 to 20 parts by weight of a polymer resin, 1 to 20 parts by weight of a thermochromic capsule powder, 1 to 20 parts by weight of a high thermal conductivity inorganic material powder and 40 to 90 parts by weight of a solvent.
[0016] Preferably, the lower electrode layer and the upper electrode layer are both composite conductive transparent films, and the composite conductive transparent film is any one of composite conductive transparent films such as PET-ITO, PET-CNT, PET-Graphene, PET-Cu, PI-ITO, PI-CNT, PI-Graphene, PI-Cu, PVC-ITO, PVC-CNT, PVC-Graphene or PVC-Cu.
[0017] Preferably, the polymer resin component in the insulating thermally conductive color-changing body slurry is any one of polyimide (PI), polyethersulfone resin (PES), polybenzimidazole (PBI), and polyurethane (PU).
[0018] Preferably, the solvent in the insulating thermally conductive color-changing body slurry is any one or more combinations of N-methylpyrrolidone (NMP), dimethylformamide (DMAc), dimethylacetamide (DMF), and acetonitrile.
[0019] Preferably, the thermochromic capsule powder in the insulating thermally conductive color-changing body slurry is a material that does not show color at room temperature but shows a specific color when reaching a specific temperature.
[0020] Preferably, the high thermal conductivity inorganic material powder in the insulating thermal conductive color-changing body slurry is aluminum nitride (AlN), silicon nitride (Si 3 N 4 ), Boron Nitride (BN), Silicon Carbide (SiC), Boron Carbide (B 4 C), diamond, alumina (Al 2 O 3 ), magnesium oxide (MgO), silicon oxide (SiO 2 ) any one or more combinations.
[0021] A second object of the present invention is to provide a method for preparing the above-mentioned high-safety composite electric heating film.
[0022] A method for preparing a high-safety composite electric heating film comprises the following steps:
[0023] S1. Preparing insulating thermal conductive color-changing body slurry: dissolving the corresponding polymer resin in a solvent, preparing a glue solution by mechanical stirring, adding an appropriate amount of high thermal conductivity inorganic material powder and thermochromic capsule powder to the glue solution, and mixing the high thermal conductivity inorganic material powder and thermochromic capsule powder with the glue solution by mechanical stirring to form an insulating thermal conductive color-changing body slurry;
[0024] S2, coating the insulating thermally conductive color-changing body slurry prepared in step S1 on the upper surface of the lower electrode layer in a preset shape, and obtaining a plurality of insulating thermally conductive color-changing bodies after curing;
[0025] S3, coating the electric heating layer slurry on the composite surface of the plurality of insulating thermally conductive color-changing bodies obtained in step S2 and the upper surface of the lower electrode layer, and obtaining the electric heating layer after curing, forming a structure in which the plurality of insulating thermally conductive color-changing bodies are embedded in the electric heating layer, and the electric heating layer is in contact with the upper surface of the lower electrode layer;
[0026] S4. The upper electrode layer is pressed together with the electric heating layer prepared in step S3 under the action of mechanical force and heat pressing to obtain a high-safety composite electric heating film.
[0027] Preferably, the curing temperature of step S2 is 60-300°C, and the curing temperature of step S3 is 60-300°C.
[0028] Preferably, the pressure in step S4 is 0.2-10 MPa.
[0029] Preferably, the hot pressing temperature in step S4 is 40-250°C.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) In the present invention, a plurality of insulating heat-conducting color-changing bodies are provided to support the internal structure, thereby preventing the upper and lower electrodes from directly contacting each other, greatly reducing the risk of short circuit, and thus improving the safety performance of the electric heating film.
[0032] (2) In the present invention, since the high thermal conductivity inorganic material powder in the insulating thermal conductive color-changing body has a good thermal conductivity, the heat conduction in the electric heating film is promoted, and the phenomenon of uneven heating of the electric heating film is improved.
[0033] (3) In the present invention, the thermochromic capsule powder in the insulating thermal conductive color-changing body can change color as the temperature of the electric heating layer changes. This enables it to have the function of real-time detection of the working status of the composite electric heating film compared to ordinary electric heating films.
[0034] (4) The present invention has a simple preparation process, low cost, strong reliability, and a wide range of applications, and is suitable for the field of low and high temperature special-shaped heating elements. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a schematic diagram of the structure of a high-safety composite electric heating film according to Example 1 of the present invention;
[0036] Figure 2 This is a cross-sectional structural diagram of a high-safety composite electric heating film according to Example 1 of the present invention;
[0037] Figure 3 A top view of the insulating thermally conductive color-changing body of Example 1;
[0038] Figure 4 A top view of the shape of the insulating thermally conductive color-changing body of Example 2;
[0039] Figure 5 A top view of the insulating thermally conductive color-changing body of Example 3;
[0040] Figure 6 The electric heating performance and resistance change of the high-safety composite electric heating film of Example 1 under repeated bending.
[0041] In the figure: ① lower electrode layer 1, ② insulating thermal conductive color-changing body 2, ③ electric heating layer 3, ④ upper electrode layer 4. DETAILED DESCRIPTION
[0042] The technical solution of the present invention is further described in detail below through specific embodiments in combination with the accompanying drawings, but the protection scope of the present invention is not limited thereto.
[0043] In the present invention, the electric heating layer slurry and the thermochromic capsule powder are common knowledge in the art and can be obtained by those skilled in the art by self-production or purchase according to actual needs, and are not limited to the materials used in the present invention.
[0044] The electric heating layer slurry of the present invention is made of the following components in parts by weight:
[0045] 5 to 10 parts by weight of polybenzimidazole powder, 1 to 5 parts by weight of conductive carbon black and 80 to 90 parts by weight of NN dimethylacetamide solution. The preparation method comprises the following steps:
[0046] S1, dissolving polybenzimidazole powder in NN dimethylacetamide solution, and preparing PBI-DMAc glue by mechanical stirring under heating conditions;
[0047] S2, adding an appropriate amount of conductive carbon black to the PBI-DMAc glue prepared in step S1, and mixing the conductive carbon black and the PBI-DMAc glue evenly by mechanical stirring to form an electric heating film slurry;
[0048] The thermochromic capsule powder is a commercially available thermochromic capsule powder, specifically the Chameleon T colorless and colored series of thermochromic microcapsule products sold by Shenzhen Jintianli New Materials Technology Co., Ltd.
[0049] Embodiment 1:
[0050] The PI polymer resin is dissolved in the NMP solvent, and the PI-NMP glue is prepared by mechanical stirring, and then an appropriate amount of boron nitride (BN) powder and thermochromic capsule powder are added to the prepared glue, and the two powders are mixed with the PI-NMP glue by mechanical stirring to form an insulating thermal conductive color-changing body slurry. The weight ratio of the insulating thermal conductive color-changing body slurry is: 20 parts by weight of PI resin, 5 parts by weight of boron nitride, 5 parts by weight of commercially available thermochromic capsule powder and 70 parts by weight of NMP solution.
[0051] The insulating thermal conductive color-changing body slurry prepared above was coated on the conductive side of the lower electrode layer 1PI-ITO in the shape of an unconnected cylindrical array, and after high-temperature curing at 120°C, a 120 μm thick insulating thermal conductive color-changing body 2 was obtained. Figure 3 The cylindrical array structure shown.
[0052] The electric heating layer slurry is evenly coated on the upper surface and gaps of the insulating thermal conductive color-changing body 2 prepared above, so that it evenly covers the upper surface of the insulating thermal conductive color-changing body 2 and fills the gaps of the insulating thermal conductive color-changing body 2, and at the same time covers the corresponding upper surface of the lower electrode layer 1PI-ITO. After high-temperature curing at 120°C, a 180μm thick electric heating layer 3 can be obtained, forming a structure in which the insulating thermal conductive color-changing body 2 is embedded in the electric heating layer 3, and the electric heating layer 3 is in contact with the upper surface of the lower electrode layer 1PI-ITO.
[0053] Finally, the upper electrode layer 4PI-ITO is tightly pressed with the above-prepared electric heating layer 3 under the mechanical force hot pressing at 150°C and 2MPa to obtain a high-safety composite electric heating film. Figure 6 As shown, the high-safety composite electric heating film of this embodiment can work stably under repeated bending conditions using 3V, 4V and 5V voltages respectively, without obvious fluctuation in resistance and without short circuit.
[0054] Embodiment 2:
[0055] PES polymer resin was dissolved in DMF solvent and PES-NMP glue was prepared by mechanical stirring. Then an appropriate amount of silicon nitride (Si 3 N 4 ) powder and thermochromic capsule powder are added to the above-prepared glue solution, and the two powders are mixed evenly with the PES-NMP glue solution by mechanical stirring to form an insulating thermal conductive color-changing body slurry. The weight ratio of the insulating thermal conductive color-changing body slurry is: 15 parts by weight of PES resin, 10 parts by weight of silicon nitride, 5 parts by weight of thermochromic capsule powder and 70 parts by weight of DMF solution.
[0056] The insulating thermal conductive color-changing body slurry prepared above was coated on the conductive side of the lower electrode layer 1 PET-Cu in a network array shape, and after high temperature curing at 120°C, a 60 μm thick insulating thermal conductive color-changing body 2 was obtained. Figure 4 The network-like array structure shown.
[0057] The electric heating layer slurry is evenly coated on the upper surface and gaps of the insulating thermal conductive color body 2 prepared above, so that it evenly covers the upper surface of the insulating thermal conductive color body 2 and fills the gaps of the insulating thermal conductive color body 2, and at the same time covers the corresponding upper surface of the lower electrode layer 1PET-Cu. After high-temperature curing at 60°C, a 100μm thick electric heating layer 3 can be obtained, forming a structure in which the insulating thermal conductive color body 2 is embedded in the electric heating layer 3, and the electric heating layer 3 is in contact with the upper surface of the lower electrode layer 1PET-Cu.
[0058] Finally, the upper electrode layer 4PET-Cu was tightly pressed with the above-prepared electric heating layer under the action of hot pressing at 60°C and 1MPa mechanical force to obtain a high-safety composite electric heating film.
[0059] Embodiment 3:
[0060] Thermoplastic polyurethane (TPU) polymer resin is dissolved in NMP solvent, and TPU-NMP glue is prepared by mechanical stirring, and then an appropriate amount of aluminum nitride (AlN) powder and thermochromic capsule powder are added to the prepared glue, and the two powders are mixed with the TPU-NMP glue by mechanical stirring to form an insulating thermal conductive color-changing body slurry. The weight ratio of the insulating thermal conductive color-changing body slurry is: 20 parts by weight of TPU resin, 5 parts by weight of aluminum nitride (AlN), 5 parts by weight of thermochromic capsule powder and 70 parts by weight of NMP solution.
[0061] The insulating thermal conductive color-changing body slurry prepared above was coated on the conductive side of the PVC-Graphene of the lower electrode layer 1 in the shape of a concentric ring array, and after high-temperature curing at 120°C, a 40 μm thick insulating thermal conductive color-changing body 2 was obtained. Figure 5 The concentric ring array structure shown.
[0062] The electric heating layer slurry is evenly coated on the upper surface and gaps of the insulating thermal conductive color body 2 prepared above, so that it evenly covers the upper surface of the insulating thermal conductive color body 2 and fills the gaps of the insulating thermal conductive color body 2, and at the same time covers the corresponding upper surface of the lower electrode layer 1PVC-Graphene. After high-temperature curing at 80°C, an 80μm thick electric heating layer 3 can be obtained, forming a structure in which the insulating thermal conductive color body 2 is embedded in the electric heating layer 3, and the electric heating layer 3 is in contact with the upper surface of the lower electrode layer 1PVC-Graphene.
[0063] Finally, the upper electrode layer 4PVC-Graphene was tightly pressed with the above-prepared electric heating layer under the action of hot pressing at 90°C and 2MPa mechanical force to obtain a high-safety composite electric heating film.
[0064] It should be noted that the above-described embodiment is only a preferred solution of the present invention and does not limit the present invention in any form. There are other variations and modifications without exceeding the technical solution described in the claims.
Claims
1. A high-safety composite electric heating film, It is characterized in that It comprises a lower electrode layer, a plurality of insulating thermally conductive color-changing bodies, an electric heating layer and an upper electrode layer, wherein the electric heating layer is arranged between the upper electrode layer and the lower electrode layer, any of the insulating thermally conductive color-changing bodies is laminated on the upper surface of the lower electrode layer, and any of the insulating thermally conductive color-changing bodies is embedded in the electric heating layer; any of the insulating thermally conductive color-changing bodies is a protrusion arranged on the upper surface of the lower electrode layer; a plurality of the insulating thermally conductive color-changing bodies are evenly distributed on the upper surface of the lower electrode layer in an array; the insulating thermally conductive color-changing body is obtained by coating insulating thermally conductive color-changing body slurry on the upper surface of the lower electrode layer and then curing it, the electric heating layer is obtained by coating electric heating layer slurry on the composite surface of the insulating thermally conductive color-changing body and the upper surface of the lower electrode layer and then curing it, and the upper electrode layer is pressed together with the electric heating layer by mechanical hot pressing; The insulating thermally conductive color-changing body slurry is composed of a polymer resin, a solvent, a thermochromic capsule powder and a high thermal conductivity inorganic material powder, and the insulating thermally conductive color-changing body slurry is made of the following components in parts by weight: 5 to 20 parts by weight of the polymer resin, 1 to 20 parts by weight of the thermochromic capsule powder, 1 to 20 parts by weight of the high thermal conductivity inorganic material powder and 40 to 90 parts by weight of the solvent; The polymer resin component in the insulating thermal conductive color-changing body slurry is any one of polyimide, polyethersulfone resin, polybenzimidazole, and polyurethane; The solvent in the insulating thermal conductive color-changing body slurry is any one or more combinations of N-methylpyrrolidone, dimethylformamide, dimethylacetamide, and acetonitrile; The high thermal conductivity inorganic material powder in the insulating thermal conductive color-changing body slurry is any one or more combinations of aluminum nitride, silicon nitride, boron nitride, silicon carbide, boron carbide, diamond, aluminum oxide, magnesium oxide, and silicon oxide.
2. A high-safety composite electric heating film according to claim 1, Features: The upper electrode layer and the lower electrode layer are both composite conductive transparent films, and the composite conductive transparent film is any one of PET-ITO, PET-CNT, PET-Graphene, PET-Cu, PI-ITO, PI-CNT, PI-Graphene, PI-Cu, PVC-ITO, PVC-CNT, PVC-Graphene or PVC-Cu.
3. A high-safety composite electric heating film according to claim 1, Features: The thickness of any of the insulating thermally conductive color-changing bodies is 10-150 μm; the thickness of the electric heating layer is 10-500 μm, and is not less than the thickness of any of the insulating thermally conductive color-changing bodies.
4. A method for preparing the high-safety composite electric heating film according to any one of claims 1 to 3, It is characterized in that The following steps are involved: S1. Preparing insulating thermal conductive color-changing body slurry: dissolving the corresponding polymer resin in a solvent, preparing a glue solution by mechanical stirring, adding an appropriate amount of high thermal conductivity inorganic material powder and thermochromic capsule powder to the glue solution, and mechanically stirring and mixing to form an insulating thermal conductive color-changing body slurry; S2, coating the insulating thermally conductive color-changing body slurry prepared in step S1 on the upper surface of the lower electrode layer according to a preset pattern, and obtaining the insulating thermally conductive color-changing body after curing; S3, coating the electric heating layer slurry on the composite surface of the plurality of insulating heat-conductive color-changing bodies obtained in step S2 and the upper surface of the lower electrode layer, and obtaining the electric heating layer after curing; S4. The upper electrode layer is pressed together with the electric heating layer prepared in step S3 under the action of mechanical force and heat pressing to obtain a high-safety composite electric heating film.
5. A method for preparing a high-safety composite electric heating film according to claim 4, Features: The curing temperature in step S2 is 60-300° C.; the curing temperature in step S3 is 60-300° C.; the pressure in step S4 is 0.2-10 MPa; and the hot pressing temperature in step S4 is 40-250° C.
Citation Information
Patent Citations
High-safety composite electrothermal film
CN213586337U