Polypropylene composite material as well as preparation method and application thereof

CN118931090APending Publication Date: 2024-11-12GUANGDONG JUSHI CHEM CO LTD

Patent Information

Application Number
CN202410886001.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing glass fiber reinforced polypropylene materials are prone to warping and floating fibers after cooling, which limits its alternative ABS materials application in the electronic and electrical industry and is costly.

Method used

Using high-flow resin substrate and non-crystalline polystyrene, combined with maleic anhydride graft compatibility agent and polar lubricant, the glass fibers are evenly dispersed, and internal stress and warping deformation are reduced, and material compatibility is improved. Mechanical properties.

Benefits of technology

A polypropylene composite material with low warpage and low floating fiber has excellent mechanical properties, reduces preparation costs, and can replace some ABS materials for electronic and electrical shells and automotive interior parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004926071980000051
    Figure BDA0004926071980000051
  • Figure BDA0004926071980000061
    Figure BDA0004926071980000061
  • Figure BDA0004926071980000062
    Figure BDA0004926071980000062
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer materials, and discloses a polypropylene composite material as well as a preparation method and application thereof. The polypropylene composite material is prepared from the following raw materials: polypropylene resin, polystyrene, glass fibers, a flexibilizer, a compatilizer, a lubricant and an antioxidant. The mass ratio of the polypropylene resin to the polystyrene is (5.5-75): 1; the melt index of the polypropylene resin under the test condition of 230 DEG C / 2.16 kg is greater than or equal to 25 g / 10 min; the cantilever beam notch impact strength of the polypropylene resin is greater than or equal to 500J / m; the melt index of the flexibilizer under the test condition of 190 DEG C / 2.16 kg is greater than or equal to 10 g / 10 min; the lubricant comprises an anti-floating fiber agent containing a polar group; the compatilizer comprises maleic anhydride grafted polypropylene and maleic anhydride grafted SEBS (Styrene-Ethylene-Butylene-Styrene); and the diameter of the glass fiber is 15-20 [mu] m.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to a polypropylene composite material and a preparation method and application thereof. Background Art

[0002] Polypropylene (PP) is one of the five general-purpose resins. It has excellent properties such as light weight, easy processing, and chemical resistance. It is widely used in chemical, electrical, packaging and other industrial fields. However, polypropylene itself still has many defects and needs to be modified to meet the needs of more application fields.

[0003] In the prior art, glass fiber reinforced polypropylene is an important modification method. Glass fiber reinforcement can make polypropylene have excellent mechanical strength and can replace some engineering plastics, such as acrylonitrile butadiene styrene (ABS) in the automotive industry, the electronic and electrical industry, and the construction industry. After adding glass fiber to polypropylene, the glass fiber has an aspect ratio and is cylindrical, so during the injection molding process, the flow direction and vertical distribution of the glass fiber in the product will be different. Polypropylene is a crystalline material. After cooling and shaping, the difference in glass fiber distribution will cause the product to warp and deform. In addition, the glass fiber itself has poor compatibility with the polypropylene substrate and is easy to float on the surface of the product, forming glass fiber exposure, that is, floating fiber phenomenon.

[0004] Therefore, although adding glass fiber to polypropylene can solve the shrinkage problem and defects in mechanical properties of polypropylene, making its shrinkage and rigidity comparable to ABS, the glass fiber reinforced polypropylene material without special treatment has serious warping and floating fiber problems, which greatly limits the use of glass fiber reinforced polypropylene material as a substitute for expensive ABS material in the electronic and electrical industry.

[0005] CN114835975A discloses a low-warpage glass fiber reinforced polypropylene composite material and its preparation method and application. The technical solution uses random copolymer polypropylene as a substrate, adds a nucleating agent and mica powder, and reduces the difference in the orientation of glass fibers in the polypropylene matrix along the flow direction and perpendicular to the flow direction, while also improving the crystallization speed of the glass fiber reinforced polypropylene composite material, thereby significantly improving the warpage deformation of the glass fiber reinforced polypropylene composite material. However, the market price of random copolymer polypropylene is relatively high, and mica powder is generally colored. The resulting glass fiber reinforced polypropylene material has a high preparation cost and is mainly black in color, making it difficult to use as a substitute for ABS. Summary of the invention

[0006] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, one of the purposes of the present invention is to provide a polypropylene composite material; the second purpose of the present invention is to provide a method for preparing the polypropylene composite material; the third purpose of the present invention is to provide a glass fiber reinforced polypropylene composite board; the fourth purpose of the present invention is to provide a polypropylene composite material, or an application of a glass fiber reinforced polypropylene composite board.

[0007] The basic principle of the present invention is described as follows:

[0008] The present invention selects a resin substrate with high fluidity and high impact resistance to make the glass fiber dispersed more evenly in the polypropylene, thereby reducing the difference in the horizontal and vertical directions, reducing the injection pressure and speed, and reducing the generation of internal stress; adding non-crystallized polystyrene and a high-fluidity toughening agent to the polypropylene can destroy the crystallization behavior of the polypropylene and reduce the warping deformation of the product after cooling; with a maleic anhydride grafted compatibilizer and a polar lubricant, the compatibility and dispersibility between the resin and the glass fiber and between the resins can be greatly improved, the mechanical properties of the material can be improved, and the phenomenon of glass fiber exposure can be reduced; through the synergistic effect of various functional components, the obtained polypropylene composite material has both excellent mechanical properties and the characteristics of low floating fiber and low warping.

[0009] In order to achieve the above object, the technical solution adopted by the present invention is:

[0010] The first aspect of the present invention provides a polypropylene composite material, comprising the following preparation raw materials: polypropylene resin, polystyrene, glass fiber, toughening agent, compatibilizer, lubricant, antioxidant;

[0011] The mass ratio of the polypropylene resin to the polystyrene is (5.5-75):1;

[0012] The melt index of the polypropylene resin under the test condition of 230°C / 2.16kg is ≥25g / 10min;

[0013] The notched Izod impact strength of the polypropylene resin is ≥500 J / m;

[0014] The melt index of the toughening agent under the test condition of 190°C / 2.16kg is ≥8g / 10min;

[0015] The lubricant includes an anti-floating agent containing a polar group;

[0016] The compatibilizer includes maleic anhydride grafted polypropylene and maleic anhydride grafted SEBS;

[0017] The diameter of the glass fiber is 15-20 μm.

[0018] Preferably, the mass ratio of the polypropylene resin to polystyrene is (5.5-13):1.

[0019] Preferably, the melt index of the polypropylene resin under the test condition of 230° C. / 2.16 kg is 25 g / 10 min to 35 g / 10 min.

[0020] Preferably, the notched Izod impact strength of the polypropylene resin is 500 to 800 J / m; the notched Izod impact strength of the polypropylene resin is tested according to standard ASTM D-256:2016, and the thickness of the specimen is 3.0 mm.

[0021] Preferably, the toughening agent has a melt index of 8 g / 10 min to 15 g / 10 min under the test condition of 190° C. / 2.16 kg.

[0022] Preferably, the diameter of the glass fiber is 15-18 μm.

[0023] Preferably, the polypropylene resin comprises block copolymer polypropylene.

[0024] Preferably, the polystyrene has a melt index of 4 g / 10 min to 8 g / 10 min under the test condition of 200° C. / 5 kg.

[0025] Preferably, the toughening agent includes an propylene-based elastomer; further preferably, the toughening agent includes one of propylene-based POE, butadiene-acrylonitrile rubber, ethylene-propylene rubber, butyl rubber, and polyurethane elastomer; further preferably, the toughening agent is propylene-based POE.

[0026] Preferably, the lubricant includes TAF, an anti-glass fiber exposure agent.

[0027] Specifically, the anti-glass fiber exposure agent TAF was purchased from Guangzhou Haocheng New Materials Co., Ltd. The anti-glass fiber exposure agent TAF is based on ethylene bis fatty acid amide (EBS). Under the action of a catalyst, a reactive monomer containing a polar group reacts with EBS to form a BAB type copolymer. It has a white powder appearance, a melting point of 130-141°C, an acid value of 10.0, and an effective content of 98%. The anti-glass fiber exposure agent TAF is a high-temperature resistant plastic processing lubricant. As a high-temperature resistant lubricating dispersant, TAF can effectively improve the appearance quality of glass fiber reinforced materials and improve the processing fluidity of composite materials in modified engineering plastics, and has no effect on the color and transparency of the resin.

[0028] Preferably, in the compatibilizer, the mass ratio of the maleic anhydride grafted polypropylene to the maleic anhydride grafted SEBS is 1:(1-5):1; further preferably, in the compatibilizer, the mass ratio of the maleic anhydride grafted polypropylene to the maleic anhydride grafted SEBS is (2-5):1.

[0029] Preferably, the linear density of the glass fiber is 1200-4800 tex; further preferably, the linear density of the glass fiber is 2400 tex.

[0030] Preferably, the glass fibers comprise continuous glass rovings.

[0031] Preferably, the antioxidant comprises a hindered phenol antioxidant; further preferably, the antioxidant comprises antioxidant B215.

[0032] Preferably, the particle length of the polypropylene composite material is 4 to 8 mm; further preferably, the particle length of the polypropylene composite material is 4 to 6 mm.

[0033] Preferably, the polypropylene composite material comprises the following raw materials in parts by mass: 55-75 parts of polypropylene resin, 1-10 parts of polystyrene, 10-25 parts of glass fiber, 5-10 parts of toughening agent, 3-8 parts of compatibilizer, 0.2-1.0 parts of lubricant, and 0.2-0.5 parts of antioxidant; further preferably, the polypropylene composite material comprises the following raw materials in parts by mass: 55-65 parts of polypropylene resin, 5-10 parts of polystyrene, 16-20 parts of glass fiber, 5-10 parts of toughening agent, 4-6 parts of compatibilizer, 0.4-0.8 parts of lubricant, and 0.2-0.4 parts of antioxidant.

[0034] The second aspect of the present invention provides a method for preparing the polypropylene composite material according to the first aspect of the present invention, comprising the following steps:

[0035] S1, mixing polypropylene resin, polystyrene, toughening agent, compatibilizer, lubricant and antioxidant to obtain a mixture;

[0036] S2. Calculating the number of glass fiber strands to be added according to the content of glass fiber in the raw material, mixing the mixed material with the glass fiber, extruding, and granulating to obtain the polypropylene composite material.

[0037] Specifically, in step S2, the calculation method of the number of added glass fiber strands is as follows:

[0038] If you plan to produce a polypropylene composite material with a glass fiber content of 20wt%, and the preset production capacity of the product is 600kg / h, then:

[0039] 1) Calculate the glass fiber content in the product produced per minute: 600kg / 60min*20wt%=2kg / min;

[0040] 2) Calculate the number of added strands of glass fiber: During production, fix the main engine speed, place 3 to 5 strands of glass fiber on a 100kg electronic scale, and time the amount of glass fiber extracted per minute. Calculate the average value multiple times. For example, if the amount of glass fiber extracted per minute is 0.2kg, then 10 strands of glass fiber are required to achieve a glass fiber output of 2kg / min.

[0041] 3) Verification of glass fiber content: After setting the main engine speed and the main feeding section’s hourly discharge, add the calculated number of glass fiber strands into the twin-screw extruder, start the machine and stabilize it, then re-measure the production capacity. If the output meets the calculated value, the glass fiber content is accurate.

[0042] Specifically, the preparation method of the polypropylene composite material comprises the following steps:

[0043] 1) Stir polypropylene resin, polystyrene, toughening agent, compatibilizer, lubricant and antioxidant in a high-speed stirring pot for 1 to 2 minutes to obtain a mixture, and let the mixture enter the intermediate hopper of the main feeding loss-in-weight scale through the discharge valve, and set the feeding amount so that the material enters the feeding section of the twin-screw extruder;

[0044] 2) By presetting the production capacity and according to the glass fiber content in the formula, the number of glass fiber strands to be added is calculated, and multiple strands of continuous glass fiber are added to the compression section of the twin-screw extruder through the fiber adding port;

[0045] 3) The mixed material and glass fiber in step 1) are melt-plasticized, extruded, cooled, dried and pelletized in a twin-screw extruder to obtain particles with a length of 4 to 8 mm, and qualified particles are screened by a vibrating screen, and are sent into a mixing barrel through a feeding fan for uniform mixing to obtain a polypropylene composite material, which can be discharged and packaged.

[0046] The preparation method of the polypropylene composite material provided by the present invention uses a stirring pot with a cooling system, and cooling water can be added to keep the stirring pot at room temperature, thereby reducing the stirring speed. During stirring, the antioxidant, polar additive and the like will not be agglomerated due to frictional heat generation, thereby affecting their function. A high-speed twin-screw extruder is used, which has high production capacity, and after the material is dried in a mixing barrel, floating fibers of the product can be reduced, and the material does not need to be dried before use, thereby facilitating operation.

[0047] The third aspect of the present invention provides a glass fiber reinforced polypropylene composite plate, comprising the polypropylene composite material described in the first aspect of the present invention.

[0048] The fourth aspect of the present invention provides the use of the polypropylene composite material described in the first aspect of the present invention, or the glass fiber reinforced polypropylene composite board described in the third aspect in the preparation of electronic and electrical housings or automobile interiors.

[0049] Compared with the prior art, the present invention has the following beneficial effects:

[0050] 1) The polypropylene composite material provided by the present invention can provide excellent mechanical properties, with a tensile strength of up to 49 MPa, a flexural strength of up to 70 MPa, a flexural modulus of up to 2650 MPa, and an Izod notched impact strength of up to 245 J / m, which are comparable to those of ABS materials.

[0051] 2) The preparation method of the polypropylene composite material provided by the present invention is simple, the process conditions are mild, and it is suitable for industrial use. The test method of the number of glass fiber added strands is simple and easy to operate, and workers can easily master it, and it can be repeated at any time, and the equipment cost is low.

[0052] 3) The glass fiber reinforced polypropylene composite plate provided by the present invention is made of a polypropylene composite material, has a glossy surface, has no warping, has few floating fibers on the surface, and has a good appearance.

[0053] 4) The polypropylene composite material and glass fiber reinforced polypropylene composite plate provided by the present invention can replace part of the ABS material and be used in the preparation of electronic and electrical housings or automotive interior decoration parts with low gloss requirements, thereby reducing the preparation cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 The following are photos of standard samples obtained by injection molding the materials in Example 2 (a) and Comparative Example 3 (b);

[0055] Figure 2 These are photos of standard samples obtained by injection molding the materials in Example 3 and Comparative Example 4. DETAILED DESCRIPTION

[0056] The present invention is further described in detail below by specific examples. Unless otherwise specified, the raw materials, reagents or devices used in the examples and comparative examples can be obtained from conventional commercial sources or can be obtained by prior art methods. Unless otherwise specified, the experiments or test methods are conventional methods in the art.

[0057] The specific information of the raw materials used in the examples and comparative examples is shown in Table 1 below:

[0058] Table 1 Specific information of raw materials used in the examples and comparative examples

[0059]

[0060]

[0061] The calculation method of the number of glass fiber added in the embodiments and comparative examples is as follows:

[0062] If you plan to produce a polypropylene composite material with a glass fiber content of 20wt%, and the preset production capacity of the product is 600kg / h, then:

[0063] 1) Calculate the glass fiber content in the product produced per minute: 600kg / 60min*20wt%=2kg / min;

[0064] 2) Calculate the number of added strands of glass fiber: During production, fix the main engine speed, place 3 to 5 strands of glass fiber on a 100kg electronic scale, and time the amount of glass fiber extracted per minute. Calculate the average value multiple times. For example, if the amount of glass fiber extracted per minute is 0.2kg, then 10 strands of glass fiber are required to achieve a glass fiber output of 2kg / min.

[0065] 3) Verification of glass fiber content: Set the main engine speed and the main feeding section hourly discharge, add the calculated number of glass fiber strands into the twin-screw extruder, start the machine and stabilize it, then re-measure the production capacity. If the output meets the calculated value, it means that the glass fiber content is accurate.

[0066] Unless otherwise specified, the "parts" of the amounts of raw materials used in the following examples and comparative examples refer to parts by mass.

[0067] Example 1

[0068] This embodiment provides a polypropylene composite material, and the raw materials and amounts thereof are shown in Table 2 below:

[0069] Table 2 Raw materials and contents of polypropylene composite materials in Example 1

[0070]

[0071]

[0072] The preparation method of the polypropylene composite material comprises the following steps:

[0073] 1) Weigh polypropylene resin, polystyrene, toughening agent, compatibilizer, lubricant and antioxidant according to proportion and add them into a high-speed stirring pot with a cooling system and stir for 1 min to obtain a mixture, feed the mixture into the intermediate hopper of the main feeding loss-in-weight scale through a discharge valve, set the feeding amount, and allow the material to enter the feeding section of the twin-screw extruder;

[0074] 2) The glass fiber content is 20wt%, the production capacity is set to 600kg / h, the main engine speed is set to 450rpm, and the number of glass fiber strands is calculated to be 10. The continuous glass fiber is fed into the compression section of the twin-screw extruder through the fiber feeding port. The machine is started and stabilized, and the production capacity is re-measured. If the output meets the calculated value, it means that the glass fiber content is accurate;

[0075] 3) In step 1), the mixed material and glass fiber are melted and plasticized in a twin-screw extruder, extruded, cooled in a water tank, dried by a water pump and a blow dryer, and then pelletized into particles of 4 to 6 mm in length. Qualified particles are screened out by a vibrating screen, and then mixed in a mixing barrel through a feeding fan, and then discharged and packaged.

[0076] Example 2

[0077] This embodiment provides a polypropylene composite material, and the raw materials and amounts thereof are shown in Table 3 below:

[0078] Table 3 Raw materials and contents of polypropylene composite materials prepared in Example 2

[0079]

[0080] The preparation method of the polypropylene composite material comprises the following steps:

[0081] 1) Weigh polypropylene resin, polystyrene, toughening agent, compatibilizer, lubricant and antioxidant according to proportion and add them into a high-speed stirring pot with a cooling system and stir for 1 min to obtain a mixture, feed the mixture into the intermediate hopper of the main feeding loss-in-weight scale through a discharge valve, set the feeding amount, and allow the material to enter the feeding section of the twin-screw extruder;

[0082] 2) The glass fiber content is 18wt%, the production capacity is set to 600kg / h, the main engine speed is set to 450rpm, and the number of glass fiber strands is calculated to be 9. The continuous glass fiber is fed into the compression section of the twin-screw extruder through the fiber feeding port. The machine is started and stabilized, and the production capacity is re-measured. If the output meets the calculated value, it means that the glass fiber content is accurate;

[0083] 3) In step 1), the mixed material and glass fiber are melted and plasticized in a twin-screw extruder, extruded, cooled in a water tank, dried by a water pump and a blow dryer, and then pelletized into particles of 4 to 6 mm in length. Qualified particles are screened out by a vibrating screen, and then mixed in a mixing barrel through a feeding fan, and then discharged and packaged.

[0084] Example 3

[0085] This embodiment provides a polypropylene composite material, and the raw materials and amounts thereof are shown in Table 4 below:

[0086] Table 4 Raw materials and contents of polypropylene composite materials prepared in Example 3

[0087]

[0088] The preparation method of the polypropylene composite material comprises the following steps:

[0089] 1) Weigh polypropylene resin, polystyrene, toughening agent, compatibilizer, lubricant and antioxidant according to proportion and add them into a high-speed stirring pot with a cooling system and stir for 1 min to obtain a mixture, feed the mixture into the intermediate hopper of the main feeding loss-in-weight scale through a discharge valve, set the feeding amount, and allow the material to enter the feeding section of the twin-screw extruder;

[0090] 2) The glass fiber content is 16wt%, the production capacity is set to 600kg / h, the main engine speed is set to 450rpm, and the number of glass fiber strands is calculated to be 8. The continuous glass fiber is fed into the compression section of the twin-screw extruder through the fiber feeding port. The machine is started and stabilized, and the production capacity is re-measured. If the output meets the calculated value, it means that the glass fiber content is accurate;

[0091] 3) In step 1), the mixed material and glass fiber are melted and plasticized in a twin-screw extruder, extruded, cooled in a water tank, dried by a water pump and a blow dryer, and then pelletized into particles of 4 to 6 mm in length. Qualified particles are screened out by a vibrating screen, and then mixed in a mixing barrel through a feeding fan, and then discharged and packaged.

[0092] Comparative Example 1

[0093] This comparative example provides a polypropylene composite material, which is different from Example 1 in that the high-impact block copolymer polypropylene K9930H is replaced with polypropylene resin EP300H-Z, and the raw materials and amounts used in the preparation are shown in Table 5 below:

[0094] Table 5 Raw materials and contents of polypropylene composite materials in comparative example 1

[0095]

[0096] The preparation method of the polypropylene composite material comprises the following steps:

[0097] 1) Weigh polypropylene resin, polystyrene, toughening agent, compatibilizer, lubricant and antioxidant according to proportion and add them into a high-speed stirring pot with a cooling system and stir for 1 min to obtain a mixture, feed the mixture into the intermediate hopper of the main feeding loss-in-weight scale through a discharge valve, set the feeding amount, and allow the material to enter the feeding section of the twin-screw extruder;

[0098] 2) The glass fiber content is 20wt%, the production capacity is set to 600kg / h, the main engine speed is set to 450rpm, and the number of glass fiber strands is calculated to be 10. The continuous glass fiber is fed into the compression section of the twin-screw extruder through the fiber feeding port. The machine is started and stabilized, and the production capacity is re-measured. If the output meets the calculated value, it means that the glass fiber content is accurate;

[0099] 3) In step 1), the mixed material and glass fiber are melted and plasticized in a twin-screw extruder, extruded, cooled in a water tank, dried by a water pump and a blow dryer, and then pelletized into particles of 4 to 6 mm in length. Qualified particles are screened out by a vibrating screen, and then mixed in a mixing barrel through a feeding fan, and then discharged and packaged.

[0100] Comparative Example 2

[0101] This comparative example provides a polypropylene composite material, which is different from Example 3 in that the high-impact block copolymer polypropylene K9930H is replaced with polypropylene resin PPH-Y26, and the raw materials and amounts used in the preparation are shown in Table 6 below:

[0102] Table 6 Raw materials and contents of polypropylene composite materials in comparative example 2

[0103]

[0104] The preparation method of the polypropylene composite material comprises the following steps:

[0105] 1) Weigh polypropylene resin, polystyrene, toughening agent, compatibilizer, lubricant and antioxidant according to proportion and add them into a high-speed stirring pot with a cooling system and stir for 1 min to obtain a mixture, feed the mixture into the intermediate hopper of the main feeding loss-in-weight scale through a discharge valve, set the feeding amount, and allow the material to enter the feeding section of the twin-screw extruder;

[0106] 2) The glass fiber content is 16wt%, the production capacity is set to 600kg / h, the main engine speed is set to 450rpm, and the number of glass fiber strands is calculated to be 8. The continuous glass fiber is fed into the compression section of the twin-screw extruder through the fiber feeding port. The machine is started and stabilized, and the production capacity is re-measured. If the output meets the calculated value, it means that the glass fiber content is accurate;

[0107] 3) In step 1), the mixed material and glass fiber are melted and plasticized in a twin-screw extruder, extruded, cooled in a water tank, dried by a water pump and a blow dryer, and then pelletized into particles of 4 to 6 mm in length. Qualified particles are screened out by a vibrating screen, and then mixed in a mixing barrel through a feeding fan, and then discharged and packaged.

[0108] Comparative Example 3

[0109] This comparative example provides a polypropylene composite material, which is different from Example 2 in that the polystyrene GPPS 525 is replaced by high-impact block copolymer polypropylene K9930H, that is, no polystyrene is added, and the raw materials and amounts used are shown in Table 7 below:

[0110] Table 7 Raw materials and contents of polypropylene composite materials in comparative example 3

[0111]

[0112]

[0113] The preparation method of the polypropylene composite material comprises the following steps:

[0114] 1) The polypropylene resin, toughening agent, compatibilizer, lubricant and antioxidant are weighed in proportion and added into a high-speed stirring pot with a cooling system and stirred for 1 min to obtain a mixture, and the mixture is fed into the intermediate hopper of the main feeding loss-in-weight scale through a discharge valve, and the feeding amount is set so that the material enters the feeding section of the twin-screw extruder;

[0115] 2) The glass fiber content is 18wt%, the production capacity is set to 600kg / h, the main engine speed is set to 450rpm, and the number of glass fiber strands is calculated to be 9. The continuous glass fiber is fed into the compression section of the twin-screw extruder through the fiber feeding port. The machine is started and stabilized, and the production capacity is re-measured. If the output meets the calculated value, it means that the glass fiber content is accurate;

[0116] 3) In step 1), the mixed material and glass fiber are melted and plasticized in a twin-screw extruder, extruded, cooled in a water tank, dried by a water pump and a blow dryer, and then pelletized into particles of 4 to 6 mm in length. Qualified particles are screened out by a vibrating screen, and then mixed in a mixing barrel through a feeding fan, and then discharged and packaged.

[0117] Comparative Example 4

[0118] This comparative example provides a polypropylene composite material, which is different from Example 3 in that the amount of high-impact block copolymer polypropylene is reduced and the amount of polystyrene is increased. The raw materials and amounts are shown in Table 8 below:

[0119] Table 8 Raw materials and contents of polypropylene composite materials in comparative example 4

[0120]

[0121]

[0122] The preparation method of the polypropylene composite material comprises the following steps:

[0123] 1) Weigh polypropylene resin, polystyrene, toughening agent, compatibilizer, lubricant and antioxidant according to proportion and add them into a high-speed stirring pot with a cooling system and stir for 1 min to obtain a mixture, feed the mixture into the intermediate hopper of the main feeding loss-in-weight scale through a discharge valve, set the feeding amount, and allow the material to enter the feeding section of the twin-screw extruder;

[0124] 2) The glass fiber content is 16wt%, the production capacity is set to 600kg / h, the main engine speed is set to 450rpm, and the number of glass fiber strands is calculated to be 8. The continuous glass fiber is fed into the compression section of the twin-screw extruder through the fiber feeding port. The machine is started and stabilized, and the production capacity is re-measured. If the output meets the calculated value, it means that the glass fiber content is accurate;

[0125] 3) In step 1), the mixed material and glass fiber are melted and plasticized in a twin-screw extruder, extruded, cooled in a water tank, dried by a water pump and a blow dryer, and then pelletized into particles of 4 to 6 mm in length. Qualified particles are screened out by a vibrating screen, and then mixed in a mixing barrel through a feeding fan, and then discharged and packaged.

[0126] Comparative Example 5

[0127] This comparative example provides a polypropylene composite material, which is different from Example 2 in that the toughening agent propylene-based elastomer 6202 is replaced by high-impact block copolymer polypropylene K9930H, that is, no toughening agent is added, and the raw materials and amounts used are shown in Table 9 below:

[0128] Table 9 Raw materials and contents of polypropylene composite materials in comparative example 5

[0129]

[0130] The preparation method of the polypropylene composite material comprises the following steps:

[0131] 1) Weigh polypropylene resin, polystyrene, compatibilizer, lubricant and antioxidant according to proportion and add them into a high-speed stirring pot with a cooling system and stir for 1 minute to obtain a mixture. Feed the mixture into the intermediate hopper of the main feeding loss-in-weight scale through the discharge valve, and set the feeding amount so that the material enters the feeding section of the twin-screw extruder;

[0132] 2) The glass fiber content is 18wt%, the production capacity is set to 600kg / h, the main engine speed is set to 450rpm, and the number of glass fiber strands is calculated to be 9. The continuous glass fiber is fed into the compression section of the twin-screw extruder through the fiber feeding port. The machine is started and stabilized, and the production capacity is re-measured. If the output meets the calculated value, it means that the glass fiber content is accurate;

[0133] 3) In step 1), the mixed material and glass fiber are melted and plasticized in a twin-screw extruder, extruded, cooled in a water tank, dried by a water pump and a blow dryer, and then pelletized into particles of 4 to 6 mm in length. Qualified particles are screened out by a vibrating screen, and then mixed in a mixing barrel through a feeding fan, and then discharged and packaged.

[0134] Comparative Example 6

[0135] This comparative example provides a polypropylene composite material, which is different from Example 2 in that the toughening agent propylene-based elastomer 6202 is replaced by toughening agent 8150, and the raw materials and amounts used in the preparation are shown in Table 10 below:

[0136] Table 10 Raw materials and contents of polypropylene composite materials in comparative example 6

[0137]

[0138] The preparation method of the polypropylene composite material comprises the following steps:

[0139] 1) Weigh polypropylene resin, polystyrene, toughening agent, compatibilizer, lubricant and antioxidant according to proportion and add them into a high-speed stirring pot with a cooling system and stir for 1 min to obtain a mixture, feed the mixture into the intermediate hopper of the main feeding loss-in-weight scale through a discharge valve, set the feeding amount, and allow the material to enter the feeding section of the twin-screw extruder;

[0140] 2) The glass fiber content is 18wt%, the production capacity is set to 600kg / h, the main engine speed is set to 450rpm, and the number of glass fiber strands is calculated to be 9. The continuous glass fiber is fed into the compression section of the twin-screw extruder through the fiber feeding port. The machine is started and stabilized, and the production capacity is re-measured. If the output meets the calculated value, it means that the glass fiber content is accurate;

[0141] 3) In step 1), the mixed material and glass fiber are melted and plasticized in a twin-screw extruder, extruded, cooled in a water tank, dried by a water pump and a blow dryer, and then pelletized into particles of 4 to 6 mm in length. Qualified particles are screened out by a vibrating screen, and then mixed in a mixing barrel through a feeding fan, and then discharged and packaged.

[0142] Comparative Example 7

[0143] This comparative example provides a polypropylene composite material, which is different from Example 1 in that the anti-glass fiber exposure agent TAF is replaced by a lubricant polyethylene wax. The raw materials and amounts used in the preparation are shown in Table 11 below:

[0144] Table 11 Raw materials and contents of polypropylene composite materials in comparative example 7

[0145]

[0146] The preparation method of the polypropylene composite material comprises the following steps:

[0147] 1) Weigh polypropylene resin, polystyrene, toughening agent, compatibilizer, lubricant and antioxidant according to proportion and add them into a high-speed stirring pot with a cooling system and stir for 1 min to obtain a mixture, feed the mixture into the intermediate hopper of the main feeding loss-in-weight scale through a discharge valve, set the feeding amount, and allow the material to enter the feeding section of the twin-screw extruder;

[0148] 2) The glass fiber content is 20wt%, the production capacity is set to 600kg / h, the main engine speed is set to 450rpm, and the number of glass fiber strands is calculated to be 10. The continuous glass fiber is fed into the compression section of the twin-screw extruder through the fiber feeding port. The machine is started and stabilized, and the production capacity is re-measured. If the output meets the calculated value, it means that the glass fiber content is accurate;

[0149] 3) In step 1), the mixed material and glass fiber are melted and plasticized in a twin-screw extruder, extruded, cooled in a water tank, dried by a water pump and a blow dryer, and then pelletized into particles of 4 to 6 mm in length. Qualified particles are screened out by a vibrating screen, and then mixed in a mixing barrel through a feeding fan, and then discharged and packaged.

[0150] Comparative Example 8

[0151] This comparative example provides a polypropylene composite material, which is different from Example 3 in that the compatibilizer is replaced by high-impact block copolymer polypropylene K9930H, that is, no compatibilizer is added, and the preparation raw materials and amounts are shown in Table 12 below:

[0152] Table 12 Raw materials and contents of polypropylene composite materials in comparative example 8

[0153]

[0154] The preparation method of the polypropylene composite material comprises the following steps:

[0155] 1) Weigh the polypropylene resin, polystyrene, toughening agent, lubricant and antioxidant according to the proportion and add them into a high-speed stirring pot with a cooling system and stir for 1 minute to obtain a mixture. Feed the mixture into the intermediate hopper of the main feeding loss-in-weight scale through the discharge valve, and set the feeding amount so that the material enters the feeding section of the twin-screw extruder;

[0156] 2) The glass fiber content is 16wt%, the production capacity is set to 600kg / h, the main engine speed is set to 450rpm, and the number of glass fiber strands is calculated to be 8. The continuous glass fiber is fed into the compression section of the twin-screw extruder through the fiber feeding port. The machine is started and stabilized, and the production capacity is re-measured. If the output meets the calculated value, it means that the glass fiber content is accurate;

[0157] 3) In step 1), the mixed material and glass fiber are melted and plasticized in a twin-screw extruder, extruded, cooled in a water tank, dried by a water pump and a blow dryer, and then pelletized into particles of 4 to 6 mm in length. Qualified particles are screened out by a vibrating screen, and then mixed in a mixing barrel through a feeding fan, and then discharged and packaged.

[0158] Comparative Example 9

[0159] This comparative example provides a polypropylene composite material, which is different from Example 3 in that the compatibilizer maleic anhydride grafted polypropylene KT-1 is replaced with maleic anhydride grafted SEBS KT-25, that is, only maleic anhydride grafted SEBS KT-25 is added as a compatibilizer. The raw materials and amounts used in the preparation are shown in Table 13 below:

[0160] Table 13 Raw materials and contents of polypropylene composite materials in comparative example 9

[0161]

[0162]

[0163] The preparation method of the polypropylene composite material comprises the following steps:

[0164] 1) Weigh polypropylene resin, polystyrene, toughening agent, compatibilizer, lubricant and antioxidant according to proportion and add them into a high-speed stirring pot with a cooling system and stir for 1 min to obtain a mixture, feed the mixture into the intermediate hopper of the main feeding loss-in-weight scale through a discharge valve, set the feeding amount, and allow the material to enter the feeding section of the twin-screw extruder;

[0165] 2) The glass fiber content is 16wt%, the production capacity is set to 600kg / h, the main engine speed is set to 450rpm, and the number of glass fiber strands is calculated to be 8. The continuous glass fiber is fed into the compression section of the twin-screw extruder through the fiber feeding port. The machine is started and stabilized, and the production capacity is re-measured. If the output meets the calculated value, it means that the glass fiber content is accurate;

[0166] 3) In step 1), the mixed material and glass fiber are melted and plasticized in a twin-screw extruder, extruded, cooled in a water tank, dried by a water pump and a blow dryer, and then pelletized into particles of 4 to 6 mm in length. Qualified particles are screened out by a vibrating screen, and then mixed in a mixing barrel through a feeding fan, and then discharged and packaged.

[0167] Comparative Example 10

[0168] This comparative example provides a polypropylene composite material, which is different from Example 3 in that the compatibilizer maleic anhydride grafted SEBS KT-25 is replaced by maleic anhydride grafted polypropylene KT-1, that is, only maleic anhydride grafted polypropylene KT-1 is added as a compatibilizer, and the raw materials and amounts used are shown in Table 14 below:

[0169] Table 14 Raw materials and contents of polypropylene composite materials in comparative example 10

[0170]

[0171]

[0172] The preparation method of the polypropylene composite material comprises the following steps:

[0173] 1) Weigh polypropylene resin, polystyrene, toughening agent, compatibilizer, lubricant and antioxidant according to proportion and add them into a high-speed stirring pot with a cooling system and stir for 1 min to obtain a mixture, feed the mixture into the intermediate hopper of the main feeding loss-in-weight scale through a discharge valve, set the feeding amount, and allow the material to enter the feeding section of the twin-screw extruder;

[0174] 2) The glass fiber content is 16wt%, the production capacity is set to 600kg / h, the main engine speed is set to 450rpm, and the number of glass fiber strands is calculated to be 8. The continuous glass fiber is fed into the compression section of the twin-screw extruder through the fiber feeding port. The machine is started and stabilized, and the production capacity is re-measured. If the output meets the calculated value, it means that the glass fiber content is accurate;

[0175] 3) In step 1), the mixed material and glass fiber are melted and plasticized in a twin-screw extruder, extruded, cooled in a water tank, dried by a water pump and a blow dryer, and then pelletized into particles of 4 to 6 mm in length. Qualified particles are screened out by a vibrating screen, and then mixed in a mixing barrel through a feeding fan, and then discharged and packaged.

[0176] Comparative Example 11

[0177] This comparative example provides a polypropylene composite material, which is different from Example 1 in that the glass fiber EDR240-17-T635 is replaced by EDR200-13.5-T635B. The raw materials and amounts used are shown in Table 15 below:

[0178] Table 15 Raw materials and contents of polypropylene composite materials in comparative example 11

[0179]

[0180] The preparation method of the polypropylene composite material comprises the following steps:

[0181] 1) Weigh polypropylene resin, polystyrene, toughening agent, compatibilizer, lubricant and antioxidant according to proportion and add them into a high-speed stirring pot with a cooling system and stir for 1 min to obtain a mixture, feed the mixture into the intermediate hopper of the main feeding loss-in-weight scale through a discharge valve, set the feeding amount, and allow the material to enter the feeding section of the twin-screw extruder;

[0182] 2) The glass fiber content is 20wt%, the production capacity is set to 600kg / h, the main engine speed is set to 450rpm, and the number of glass fiber strands is calculated to be 10. The continuous glass fiber is fed into the compression section of the twin-screw extruder through the fiber feeding port. The machine is started and stabilized, and the production capacity is re-measured. If the output meets the calculated value, it means that the glass fiber content is accurate;

[0183] 3) In step 1), the mixed material and glass fiber are melted and plasticized in a twin-screw extruder, extruded, cooled in a water tank, dried by a water pump and a blow dryer, and then pelletized into particles of 4 to 6 mm in length. Qualified particles are screened out by a vibrating screen, and then mixed in a mixing barrel through a feeding fan, and then discharged and packaged.

[0184] Comparative Example 12

[0185] This comparative example uses ABS resin 8391 as a comparison.

[0186] Performance Testing

[0187] 1) The materials of Examples 1-3 and Comparative Examples 1-12 were respectively injection molded using a horizontal injection molding machine to obtain standard specimens. The molding process conditions were: injection temperature (feeding port) 195 / 200 / 200 / 195°C (nozzle); injection pressure 55-75MPa; holding time 8s; cooling time 8s, and drying at 105°C for 2h before injection molding.

[0188] 2) The performance tests were performed on the standard samples obtained by injection molding the materials in Examples 1-3 and Comparative Examples 1-12. The performance test standards are as follows:

[0189] Melt index: tested according to ASTM D1238-04a standard, test conditions: 230℃ / 2.16Kg, unit: g / 10min;

[0190] Density: tested according to ASTM D792 standard, unit: g / cm 3 ;

[0191] Tensile strength: tested according to ASTM D638-2016 standard, unit: MPa;

[0192] Bending properties: including bending strength and bending modulus, in accordance with ASTM D790-2016 standard, unit: MPa;

[0193] Izod notched impact performance (impact strength): tested according to ASTM D256-2016 standard, specimen thickness 3.0mm, unit: J / m;

[0194] Flat plate warping height test: Fix one end of a long light plate (150mm*450mm*1.5mm) and measure the warping height at the end of the plate, unit: mm.

[0195] Assessment of floating fiber condition: Compare the floating fiber condition of the long light board (150mm*450mm*1.5mm) visually.

[0196] The performance test results of the standard samples obtained by injection molding of the materials in Examples 1-3 and Comparative Examples 1-12 are shown in Table 16:

[0197] Table 16 Performance test results of standard samples obtained by injection molding of materials in Examples 1-3 and Comparative Examples 1-12

[0198]

[0199] Table 16 shows the performance test results of the standard samples obtained by injection molding of the materials in Examples 1-3 and Comparative Examples 1-12. It can be seen from Table 16 that the standard samples made of the polypropylene composite materials in Examples 1-3 have a tensile strength of up to 49MPa, a flexural strength of up to 70MPa, a flexural modulus of up to 2650MPa, and an impact strength of more than 220J / m, and the flat plate warping height is less than 1mm, and there are few floating fibers on the surface. The polypropylene composite materials in Examples 1-3 can provide mechanical properties comparable to those of ABS materials, with excellent mechanical properties, and the warping deformation of the obtained specimens is not obvious, and there are fewer floating fibers, indicating that the polypropylene composite materials can be used to replace part of the ABS materials in the preparation of electronic and electrical housings or automotive interiors. In addition, compared with ABS materials, the price fluctuation of glass fiber reinforced polypropylene materials is small, and each ton can save 500 to 3000 yuan compared to ABS materials, which can greatly reduce the preparation cost of electronic and electrical housings or automotive interiors.

[0200] Compared with Example 1, Comparative Example 1 uses the substrate EP300H-Z with a lower melt index, which results in lower fluidity of the glass fiber reinforced polypropylene material. The glass fiber cannot be well dispersed during the injection molding process, resulting in severe warping and more floating fibers after the part is cooled.

[0201] Compared with Example 3, in Comparative Example 2, since the high-impact block copolymer polypropylene K9930H is replaced by the polypropylene resin PPH-Y26 with a higher melt index but lower impact strength, the cantilever beam notched impact strength of the obtained glass fiber reinforced polypropylene material is only 100 J / m, which is inferior to the relevant performance of ABS material and cannot replace ABS material well.

[0202] Comparative Example 3 Compared with Example 2, since no polystyrene is added, the proportion of polypropylene substrate K9930H increases. Figure 1 The standard sample photos obtained by injection molding of the materials in Example 2 (a) and Comparative Example 3 (b) are shown in FIG. Figure 1 (a) It can be seen that the corresponding product of Example 2 has no warping. Figure 1 (b) It can be seen that compared with Example 2, the corresponding product of Comparative Example 3 has serious shrinkage deformation and obvious warping due to the crystallization behavior of polypropylene.

[0203] In Comparative Example 4, compared with Example 3, the amount of high-impact block copolymer polypropylene is reduced and the amount of polystyrene is increased. Since polystyrene and polypropylene have poor compatibility, adding too much polystyrene will seriously damage the mechanical properties of glass fiber reinforced polypropylene. Figure 2 The standard sample photos obtained by injection molding of the materials in Example 3 and Comparative Example 4 are shown from left to right, respectively, the corresponding parts of Example 3 and the corresponding parts of Comparative Example 4. Figure 2 It can be seen that the corresponding product of Example 3 has a bright surface, less floating fibers and a good appearance. Compared with Example 3, the corresponding product of Comparative Example 4 has a serious white surface and a poor appearance, and cannot replace the ABS material well.

[0204] Compared with Example 2, Comparative Example 5 does not add the toughening agent propylene-based elastomer 6202, the system lacks reinforcement effect, the impact strength does not reach the level of ABS material, the inhibition of polypropylene crystallization behavior is weakened, and the dispersion of glass fiber is reduced, so it leads to obvious warping of the product and is not suitable for replacing ABS material.

[0205] Compared with Example 2, in Comparative Example 6, the toughening agent propylene-based elastomer 6202 is replaced by toughening agent 8150. The melt index of the toughening agent is reduced, which affects the overall fluidity and fails to improve the dispersion of the glass fiber. As a result, the product warps significantly and is not suitable for replacing ABS materials.

[0206] Comparative Example 7 compares Example 1 with common lubricant polyethylene wax instead of TAF containing polar group anti-glass fiber exposure agent. The lubricant has no polar functional group, has weak dispersion effect on glass fiber, and has serious fiber floating problem, so it is not suitable to replace ABS material.

[0207] Compared with Example 3, Comparative Example 8 does not add a compatibilizer, lacks a bridge between polypropylene / polystyrene and glass fiber, has poor compatibility, reduces overall strength, and has relatively serious floating fibers and warping, making it unsuitable for replacing ABS materials.

[0208] Compared with Example 3, Comparative Example 9 only adds maleic anhydride grafted SEBS as a compatibilizer, which has limited effect on improving compatibility and has low overall performance, making it unsuitable for replacing ABS materials.

[0209] Compared with Example 3, Comparative Example 10 only adds maleic anhydride grafted polypropylene as a compatibilizer, which has limited effect on improving compatibility. The compatibility between polystyrene and glass fiber / polypropylene is poor. Polystyrene cannot enhance the rigidity of the material. The overall performance of the material is poor and is not suitable for replacing ABS material.

[0210] Compared with Example 1, Comparative Example 11 changes the glass fiber model. The glass fiber monofilament has a thinner wire diameter and is not easily damaged or sheared in the twin-screw. The glass fiber length is uneven. There is a significant difference in the flow direction and vertical direction of the injection molded parts. The warping is relatively obvious, and it is not suitable for replacing ABS material.

[0211] The parts prepared by the polypropylene composite material provided by the present invention have a tensile strength of ≥46MPa, a flexural strength of ≥65MPa, a flexural modulus of ≥2370MPa, and an Izod notched impact strength of ≥225J / m, which can provide excellent mechanical properties, which are comparable to ABS materials; and the surface of the polypropylene composite material parts is glossy, without warping, with less floating fibers on the surface, and good appearance, indicating that the polypropylene composite material can replace part of the ABS material for the preparation of electronic and electrical housings or automotive interior parts with low gloss requirements, thereby reducing costs. The preparation method of the polypropylene composite material provided by the present invention uses a stirring pot with a self-cooling system, and cooling water can be added to keep the stirring pot at room temperature, reduce the stirring speed, and will not cause agglomeration of antioxidants, polar additives, etc. due to frictional heat during stirring, which affects their function; a high-speed twin-screw extruder is used, which has high production capacity, and after the material is dried in the mixing barrel, the floating fibers of the product can be reduced, and the material does not need to be dried before use, which is convenient to operate. In the preparation process of the polypropylene composite material, the glass fiber content can be tested by a simple method, which is simple to operate, easy for workers to master, can be retested at any time, and has low equipment cost.

Claims

1. A polypropylene composite material, characterized in that: The preparation comprises the following raw materials: polypropylene resin, polystyrene, glass fiber, toughening agent, compatibilizer, lubricant, antioxidant; The mass ratio of the polypropylene resin to the polystyrene is (5.5-75):1; The melt index of the polypropylene resin under the test condition of 230°C / 2.16kg is ≥25g / 10min; The notched Izod impact strength of the polypropylene resin is ≥500 J / m; The melt index of the toughening agent under the test condition of 190°C / 2.16kg is ≥8g / 10min; The lubricant includes an anti-floating agent containing a polar group; The compatibilizer includes maleic anhydride grafted polypropylene and maleic anhydride grafted SEBS; The diameter of the glass fiber is 15-20 μm.

2. The polypropylene composite material according to claim 1, characterized in that: The polypropylene resin includes block copolymer polypropylene.

3. The polypropylene composite material according to claim 1, characterized in that: The polystyrene has a melting index of ≥4 g / 10 min under the test condition of 200° C. / 5 kg.

4. The polypropylene composite material according to claim 1, characterized in that: The toughening agent includes a propylene-based elastomer; And / or, the lubricant includes a glass fiber exposure prevention agent TAF.

5. The polypropylene composite material according to claim 1, characterized in that: In the compatibilizer, the mass ratio of the maleic anhydride grafted polypropylene to the maleic anhydride grafted SEBS is (1-5):

1.

6. The polypropylene composite material according to claim 1, characterized in that: The linear density of the glass fiber is 1200-4800tex; And / or, the glass fibers include continuous glass rovings.

7. The polypropylene composite material according to claim 1, characterized in that: The polypropylene composite material comprises the following raw materials in parts by weight: 55-75 parts of polypropylene resin, 1-10 parts of polystyrene, 10-25 parts of glass fiber, 5-10 parts of toughening agent, 3-8 parts of compatibilizer, 0.2-1.0 parts of lubricant and 0.2-0.5 parts of antioxidant.

8. The method for preparing the polypropylene composite material according to claim 7, characterized in that: The following steps are involved: S1, mixing polypropylene resin, polystyrene, toughening agent, compatibilizer, lubricant and antioxidant to obtain a mixture; S2. Calculating the number of glass fiber strands to be added according to the content of glass fiber in the raw material, mixing the mixed material with the glass fiber, extruding, and granulating to obtain the polypropylene composite material.

9. A glass fiber reinforced polypropylene composite board, characterized in that: The polypropylene composite material comprises the polypropylene composite material according to any one of claims 1 to 7.

10. Use of the polypropylene composite material according to any one of claims 1 to 7, or the glass fiber reinforced polypropylene composite board according to claim 9, in the preparation of electronic and electrical appliance housings or automobile interiors.

Citation Information

Patent Citations

  • Low-warpage glass fiber reinforced polypropylene composite material as well as preparation method and application thereof

    CN114835975A

Cited By

  • High-toughness anti-cracking polypropylene composite material as well as preparation method and application thereof

    CN121378962A

  • High toughness anti-cracking polypropylene composite material, its preparation method and application

    CN121378962B