Adhesive sheet, backlight unit and display device

By using an adhesive layer containing light-diffusing particles on the backlight, the problem of accidental coloring of diffused light in the adhesive layer is solved, high haze value and color uneven suppression are achieved, and the image quality and water resistance of the display device are improved. .

CN112442321BActive Publication Date: 2024-10-29LINTEC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202010819337.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-14
Publication Date
2024-10-29
Estimated Expiration
2040-08-14

AI Technical Summary

Technical Problem

The adhesive layer of the existing backlight is easily accidentally colored when diffusing light, resulting in uneven colors. The water resistance of the luminous body is low, which affects the image quality of the display device.

Method used

An adhesive layer containing light-diffusing particles is used to ensure that the haze value and standard deviation of light of different wavelengths are within a specific range, and the total light transmittance reaches more than 70%, and the adhesive layer is formed by cross-linking the adhesive composition to improve Adhesion and concave-convex embedding.

Benefits of technology

It achieves high haze value and suppression of color unevenness, improves the image visibility and brightness uniformity of the display device, and enhances the water resistance and concave-convex embedding ability of the backlight.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112442321B_ABST
    Figure CN112442321B_ABST
Patent Text Reader

Abstract

The present invention provides an adhesive sheet, a backlight unit and a display device that exhibit a high haze value and excellent color unevenness suppression. The adhesive sheet is an adhesive sheet (1) having an adhesive layer (11), wherein the adhesive constituting the adhesive layer (11) contains light diffusion particles, the average value of the haze value of the adhesive layer (11) for light with a wavelength of 380nm, the haze value of the adhesive layer (11) for light with a wavelength of 580nm and the haze value of the adhesive layer (11) for light with a wavelength of 780nm is 70% or more and 100% or less, the standard deviation of the haze value of the adhesive layer (11) for light with a wavelength of 380nm, the haze value of the adhesive layer (11) for light with a wavelength of 580nm and the haze value of the adhesive layer (11) for light with a wavelength of 780nm is 7.50 or less, and the total light transmittance of the adhesive layer (11) is 70% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive sheet including an adhesive layer having light diffusing properties, and a backlight unit and a display device using the adhesive sheet. Background Art

[0002] In recent years, liquid crystal displays (LCDs) have been widely used as display devices in electronic devices such as portable telephones, smartphones, tablets, and game consoles. Since the display section formed by the liquid crystal panel does not emit light itself, display devices using such a display section require a backlight to illuminate it.

[0003] Until now, the light source configuration of the backlight in the display device described above has generally been a side-entry type in which the light source is configured on the side of the light guide plate. On the other hand, recently, from the perspective of screen brightness and contrast, research has begun on direct-type backlights in which the light source is configured directly below the display unit. For direct-type backlights, in order to obtain light quantity and to make the light quantity uniform between the center and the ends of the screen when manufacturing a display device, research is being conducted in the direction of arranging multiple light-emitting bodies, typically light-emitting diodes (LEDs), on a substrate.

[0004] However, when multiple light-emitting elements are used as the light source for a direct-lit backlight, it is desirable to seal the light-emitting elements with resin or the like due to their low water resistance. Furthermore, when a display device is manufactured using a backlight with multiple light-emitting elements as the light source, uneven brightness occurs in the resulting image due to the presence and absence of the light-emitting elements.

[0005] Patent Document 1 proposes providing an adhesive layer containing light-scattering particles on the light-emitting element of the above-mentioned backlight.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent No. 5590582 Summary of the Invention

[0009] Technical Problems to be Solved by the Invention

[0010] However, in Patent Document 1, the adhesive layer must be formed by directly coating the adhesive onto the backlight. Furthermore, when using conventional adhesives, the light from the light source or its diffused light can sometimes be accidentally colored, resulting in uneven color.

[0011] In view of such circumstances, an object of the present invention is to provide an adhesive sheet, a backlight unit, and a display device that exhibit a high haze value and are excellent in suppressing color unevenness.

[0012] Technical means to solve technical problems

[0013] In order to achieve the above-mentioned purpose, first, the present invention provides an adhesive sheet having an adhesive layer, characterized in that the adhesive constituting the adhesive layer contains light-diffusing particles, the average value of the haze value of the adhesive layer for light with a wavelength of 380nm, the haze value of the adhesive layer for light with a wavelength of 580nm, and the haze value of the adhesive layer for light with a wavelength of 780nm is greater than 70% and less than 100%, the standard deviation of the haze value of the adhesive layer for light with a wavelength of 380nm, the haze value of the adhesive layer for light with a wavelength of 580nm, and the haze value of the adhesive layer for light with a wavelength of 780nm is less than 7.50, and the total light transmittance of the adhesive layer is greater than 70% (Invention 1).

[0014] The invention (Invention 1) exhibits a high haze value, suppresses unintended coloring of light from a light source and its diffused light, and suppresses color unevenness. Furthermore, the image and video visibility when used in a display device is excellent.

[0015] In the above invention (Invention 1), the total value of the image sharpness of the optical combs (optical combs) of 0.125 mm, 0.25 mm, 0.5 mm, 1.0 mm, and 2.0 mm of the adhesive layer is preferably 0.2 or more and 400 or less.

[0016] In the above inventions (Inventions 1 and 2), it is preferred that the thickness of the adhesive layer be 10 μm or more and 500 μm or less (Invention 3).

[0017] In the above inventions (Inventions 1 to 3), the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer preferably has a storage elastic modulus G′ at 23° C. of 0.001 MPa to 10 MPa (Invention 4).

[0018] In the above inventions (Inventions 1 to 4), it is preferred that the adhesive strength of the adhesive sheet to soda-lime glass is 0.1 N / 25 mm or more (Invention 5).

[0019] In the above inventions (Inventions 1 to 5), it is preferred that the adhesive is an acrylic adhesive (Invention 6).

[0020] In the above inventions (Inventions 1 to 6), preferably, the adhesive sheet includes two release sheets, and the adhesive layer is sandwiched between the release sheets so as to contact release surfaces of the two release sheets (Invention 7).

[0021] The adhesive sheet of the above inventions (Inventions 1 to 7) is preferably used for bonding two hard bodies together (Invention 8).

[0022] Second, the present invention provides a backlight unit comprising a backlight having a plurality of light emitters and an adhesive layer stacked on the backlight, wherein the backlight is characterized in that the adhesive layer is the adhesive layer (invention 9) of the adhesive sheet (invention 1-8).

[0023] In the above invention (Invention 9), it is preferred that the light-emitting body is a light-emitting diode (Invention 10).

[0024] Thirdly, the present invention provides a display device comprising the backlight unit (Inventions 9 and 10) and a display portion stacked on the adhesive layer of the backlight unit (Invention 11).

[0025] Effects of the Invention

[0026] The adhesive sheet, backlight unit, and display device of the present invention exhibit high haze values ​​and excellent color unevenness suppression. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a cross-sectional view of an adhesive sheet according to one embodiment of the present invention.

[0028] Figure 2 This is a cross-sectional view of a backlight unit according to one embodiment of the present invention.

[0029] Figure 3 This is a cross-sectional view of a display device according to one embodiment of the present invention.

[0030] Description of Reference Numerals

[0031] 1: Adhesive sheet; 11: Adhesive layer; 12a, 12b: Release sheets; 2: Backlight unit; 20: Backlight; 21: Substrate; 22: Light emitter; 3: Display device; 30: Display section. DETAILED DESCRIPTION

[0032] The embodiments of the present invention will be described below.

[0033] [Adhesive sheet]

[0034] An adhesive sheet according to one embodiment of the present invention has an adhesive layer. Figure 1 Detailed structure of an example of an adhesive sheet according to this embodiment is shown in FIG. Figure 1As shown, an adhesive sheet 1 according to one embodiment is composed of two release sheets 12a and 12b and an adhesive layer 11. The adhesive layer 11 is sandwiched between the two release sheets 12a and 12b in a manner that the adhesive layer 11 contacts the release surfaces of the two release sheets 12a and 12b. In addition, the release surface of the release sheet in this specification refers to the surface of the release sheet that has releasability, including any of the surfaces that have been subjected to a release treatment and the surfaces that exhibit releasability even without a release treatment.

[0035] 1. Components

[0036] 1-1. Adhesive layer

[0037] The adhesive constituting the adhesive layer 11 contains light-diffusing particles. The adhesive layer 11 has the following physical properties: The average haze value for light with a wavelength of 380 nm, the haze value for light with a wavelength of 580 nm, and the haze value for light with a wavelength of 780 nm is 70% or greater and 100% or less; the standard deviation of the haze value for light with a wavelength of 380 nm, the haze value for light with a wavelength of 580 nm, and the haze value for light with a wavelength of 780 nm is 7.50 or less; and the total light transmittance is 70% or greater. The haze values ​​for each light beam and the total light transmittance are values ​​measured in accordance with JIS K7375:2008.

[0038] While an average haze value of 70% or greater can easily suppress brightness unevenness, it can also easily cause color unevenness. However, by setting the standard deviation of the haze value to 7.50 or less, color unevenness can be suppressed, preventing unintended coloration of light from the light source and its diffused light. Furthermore, by setting the total light transmittance to 70% or greater, the visibility of images and videos (visibility of the display device) when used in a display device is excellent.

[0039] From the perspective of suppressing brightness unevenness, the average haze value is preferably 80% or higher, preferably 86% or higher, particularly preferably 88% or higher, and even more preferably 90% or higher. Furthermore, the average haze value is 100% or lower. From the perspective of achieving high total light transmittance, it is preferably 98% or lower, particularly preferably 95% or lower, and even more preferably less than 94%.

[0040] Furthermore, from the perspective of suppressing color unevenness, the standard deviation should be 7.50 or less, preferably 5.00 or less, particularly preferably 2.50 or less, and even more preferably 1.50 or less. On the other hand, from the perspective of suppressing color unevenness, the lower limit of the standard deviation is most preferably 0. From the perspective of ease of adjusting the standard deviation, it is preferably 0.01 or more, particularly preferably 0.10 or more, and even more preferably 0.50 or more.

[0041] From the perspective of the visibility of the display device, the total light transmittance should be 70% or more, preferably 80% or more, particularly preferably 90% or more, and even more preferably 99% or more. Furthermore, from the perspective of the visibility of the display device, the upper limit of the total light transmittance is most preferably 100%.

[0042] The total value of the image clarity of the optical combs of 0.125 mm, 0.25 mm, 0.5 mm, 1.0 mm, and 2.0 mm, measured in accordance with JIS K7374:2007, for the adhesive layer 11 of this embodiment is preferably 400 or less, more preferably 300 or less, particularly preferably 200 or less, and even more preferably 180 or less. Conventionally, when a display device is manufactured using a backlight having multiple luminous elements as a light source, uneven brightness may sometimes occur in the displayed image due to the presence and absence of the luminous elements. However, by making the total value of the image clarity relatively small as described above, an excellent effect of suppressing uneven brightness can be achieved.

[0043] Furthermore, the total value of the aforementioned image sharpness is preferably 0.1 or higher, more preferably 1 or higher, particularly preferably 10 or higher, and even more preferably 30 or higher. As a result, the visibility of the image and image of the obtained display becomes excellent.

[0044] Here, image sharpness is obtained by measuring the amount of parallel light rays transmitted through the test specimen using an optical comb with a transmitting and blocking section. The smaller the width (comb width) of the transmitting and blocking sections of the optical comb, the higher the image sharpness. Image sharpness is measured according to the transmission method of JIS K7374:2007. Specific measurement methods are shown in the test examples described later.

[0045] The storage modulus G' of the adhesive constituting the adhesive layer 11 of the present embodiment at 23°C is preferably 0.001MPa or more, more preferably 0.01MPa or more, particularly preferably 0.03MPa or more, and further preferably 0.05MPa or more. In addition, the above-mentioned storage modulus G' is preferably 10MPa or less, more preferably 1MPa or less, particularly preferably 0.20MPa or less, and further preferably 0.09MPa or less. By making the storage modulus G' within the above-mentioned range, excellent concave-convex embedding properties can be obtained, not only in the initial stage, but also under high temperature and high humidity conditions (for example, 85°C, 85%RH, 72 hours), it is possible to maintain the state of fully embedding the concave-convex due to the luminous body, etc. using the adhesive layer, and it is also possible to suppress the occurrence of floating, peeling, etc. at the interface between the concave-convex and the adhesive layer. In addition, the method for measuring the storage modulus G' in this specification is as shown in the test examples described later.

[0046] From the perspective of reducing the standard deviation of the haze value and reducing the image clarity, the average particle size of the light-diffusing particles contained in the adhesive constituting the adhesive layer 11, obtained by centrifugal sedimentation light transmission method, is preferably 0.5 μm or more, more preferably 1 μm or more, particularly preferably 2 μm or more, and even more preferably 4 μm or more.

[0047] Furthermore, from the perspective of improving the average haze value with a smaller amount of light-diffusing particles, the average particle size of the light-diffusing particles is preferably 50 μm or less, more preferably 30 μm or less, particularly preferably 17 μm or less, and even more preferably 13 μm or less.

[0048] In addition, the average particle size obtained by the centrifugal sedimentation light transmission method is the value obtained by using a sample of 1.2g of light-diffusing microparticles and 98.8g of isopropanol, which were thoroughly stirred, as a test sample, and measuring it using a centrifugal automatic particle size distribution measuring device (manufactured by HORIBA, Ltd., product name "CAPA-700").

[0049] The adhesive constituting the adhesive layer 11 is formed of light-diffusing fine particles and a matrix.

[0050] In this embodiment, from the perspective of increasing the average value of the haze value while suppressing the standard deviation of the haze value to a low level, the absolute value of the difference between the refractive index of the adhesive matrix and the refractive index of the light-diffusing particles (refractive index difference) is preferably 0.001 or more, more preferably 0.010 or more, particularly preferably 0.020 or more, further preferably 0.030 or more, and most preferably 0.040 or more. Furthermore, from the perspective of increasing total light transmittance and reducing image sharpness, the absolute value of the refractive index difference is preferably 0.5 or less, more preferably 0.2 or less, particularly preferably 0.15 or less, and further preferably 0.10 or less.

[0051] Here, the method for measuring the refractive index of the matrix is ​​as described in the test examples described later. In addition, the refractive index of the light-diffusing fine particles can be obtained by method B of JIS K7142:2008.

[0052] The refractive index of the matrix of the adhesive is preferably 1.10 or higher, more preferably 1.20 or higher, particularly preferably 1.30 or higher, further preferably 1.40 or higher, and most preferably 1.45 or higher. Furthermore, the refractive index of the matrix of the adhesive is preferably 2.00 or lower, more preferably 1.80 or lower, particularly preferably 1.60 or lower, and further preferably 1.50 or lower. By ensuring that the refractive index of the matrix of the adhesive is within the above-mentioned range, the absolute value of the refractive index difference is more likely to fall within the above-mentioned range.

[0053] The refractive index of the light-diffusing particles is preferably 1.10 or higher, more preferably 1.20 or higher, particularly preferably 1.30 or higher, and even more preferably 1.40 or higher. Furthermore, the refractive index of the light-diffusing particles is preferably 2.00 or lower, more preferably 1.80 or lower, particularly preferably 1.60 or lower, and even more preferably 1.58 or lower. Therefore, the absolute value of the aforementioned refractive index difference readily falls within the above-mentioned range.

[0054] From the perspective of reducing the standard deviation of the haze value and easily obtaining an adhesive with high haze and low image clarity, the content of the light-diffusing fine particles in the adhesive is preferably 0.1% by mass or more, more preferably 1% by mass or more, particularly preferably 3% by mass or more, and even more preferably 5% by mass or more. Furthermore, from the perspective of suppressing the storage modulus G' of the adhesive to a low level, the content of the light-diffusing fine particles in the adhesive is preferably 40% by mass or less, more preferably 30% by mass or less, particularly preferably 20% by mass or less, even more preferably 10% by mass or less, and most preferably 8% by mass or less.

[0055] As long as the adhesive layer 11 of the adhesive sheet 1 of the present embodiment satisfies the above-mentioned physical properties and does not hinder the effect brought by the light diffusion particles, its type is not particularly limited. For example, it can be any one of acrylic adhesives, polyester adhesives, polyurethane adhesives, rubber adhesives, silicone adhesives, etc. In addition, the adhesive can be any one of emulsion type, solvent type or solvent-free type, and can also be any one of cross-linked type or non-cross-linked type. Among them, acrylic adhesives with excellent adhesive physical properties, optical characteristics, etc. are preferred. As acrylic adhesives, cross-linked acrylic adhesives are preferred, and thermally cross-linked acrylic adhesives are further preferred.

[0056] The adhesive of the present embodiment may be non-active energy ray-curable or active energy ray-curable. Hereinafter, the description will focus on the non-active energy ray-curable adhesive.

[0057] Specifically, the adhesive of the present embodiment is preferably formed by crosslinking an adhesive composition (hereinafter sometimes referred to as "adhesive composition P") containing a (meth)acrylate polymer (A), a crosslinking agent (B), and light-diffusing particles (C). The adhesive obtained by crosslinking the adhesive composition P easily satisfies the above-mentioned physical properties. In addition, in this specification, (meth)acrylic acid refers to acrylic acid and methacrylic acid. Other similar terms are also the same. In addition, the concept of "polymer" also includes "copolymer".

[0058] (1) Components of adhesive composition P

[0059] (1-1) (Meth)acrylate polymer (A)

[0060] The (meth)acrylate polymer (A) of this embodiment preferably contains a reactive group-containing monomer as a monomer unit constituting the polymer, wherein the reactive group-containing monomer has a reactive group within the molecule that reacts with the crosslinking agent (B). By reacting the reactive group derived from the reactive group-containing monomer with the crosslinking agent (B), a crosslinked structure (three-dimensional network structure) is formed, resulting in an adhesive having the desired cohesive strength.

[0061] As monomers containing reactive groups, preferred examples include monomers with intramolecular hydroxyl groups (hydroxyl-containing monomers) and monomers with intramolecular carboxyl groups (carboxyl-containing monomers). Among these, monomers containing hydroxyl groups or carboxyl groups that exhibit excellent reactivity with the crosslinking agent (B) are preferred.

[0062] Examples of hydroxyl-containing monomers include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Among these, hydroxyalkyl (meth)acrylates having a hydroxyalkyl group having 1 to 4 carbon atoms are preferred from the perspective of reactivity with the crosslinking agent (B) and copolymerizability with other monomers. Specifically, examples include 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate, and particularly preferably, 2-hydroxyethyl acrylate or 4-hydroxybutyl acrylate. These may be used alone or in combination of two or more.

[0063] Examples of carboxyl-containing monomers include acrylic acid, methacrylic acid, crotonic acid, maleic acid, itaconic acid, and citraconic acid, among other olefinic unsaturated carboxylic acids. Among these, acrylic acid is preferred based on the reactivity of the carboxyl group in the resulting (meth)acrylate polymer (A) with the crosslinking agent (B) and its copolymerization with other monomers. These monomers can be used alone or in combination of two or more.

[0064] Based on the following limit, the (meth)acrylate polymer (A) preferably contains 1% by mass or more, particularly preferably 6% by mass or more, further preferably 12% by mass or more, and most preferably 17% by mass or more of a monomer containing a reactive group as a monomer unit constituting the polymer. In addition, based on the upper limit, the (meth)acrylate polymer (A) preferably contains 40% by mass or less, particularly preferably 35% by mass or less, further preferably 30% by mass or less, and most preferably 25% by mass or less of a monomer containing a reactive functional group as a monomer unit constituting the polymer. If the (meth)acrylate polymer (A) contains the reactive group-containing monomer as a monomer unit in the above amount, a good cross-linked structure can be formed in the resulting adhesive, which is easy to satisfy the above-mentioned physical properties such as the storage modulus G'. In addition, the dispersibility of the light-diffusing particles (C) in the resulting adhesive tends to become better.

[0065] In addition, the (meth)acrylate polymer (A) also preferably does not contain a carboxyl-containing monomer as a monomer unit constituting the polymer. Since the carboxyl group is an acid component, by not containing a carboxyl-containing monomer, even when there is a substance that produces adverse conditions due to acid in the adhesive's attachment object, such as a transparent conductive film or metal film such as tin-doped indium oxide (ITO), the above-mentioned adverse conditions (corrosion, resistance value change, etc.) caused by the acid can be suppressed. However, it is also allowed to contain a specified amount of carboxyl-containing monomer to the extent that the above-mentioned adverse conditions are not produced. Specifically, in the (meth)acrylate polymer (A), it is allowed to contain a carboxyl-containing monomer as a monomer unit in an amount of less than 0.1% by mass, preferably in an amount of less than 0.01% by mass, and further preferably in an amount of less than 0.001% by mass.

[0066] The (meth)acrylate polymer (A) preferably contains an alkyl (meth)acrylate as a monomer unit constituting the polymer. This allows for excellent adhesiveness. The alkyl group may be linear or branched.

[0067] From the perspective of adhesiveness, alkyl (meth)acrylates having an alkyl group with 1 to 20 carbon atoms are preferred. Examples of alkyl (meth)acrylates having an alkyl group with 1 to 20 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, and octadecyl (meth)acrylate. Among these, alkyl (meth)acrylates having an alkyl group with 4 to 8 carbon atoms are preferred from the perspective of further improving adhesiveness and facilitating satisfaction of the aforementioned physical properties. Specifically, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, or isooctyl (meth)acrylate are preferred, and n-butyl acrylate, 2-ethylhexyl acrylate, or isooctyl acrylate are even more preferred. These may be used alone or in combination of two or more.

[0068] The (meth)acrylate polymer (A) preferably contains 30% by mass or more, more preferably 40% by mass or more, particularly preferably 50% by mass or more, and further preferably 55% by mass or more of (meth)acrylate alkyl ester as the monomer unit constituting the polymer. If the lower limit of the content of the (meth)acrylate alkyl ester is as described above, the (meth)acrylate polymer (A) can exhibit suitable adhesion while making the storage modulus G' low. On the other hand, the (meth)acrylate polymer (A) preferably contains 85% by mass or less, more preferably 80% by mass or less, particularly preferably 75% by mass or less, and further preferably 70% by mass or less of (meth)acrylate alkyl ester as the monomer unit constituting the polymer. If the upper limit of the content of the (meth)acrylate alkyl ester is as described above, it is possible to introduce an appropriate amount of other monomer components such as a reactive functional group-containing monomer into the (meth)acrylate polymer (A).

[0069] The (meth)acrylate polymer (A) also preferably contains a monomer having an alicyclic structure in its molecule (alicyclic structure-containing monomer) as a monomer unit constituting the polymer. Since alicyclic structure-containing monomers are bulky, their presence in the polymer is presumably believed to increase the spacing between the polymers, thereby facilitating satisfaction of the aforementioned physical properties, particularly the storage modulus G'.

[0070] The alicyclic carbon rings in the alicyclic monomer can be saturated or partially unsaturated. Furthermore, the alicyclic structure can be monocyclic, bicyclic, tricyclic, or multicyclic. From the perspective of ensuring appropriate spacing between the resulting (meth)acrylate polymers (A) and reducing the storage modulus G', a multicyclic alicyclic structure is preferred. Furthermore, considering the compatibility of the (meth)acrylate polymer (A) with other components, the multicyclic structure is particularly preferred to be bicyclic to tetracyclic. Also, from the same perspective, the number of carbon atoms in the alicyclic structure (referring to the total number of carbon atoms in the ring-forming portion; when multiple rings exist independently, it refers to their total number of carbon atoms) is generally preferred to be 5 or more, and particularly preferred to be 7 or more. On the other hand, while there is no particular upper limit to the number of carbon atoms in the alicyclic structure, from the same perspective, it is preferably 15 or less, and particularly preferred to be 10 or less.

[0071] Specifically, examples of the aforementioned alicyclic monomers include cyclohexyl methacrylate, dicyclopentyl methacrylate, adamantyl methacrylate, isobornyl methacrylate, dicyclopentenyl methacrylate, and dicyclopentenyloxyethyl methacrylate. Among these, dicyclopentyl methacrylate (10 carbon atoms in the alicyclic structure), adamantyl methacrylate (10 carbon atoms in the alicyclic structure), or isobornyl methacrylate (7 carbon atoms in the alicyclic structure) are preferred for their superior encapsulation properties. Isobornyl methacrylate is particularly preferred, and isobornyl methacrylate is even more preferred. They can be used alone or in combination of two or more.

[0072] When the (meth)acrylate polymer (A) contains an alicyclic monomer as a monomer unit constituting the polymer, from the perspective of easily satisfying the aforementioned storage modulus G', it is preferable to contain 1% or more by mass, particularly preferably 5% or more by mass, and even more preferably 10% or more of the alicyclic monomer. Furthermore, from the same perspective, it is preferable to set the content of the alicyclic monomer to 40% or less by mass, particularly preferably 30% or less by mass, and even more preferably 20% or less by mass.

[0073] The aforementioned (meth)acrylate polymer (A) preferably contains a nitrogen-containing monomer as a monomeric unit constituting the polymer. By having a nitrogen-containing monomer as a structural unit in the polymer, the adhesive can be endowed with a specified polarity, resulting in excellent affinity for adhesives even to substrates with a certain degree of polarity, such as glass. From the perspective of giving the (meth)acrylate polymer (A) suitable rigidity, the aforementioned nitrogen-containing monomer is preferably a monomer having a nitrogen-containing heterocycle. Furthermore, from the perspective of increasing the degree of freedom of the portion derived from the aforementioned nitrogen-containing monomer in the high-dimensional structure of the constructed adhesive, it is preferable that the nitrogen-containing monomer, apart from containing one polymerizable group used in the polymerization of the (meth)acrylate polymer (A), does not contain reactive unsaturated double bond groups.

[0074] Examples of monomers having nitrogen-containing heterocycles include N-(meth)acryloylmorpholine, N-vinyl-2-pyrrolidone, N-(meth)acryloylpyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-(meth)acryloylaziridine, aziridineylethyl(meth)acrylate, 2-vinylpyridine, 4-vinylpyridine, 2-vinylpyrazine, 1-vinylimidazolium, N-vinylcarbazole, and N-vinylphthalimide. Among these, N-(meth)acryloylmorpholine, which exhibits superior adhesive properties, is preferred, and N-acryloylmorpholine is particularly preferred. They can be used alone or in combination of two or more.

[0075] When the (meth)acrylate polymer (A) contains a nitrogen-containing monomer as a monomer unit constituting the polymer, it is preferable to contain 0.1% by mass or more, more preferably 1% by mass or more, particularly preferably 3% by mass or more, and even more preferably 8% by mass or more of the nitrogen-containing monomer as a monomer unit constituting the polymer. Furthermore, the (meth)acrylate polymer (A) preferably contains 30% by mass or less, particularly preferably 20% by mass or less, and even more preferably 14% by mass or less of the nitrogen-containing monomer as a monomer unit constituting the polymer. If the content of the nitrogen-containing monomer is within the above range, the resulting adhesive can fully exert excellent adhesion to glass.

[0076] Depending on the requirements, the (meth)acrylate polymer (A) may also contain other monomers as monomeric units constituting the polymer. To avoid hindering the aforementioned effects of monomers containing reactive functional groups, monomers without reactive functional groups are preferred as other monomers. Examples of such monomers include, for instance, methoxyethyl methacrylate, ethoxyethyl methacrylate, alkoxyalkyl methacrylates, vinyl acetate, and styrene. They can be used alone or in combination of two or more.

[0077] The (meth)acrylate polymer (A) is preferably a linear polymer because a linear polymer facilitates entanglement of molecular chains and can be expected to improve cohesive strength, thereby easily obtaining an adhesive with excellent unevenness embedding properties under high temperature and high humidity conditions.

[0078] Furthermore, the (meth)acrylate polymer (A) is preferably a solution polymer obtained by solution polymerization. This is because a high molecular weight polymer can be easily obtained, and improved cohesive strength can be expected, thereby easily obtaining an adhesive with excellent uneven embedding properties under high temperature and high humidity conditions.

[0079] The polymerization form of the (meth)acrylate polymer (A) may be a random copolymer or a block copolymer.

[0080] The weight average molecular weight of (meth)acrylate polymer (A) is preferably more than 100,000, more preferably more than 250,000, and particularly preferably more than 400,000. In addition, the weight average molecular weight of (meth)acrylate polymer (A) is preferably less than 3,000,000, particularly preferably less than 2,000,000, and further preferably less than 1,000,000. If the weight average molecular weight of (meth)acrylate polymer (A) is within the above range, the storage modulus G' and the adhesion of the obtained adhesive are easily suitable. Here, the weight average molecular weight in this specification is the value converted to standard polystyrene measured by gel permeation chromatography (GPC).

[0081] In the adhesive composition P, the (meth)acrylate polymer (A) may be used alone or in combination of two or more.

[0082] (1-2) Cross-linking agent (B)

[0083] The crosslinking agent (B) can react with the reactive group possessed by the (meth)acrylate polymer (A). Examples of the crosslinking agent (B) include isocyanate crosslinking agents, epoxy crosslinking agents, amine crosslinking agents, melamine crosslinking agents, aziridine crosslinking agents, hydrazine crosslinking agents, aldehyde crosslinking agents, oxazoline crosslinking agents, metal alkoxide crosslinking agents, metal chelate crosslinking agents, metal salt crosslinking agents, and ammonium salt crosslinking agents. In addition, the crosslinking agent (B) can be used alone or in combination of two or more.

[0084] When the reactive groups of the (meth)acrylate polymer (A) are hydroxyl groups, it is preferred to use an isocyanate crosslinking agent that is highly reactive with the hydroxyl groups. Furthermore, when the reactive groups of the (meth)acrylate polymer (A) are carboxyl groups, it is preferred to use an epoxy crosslinking agent that is highly reactive with the carboxyl groups.

[0085] Isocyanate crosslinking agents contain at least a polyisocyanate compound. Examples of polyisocyanate compounds include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate; aliphatic polyisocyanates such as hexamethylene diisocyanate; alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate; and biuret and isocyanurate forms of these compounds. Further examples include adducts formed as reaction products with low-molecular-weight active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil. Among these, trimethylolpropane-modified aromatic polyisocyanates are preferred due to their reactivity with hydroxyl groups, and trimethylolpropane-modified tolylene diisocyanate is particularly preferred.

[0086] Examples of epoxy crosslinking agents include 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m-xylenediamine, ethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, diglycidylaniline, and diglycidylamine. Among these, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane is preferred from the perspective of reactivity with carboxyl groups.

[0087] The content of the crosslinking agent (B) in the adhesive composition P is preferably 0.001 parts by mass or more, particularly preferably 0.01 parts by mass or more, and more preferably 0.1 parts by mass or more, relative to 100 parts by mass of the (meth)acrylate polymer (A). In addition, the content of the crosslinking agent (B) is preferably 10 parts by mass or less, particularly preferably 1 part by mass or less, and more preferably 0.5 parts by mass or less, relative to 100 parts by mass of the (meth)acrylate polymer (A). By making the content of the crosslinking agent (B) within the above range, the storage modulus G', adhesion, etc. of the resulting adhesive are easily suitable.

[0088] (1-3) Light-diffusing particles (C)

[0089] The light-diffusing microparticles (C) only need to exhibit the specified light-diffusing properties, and the resulting adhesive layer 11 needs to satisfy the above-mentioned physical properties.

[0090] Examples of light-diffusing microparticles (C) include inorganic light-diffusing microparticles such as silica, calcium carbonate, aluminum hydroxide, magnesium hydroxide, clay, talc, and titanium dioxide; organic light-diffusing microparticles such as acrylic resins, polystyrene resins, polyethylene resins, epoxy resins, copolymers of these, or mixtures thereof; light-diffusing microparticles formed from silicon-containing compounds with intermediate inorganic and organic structures, such as silicone resins (e.g., the TOSPEARL series manufactured by Momentive Performance Materials Japan); and composite light-diffusing microparticles of organic resins and silicone resins. Among these, light-diffusing microparticles formed from polymethyl methacrylate-polystyrene copolymers, light-diffusing microparticles formed from silicone resins, or composite light-diffusing microparticles of polystyrene resins and silicone resins are preferred. Therefore, the resulting adhesive layer 11 readily satisfies the aforementioned physical properties. The above-mentioned light-diffusing microparticles (C) can be used alone or in combination of two or more.

[0091] As the shape of the light-diffusing fine particles (C), spherical light-diffusing fine particles that diffuse light uniformly are preferred, but the present invention is not limited thereto. The average particle size of the light-diffusing fine particles (C) is as described above.

[0092] The content of light-diffusing microparticles (C) in the adhesive composition P is the same as the content of light-diffusing microparticles in the adhesive described above.

[0093] (1-4) Various additives

[0094] If necessary, various additives commonly used in acrylic adhesives, such as silane coupling agents, rust inhibitors, ultraviolet absorbers, antistatic agents, tackifiers, antioxidants, light stabilizers, softeners, and refractive index modifiers, can be added to the adhesive composition P. The polymerization solvent or dilution solvent described below is not included in the additives constituting the adhesive composition P.

[0095] The adhesive composition P preferably contains a silane coupling agent among the above. This improves adhesion to the adherend, whether it is a plastic component or a glass member, and further improves the unevenness embedding property under high temperature and high humidity conditions.

[0096] As a silane coupling agent, an organosilicon compound that is well compatible with (meth)acrylate polymer (A), has light transmittance, and has at least one alkoxysilyl group in the molecule is preferred.

[0097] Examples of silane coupling agents include, for example, silicon compounds containing polymerizable unsaturated groups such as vinyltrimethoxysilane, vinyltriethoxysilane, and methacryloxypropyltrimethoxysilane; silicon compounds with epoxy structures such as 3-glycidyl etheroxypropyltrimethoxysilane and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; silicon compounds containing thiol groups such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-mercaptopropyldimethoxymethylsilane; and 3-aminopropyltrimethoxysilane. Amino-containing silicon compounds such as methyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane; 3-chloropropyltrimethoxysilane; propyltriethoxysilane isocyanate; 1,6-bis(trimethoxysilyl)hexane; or condensates of at least one of these silane coupling agents with alkyl-containing silicon compounds such as methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane, and ethyltrimethoxysilane. They can be used alone or in combination of two or more.

[0098] The content of the silane coupling agent in the adhesive composition P is preferably 0.01 parts by mass or more, particularly preferably 0.05 parts by mass or more, and further preferably 0.1 parts by mass or more, relative to 100 parts by mass of the (meth)acrylate polymer (A). Furthermore, the content is preferably 1.2 parts by mass or less, particularly preferably 0.8 parts by mass or less, and further preferably 0.4 parts by mass or less.

[0099] (2) Preparation of adhesive composition P

[0100] The adhesive composition P can be prepared by preparing a (meth)acrylate polymer (A), mixing the obtained (meth)acrylate polymer (A), a crosslinking agent (B) and light-diffusing fine particles (C), and adding additives as needed.

[0101] (Meth)acrylate polymer (A) can be prepared by polymerizing a mixture of monomers constituting the polymer using conventional free radical polymerization. The polymerization of (meth)acrylate polymer (A) is preferably carried out using a polymerization initiator and via solution polymerization, as needed. However, the invention is not limited thereto, and polymerization can also be carried out in a solvent-free environment. Examples of polymerization solvents include ethyl acetate, n-butyl acetate, isobutyl acetate, toluene, acetone, hexane, methyl ethyl ketone, etc., and two or more may be used simultaneously.

[0102] Examples of polymerization initiators include azo compounds and organic peroxides, and more than one type can be used simultaneously. Examples of azo compounds include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-formonitrile), 2,2'-azobis(2,4-dimethylpentanonitrile), 2,2'-azobis(2,4-dimethyl-4-methoxypentanonitrile), 2,2'-azobis(methyl 2-methylpropionate), 4,4'-azobis(4-cyanopentanoic acid), 2,2'-azobis(2-hydroxymethylpropionitrile), and 2,2'-azobis[2-(2-imidazolin-2-yl)propane].

[0103] Examples of the organic peroxide include benzoyl peroxide, tert-butyl perbenzoate, cumene hydroperoxide, diisopropyl peroxydicarbonate, di-n-propyl peroxydicarbonate, di(2-ethoxyethyl) peroxydicarbonate, tert-butyl peroxyneodecanoate, tert-butyl peroxypivalate, (3,5,5-trimethylhexanoyl) peroxide, dipropionyl peroxide, and diacetyl peroxide.

[0104] Furthermore, in the polymerization step, the weight average molecular weight of the obtained polymer can be adjusted by adding a chain transfer agent such as 2-mercaptoethanol.

[0105] After obtaining (meth)acrylate polymer (A), a crosslinking agent (B), light-diffusing microparticles (C), and appropriate diluting solvents and additives are added to a solution of (meth)acrylate polymer (A), and the mixture is thoroughly mixed to obtain a solvent-diluted adhesive composition P (coating solution). Alternatively, for any of the above components, if a solid substance is used, or if precipitation occurs when mixed with other components in an undiluted state, that component can be dissolved or diluted separately in a diluting solvent beforehand, and then mixed with the other components.

[0106] The dilution solvent is not particularly limited as long as it can maintain the adhesive composition P in a dissolved or dispersed state, and preferred examples include the same solvents as the polymerization solvent.

[0107] The concentration and viscosity of the coating solution prepared by the above method are not particularly limited as long as they are within the coating range, and can be appropriately selected according to the situation. For example, the adhesive composition P can be diluted to a concentration of 10-60% by mass. Furthermore, adding a diluent is not necessary when obtaining the coating solution; if the adhesive composition P has a coating viscosity suitable for coating, a diluent may not be added. In this case, the adhesive composition P is a coating solution in which the polymerization solvent of the (meth)acrylate polymer (A) is used directly as the diluent.

[0108] (3) Formation of adhesive layer

[0109] The adhesive layer 11 of this embodiment is preferably composed of an adhesive formed by crosslinking (the coating layer of) the adhesive composition P. Crosslinking of the adhesive composition P can generally be performed by heat treatment. Alternatively, the drying process during which the dilution solvent or the like is volatilized from the coating layer of the adhesive composition P applied to the desired object can also serve as the heat treatment.

[0110] The heating temperature of the heat treatment is preferably 50 to 150° C., particularly preferably 70 to 120° C. The heating time is preferably 10 seconds to 10 minutes, particularly preferably 50 seconds to 2 minutes.

[0111] If necessary, a 1-2 week aging period at room temperature (e.g., 23°C, 50% RH) may be provided after the heat treatment. If this aging period is required, the adhesive is formed after the aging period. If this aging period is not required, the adhesive is formed directly after the heat treatment.

[0112] By the above-mentioned heat treatment (and aging), the (meth)acrylate polymer (A) is crosslinked via the crosslinking agent (B), thereby obtaining a pressure-sensitive adhesive.

[0113] (4) Composition of adhesive layer

[0114] The adhesive layer 11 of the present embodiment can be formed by a single layer or by laminating multiple layers. In addition, in the adhesive layer 11 of the present embodiment, an adhesive layer (transparent adhesive layer) not containing light-diffusing particles can be laminated on one side or both sides of the adhesive layer (light-diffusing adhesive layer) containing light-diffusing particles.

[0115] When a transparent adhesive layer is present as described above, it is preferred that the transparent adhesive layer be positioned on the surface in contact with the adherend having irregularities. This prevents the light-diffusing adhesive layer from being compressed or deformed by the irregularities of the adherend, thereby obtaining an optical laminate (display) with even better color and brightness unevenness suppression properties.

[0116] 1-2. Peel sheet

[0117] The release sheets 12a and 12b protect the adhesive layer 11 until the adhesive sheet 1 is used and are peeled off when the adhesive sheet 1 (adhesive layer 11) is used. In the adhesive sheet 1 of this embodiment, one or both of the release sheets 12a and 12b are not necessarily required.

[0118] As the release sheets 12a and 12b, for example, polyethylene film, polypropylene film, polybutylene film, polybutadiene film, polymethylpentene film, polyvinyl chloride film, vinyl chloride copolymer film, polyethylene terephthalate film, polyethylene naphthalate film, polybutylene terephthalate film, polyurethane film, ethylene-vinyl acetate film, ionomer resin film, ethylene-(meth)acrylic acid copolymer film, ethylene-(meth)acrylate copolymer film, polystyrene film, polycarbonate film, polyimide film, fluororesin film, etc. can be used. In addition, cross-linked films of the above films can also be used. Furthermore, laminated films of the above films can also be used.

[0119] The release surfaces of the release sheets 12a and 12b (particularly the surface in contact with the adhesive layer 11) are preferably subjected to a release treatment. Examples of release agents used for the release treatment include alkyd, silicone, fluorine, unsaturated polyester, polyolefin, and wax release agents. Furthermore, it is preferred that one of the release sheets 12a and 12b be a heavy-release type with a high release force, and the other be a light-release type with a low release force.

[0120] The thickness of the release sheets 12a and 12b is not particularly limited, but is generally about 20 to 150 μm.

[0121] 2.Physical properties

[0122] (1) Thickness of adhesive layer

[0123] According to the following limit value, the thickness of the adhesive layer 11 in the adhesive sheet 1 of the present embodiment (the value measured according to JIS K7130) is preferably 10 μm or more, more preferably 20 μm or more, particularly preferably 30 μm or more, and further preferably 40 μm or more. Thus, the concave and convex of the backlight source can be embedded using the adhesive layer 11, and the desired light diffusion can be obtained. In addition, according to the upper limit value, the thickness of the adhesive layer 11 is preferably 500 μm or less, more preferably 300 μm or less, particularly preferably 200 μm or less, and further preferably 150 μm or less. Thus, it is easy to obtain the desired light diffusion, and the processability also becomes good.

[0124] (2) Adhesion

[0125] According to the following limit, the adhesion of the adhesive sheet 1 of the present embodiment to the soda-lime glass is preferably 0.1N / 25mm or more, more preferably 1N / 25mm or more, particularly preferably 10N / 25mm or more, and further preferably 20N / 25mm or more. If the lower limit of the adhesion is as described above, the concave-convex embedding property under high temperature and high humidity conditions is more excellent. In addition, according to the upper limit, the adhesion of the adhesive sheet 1 of the present embodiment to the soda-lime glass is preferably 70N / 25mm or less, more preferably 50N / 25mm or less, and particularly preferably 40N / 25mm or less. If the upper limit of the adhesion of the adhesive sheet is as described above, good reoperability can be obtained, and when a lamination error occurs, the expensive display body constituent member can be reused.

[0126] The adhesive strength referred to in this specification is basically the adhesive strength measured by the 180-degree peel method in accordance with JIS Z0237:2009. A 25 mm wide and 100 mm long sample is attached to an adherend and pressurized at 0.5 MPa and 50°C for 20 minutes. The sample is then left at atmospheric pressure, 23°C, and 50% RH for 24 hours, and then measured at a peel rate of 300 mm / min.

[0127] 3. Manufacturing of adhesive sheets

[0128] As a manufacturing example of the adhesive sheet 1, the case of using the above-mentioned adhesive composition P is described. A coating liquid of the adhesive composition P is applied to the release surface of a release sheet 12a (or 12b), and the adhesive composition P is heat-crosslinked to form a coating layer. Then, the release surface of another release sheet 12b (or 12a) is superimposed on the coating layer. When a maturation period is required, the above-mentioned coating layer becomes the adhesive layer 11 by setting the maturation period. When a maturation period is not required, the above-mentioned coating layer directly becomes the adhesive layer 11. Thus, the above-mentioned adhesive sheet 1 is obtained. The conditions for the heat treatment and maturation are as described above.

[0129] As another manufacturing example of the adhesive sheet 1, a coating liquid of an adhesive composition P is applied to the release surface of a release sheet 12a, and the adhesive composition P is heat-treated to thermally crosslink the adhesive composition P to form a coating layer, thereby obtaining a release sheet 12a with a coating layer. In addition, a coating liquid of the adhesive composition P is applied to the release surface of another release sheet 12b, and the adhesive composition P is heat-treated to thermally crosslink the adhesive composition P to form a coating layer, thereby obtaining a release sheet 12b with a coating layer. Then, the release sheet 12a with a coating layer and the release sheet 12b with a coating layer are laminated so that the two coating layers are in contact with each other. When a maturation period is required, the laminated coating layer becomes the adhesive layer 11 by providing the maturation period. When a maturation period is not required, the laminated coating layer directly becomes the adhesive layer 11. Thus, the above-mentioned adhesive sheet 1 is obtained. According to this manufacturing example, even when the adhesive layer 11 is thick, stable manufacturing can be carried out.

[0130] Methods for applying the coating liquid to the adhesive composition P can include, for example, bar coating, blade coating, roller coating, blade coating, mold coating, gravure coating, etc.

[0131] 4. Application of adhesive sheet

[0132] The adhesive sheet 1 of this embodiment can be suitably used to bond two rigid bodies. Bonding rigid bodies together using an adhesive layer is more difficult than bonding films together or bonding a film to a rigid body, and the yield rate during bonding is easily reduced. However, according to the adhesive sheet 1 of this embodiment, two rigid bodies can be bonded well.

[0133] In addition, the hard body in this specification refers to a component whose structure does not undergo irreversible deformation and whose bendable angle is less than 90°. The angle is preferably less than 60°, more preferably less than 45°, particularly preferably less than 10°, and further preferably less than 5°. In addition, the bendable angle (bending angle) refers to the angle at which the hard body is lifted from the horizontal plane when it is placed on a horizontal surface, one end is fixed and the end on the opposite side is lifted. The hard body can be formed by a single layer or a single component, or by multiple layers or multiple components. In the latter case, the hard body refers to an object formed by multiple layers or multiple components that is used as an object when attached to an adhesive layer and the object as a whole meets the above-mentioned bending angle. Even if a part of the layer or component of the object does not meet the above-mentioned bending angle, the object can be called a hard body.

[0134] Specifically, as described below, the adhesive sheet 1 of this embodiment can be suitably used to bond backlights and display units such as liquid crystal panels or other rigid optical components. Backlights and display units are typically formed of rigid materials. However, the present invention is not limited to this, and can also be used to bond display components that are desired rigid materials to each other.

[0135] [Backlight Unit]

[0136] A backlight unit according to one embodiment of the present invention includes a backlight having a plurality of light-emitting elements and an adhesive layer laminated on the backlight. Since the backlight unit includes a plurality of light-emitting elements, the adhesive layer often has irregularities on its surface.

[0137] The specific structure of an example of the backlight unit of this embodiment is shown in FIG. Figure 2 .like Figure 2 As shown, the backlight unit 2 according to one embodiment includes a backlight 20 and an adhesive layer 11 stacked on the backlight 20 .

[0138] 1. Constituent elements

[0139] (1) Backlight

[0140] The backlight 20 is composed of one or more substrates 21 and a plurality of light-emitting bodies 22 provided on the substrate 21. The backlight 20 has concavities and convexities generated by the plurality of light-emitting bodies 22.

[0141] The substrate 21 is not particularly limited, and a substrate commonly used for backlights can be used. The substrate 21 is generally a printed circuit board (PCB).

[0142] The substrate 21 can be formed integrally by mounting a plurality of light emitting bodies 22 uniformly, or can be formed separately by mounting one light emitting body 22 on one substrate 21. When formed separately, each substrate 21 is usually fixed to a frame, a support, a housing, etc. In this embodiment, Figure 2 As shown, the substrate 21 is preferably formed integrally so as to collectively mount a plurality of light-emitting bodies 22 .

[0143] A reflective layer or a reflective member may be formed on the adhesive layer 11 side surface of the substrate 21. This can effectively increase the brightness of the backlight 20. The reflective layer or the reflective member can be made of known materials.

[0144] Examples of the light emitting body 22 include light emitting diodes (LEDs), laser diodes (LDs), organic electroluminescent elements, and inorganic electroluminescent elements. Among these, LEDs are preferred from the perspective of sealing performance with the adhesive layer 11, and Mini LEDs or Micro LEDs are particularly preferred.

[0145] The thickness of the luminous body 22 is preferably 5 μm or more, more preferably 50 μm or more, particularly preferably 100 μm or more, and further preferably 200 μm or more. Furthermore, the thickness of the luminous body 22 is preferably 1000 μm or less, particularly preferably 500 μm or less, and further preferably 250 μm or less.

[0146] Furthermore, the width of the gap between adjacent light emitters 22 is preferably 0.01 mm or greater, particularly preferably 0.1 mm or greater, and further preferably 0.5 mm or greater. Furthermore, the width of the gap is preferably 100 mm or less, more preferably 10 mm or less, particularly preferably 4 mm or less, and further preferably 2 mm or less.

[0147] The shape of the luminous body 22 is not particularly limited, and is generally a rectangular parallelepiped, a hemispherical shape, etc. The size of the luminous body 22 is also not particularly limited. From the perspective of the sealing performance of the luminous body, a side or diameter when viewed from above is preferably 0.01 to 100 mm, more preferably 0.1 to 10 mm, particularly preferably 0.2 to 5 mm, and even more preferably 0.5 to 2 mm.

[0148] (2)Adhesive layer

[0149] The adhesive layer 11 of the present embodiment is preferably the adhesive layer 11 of the above-mentioned adhesive sheet 1. Furthermore, the adhesive layer 11 of the present embodiment is preferably composed of an adhesive obtained by crosslinking the adhesive composition P.

[0150] The adhesive layer 11 of this embodiment embeds the unevenness caused by the light-emitting elements 22. Specifically, the adhesive layer 11 can seal the plurality of light-emitting elements 22 without any gaps. This improves water resistance and protects the light-emitting elements 22 (particularly LEDs) from moisture. Furthermore, the adhesive layer 11 diffuses the light emitted from the backlight 20. Furthermore, by possessing these physical properties, the light from the light source and its diffused light are prevented from being accidentally colored, effectively suppressing the occurrence of color unevenness.

[0151] The adhesive layer 11 may be laminated in direct contact with the backlight 20 , or may be laminated indirectly via another layer or member.

[0152] 2. Manufacturing of the backlight unit

[0153] To manufacture the backlight unit 2 of this embodiment, for example, one release sheet 12 a of the adhesive sheet 1 is peeled off, and the exposed adhesive layer of the adhesive sheet 1 is bonded to the surface of the backlight 20 on the side where the light-emitting body 22 is located.

[0154] Next, at a desired timing, another release sheet 12b is peeled off from the adhesive layer 11 of the adhesive sheet 1. The release sheet 12b is preferably peeled off when manufacturing the display device 3 described below. Before this, the adhesive layer 11 is preferably protected by the release sheet 12b.

[0155] 3. Other components

[0156] A sealing material may be provided between the backlight 20 and the adhesive layer 11. In this case, the surface of the sealing material opposite to the backlight 20 often has irregularities, and the adhesive layer 11 can absorb these irregularities.

[0157] Furthermore, another adhesive layer may be stacked between the backlight 20 and the adhesive layer 11. Even in such a case, the adhesive layer 11 can alleviate the influence of the other adhesive layer on the embedding of the unevenness.

[0158] Furthermore, two or more layers of the sealing material and adhesive layer may be stacked between the backlight 20 and the adhesive layer 11 .

[0159] [Display device]

[0160] A display device according to one embodiment of the present invention comprises the backlight unit according to the above embodiment and a display portion laminated on the adhesive layer of the backlight unit. The display portion may be laminated in direct contact with the adhesive layer or may be laminated indirectly via another layer or member.

[0161] A display device as an example of this embodiment is shown in FIG. Figure 3 .

[0162] like Figure 3 As shown, the display device 3 of this embodiment includes the above-mentioned backlight unit 2 and a display portion 30 stacked on the adhesive layer 11 of the backlight unit 2. The backlight 20 in the display device 3 corresponds to a direct-type backlight.

[0163] Examples of the display device 3 include a liquid crystal display (LCD), a light emitting diode (LED) display, an organic electroluminescent (organic EL) display, and electronic paper. The display device 3 may also be a touch panel. Among these, a liquid crystal display (liquid crystal display device) is preferred, as it requires a backlight.

[0164] The display unit 30 may be, for example, a liquid crystal panel, but is not limited thereto. For example, it may be a portion of a component of the liquid crystal panel, or an optical component (e.g., a light diffuser or ultraviolet absorption filter) used in conjunction with the display unit 30 to add or enhance the functions of the liquid crystal panel. A known display unit may be used for the display unit 30.

[0165] In order to manufacture the display device 3 of this embodiment, the adhesive layer 11 exposed by the backlight unit 2 is bonded to the display part 30. In addition, when a release sheet 12b is stacked on the adhesive layer 11, the release sheet 12b is peeled off to expose the adhesive layer 11, and on this basis, the adhesive layer 11 is bonded to the display part 30.

[0166] When manufacturing the display device 3 of this embodiment, the adhesive layer 11 can be first attached to the display part 30, and then the adhesive layer 11 can be attached to the backlight 20.

[0167] Here, the desired optical component can be provided between the adhesive layer 11 and the display portion 30, or on the surface of the display portion 30 opposite to the adhesive layer 11. Examples of such optical components include brightness enhancement films, contrast enhancement films, viewing angle compensation films, transparent conductive films, liquid crystal polymer films, semi-transparent reflective films, anti-scattering films, and light diffusion plates.

[0168] The embodiments described above are for the purpose of understanding the present invention and are not intended to limit the present invention. Therefore, the elements disclosed in the above embodiments also cover all design changes or equivalents that fall within the technical scope of the present invention.

[0169] For example, either of the release tabs 12a and 12b of the adhesive tab 1 can be omitted.

[0170] Example

[0171] Hereinafter, the present invention will be described in more detail with reference to Examples and the like, but the scope of the present invention is not limited to these Examples and the like.

[0172] [Example 1]

[0173] 1. Preparation of (meth)acrylate polymers

[0174] A (meth)acrylate polymer (A) was prepared by copolymerizing 30 parts by weight of 2-ethylhexyl acrylate, 30 parts by weight of n-butyl acrylate, 10 parts by weight of isobornyl acrylate, 10 parts by weight of N-acryloylmorpholine, and 20 parts by weight of 2-hydroxyethyl acrylate. The molecular weight of the (meth)acrylate polymer (A) was determined using the method described below, and the weight-average molecular weight (Mw) was 500,000.

[0175] 2. Preparation of adhesive compositions

[0176] 100 parts by mass (solid content conversion value; the same applies hereinafter) of the (meth)acrylate polymer (A) obtained in the above step 1, 0.2 parts by mass of trimethylolpropane-modified toluene diisocyanate (manufactured by TOYOCHEM CO., LTD., product name "BHS8515") as a crosslinking agent (B), 7.5 parts by mass of light-diffusing fine particles (C) composed of a silicone resin (a silicon-containing compound having an intermediate structure between inorganic and organic) (C1; manufactured by Momentive Performance Materials Japan, product name "TOSPEARL 145", average particle size: 4.5 μm, refractive index: 1.43), and 0.13 parts by mass of 3-glycidoxypropyltrimethoxysilane (Si1) as a silane coupling agent were mixed, stirred thoroughly, and diluted with methyl ethyl ketone to obtain a coating solution of an adhesive composition.

[0177] Table 1 shows the respective proportions (solid content conversion values) of the adhesive composition when the (meth)acrylate polymer (A) is 100 parts by mass (solid content conversion value). Detailed descriptions of the abbreviations and the like described in Table 1 are as follows.

[0178] [(Meth)acrylate polymer (A)]

[0179] 2EHA: 2-ethylhexyl acrylate

[0180] BA: n-Butyl acrylate

[0181] IBXA: Isobornyl acrylate

[0182] ACMO: N-Acryloylmorpholine

[0183] HEA: 2-Hydroxyethyl Acrylate

[0184] AA: Acrylic acid

[0185] 4HBA: 4-Hydroxybutyl acrylate

[0186] EA: Ethyl acrylate

[0187] [Crosslinking agent (B)]

[0188] B1: Trimethylolpropane-modified toluene diisocyanate (manufactured by TOYOCHEM CO., LTD., product name "BHS8515")

[0189] B2: Trimethylolpropane-modified diphenylmethylene diisocyanate (manufactured by Soken Chemical & Engineering Co., Ltd., product name "TD-75")

[0190] B3: 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane

[0191] B4: Aluminum triacetylacetonate

[0192] [Light Diffusing Particles (C)]

[0193] C1: Light-diffusing fine particles made of silicone resin (a silicon-containing compound having an intermediate structure between inorganic and organic) (manufactured by Momentive Performance Materials Japan, product name "TOSPEARL 145", average particle size: 4.5 μm, refractive index: 1.43)

[0194] C2: Light-diffusing fine particles made of silicone resin (a silicon-containing compound having an intermediate structure between inorganic and organic) (manufactured by Momentive Performance Materials Japan, product name "TOSPEARL 1100", average particle size: 11 μm, refractive index: 1.43)

[0195] C3: spherical polymethyl methacrylate-polystyrene copolymer microparticles (manufactured by Sekisui Kasei Co., Ltd., product name "XX-13LA", average particle size: 4 μm, refractive index: 1.565)

[0196] C4: Light-diffusing fine particles formed of silicone resin and polystyrene resin (manufactured by Nippon Shokubai Co., Ltd., product name "SOLIOSTAR RA-Y50X", average particle size: 5 μm, refractive index: 1.57)

[0197] C5: Light-diffusing fine particles made of silicone resin (a silicon-containing compound having an intermediate structure between inorganic and organic) (manufactured by Momentive Performance Materials Japan, product name "TOSPEARL 120," average particle size: 2 μm, refractive index: 1.43)

[0198] C6: Light-diffusing fine particles made of melamine resin and benzoguanamine resin (manufactured by Nippon Shokubai Co., Ltd., product name "EPOSTAR M-30", average particle size: 3 μm, refractive index: 1.66)

[0199] [Silane coupling agent]

[0200] Si1: 3-glycidoxypropyltrimethoxysilane

[0201] Si2: A-50 (manufactured by Soken Chemical & Engineering Co., Ltd.)

[0202] 3. Manufacturing of adhesive sheets

[0203] The obtained coating solution of the adhesive composition was applied using a knife coater onto the release-treated surface of a heavy-release release sheet (manufactured by LINTEC CORPORATION, product name "SP-PET752150") having one side of a polyethylene terephthalate film release-treated with a silicone release agent, and then heated at 90°C for 1 minute to form a coating layer.

[0204] Next, the coating layer on the heavy-peel release sheet obtained above was attached to a light-peel release sheet (manufactured by LINTEC CORPORATION, product name "SP-PET381031") obtained by peeling a single surface of a polyethylene terephthalate film with a silicone release agent, with the peeling-treated surface of the light-peel release sheet in contact with the coating layer, thereby producing an adhesive sheet consisting of a heavy-peel release sheet / adhesive layer coating layer (thickness: 50 μm) / light-peel release sheet.

[0205] The thickness of the adhesive layer is a value measured using a constant pressure thickness gauge (manufactured by TECLOCK CO., LTD., product name “PG-02”) in accordance with JIS K7130 (the same shall apply hereinafter).

[0206] [Examples 2-10, Comparative Example 1]

[0207] An adhesive sheet was produced in the same manner as in Example 1, except that the types and ratios of the monomers constituting the (meth)acrylate polymer (A), the weight average molecular weight (Mw) of the (meth)acrylate polymer (A), the type and blending amount of the crosslinking agent (B), the type and blending amount of the light-diffusing fine particles (C), the type and blending amount of the silane coupling agent, and the thickness of the adhesive layer were changed to those shown in Table 1. In Example 7, a 100 μm thick adhesive layer was prepared by laminating two 50 μm thick adhesive layers.

[0208] The weight average molecular weight (Mw) is a polystyrene-equivalent weight average molecular weight measured using gel permeation chromatography (GPC) under the following conditions (GPC measurement).

[0209] <Measurement Conditions>

[0210] GPC measurement equipment: HLC-8020 manufactured by TOSOH CORPORATION

[0211] • GPC column (passes through in the following order): Manufactured by TOSOH CORPORATION

[0212] TSK guard column HXL-H

[0213] TSK gel GMHXL (×2)

[0214] TSK gel G2000HXL

[0215] ·Test solvent: tetrahydrofuran

[0216] ·Measurement temperature: 40℃

[0217] [Test Example 1] (Measurement of refractive index)

[0218] Except that light diffusion particles are not mixed, an adhesive composition is prepared in the same manner as in each embodiment and comparative example. Then, using the adhesive composition, an adhesive sheet is manufactured in the same manner as in each embodiment and comparative example. An Abbe refractometer (manufactured by ATAGO CO., LTD., product name "Abbe Refractometer DR-M2", Na light source, wavelength: 589nm) is used to measure the refractive index of the adhesive layer of the obtained adhesive sheet in accordance with JIS K0062-1992. The measurement result is equivalent to the refractive index of the matrix of the adhesive. The results are shown in Table 1.

[0219] Furthermore, the difference between the measured refractive index of the adhesive matrix and the refractive index of the light-diffusing fine particles used in each example and comparative example was calculated as an absolute value.

[0220] [Test Example 2] (Measurement of Haze Value)

[0221] The adhesive layer of the adhesive sheet manufactured in the embodiment and the comparative example is attached to the glass and used as a sample for measurement. Based on the background measurement using glass, according to JIS K7375:2008, a haze meter (manufactured by NIPPON DENSHOKU INDUSTRIES Co., LTD., product name "NDH7000") is used to measure the haze value (%) of light with a wavelength of 5 nm from 380 nm to 780 nm. The haze values ​​(%) of light with a wavelength of 380 nm, 580 nm and 780 nm are shown in Table 2. In addition, the average value and standard deviation of the haze values ​​of light with a wavelength of 380 nm, 580 nm and 780 nm are calculated. The results are shown in Table 2.

[0222] [Test Example 3] (Measurement of total light transmittance)

[0223] The adhesive layer of the adhesive sheet produced in the Examples and Comparative Examples was bonded to glass to serve as the measurement sample. Based on background measurement using the glass, the total light transmittance (%) was measured using a haze meter (manufactured by Nippo Ndenshoku Industries Co., Ltd., product name "NDH5000") in accordance with JIS K7375:2008. The results are shown in Table 2.

[0224] [Test Example 4] (Measurement of Image Clarity)

[0225] The adhesive layers of the adhesive sheets produced in the Examples and Comparative Examples were measured for image clarity (%) using five optical combs (comb widths: 0.125 mm, 0.25 mm, 0.5 mm, 1.0 mm, and 2.0 mm) using an imaging property meter (product name: "ICM-10P" manufactured by Suga Test Instruments Co., Ltd.) in accordance with the transmission method of JIS K7374:2007. The total value was calculated. The results are shown in Table 2.

[0226] [Test Example 5] (Measurement of storage modulus)

[0227] The release sheet was peeled off from the adhesive sheet produced in each example and comparative example, and multiple adhesive layers were laminated to a thickness of 800 μm. Columns with a diameter of 8 mm (height of 800 μm) were punched out from the obtained adhesive layer laminates to prepare samples.

[0228] The storage modulus (G') (MPa) of the samples at 23°C was measured using a viscoelasticity measuring apparatus (product name "MCR300" manufactured by Physica Corporation) according to JIS K7244-6 by the torsional shear method under the following conditions.

[0229] Measuring frequency: 1Hz

[0230] Measurement temperature: 23°C

[0231] [Test Example 6] (Measurement of Adhesion Strength)

[0232] The light-release release sheet was peeled off from the adhesive sheets produced in the Examples and Comparative Examples, and the exposed adhesive layer was attached to the easy-adhesive layer of a polyethylene terephthalate (PET) film (manufactured by TOYOBO CO., LTD., product name "PET A4300," thickness: 100 μm) having an easy-adhesive layer to produce a heavy-release release sheet / adhesive layer / PET film laminate. The resulting laminate was cut into pieces 25 mm wide and 100 mm long.

[0233] Under the environment of 23 ℃ and 50% RH, the heavy peeling type peeling sheet was peeled off from the above-mentioned laminate, and the exposed adhesive layer was attached to soda-lime glass (manufactured by Nippon Sheet Glass Co., Ltd.), and then pressurized at 0.5 MPa and 50 ℃ for 20 minutes using an autoclave manufactured by KURIHARASEISAKUSHO Co., Ltd. Then, it was left for 24 hours under the conditions of 23 ℃ and 50% RH as a sample. Then, using a tensile testing machine (manufactured by ORIENTEC Co., Ltd., product name "TENSILON"), the adhesion force (before UV; mN / 25mm) was measured at a peeling speed of 300 mm / min and a peeling angle of 180 degrees. For conditions not described herein, the measurements were performed in accordance with JIS Z0237:2009. The results are shown in Table 2.

[0234] [Test Example 7] (Evaluation of Color Unevenness Suppression)

[0235] The light-release type release sheet is peeled off from the adhesive sheet manufactured in the examples and comparative examples, and the exposed adhesive layer is bonded to a soda-lime glass plate (manufactured by Nippon Sheet Glass Co., Ltd., thickness: 0.7 mm) to obtain a laminate formed by a heavy-release type release sheet / adhesive layer / soda-lime glass plate.

[0236] The three-wavelength fluorescent lamps were covered by the aforementioned laminate (distance from the lamps: 200 cm), and the colors of the fluorescent lamps and the light diffused into their surroundings, observable through the laminate, were observed. The color non-uniformity suppression was then evaluated according to the following criteria. The results are shown in Table 2.

[0237] ◎…There is no color unevenness even when changing the covering angle, and the whole image is white.

[0238] ○...Depending on the shielding angle, the fluorescent light portion was slightly colored (red, etc.), but at angles where no coloring was observed, the entire portion was white.

[0239] △ ...Whether the shielding angle is different, the fluorescent lamp portion is slightly colored (red, etc.), but the light diffused around the fluorescent lamp is white.

[0240] ×... Regardless of the shielding angle, the fluorescent lamp portion was clearly colored (red, etc.), and the light diffused around the fluorescent lamp was also observed to be colored.

[0241] [Test Example 8] (Evaluation of Brightness Unevenness Suppression)

[0242] Using a lead frame manufactured by ENOMOTO CO., LTD. (product name "5050D / G PKG"), an LED manufactured by GeneLite Inc. (product name "B3838ECI1"), a gold wire manufactured by Tanaka Kikinzoku Co., Ltd. (product name "GLF=30"), a sealing resin manufactured by Shin-Etsu Chemical Co., Ltd. (product name "KJR-9022"), and a die-bonding adhesive manufactured by Shin-Etsu Chemical Co., Ltd. (product name "KER3000-M2"), a 5mm×5mm square LED point light source (total light beam 20 lumens) was produced. Next, four of the obtained LED point light sources were fixed on a black resin substrate in a square arrangement at intervals of 5mm to obtain a pseudo backlight source.

[0243] The laminate produced in Test Example 7 was placed on the pseudo-backlight lamp with its heavy-peel release sheet in contact with the pseudo-backlight, yielding a pseudo-display device having a backlight unit. The LED point light source was illuminated, and the point light source's shape was visually inspected from a position 30 cm directly above the pseudo-display device. The brightness unevenness suppression was evaluated according to the following criteria. The results are shown in Table 2.

[0244] ◎…point light sources are completely unrecognizable.

[0245] 0…If you stare closely, you can recognize the point light source, but it is almost unnoticeable.

[0246] ×… can clearly identify point light sources.

[0247] [Test Example 9] (Evaluation of uneven embedding properties)

[0248] UV curable ink (manufactured by TEIKOKU PRINTING INKS MFG.CO.,LTD., product name "POS-911SUMI") was screen printed in a frame shape (external dimensions: 90 mm long × 50 mm wide, 5 mm thick) on the surface of a glass plate (manufactured by NSG PrecisionCells, Inc., product name "CORNING Glass EAGLE XG", 90 mm long × 50 mm wide × 0.5 mm thick). 2 , 2 metal halide lamps, lamp height 15 cm, belt speed 10-15 m / min), cure the printed ultraviolet curing ink to produce a stepped glass plate with a printed step (the height of the step: any one of 15 μm, 20 μm, 25 μm and 50 μm).

[0249] The light-peelable release sheet was peeled off from the adhesive sheet manufactured in the Examples and Comparative Examples, and the exposed adhesive layer was attached to the easy-adhesive layer of a polyethylene terephthalate film (manufactured by TOYOBO CO., LTD., product name "PETA4300", thickness: 100 μm) having an easy-adhesive layer. Next, the heavy-peelable release sheet was peeled off to expose the adhesive layer. Then, using a laminator (manufactured by FUJIPLA INC., product name "LPD3214"), the above-mentioned laminate was laminated on each stepped glass plate in such a way that the adhesive layer covered the entire frame-shaped printed surface. This was used as an evaluation sample.

[0250] Under the conditions of 50°C and 0.5MPa, the obtained evaluation sample was subjected to a heat-pressing treatment for 30 minutes, and then placed at room temperature, 23°C, and 50%RH for 24 hours. Then, after being stored under high temperature and high humidity conditions of 85°C and 85%RH for 72 hours (durability test), the concave-convex embedding property was evaluated. The concave-convex embedding property is judged by whether the printed step (concave-convex) is completely embedded in the adhesive layer. If bubbles, floating, peeling, etc. are observed at the interface between the printed step and the adhesive layer, it is judged that the printed step (concave-convex) is not embedded in the adhesive layer. Here, the concave-convex embedding property is calculated as the step following rate (%) shown in the following formula, and is evaluated using the following benchmarks. The results are shown in Table 2.

[0251] Step follow-through rate (%) = {(height of the step without bubbles, floating, peeling, etc., and maintaining the embedded state after durability testing (μm)) / (thickness of the adhesive layer (μm)} × 100

[0252] <Evaluation Criteria for Concave / Concave Embedding Properties>

[0253] ◎…The rate of following the segment difference is over 40%.

[0254] ○…The step difference following rate is less than 40% and is 30% or more

[0255] ×…The step difference following rate is less than 30%.

[0256] [Table 1]

[0257]

[0258]

[0259] As shown in Table 2, the adhesive sheets produced in Examples 1 to 8 and 10 also exhibited excellent suppression of color unevenness. Furthermore, the adhesive sheets produced in Examples 1 to 9 also exhibited excellent unevenness embedding properties.

[0260] Industrial Applicability

[0261] The adhesive sheet and backlight unit of the present invention are suitable for display devices, particularly liquid crystal display devices, which require suppression of color unevenness.

Claims

1. A backlight unit, which is a direct-type backlight unit comprising a backlight having a plurality of light emitters and an adhesive layer stacked on the backlight, wherein the backlight unit is characterized in that: The adhesive constituting the adhesive layer contains light-diffusing fine particles. The average value of the haze value of the adhesive layer for light with a wavelength of 380 nm, the haze value for light with a wavelength of 580 nm, and the haze value for light with a wavelength of 780 nm is 70% or more and 100% or less, The standard deviation of the haze value of the adhesive layer for light with a wavelength of 380 nm, the haze value for light with a wavelength of 580 nm, and the haze value for light with a wavelength of 780 nm is 7.50 or less, The total light transmittance of the adhesive layer is above 70%. The width of the gap between the adjacent light emitters is greater than or equal to 0.1 mm and less than or equal to 10 mm. The size of the light-emitting body is 0.1 to 10 mm in terms of one side or diameter when viewed from above.

2. The backlight unit according to claim 1, wherein: The total value of the image sharpness of the optical combs of 0.125 mm, 0.25 mm, 0.5 mm, 1.0 mm, and 2.0 mm of the adhesive layer is 0.1 or more and 400 or less.

3. The backlight unit according to claim 1, wherein: The adhesive layer has a thickness of 10 μm or more and 500 μm or less.

4. The backlight unit according to claim 1, wherein: The storage modulus G′ of the adhesive constituting the adhesive layer at 23° C. is 0.001 MPa or more and 10 MPa or less.

5. The backlight unit according to claim 1, wherein: The adhesive layer has an adhesive force to the soda-lime glass of 0.1 N / 25 mm or more.

6. The backlight unit according to claim 1, wherein: The adhesive is an acrylic adhesive.

7. The backlight unit according to claim 6, wherein: The acrylic adhesive is obtained by cross-linking an adhesive composition containing a (meth)acrylate polymer (A), a cross-linking agent (B) and light-diffusing fine particles (C). The (meth)acrylate polymer (A) contains a monomer having an alicyclic structure in the molecule as a monomer unit constituting the polymer.

8. The backlight unit according to claim 1, wherein: The light emitting body is a light emitting diode.

9. A display device, characterized in that: It has: The backlight unit according to any one of claims 1 to 8, and A display unit is stacked on the adhesive layer of the backlight unit.

Citation Information

Patent Citations

  • Pressure sensitive adhesive sheet for optics

    CN102791816A

  • Adhesive layer for optical members, adhesive layer-provided optical member, and image display device

    CN107922807A

  • Adhesive sheet and liquid crystal display member

    CN108239487A

  • Adhesive sheet, structure, and method for producing same

    CN110093109A

  • Pressure-sensitive adhesive sheet

    JP2010229246A