A method for preparing a micro-crosslinked antistatic graphene-based polypropylene composite material

Through the preparation of micro-crosslinked antistatic graphene-based polypropylene composite materials, the electrostatic problem of polypropylene materials is solved, and efficient antistatic performance and mechanical performance improvement are achieved, which is suitable for large-scale production.

CN112457571BActive Publication Date: 2024-10-11ZHEJIANG PRET NEW MATERIALS +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011372692.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-30
Publication Date
2024-10-11
Estimated Expiration
2040-11-30

AI Technical Summary

Technical Problem

Due to its high surface resistivity, polypropylene materials are prone to static electricity, leading to charge accumulation and fire risks. Existing antistatic agents require a large amount, are costly, and are difficult to produce on a large scale.

Method used

Micro-crosslinked antistatic graphene-based polypropylene composite materials are used to prepare graphene-based antistatic masterbatch through melt blending method, and are evenly dispersed in polypropylene. The cross-linked structure of the carrier polymer is used to build an electron flow path. Reduce the amount of graphene added and improve the antistatic performance.

Benefits of technology

It achieves the simple and efficient preparation of well-dispersed antistatic materials with low graphene usage, improves the antistatic and mechanical properties of polypropylene composites, reduces processing costs, and facilitates mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112457571B_ABST
    Figure CN112457571B_ABST
Patent Text Reader

Abstract

The invention discloses a micro-crosslinked antistatic graphene-based polypropylene composite material and a preparation method thereof, which is prepared from the following raw materials in parts by weight: polypropylene: 70-90 parts, inorganic filler: 0-20 parts, processing aid: 2-3 parts, initiator: 0.01-0.1 parts, graphene-based antistatic masterbatch: 5-10 parts; the graphene-based antistatic masterbatch is prepared from the following raw materials in parts by weight: elastomer: 85-95 parts, graphene microsheets: 5-20 parts, coupling agent: 1-5 parts, processing aid: 2-5 parts, initiator: 0.01-0.1 parts, crosslinking aid: 0.1-2 parts. Under the micro-crosslinking system, the amount of crosslinking agent added to the resin phase and the reinforcing phase is relatively low, and the composite material still has a certain fluidity and is easy to process while meeting the antistatic requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a functional polypropylene material and a preparation method thereof, in particular to a micro-crosslinked antistatic graphene-based polypropylene composite material and a preparation method thereof, belonging to the technical field of polypropylene. Background Art

[0002] Polypropylene material has become one of the most widely used and fastest growing plastics due to its low density, low price, easy processing and molding, and certain heat resistance and chemical resistance. It is widely used in daily necessities, food packaging, household appliances, auto parts and other products. Although polypropylene has many advantages, it is an insulating material with a high surface resistivity of >10 15 Ω·m -2 This makes it easy for PP products to accumulate electric charges during use. When the charge accumulates to a certain level, static electricity will be generated to absorb dust, thus affecting the appearance quality of the material products. More seriously, it will induce fire, which seriously affects the application of polypropylene and its composite materials.

[0003] In order to solve this problem of polypropylene materials, the modified plastics industry currently mainly improves the antistatic properties of polypropylene by adding a certain amount of antistatic agents. Common antistatic agents on the market include ionic and non-ionic types. These antistatic agents mainly have the disadvantages of large dosage and easy precipitation. For example, in a high-strength antistatic polypropylene structural sheet disclosed in patent CN102485786A, a composite antistatic masterbatch is prepared by blending 20 to 40 parts of ionic, polyol ester and polyether hindered amine antistatic agents to achieve antistatic properties for the polypropylene structural sheet. In addition to conventional antistatic agents such as ionic and non-ionic antistatic agents, new antistatic agents such as carbon nanotubes, fullerenes and graphene have also emerged in recent years. The advantages of this type of antistatic agent are that the amount added is small, the antistatic efficiency is high, and other properties of the composite material can be improved while antistatic. However, the disadvantages are also obvious. The compatibility of carbon materials with polypropylene is poor, it is difficult to disperse, the processing cost is high, and it lacks market competitiveness. For example, patent CN109897279A discloses a method for preparing a polypropylene / graphene nanocomposite material. This method uses solution blending and melt blending to disperse graphene when preparing graphene-based masterbatch, which has many steps and is time-consuming. Patent CN105273309B discloses an anti-static flame-retardant graphene-based polypropylene composite material and a preparation method thereof. This method directly blends graphene microsheets and thermally conductive carbon fibers to prepare the composite material, which is costly and difficult to mass produce. Summary of the invention

[0004] The objects of the present invention are: (1) to solve the problem that excessive use of conventional antistatic agents leads to reduced mechanical properties and mechanical properties of polypropylene composite materials; and (2) to find a simple and efficient method for preparing graphene-based antistatic materials with good dispersion and excellent performance under the premise of low graphene usage.

[0005] In order to achieve the above object, the present invention provides a micro-crosslinked antistatic graphene-based polypropylene composite material, which is prepared from the following raw materials in parts by weight:

[0006] Polypropylene: 70-90 parts,

[0007] Inorganic filler: 0-20 parts,

[0008] Processing aids: 2-3 parts,

[0009] Initiator: 0.01~0.1 parts

[0010] Graphene-based antistatic masterbatch: 5-10 parts;

[0011] The graphene-based antistatic masterbatch is prepared from the following raw materials in parts by weight:

[0012] Elastomer: 85-95 parts,

[0013] Graphene microsheets: 5-20 parts,

[0014] Coupling agent: 1 to 5 parts,

[0015] Processing aids: 2-5 parts,

[0016] Initiator: 0.01~0.1 parts,

[0017] Cross-linking aid: 0.1 to 2 parts.

[0018] The polypropylene material is one or more of homopolymer polypropylene and copolymer polypropylene, and the specific requirement is that the melt flow rate is above 100g / 10min under the conditions of 230°C and 2.16Kg.

[0019] The inorganic filler is one of talcum powder, barium sulfate and calcium carbonate.

[0020] The elastomer is preferably one or more of ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-hexene copolymer, ethylene-octene copolymer, and ethylene-propylene-diene terpolymer. The specific requirements are that the melting temperature is within 70-120°C and the melt flow rate is above 30 / 10min.

[0021] The auxiliary agent is one of antioxidant 1010, antioxidant 168, antioxidant DSTP, light stabilizer V703, 5589, 531, lubricant white oil, and vinyl bis stearamide (EBS) or a mixture of several of them.

[0022] The graphene microsheet has a thickness of 1 to 5 nm and a sheet diameter of 10 to 25 μm.

[0023] The coupling agent is one of KH550, KH560, KH570, KH580, VTM0S and VTES.

[0024] The initiator is preferably one of benzoyl peroxide, 2,5-dimethyl-2,5-bis(tert-butyl peroxide)hexane, di-tert-butyl peroxide, isopropylbenzene hydroperoxide, tert-butyl hydroperoxide, tert-butyl perbenzoate, tert-butyl pervalerate, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, triallyl isocyanurate and 2,2,6,6-tetramethylpiperidinol oxide.

[0025] The crosslinking aid is preferably one of methyl methacrylate, ethylene glycol dimethacrylate, triethylhexyl dimethacrylate, allyl phthalate, triethylene glycol dimethacrylate, triallyl cyanurate and divinylbenzene.

[0026] The method for preparing a micro-crosslinked antistatic graphene-based polypropylene composite material of the present invention comprises the following preparation steps:

[0027] (1) Preparation of graphene-based antistatic masterbatch:

[0028] According to weight, 85-95 parts of elastomer, 5-20 parts of graphene microsheets, 1-5 parts of coupling agent, 2-5 parts of processing aid, 0.01-0.1 parts of initiator and 0.1-2 parts of cross-linking agent are added to the Haake torque rheometer in order for melt blending. After the banburying is completed, the product is collected for granulation to obtain the graphene-based antistatic masterbatch.

[0029] The rotation speed of the Haake torque rheometer is 60r / min, and the mixing time is 10 to 15min.

[0030] The processing temperature of the Haake torque rheometer should be set within the melting temperature of the elastomer and the decomposition temperature of the co-crosslinking agent, ranging from 90 to 130°C.

[0031] (2) Preparation of micro-crosslinked antistatic graphene-based polypropylene composite materials:

[0032] According to weight proportions, 5-10 parts of the graphene-based antistatic masterbatch prepared in step (1), 50-90 parts of polypropylene, 0-20 parts of inorganic filler, 0-20 parts of elastomer, 2-5 parts of auxiliary agent, and 0.01-0.1 parts of initiator are added together in a high-speed mixer and mixed evenly, and then added to a twin-screw extruder, and melted, extruded, cooled, and pelletized in the twin-screw extruder to prepare a slightly cross-linked antistatic graphene-based polypropylene composite material;

[0033] The processing temperatures of zones I to X of the twin-screw extruder are 155° C., 185° C., 195° C., 195° C., 200° C., 205° C., 210° C., 215° C., 215° C., 220° C. The main screw speed is 400 to 450 r / min, and the water tank temperature is 23° C. to 50° C.

[0034] The beneficial effects of the present invention are:

[0035] (1) Using elastomer as a filler carrier, a graphene-based antistatic masterbatch was prepared by melt blending, which solved the problem that graphene was difficult to disperse evenly in a polypropylene matrix and was very easy to agglomerate. The process was simple and easy to mass produce.

[0036] (2) Pre-crosslinked graphene-based antistatic masterbatch was prepared by using the crosslinking system in the carrier polymer. The difference in processing temperature and melt fluidity between the carrier polymer and polypropylene was used to allow the carrier polymer to fully penetrate into the polypropylene material. With the help of chemical crosslinking, the carrier polymer was distributed throughout the polypropylene matrix in the form of a network structure during the subsequent processing, forming a path for electron flow, so that the composite material has good antistatic properties.

[0037] (3) In the micro-cross-linking system, the amount of cross-linking agent added to the resin phase and the reinforcement phase is relatively low. The composite material still has a certain fluidity while meeting the antistatic requirements, which is easy to process.

[0038] (4) When the materials meet the same antistatic standard, the amount of graphene added in the present invention is significantly less than the amount of graphene added in the currently commonly used graphene-based composite materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 A model diagram of the preparation process of a micro-crosslinked antistatic graphene-based polypropylene composite material

[0040] Figure 2 This is a cross-sectional microstructure diagram of Example 6# of a micro-cross-linked antistatic graphene-based polypropylene composite material. DETAILED DESCRIPTION

[0041] Below in conjunction with specific embodiment, further elaborate content of the present invention.It should be emphasized that these embodiments are only used for further explanation of the present invention, and can not be interpreted as limiting the scope of protection of the present invention.In addition, it should be understood that after reading the content described in the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope limited by the appended claims of the application.

[0042] Example 1

[0043] (1) Preparation of graphene-based antistatic masterbatch:

[0044] According to weight, 90 parts of elastomer EVA, 5 parts of graphene microsheets, 4 parts of coupling agent VTES, 0.02 parts of initiator DCP and 2 parts of crosslinking aid TAC were added to the Haake torque rheometer in order for melt blending. After the banburying was completed, the product was collected for granulation to obtain the graphene-based antistatic masterbatch.

[0045] The rotation speed of the Haake torque rheometer is 60r / min, the mixing time is 10-15min, and the processing temperature is 90°C.

[0046] (2) Preparation of micro-crosslinked antistatic graphene-based polypropylene composite materials:

[0047] According to weight proportions, 10 parts of the graphene-based antistatic masterbatch prepared in step (1) are added together with 75 parts of polypropylene, 15 parts of talcum powder, 0.02 parts of initiator DCP, 0.2 parts of antioxidant 168, 0.1 parts of antioxidant 1010 and 1 part of white oil into a high-speed mixer and mixed evenly, and then added into a twin-screw extruder, and melted, extruded, cooled and pelletized by the twin-screw extruder to prepare a slightly cross-linked antistatic graphene-based polypropylene composite material;

[0048] The processing temperatures of zones I to X of the twin-screw extruder are 145° C., 180° C., 180° C., 185° C., 190° C., 190° C., 200° C., 200° C., 205° C., and 210° C. The main screw speed is 400 to 450 r / min, and the water tank temperature is 23° C. to 50° C.

[0049] Example 2

[0050] (1) Preparation of graphene-based antistatic masterbatch:

[0051] According to weight, 90 parts of elastomer POE, 5 parts of graphene microsheets, 3 parts of coupling agent VTMOS, 0.03 parts of initiator TAIC and 1.5 parts of crosslinking aid DAP were added to the Haake torque rheometer in order for melt blending. After the banburying was completed, the product was collected for granulation to obtain the graphene-based antistatic masterbatch.

[0052] The rotation speed of the Haake torque rheometer is 60r / min, the mixing time is 10-15min, and the processing temperature is 90°C.

[0053] (2) Preparation of micro-crosslinked antistatic graphene-based polypropylene composite materials:

[0054] By weight, 8 parts of the graphene-based antistatic masterbatch prepared in step (1) are added together with 70 parts of polypropylene, 15 parts of calcium carbonate, 7 parts of elastomer POE, 0.03 parts of initiator TAIC, 0.2 parts of antioxidant DSTP and 0.08 parts of zinc stearate, and mixed evenly in a high-speed mixer, and then added to a twin-screw extruder, and melted, extruded, cooled and pelletized in the twin-screw extruder to prepare a slightly cross-linked antistatic graphene-based polypropylene composite material;

[0055] The processing temperatures of zones I to X of the twin-screw extruder are 155° C., 185° C., 195° C., 195° C., 200° C., 205° C., 210° C., 215° C., 215° C., 220° C. The main screw speed is 400 to 450 r / min, and the water tank temperature is 23° C. to 50° C.

[0056] Example 3

[0057] (1) Preparation of graphene-based antistatic masterbatch:

[0058] According to weight, 87 parts of elastomer PBE, 8 parts of graphene microsheets, 4 parts of coupling agent KH560, 0.02 parts of initiator DTBP and 1.5 parts of crosslinking aid TEGDMA were added to the Haake torque rheometer in order for melt blending. After the banburying was completed, the product was collected for granulation to obtain the graphene-based antistatic masterbatch.

[0059] The rotation speed of the Haake torque rheometer is 60r / min, the mixing time is 10-15min, and the processing temperature is 125°C.

[0060] (2) Preparation of micro-crosslinked antistatic graphene-based polypropylene composite materials:

[0061] According to weight proportions, 5 parts of the graphene-based antistatic masterbatch prepared in step (1) are added together with 75 parts of polypropylene, 10 parts of barium sulfate, 10 parts of PBE, 0.02 parts of initiator DTBP, 0.2 parts of antioxidant 168, 0.1 parts of antioxidant 1010 and 1 part of calcium stearate into a high-speed mixer and mixed evenly, and then added into a twin-screw extruder, and melted, extruded, cooled and pelletized by the twin-screw extruder to prepare a slightly cross-linked antistatic graphene-based polypropylene composite material;

[0062] The processing temperatures of zones I to X of the twin-screw extruder are 155° C., 185° C., 195° C., 195° C., 200° C., 205° C., 210° C., 215° C., 215° C., 220° C. The main screw speed is 400 to 450 r / min, and the water tank temperature is 23° C. to 50° C.

[0063] Example 4

[0064] (1) Preparation of graphene-based antistatic masterbatch:

[0065] According to weight, 85 parts of elastomer EVA, 10 parts of graphene microsheets, 4 parts of coupling agent KH550, 0.02 parts of initiator BPO and 2 parts of crosslinking aid EGDMA were added to the Haake torque rheometer in order for melt blending. After the banburying was completed, the product was collected for granulation to obtain the graphene-based antistatic masterbatch.

[0066] The rotation speed of the Haake torque rheometer is 60r / min, the mixing time is 10-15min, and the processing temperature is 90°C.

[0067] (2) Preparation of micro-crosslinked antistatic graphene-based polypropylene composite materials:

[0068] According to weight proportions, 5 parts of the graphene-based antistatic masterbatch prepared in step (1) are added together with 80 parts of polypropylene, 10 parts of talcum powder, 5 parts of elastomer EVA, 0.02 parts of initiator BPO, 0.2 parts of antioxidant DSTP and 1 part of white oil into a high-speed mixer and mixed evenly, and then added into a twin-screw extruder, and melted, extruded, cooled and pelletized in the twin-screw extruder to prepare a slightly cross-linked antistatic graphene-based polypropylene composite material;

[0069] The processing temperatures of zones I to X of the twin-screw extruder are 145° C., 180° C., 180° C., 185° C., 190° C., 190° C., 200° C., 200° C., 205° C., and 210° C. The main screw speed is 400 to 450 r / min, and the water tank temperature is 23° C. to 50° C.

[0070] Example 5

[0071] (1) Preparation of graphene-based antistatic masterbatch:

[0072] According to weight, 87 parts of elastomer POE, 8 parts of graphene microsheets, 4 parts of coupling agent KH580, 0.03 parts of initiator TBPO and 1.5 parts of crosslinking aid DAP were added to the Haake torque rheometer in order for melt blending. After the banburying was completed, the product was collected for granulation to obtain the graphene-based antistatic masterbatch.

[0073] The rotation speed of the Haake torque rheometer is 60r / min, the mixing time is 10-15min, and the processing temperature is 90°C.

[0074] (2) Preparation of micro-crosslinked antistatic graphene-based polypropylene composite materials:

[0075] By weight, 8 parts of the graphene-based antistatic masterbatch prepared in step (1) are added together with 85 parts of polypropylene, 7 parts of elastomer POE, 0.01 parts of initiator TBPO, 0.2 parts of antioxidant 168, 0.1 parts of antioxidant 1010 and 0.08 parts of zinc stearate, and mixed evenly in a high-speed mixer, and then added to a twin-screw extruder, and melted, extruded, cooled and pelletized in the twin-screw extruder to prepare a slightly cross-linked antistatic graphene-based polypropylene composite material;

[0076] The processing temperatures of zones I to X of the twin-screw extruder are 145° C., 180° C., 180° C., 185° C., 190° C., 190° C., 200° C., 200° C., 205° C., and 210° C. The main screw speed is 400 to 450 r / min, and the water tank temperature is 23° C. to 50° C.

[0077] Example 6

[0078] (1) Preparation of graphene-based antistatic masterbatch:

[0079] According to weight, 90 parts of elastomer PBE, 5 parts of graphene microsheets, 3 parts of coupling agent VTMOS, 0.02 parts of initiator DCP and 2 parts of crosslinking aid DVB were added to the Haake torque rheometer in order for melt blending. After the banburying was completed, the product was collected for granulation to obtain the graphene-based antistatic masterbatch.

[0080] The rotation speed of the Haake torque rheometer is 60r / min, the mixing time is 10-15min, and the processing temperature is 125°C.

[0081] (2) Preparation of micro-crosslinked antistatic graphene-based polypropylene composite materials:

[0082] According to weight proportions, 10 parts of the graphene-based antistatic masterbatch prepared in step (1) are added together with 90 parts of polypropylene, 0.02 parts of initiator DCP, 0.2 parts of antioxidant DSTP and 1 part of calcium stearate, and mixed uniformly in a high-speed mixer, and then added to a twin-screw extruder, and melted, extruded, cooled and pelletized in the twin-screw extruder to prepare a slightly cross-linked antistatic graphene-based polypropylene composite material;

[0083] The processing temperatures of zones I to X of the twin-screw extruder are 155° C., 185° C., 195° C., 195° C., 200° C., 205° C., 210° C., 215° C., 215° C., 220° C. The main screw speed is 400 to 450 r / min, and the water tank temperature is 23° C. to 50° C.

[0084] Comparative Example 1

[0085] In order to better reflect the antistatic performance of a micro-crosslinked antistatic graphene-based polypropylene composite material of the present invention in contrast to Example 1, the corresponding comparative example 1 adopts a traditional method to prepare a graphene-based polypropylene composite material, wherein the addition amount of graphene microsheets is increased to 1 part, no initiator and crosslinking auxiliary agent are added, and the amount of other auxiliary agents is the same as that of Example 1, and mainly includes the following specific implementation steps:

[0086] According to weight proportions, 75 parts of polypropylene, 15 parts of talc, 9 parts of EVA elastomer, 0.5 parts of graphene microsheets, 0.4 parts of VTES coupling agent, 0.2 parts of antioxidant 168, 0.1 parts of antioxidant 1010 and 1 part of lubricant white oil were added in sequence, added into a high-speed mixer and mixed evenly, and then added into a twin-screw extruder, and melted, extruded, cooled and pelletized by the twin-screw extruder to prepare a modified polypropylene composite material.

[0087] Comparative Example 2

[0088] In order to form a comparison with Example 1 and better reflect the antistatic performance of a slightly cross-linked antistatic graphene-based polypropylene composite material of the present invention, the corresponding comparative example 2 adopts a masterbatch method to prepare a graphene-based polypropylene composite material, and directly adds the same weight parts of materials as in Example 1 except for an initiator and a cross-linking aid, and mainly includes the following specific implementation steps:

[0089] (1) Preparation of graphene-based antistatic masterbatch:

[0090] According to the weight percentage, 90 parts of elastomer EVA, 5 parts of graphene microsheets and 4 parts of coupling agent VTES were added to the Haake torque rheometer in order for melt blending. After the banburying was completed, the product was collected for granulation, and finally the graphene-based antistatic masterbatch was obtained.

[0091] (2) Preparation of micro-crosslinked antistatic graphene-based polypropylene composite materials:

[0092] According to weight proportions, 10 parts of the graphene-based antistatic masterbatch prepared in step (1) are added together with 75 parts of polypropylene, 15 parts of talcum powder, 0.2 parts of antioxidant 168, 0.1 parts of antioxidant 1010 and 1 part of white oil into a high-speed mixer and mixed evenly, and then added into a twin-screw extruder, and melted, extruded, cooled and pelletized in the twin-screw extruder to prepare a slightly cross-linked antistatic graphene-based polypropylene composite material;

[0093] Comparative Example 3

[0094] In order to form a comparison with Example 1, and to better reflect that a micro-crosslinked antistatic graphene-based polypropylene composite material of the present invention has both processability and antistatic performance, the corresponding comparative example 3 is based on Example 1, and more initiators and crosslinking aids are added, and mainly includes the following specific implementation steps:

[0095] (1) Preparation of graphene-based antistatic masterbatch:

[0096] According to weight, 90 parts of elastomer EVA, 5 parts of graphene microsheets, 4 parts of coupling agent VTES, 0.1 parts of initiator DCP and 2 parts of crosslinking aid TAC were added to the Haake torque rheometer in order for melt blending. After the banburying was completed, the product was collected for granulation to obtain the graphene-based antistatic masterbatch.

[0097] (2) Preparation of micro-crosslinked antistatic graphene-based polypropylene composite materials:

[0098] According to weight proportions, 10 parts of the graphene-based antistatic masterbatch prepared in step (1) are added together with 75 parts of polypropylene, 15 parts of talcum powder, 0.1 parts of initiator DCP, 0.2 parts of antioxidant 168, 0.1 parts of antioxidant 1010 and 1 part of white oil into a high-speed mixer and mixed evenly, and then added into a twin-screw extruder, and melted, extruded, cooled and pelletized by the twin-screw extruder to prepare a slightly cross-linked antistatic graphene-based polypropylene composite material;

[0099] The material particles of the above Examples 1 to 6 and Comparative Examples 1 to 3 were dried in an oven at 90°C for 8 hours, and then the relevant tests in Table 1 were performed, wherein only the particles were tested in Items 1 and 2, and the surface resistivity test was performed in Item 3. All particles were made into discs with a radius of 40 mm and a thickness of 2 mm according to a unified process. The test results are shown in Table 2.

[0100] Table 1 Test items and test methods

[0101]

[0102] Table 2 Test data of Examples 1 to 6 and Comparative Examples 1 to 3

[0103]

[0104] Examples 1 to 6 in Table 2 are test results of modified polypropylene composite materials prepared according to some representative embodiments of a micro-crosslinked antistatic graphene-based polypropylene composite material in the present invention. In order to better reflect the antistatic property and processability of the present invention, corresponding comparative examples 1 to 3 are used as controls for the examples. The following conclusions can be drawn from Table 2:

[0105] (1) The micro-crosslinked antistatic graphene-based polypropylene composite material of the present invention effectively reduces the amount of graphene microsheets and improves its antistatic efficiency through the masterbatch method and micro-crosslinking structure;

[0106] (2) Since the amount of initiator and cross-linking aid used in the present invention is relatively small, the graphene microsheets in the composite material are guaranteed to form a path for the flow of electrons, but a complete cross-linking structure cannot be formed. This method combines the antistatic properties and flow properties of the composite material, and is convenient for industrial production.

Claims

1. A micro-crosslinked antistatic graphene-based polypropylene composite material, characterized in that: It is prepared from the following raw materials in parts by weight: Polypropylene: 70-90 parts, Inorganic filler: 0-20 parts, Antioxidant 1680.2 parts, Antioxidant 1010 0.1 parts, 1 part white oil, Initiator: 0.01~0.1 parts, Graphene-based antistatic masterbatch: 5-10 parts; The graphene-based antistatic masterbatch is prepared from the following raw materials in parts by weight: Elastomer: 85-95 parts, Graphene microsheets: 5-20 parts, Coupling agent: 1 to 5 parts, Initiator: 0.01~0.1 parts, Cross-linking aid: 0.1-2 parts; The elastomer is one or more of ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-hexene copolymer, ethylene-octene copolymer, and ethylene-propylene-diene terpolymer. The specific requirements are that the melting temperature is within 70-120°C and the melt flow rate is above 30 / 10min.

2. A micro-crosslinked antistatic graphene-based polypropylene composite material, characterized in that: It is prepared from the following raw materials in parts by weight: Polypropylene: 70-90 parts, Inorganic filler: 0-20 parts, Antioxidant DSTP 0.2 parts Zinc stearate 0.08 parts Initiator: 0.01~0.1 parts Graphene-based antistatic masterbatch: 5-10 parts; The graphene-based antistatic masterbatch is prepared from the following raw materials in parts by weight: Elastomer: 85-95 parts, Graphene microsheets: 5-20 parts, Coupling agent: 1 to 5 parts, Initiator: 0.01~0.1 parts, Cross-linking aid: 0.1-2 parts; The elastomer is one or more of ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-hexene copolymer, ethylene-octene copolymer, and ethylene-propylene-diene terpolymer. The specific requirements are that the melting temperature is within 70-120°C and the melt flow rate is above 30 / 10min.

3. A micro-crosslinked antistatic graphene-based polypropylene composite material, characterized in that: It is prepared from the following raw materials in parts by weight: Polypropylene: 70-90 parts, Inorganic filler: 0-20 parts, Antioxidant 168 0.2 parts, Antioxidant 1010 0.1 parts, 1 part calcium stearate, Initiator: 0.01~0.1 parts Graphene-based antistatic masterbatch: 5-10 parts; The graphene-based antistatic masterbatch is prepared from the following raw materials in parts by weight: Elastomer: 85-95 parts, Graphene microsheets: 5-20 parts, Coupling agent: 1 to 5 parts, Initiator: 0.01~0.1 parts, Cross-linking aid: 0.1-2 parts; The elastomer is one or more of ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-hexene copolymer, ethylene-octene copolymer, and ethylene-propylene-diene terpolymer. The specific requirements are that the melting temperature is within 70-120°C and the melt flow rate is above 30 / 10min.

4. A micro-crosslinked antistatic graphene-based polypropylene composite material, characterized in that: It is prepared from the following raw materials in parts by weight: Polypropylene: 70-90 parts, Inorganic filler: 0-20 parts, Antioxidant DSTP 0.2 parts, 1 part white oil, Initiator: 0.01~0.1 parts, Graphene-based antistatic masterbatch: 5-10 parts; The graphene-based antistatic masterbatch is prepared from the following raw materials in parts by weight: Elastomer: 85-95 parts, Graphene microsheets: 5-20 parts, Coupling agent: 1 to 5 parts, Initiator: 0.01~0.1 parts, Cross-linking aid: 0.1-2 parts; The elastomer is one or more of ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-hexene copolymer, ethylene-octene copolymer, and ethylene-propylene-diene terpolymer. The specific requirements are that the melting temperature is within 70-120°C and the melt flow rate is above 30 / 10min.

5. A micro-crosslinked antistatic graphene-based polypropylene composite material, characterized in that: It is prepared from the following raw materials in parts by weight: Polypropylene: 70-90 parts, Inorganic filler: 0-20 parts, Antioxidant 168 0.2 parts, Antioxidant 1010 0.1 parts, 0.08 parts of zinc stearate, Initiator: 0.01~0.1 parts, Graphene-based antistatic masterbatch: 5-10 parts; The graphene-based antistatic masterbatch is prepared from the following raw materials in parts by weight: Elastomer: 85-95 parts, Graphene microsheets: 5-20 parts, Coupling agent: 1 to 5 parts, Initiator: 0.01~0.1 parts, Cross-linking aid: 0.1-2 parts; The elastomer is one or more of ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-hexene copolymer, ethylene-octene copolymer, and ethylene-propylene-diene terpolymer. The specific requirements are that the melting temperature is within 70-120°C and the melt flow rate is above 30 / 10min.

6. A micro-crosslinked antistatic graphene-based polypropylene composite material, characterized in that: It is prepared from the following raw materials in parts by weight: Polypropylene: 70-90 parts, Inorganic filler: 0-20 parts, Antioxidant DSTP 0.2 parts, 1 part calcium stearate, Initiator: 0.01~0.1 parts, Graphene-based antistatic masterbatch: 5-10 parts; The graphene-based antistatic masterbatch is prepared from the following raw materials in parts by weight: Elastomer: 85-95 parts, Graphene microsheets: 5-20 parts, Coupling agent: 1 to 5 parts, Initiator: 0.01~0.1 parts, Cross-linking aid: 0.1-2 parts; The elastomer is one or more of ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-hexene copolymer, ethylene-octene copolymer, and ethylene-propylene-diene terpolymer. The specific requirements are that the melting temperature is within 70-120°C and the melt flow rate is above 30 / 10min.

7. The slightly cross-linked antistatic graphene-based polypropylene composite material according to any one of claims 1 to 6, characterized in that: The polypropylene material is one or more of homopolymer polypropylene and copolymer polypropylene, and the specific requirement is that the melt flow rate is above 100g / 10min under the conditions of 230°C and 2.16Kg.

8. The slightly cross-linked antistatic graphene-based polypropylene composite material according to any one of claims 1 to 6, characterized in that: The inorganic filler is one of talcum powder, barium sulfate and calcium carbonate.

9. The slightly cross-linked antistatic graphene-based polypropylene composite material according to any one of claims 1 to 6, characterized in that: The graphene microsheet has a thickness of 1 to 5 nm and a sheet diameter of 10 to 25 μm.

10. The slightly cross-linked antistatic graphene-based polypropylene composite material according to any one of claims 1 to 6, characterized in that: The coupling agent is one of KH550, KH560, KH570, KH580, VTM0S and VTES.

11. The slightly cross-linked antistatic graphene-based polypropylene composite material according to any one of claims 1 to 6, characterized in that: The initiator is one of benzoyl peroxide, 2,5-dimethyl-2,5-bis(tert-butyl peroxide)hexane, di-tert-butyl peroxide, isopropylbenzene hydroperoxide, tert-butyl hydroperoxide, tert-butyl perbenzoate, tert-butyl pervalerate, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, triallyl isocyanurate and 2,2,6,6-tetramethylpiperidinol oxide.

12. The slightly cross-linked antistatic graphene-based polypropylene composite material according to any one of claims 1 to 6, characterized in that: The cross-linking auxiliary agent is one of methyl methacrylate, ethylene glycol dimethacrylate, triethylhexyl dimethacrylate, allyl phthalate, triethylene glycol dimethacrylate, triallyl cyanurate and divinyl benzene.