Antistatic polypropylene sheet and fabric thereof, high-strength high-impact-resistance antistatic polypropylene composite material and preparation method and application of high-strength high-impact-resistance antistatic polypropylene composite material
Through multi-layer structure of antistatic polypropylene sheets and fabrics, using melting point differences and conductive fillers, the deficiencies in mechanical properties and interlayer peeling strength of polypropylene composites are solved, and the hot pressing temperature is reduced, achieving high efficiency and Safe polypropylene composite preparation.
Patent Information
- Application Number
- CN202310485595.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-29
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-29
AI Technical Summary
It is difficult for existing polypropylene composite materials to have a wide processing temperature, strong mechanical properties and high interlayer peeling strength at the same time, and it is easy to accumulate static electricity, leading to safety hazards during production and processing.
It adopts multi-layer structure of antistatic polypropylene sheets and fabrics, prepared by co-extrusion molding and hot pressing methods, including homopolymer polypropylene, impact copolymer polypropylene, random copolymer polypropylene and conductive fillers, layer A and layer The melting point difference of B and the conductive filler content are optimized to form a high-strength, high-impact antistatic polypropylene composite material.
It achieves high-layer peeling strength and good mechanical properties at a lower hot pressing temperature, while reducing equipment energy consumption and production costs, and improving the safety and application breadth of composite materials.
Smart Images

Figure BDA0004209800350000211
Abstract
Description
Technical Field
[0001] The invention relates to the field of polypropylene materials, and more particularly to an antistatic polypropylene sheet, an antistatic polypropylene fabric, a high-strength and high-impact antistatic polypropylene composite material, and a preparation method and application thereof. Background Art
[0002] Polypropylene (PP) resin has low density, good heat resistance, and good stiffness, hardness and weldability, which makes it widely used.
[0003] The matrix and reinforcing phase of self-reinforced polymer composites are composed of different forms of the same polymer, and the reinforcing phase is usually a highly oriented fiber or flat ribbon. Most self-reinforced polymer composites are prepared using a hot pressing method. When the reinforcing phase is hot pressed at a certain pressure and temperature, the surface of the reinforcing phase fiber melts to become a matrix melt. The matrix melt and the reinforcing phase surface co-crystallize when melted, thereby providing sufficient interfacial bonding strength. As in US6312638B1, melt-spun oriented polyolefin fibers are hot pressed, and a specific temperature and pressure are used to partially melt-bond the surface layer of the polyolefin to prepare a polyolefin sheet. This preparation method is not only sensitive to the temperature of hot pressing, but also has a high hot pressing temperature. In addition, the oriented fibers produce a large decomposition orientation after hot pressing, and the mechanical strength decreases significantly.
[0004] In order to widen the hot pressing window and reduce the hot pressing pressure, polyolefins with different melting points can be hot pressed. For example, US8133537B2 hot presses three layers of polyolefin fibers with different melting points to obtain a polyolefin composite material, wherein the melting temperatures of the first and second layers of polyolefins are lower than the core layer. However, the hot pressing composite material prepared by this method has low impact strength and interlayer peeling strength.
[0005] Polypropylene molecules are completely non-polar and have high electrical insulation properties. Their surface resistivity is 10 16 -10 17 Ω, volume resistivity is 10 16 -10 18 Ω·m, it is easy to accumulate static charge, which will cause polypropylene to carry static electricity due to friction and other reasons during production or processing, which is difficult to eliminate through conduction, causing problems and safety hazards in the production, processing, storage, transportation and application of polypropylene. Summary of the invention
[0006] The purpose of the present invention is to overcome the technical defect that the existing polypropylene composite material is difficult to have a wide processing temperature, strong mechanical properties and high interlayer peeling strength at the same time, and provide an antistatic polypropylene sheet, an antistatic polypropylene fabric, a high-strength and high-impact antistatic polypropylene composite material and a preparation method and application thereof. The antistatic polypropylene sheet of the present invention is subjected to hot pressing and the like to obtain the antistatic polypropylene composite material. The antistatic polypropylene composite material has excellent mechanical properties and good interlayer peeling strength. Even at a lower hot pressing temperature and a wider hot pressing temperature range, the interlayer peeling strength of the obtained polypropylene composite material is still high.
[0007] The first aspect of the present invention is to provide an antistatic polypropylene sheet, comprising a layer A and layers B and B' located on both sides of the layer A, with a structure of BAB';
[0008] Wherein layer A contains a polypropylene composition A and a conductive filler, layer B and layer B' are the same or different, each containing a conductive filler and each correspondingly containing a polypropylene composition B and a polypropylene composition B', and the melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B';
[0009] The polypropylene composition A comprises homopolypropylene a and impact copolymer polypropylene b; the polypropylene composition B and the polypropylene composition B' each comprise random copolymer polypropylene x and thermal bonding enhancer y.
[0010] According to the present invention, the content of each component in the polypropylene composition A can be selected within a wide range. In a preferred embodiment of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-99wt% of homopolypropylene a and 1-50wt% of impact copolymer polypropylene b; preferably, the polypropylene composition A comprises 70-90wt% of homopolypropylene a and 10-30wt% of impact copolymer polypropylene b.
[0011] According to the present invention, the content of the conductive filler in layer A can be selected within a wide range. In a preferred embodiment of the present invention, the content of the conductive filler in layer A is 0.1-10 parts by weight, preferably 1-3 parts by weight, relative to 100 parts by weight of the polypropylene composition A.
[0012] According to the present invention, the content of each component in the polypropylene composition B and the polypropylene composition B' can be selected within a wide range. In a preferred embodiment of the present invention, based on the total weight of the polypropylene composition B and the polypropylene composition B', the polypropylene composition B and the polypropylene composition B' each include 70-99wt% of random copolymer polypropylene x and 1-30wt% of thermal adhesion enhancer y; preferably, the polypropylene composition B and the polypropylene composition B' each include 80-90wt% of random copolymer polypropylene x and 10-20wt% of thermal adhesion enhancer y.
[0013] According to the present invention, the content of the conductive filler in layer B and layer B' can be selected within a wide range. In a preferred embodiment of the present invention, the content of the conductive filler in layer B and layer B' is 0.1-10 parts by weight, preferably 1-3 parts by weight, relative to 100 parts by weight of the polypropylene composition B and the polypropylene composition B' respectively.
[0014] According to the present invention, the ratio of the thickness of layer A to the total thickness can be selected within a wide range. In a preferred embodiment of the present invention, based on the total thickness of the polypropylene sheet, the thickness of layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%. The thicknesses of film layers B and B' on both sides of film layer A can be the same or different, preferably the same.
[0015] The present invention does not limit the thickness of the antistatic polypropylene sheet, and can be selected in a wide range according to its practical application field. Preferably, the thickness of the antistatic polypropylene sheet can be 10-1000 μm, preferably 30-500 μm, and more preferably 50-300 μm.
[0016] According to the present invention, the thickness of the film layers A, B, B' can be controlled by the melt pump of the extruder during the processing.
[0017] The homopolypropylene a has a wide range of material selection. In a preferred embodiment of the present invention, the homopolypropylene a has:
[0018] The melting point is 150-170°C, preferably 160-170°C; and / or,
[0019] The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or,
[0020] In a preferred embodiment of the present invention, the isotacticity (mm) of the homopolypropylene a is not less than 96%.
[0021] In a more preferred embodiment of the present invention, the melting point of the homopolypropylene a is 160-170°C, and the melt flow rate at 230°C and 2.16kg load is 0.5-50g / 10min, preferably 1-20g / 10min, and more preferably 2.5-18g / 10min; the isotacticity (mm) of the homopolypropylene is not less than 96%.
[0022] The material selection range of the high impact copolymer polypropylene b is relatively wide. In a preferred embodiment of the present invention, the high impact copolymer polypropylene b has:
[0023] The melting point of the impact-resistant copolymer polypropylene b is 150-170° C.: and / or,
[0024] The monomer of the impact copolymer polypropylene b and propylene copolymer is ethylene or butene, preferably butene; and / or,
[0025] The impact copolymer polypropylene b has a melt flow rate of 0.5-50 g / 10 min at 230° C. and a load of 2.16 kg, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or,
[0026] The cantilever beam impact strength of the impact-resistant copolymer polypropylene b is not less than 20KJ / m 2 (Test conditions: 23℃).
[0027] In a more preferred embodiment of the present invention, the melting point of the high impact copolymer polypropylene b is 150-170°C, and the monomer copolymerized with propylene is ethylene or butene, preferably butene; the melt flow rate of the high impact copolymer polypropylene b at 230°C and a load of 2.16 kg is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and further preferably 2.5-18 g / 10 min.
[0028] According to the research of the inventors, when the melt mass flow rate and polymer composition ratio of the antistatic polypropylene composition A are within the above preferred ranges, the high impact copolymer polypropylene b in the composition can absorb impact energy well, meet the requirements of impact performance, and make the sheet have good impact performance. At the same time, since the macromolecular segments in the homopolymer polypropylene a are relatively regular, crystallization occurs during the sheet preparation process, so the sheet also has good tensile properties.
[0029] The random copolymer polypropylene x has a wide range of material selection. In a preferred embodiment of the present invention, the random copolymer polypropylene x has:
[0030] The melting point is 110-150°C, preferably 120-140°C; and / or,
[0031] The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 3-18 g / 10 min; and / or,
[0032] The molecular weight distribution Mw / Mn is 5-12, preferably 7-10; and / or,
[0033] It is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene binary copolymer.
[0034] The thermal adhesion enhancer y has a wide range of material selection. In a preferred embodiment of the present invention, the thermal adhesion enhancer y has:
[0035] The melting point or viscosity flow temperature is 70-110°C; and / or,
[0036] The melt flow rate at 190°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 1-18 g / 10 min; and / or,
[0037] One or more selected from polyolefin elastomer, EPDM rubber, SEBS, SBS, EVA, petroleum resin; preferably, polyolefin elastomer and / or petroleum resin; preferably,
[0038] The polyolefin elastomer is a copolymer elastomer of ethylene and propylene and / or alpha olefin, wherein the alpha olefin is preferably a C4-C12 alpha olefin, more preferably 1-butene and / or 1-octene; and / or,
[0039] The petroleum resin is a C5 and / or C9 hydrogenated petroleum resin with a softening point of 100-150° C. and is preferably a cyclopentadiene type resin.
[0040] In another more preferred embodiment of the present invention, the thermal adhesion enhancer y is a petroleum resin, and the petroleum resin is a hydrogenated petroleum resin of C5 and / or C9, preferably with a softening point of 100-150°C; more preferably, the petroleum resin is a cyclopentadiene type resin.
[0041] According to the research conducted by the inventors, when the antistatic polypropylene composition B i When the melt mass flow rate and the polymer composition ratio are within the preferred range, the low melting point random copolymer polypropylene x and the thermal bonding enhancer y in the composition can significantly reduce the hot pressing temperature and broaden the hot pressing temperature window, and the thermal bonding enhancer y provides good bonding properties for the sheet, which can further improve the interlayer peeling strength.
[0042] In a preferred embodiment of the present invention, the layer A further contains a β-crystal nucleating agent; preferably,
[0043] The β-crystal nucleating agent is selected from at least one of condensed ring aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates.
[0044] The amount of the β-crystal nucleating agent can be selected in a wide range. In a preferred embodiment of the present invention, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight relative to 100 parts by weight of the polypropylene composition A. For example, the content of the β-crystal nucleating agent can be 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, or 0.5 parts by weight.
[0045] According to the present invention, the conductive filler can be selected from a wide range. In a preferred embodiment of the present invention, the conductive filler is selected from at least one of carbon black conductive fillers, graphite conductive fillers, carbon nanotube conductive fillers, carbon fiber conductive fillers, conductive metal particles, conductive metal fibers, fillers coated with conductive metals, and metal oxides; preferably,
[0046] The carbon black conductive filler is at least one of acetylene black, superconducting carbon black and special conductive carbon black; and / or, the graphite conductive filler is at least one of natural graphite, expandable graphite, expanded graphite and graphene; and / or, the carbon nanotube conductive filler is at least one of the following carbon nanotubes that are not surface-modified or surface-modified: single-walled carbon nanotubes and / or multi-walled carbon nanotubes; and / or, the conductive metals in the conductive metal particles and conductive metal fibers are each independently at least one of silver, aluminum, copper, iron, nickel and stainless steel; and / or, the filler coated with conductive metal is selected from at least one of the following materials plated with lead, nickel and silver: glass balls, glass fibers and mica sheets; and / or, the metal oxide is at least one of titanium oxide, zinc oxide, tin oxide, indium oxide and cadmium oxide.
[0047] In a preferred embodiment of the present invention, the melting point of the homopolymerized polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymerized polypropylene x in the polypropylene composition B and the polypropylene composition B', and the temperature difference of the corresponding melting points is preferably greater than or equal to 10 degrees. In this preferred embodiment, the inventors of the present invention surprisingly found that the obtained polypropylene sheet is subjected to hot pressing to obtain a polypropylene composite material, and the polypropylene composite material has more excellent mechanical properties and better interlayer peel strength. Even at a lower hot pressing temperature and a wider hot pressing temperature range, the obtained polypropylene composite material has a higher interlayer peel strength.
[0048] More preferably, the difference between the melting points of polypropylene composition A and polypropylene composition B and the difference between the melting points of polypropylene composition A and polypropylene composition B' are each equal to or greater than 5°C, preferably equal to or greater than 10°C, more preferably equal to or greater than 20°C.
[0049] According to the research conducted by the inventors, when the antistatic polypropylene composition A i When the melt mass flow rate, polymer composition ratio and thickness distribution of the antistatic polypropylene combination B and B' are within the preferred range, the sheet preparation process can be smoother, thereby making the sheet have better uniformity, tensile strength, impact performance and interlayer peeling strength.
[0050] In a preferred embodiment of the present invention, the BAB' layer structure of the polypropylene sheet is obtained by co-extruding a layer A raw material comprising a polypropylene composition A and a conductive filler, a layer B raw material comprising a polypropylene composition B and a conductive filler, and a layer B' raw material comprising a polypropylene composition B' and a conductive filler.
[0051] The second aspect of the present invention is to provide a method for preparing the antistatic polypropylene sheet described in the first aspect, comprising co-extruding, casting or calendering, and stretching a layer A raw material containing a polypropylene composition A and a conductive filler, a layer B raw material containing a polypropylene composition B and a conductive filler, and a layer B' raw material containing a polypropylene composition B' and a conductive filler according to a BAB' structure to obtain the antistatic polypropylene sheet.
[0052] In a preferred embodiment of the present invention, the preparation of the raw material of layer A comprises melt blending the components including the homopolypropylene a, the impact copolymer polypropylene b and the conductive filler. The conditions and equipment for melt blending of the antistatic polypropylene composition A are the conditions and equipment for melt blending of polyolefins in the prior art, preferably, the melting temperature is 150-170°C, and the equipment is preferably a twin-screw extruder.
[0053] In a preferred embodiment of the present invention, the preparation of the raw materials of the layer B and the layer B' comprises melt blending the components including the random copolymer polypropylene x, the thermal adhesion enhancer y and the conductive filler. The conditions and equipment for melt blending of the antistatic polypropylene compositions B and B' are the conditions and equipment for melt blending of polyolefins in the prior art, preferably, the melting temperature is 110-150°C, and the equipment is preferably a twin-screw extruder.
[0054] Preferably, the co-extrusion and casting temperatures are independently selected from 200-240°C.
[0055] Preferably, the temperature of the calendering roller is 50-70°C.
[0056] The selection range of stretching conditions is relatively wide. In a preferred embodiment of the present invention, the stretching conditions include: the stretching method is free stretching, and / or solid phase stretching, and / or multi-stage stretching; the stretching temperature is 90-165°C, preferably 90-140°C, and further preferably 90-119°C; the stretching ratio is 1-20 times, preferably 2-15 times.
[0057] In a preferred embodiment of the present invention, the longitudinal tensile strength of the antistatic polypropylene sheet after stretching is greater than or equal to 30 MPa, more preferably 30 MPa-1 GPa; most preferably 300-800 MPa.
[0058] According to some embodiments of the present invention, the antistatic polypropylene composition A, the antistatic polypropylene composition B, and B' are co-extruded and cast or calendered according to the BAB' structure to obtain a polypropylene co-extruded sheet. The process of the extrusion calendering method may include passing the polypropylene co-extruded sheet through a calendering roller and a traction roller in sequence, and then solid phase stretching, trimming and winding to obtain the antistatic sheet. The temperature of the extrusion casting is 200-230°C, and the temperature of the calendering roller is 50-70°C. The specific process of preparing the film by the extrusion calendering method is a commonly used choice in the art and will not be repeated here.
[0059] The third aspect of the present invention is to provide an antistatic polypropylene fabric, which is a three-dimensional polypropylene fabric obtained by weaving the antistatic polypropylene sheet described in the first aspect;
[0060] Preferably, the antistatic polypropylene fabric is obtained by slitting and weaving the antistatic polypropylene sheet; and / or the antistatic polypropylene fabric has a three-dimensional structure of plain, twill and / or satin.
[0061] In order to facilitate weaving, the antistatic polypropylene sheet is preferably cut into polypropylene sheets with a width of 2-5 mm, and then the antistatic polypropylene fabric is obtained by weaving.
[0062] In a more preferred embodiment of the present invention, the antistatic polypropylene fabric is a plain, twill, satin or three-dimensional antistatic polypropylene fabric obtained by weaving three-layer co-extruded antistatic polypropylene stretch flat tape, and the three-layer co-extruded polypropylene stretch flat tape includes at least one film layer A formed by a high-melting point polypropylene combination A and at least one film layer B formed by a low-melting point polypropylene composition B, wherein the polypropylene composition A includes homopolymer polypropylene a and impact copolymer polypropylene b; the polypropylene composition B includes random copolymer polypropylene x and thermal bonding enhancement enhancer y, and the polymer film B layer is located on both sides of the A layer.
[0063] The fourth aspect of the present invention provides an antistatic polypropylene composite material, which is prepared by hot pressing multiple layers of the antistatic polypropylene sheets described in the first aspect and / or the antistatic polypropylene fabric described in the third aspect.
[0064] Preferably, the antistatic polypropylene composite material is prepared by thermally pressing multiple layers of the antistatic polypropylene sheets or the antistatic polypropylene fabric.
[0065] Preferably, the multi-layer antistatic polypropylene sheets are stacked from top to bottom in the angle of 0-90° along the respective machine directions.
[0066] Preferably, the multi-layer antistatic polypropylene fabric is stacked from top to bottom with the warp direction being 0-90° with the warp direction being the other direction.
[0067] Preferably, the number of layers of the multi-layer antistatic polypropylene sheet and / or the multi-layer antistatic polypropylene fabric is greater than or equal to 2 layers, more preferably 2-200 layers; most preferably 4-100 layers.
[0068] Preferably, the surface density of the multi-layer antistatic polypropylene composite material is greater than or equal to 110 g / m 2 , more preferably 110g / m 2 -14000g / m 2 ; The most preferred is 220g / m 2 -7000g / m 2 .
[0069] In a preferred embodiment of the present invention, the antistatic polypropylene composition A contained in each stacked layer of antistatic polypropylene fabric may be the same or different, and the antistatic polypropylene fabric A contained in each layer may be independently selected, and preferably the antistatic polypropylene composition A of each layer is the same.
[0070] In a more preferred embodiment of the present invention, the antistatic polypropylene composite material comprises a plurality of antistatic polypropylene sheet unit groups stacked in sequence; each antistatic polypropylene sheet unit group comprises at least one identical or different antistatic polypropylene sheet unit, and each antistatic polypropylene sheet unit comprises an antistatic core layer A i and located in the core layer A i Antistatic outer layer B on both sides i , B' i , structure B i A i B' iThe structure of the antistatic polypropylene composite material is, from bottom to top, the nth group... the ith group... the second group, the first group, the second group... the ith group... the nth group, and the total number of stacked antistatic polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n; wherein the core layer A in the antistatic polypropylene sheet unit i Containing antistatic polypropylene composition A i , antistatic outer layer B i With antistatic outer layer B' i The same or different, each corresponding to an antistatic polypropylene composition B i , antistatic polypropylene composition B' i , the antistatic polypropylene composition A i The melting point is greater than that of the antistatic polypropylene composition B i , the antistatic polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than or equal to the average melting point of all outer layers in the i-1-th group.
[0071] More preferably, the average value of the melting points of all the outer layers in the i-th group is greater than the average value of the melting points of all the outer layers in the i-1-th group.
[0072] Preferably, the antistatic polypropylene composition A i Melting point and antistatic polypropylene composition B i The difference in melting points, antistatic polypropylene composition A i Melting point and antistatic polypropylene composition B' i The difference in melting points is 5°C or more, preferably 10°C or more, and more preferably 20°C or more.
[0073] Preferably, the difference between the average melting point of all outer layers in the i-th group and the average melting point of all outer layers in the i-1-th group is the same or different, and is 1-40°C, preferably 1-10°C, more preferably 1-5°C.
[0074] Preferably, 2≤n≤100, preferably, 2≤n≤50.
[0075] Preferably, each group of antistatic polypropylene sheet units independently comprises 1 to 10, preferably 1 to 5, identical or different antistatic polypropylene sheet units.
[0076] In a preferred embodiment of the present invention, the antistatic polypropylene composite material has at least one of the following characteristics:
[0077] Longitudinal tensile strength ≥150MPa, preferably ≥170MPa;
[0078] Interlayer peel strength ≥1N / mm, preferably ≥1.2N / mm;
[0079] The tensile strength is measured according to the method specified in GB / T1040.1-2018, and the interlayer peel strength is measured according to the method specified in GB / T2358-98. The corresponding specimens in the above two tests are the standard specimens required in the above-mentioned test standards.
[0080] When the antistatic polypropylene composite material is obtained by hot pressing 24 layers of antistatic polypropylene fabrics and has a thickness of about 1.6 mm, the drop weight impact strength is ≥226 J, preferably ≥240 J.
[0081] The drop weight impact strength is measured according to the method specified in GB / T14153-1993, and the thickness of the sample is the thickness of the prepared product.
[0082] As an example, in a preferred embodiment of the present invention, the polypropylene composite material is obtained by sequentially stacking the antistatic polypropylene sheets and / or fabrics described above to obtain a melting point gradient structure antistatic polypropylene sheet composition; preferably, the structure is B from bottom to top. n A n B n ……B i A i B i ……B 2 A 2 B 2 , B 1 A 1 B 1 , B 2 A 2 B 2 ……B i A i B i ……B n A n B n , the total number of stacked layers of the polypropylene sheet unit is 2n-1; i and n are both integers not less than 2, and i≤n; the antistatic polypropylene sheets are stacked from top to bottom at 0-90° between the warp and the warp, preferably with more than or equal to 2 layers, more preferably 2-200 layers; most preferably 4-100 layers, the antistatic polypropylene composition A i The melting point is greater than that of the antistatic polypropylene composition B i , the antistatic polypropylene composition B i The melting point is greater than or equal to that of the adjacent antistatic polypropylene composition B i-1 Melting point.
[0083] The fifth aspect of the present invention is to provide a method for preparing the antistatic polypropylene composite material described in the fourth aspect, which comprises laminating and hot-pressing the antistatic polypropylene sheet and / or the antistatic polypropylene fabric, and then cooling and shaping to prepare the antistatic polypropylene composite material.
[0084] Preferably, the temperature of the hot pressing fusion is 115-170°C, preferably 115-159°C, and more preferably 140-159°C.
[0085] Preferably, the pressure of the hot pressing fusion is 2-10 MPa.
[0086] Preferably, the preheating time of the hot pressing fusion is 5-600s, and the hot pressing time is 1-600s, preferably 10-500s.
[0087] Preferably, the cooling and shaping pressure is 2-8 MPa, and the cooling and shaping time is 30-700 s.
[0088] Preferably, the number of layers of the antistatic polypropylene sheet and / or the antistatic polypropylene fabric laminate is greater than or equal to 2 layers, preferably 2-200 layers; more preferably 4-100 layers.
[0089] Preferably, adjacent layers of the antistatic polypropylene fabric laminate are placed at an angle of 0-90° between the warp directions.
[0090] Preferably, adjacent layers of the antistatic polypropylene sheet laminate are placed at 0-90° along the respective machine directions.
[0091] As an example, in a more preferred embodiment of the present invention, the method for preparing the high-strength, high-impact, antistatic polypropylene composite material comprises the following steps:
[0092] Step a: co-extrude the antistatic polypropylene composition A and the antistatic polypropylene composition B according to the BAB structure and cast or calender to obtain an antistatic polypropylene co-extruded sheet; preferably, the extrusion casting or calendering temperature is 200-240° C., and the temperature of the calendering roller is 50-70° C.;
[0093] Step b: stretching the antistatic polypropylene coextruded sheet at a certain temperature to obtain an antistatic polypropylene stretched sheet; the stretching method is free stretching, and / or solid phase stretching, and / or multi-stage stretching; the stretching temperature is preferably 90-165°C, preferably 90-140°C, and more preferably 90-119°C; the stretching ratio is 1-20 times, preferably 2-15 times.
[0094] Step c: cutting the antistatic polypropylene stretched sheet to prepare antistatic polypropylene flat strips, and weaving the flat strips to prepare antistatic polypropylene fabrics; preferably, the width of the polypropylene flat strips is 2-5 mm, and the antistatic polypropylene fabrics include plain weave, twill, satin weave or other three-dimensional polypropylene fabrics;
[0095] Step d: stacking the antistatic polypropylene fabrics in sequence, hot pressing and fusing them, and then cooling and shaping them to form an antistatic polypropylene composite material; preferably, in the step d, the hot pressing conditions are: hot pressing temperature 115-170°C, preferably 115-159°C, and more preferably 140-159°C; hot pressing pressure 2-10MPa, preheating time 5-600s, hot pressing time 1-600s, preferably 10-500s, cooling pressure 2-8MPa, cooling time 30s-700s; preferably, adjacent polypropylene fabrics in the antistatic polypropylene composite material can be placed at 0-90° between the warp and the warp.
[0096] According to some embodiments of the present invention, in step c, a high-speed slitting machine with multiple blades can be used for cutting to obtain an oriented polypropylene flat ribbon with a width of 2-5 mm; a commercial weaving machine is used to weave the oriented flat ribbon according to the designed fabric structure to obtain plain, twill, satin or other three-dimensional antistatic polypropylene fabrics.
[0097] According to the present invention, in a preferred specific embodiment, the pressure is preferably maintained continuously during the hot pressing and cooling process without being reduced. The hot pressing process is carried out continuously, and preferably a continuous hot pressing composite material molding equipment consisting of a preheating machine, a crawler-type continuous flat hot press, a crawler-type continuous flat cooling press, a sheet cutting machine and a sheet stacking machine arranged in sequence is used; preferably, the crawler-type continuous flat hot press has a preheating unit, an independent heating and pressurizing unit, an air cooling unit and a lifting mechanism.
[0098] During the preparation, the antistatic polypropylene sheet and / or the antistatic polypropylene fabric are stacked in sequence and then preheated by a preheater. The preheated samples are sequentially hot-pressed and fused by a crawler-type flat hot press, and then cooled and shaped by a crawler-type continuous flat cooling press to form a polypropylene composite material, i.e., a stacked hot-pressed product. Afterwards, the sheets are sliced by a sheet cutter as needed, and the hot-pressed products are stacked and arranged by a sheet stacker. The hot-pressing temperature is controlled by a preheating unit, an independent heating and pressing unit, and an air-cooling unit in a crawler-type flat hot press, and the hot-pressing pressure is controlled by a lifting mechanism. According to the inventor's research, when the preparation process parameters are within a preferred range, the antistatic polymer composite material is preferably prepared using the preparation equipment, and the polymer composite material has better tensile strength, impact resistance, and interlayer peeling strength.
[0099] The sixth aspect of the present invention is to provide an application of the antistatic polypropylene sheet described in the first aspect, the antistatic polypropylene fabric described in the third aspect, the antistatic polypropylene composite material described in the fourth aspect, and the antistatic polypropylene composite material prepared by the preparation method described in the fifth aspect in the fields of sports protection, automobile manufacturing, military materials and consumer goods.
[0100] According to a specific embodiment of the present invention, the material fields include luggage and transportation industry, shoemaking industry, automobile manufacturing industry, sports equipment manufacturing industry, audio equipment manufacturing industry and military field.
[0101] Compared with the prior art, the present invention has the following beneficial effects:
[0102] (1) The antistatic polypropylene composite material is obtained by hot pressing the antistatic polypropylene sheet, which has good tensile properties, impact resistance and electrical properties at the same time, and still has good interlayer peeling strength when prepared at a lower hot pressing temperature.
[0103] (2) The antistatic polypropylene composite material of the present invention has good tensile strength, impact resistance, interlayer peeling strength and antistatic properties;
[0104] The antistatic polypropylene composite material has the following characteristics:
[0105] Longitudinal (MD) tensile strength ≥150MPa, preferably ≥170MPa; interlayer peel strength ≥1N / mm, preferably ≥1.2N / mm; volume resistivity ≥10 2 -10 9 Ω·m, preferably 10 2 -10 6 Ω·m; when the composite material is only composed of 24 layers of antistatic polypropylene fabrics hot pressed together and has a thickness of about 1.6 mm, the drop weight impact strength is ≥226 J, preferably ≥240 J.
[0106] (3) The antistatic polypropylene composite material of the present invention can be prepared at a relatively low hot pressing temperature and within a relatively wide hot pressing temperature range, which effectively reduces the energy consumption of the equipment and the damage to the composite material caused by high-temperature operation. At the same time, when prepared at a relatively low hot pressing temperature, it still has good interlayer peeling strength.
[0107] (4) The preparation method can reduce the hot pressing operation time, while improving production efficiency and reducing production energy consumption.
[0108] (5) The present invention reduces the hot pressing temperature and expands the hot pressing temperature range to 50°C; it effectively reduces the energy consumption of the equipment and the damage to the composite material caused by high temperature operation. DETAILED DESCRIPTION
[0109] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0110] The properties of the polypropylene composition and sheet were tested according to the following method, and the product test results are shown in Table 1:
[0111] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682-2000, wherein for polypropylene (including homopolypropylene, impact copolymer polypropylene and random copolymer polypropylene), the test temperature is 230°C and the load is 2.16 kg; for thermal adhesion enhancers, the test temperature is 190°C and the load is 2.16 kg.
[0112] (2) Molecular weight distribution (Mw / Mn): measured according to the method specified in GB / T 36214.1-2018, where Mw is the weight average molecular weight in g / mol and Mn is the number average molecular weight in g / mol.
[0113] (3) The melting point of the material is determined by the method of GB / T 28724-2012. The sample mass is 5 mg. The temperature is increased from 50°C to 230°C at a rate of 10°C / min, and the temperature is maintained at 230°C for 3 min to eliminate the thermal history. The temperature is then decreased from 230°C to 50°C at a rate of 10°C / min, and the temperature is maintained at 50°C for 1 min. Finally, the temperature is increased from 50°C to 230°C at a rate of 10°C / min. The last temperature increase curve is used to determine the melting point or melting range of the material.
[0114] (4) Sheet tensile strength: measured according to the method specified in GB / T1040.1-2018.
[0115] (5) Drop weight impact strength: measured according to the method specified in GB / T14153-1993.
[0116] (6) Interlayer peel strength: measured according to the method specified in QB / T2358-98.
[0117] (7) Density: measured according to the method specified in GB / T 1033.1-2008;
[0118] (8) Volume resistivity: measured using Keithley 6517B Electrometer.
[0119] In the following examples, the β-crystal nucleating agent with the brand name VP101B is sourced from Beijing Research Institute of Chemical Industry of Sinopec Corporation; the sources of some raw materials are described in the examples, and the other raw materials are commercially available unless otherwise specified.
[0120] Example 1
[0121] This example is used to illustrate the preparation of the antistatic polypropylene composition, the three-layer co-extruded antistatic polypropylene sheet, the antistatic polypropylene fabric, and the antistatic polypropylene composite material provided by the present invention.
[0122] (1) Preparation of antistatic polypropylene composition A:
[0123] Component a is a homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 160°C, a melt flow rate of 3.2g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry (under 23°C test conditions, the impact strength is 23KJ / m 2 ), the ethylene content is 11%wt, the melt flow rate is 2.0g / 10min, and the melting point is 155°C; the conductive filler is multi-walled carbon nanotubes purchased from Cheap Tubes Company in the United States.
[0124] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 80 parts by weight, the mass fraction Wb of component b is 20 parts by weight, and the carbon nanotubes are 3 parts by weight. 0.05 parts by weight of a β-crystal nucleating agent with the grade VP101B is added. Then the mixture is added to a high-speed stirrer and mixed evenly, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 200-230°C. After the screw is melt-mixed, extruded, granulated and dried, an antistatic polypropylene composition pellet is obtained. The melt mass flow rate MFRA is detected to be 4.5 / 10min; the melting point of the antistatic polypropylene composition A is 157°C.
[0125] (2) Preparation of antistatic polypropylene composition B:
[0126] Component x is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C and a melt flow rate of 6.6 g / 10 min; component y is a polyolefin elastomer with brand number 6102, purchased from Exxon, which is an ethylene-propylene copolymer with an ethylene content of 16%wt and a melt flow rate of 1.4 g / 10 min at 230°C and a load of 2.16 kg; the conductive filler is multi-walled carbon nanotubes purchased from Cheap Tubes, USA.
[0127] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 85 parts by weight, the mass fraction Wy of component y is 15 parts by weight, and the carbon nanotubes are 3 parts by weight. The other steps are the same as step (1), and finally an antistatic polypropylene composition B pellet is obtained. The melt mass flow rate MFRB is 5.1 g / 10 min and the melting point is 138° C.
[0128] (3) Preparation of three-layer co-extruded antistatic polypropylene sheet:
[0129] The antistatic polypropylene composition A and the antistatic polypropylene composition B pellets prepared in the above steps (1) and (2) are dried, and then the antistatic polypropylene composition A is added to the core layer extruder of the multi-layer extrusion calendering, and the antistatic polypropylene composition B is added to the upper and lower surface layer extruders of the multi-layer extrusion casting machine.
[0130] After the pellets are co-extruded and compounded out from the die of the extruder, they are sequentially passed through a calendering roller and a traction roller, and then subjected to solid phase stretching, edge cutting and winding, thereby obtaining the sheet.
[0131] The temperature of the extrusion casting is 230°C, and the temperature of the calendering roller is 55°C. The temperature during the solid phase stretching is 135°C, the stretching rate is 2m / min, and the stretching ratio is 7 times. After stretching, the sheet is rolled up to form an antistatic polypropylene sheet (composite film), which consists of an upper surface layer (antistatic film layer B), a core layer (antistatic film layer A) and a lower surface layer (antistatic film layer B).
[0132] The thickness of the antistatic polypropylene sheet (composite film) is 82 μm, wherein the thickness of the film layer A accounts for 80% of the total thickness of the sheet.
[0133] (4) Preparation of antistatic polypropylene fabric:
[0134] The three-layer co-extruded antistatic polypropylene sheet obtained in the above step (3) is cut by a high-speed slitting machine with multiple blades to obtain an oriented antistatic polypropylene flat ribbon with a width of 3 mm; the oriented flat ribbon is woven by a commercial weaving machine according to the designed fabric structure to obtain a plain antistatic polypropylene fabric.
[0135] (5) Preparation of antistatic polypropylene composite materials:
[0136] The antistatic polypropylene fabric obtained in the above step (4) is laminated and hot-pressed in sequence to form a laminated antistatic polypropylene sheet. The laminated antistatic polypropylene sheet includes 24 layers of antistatic polypropylene fabric, and the polypropylene fabric is placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 150°C, hot pressing pressure 5MPa, preheating time 180s, hot pressing time 180s, and cooling time 600s. The thickness of the prepared antistatic polypropylene composite material is 1.70mm.
[0137] Example 2
[0138] This example is used to illustrate the preparation of the antistatic polypropylene composition, the three-layer co-extruded antistatic polypropylene sheet, the antistatic polypropylene fabric, and the antistatic polypropylene composite material provided by the present invention.
[0139] (1) Preparation of antistatic polypropylene composition A:
[0140] Component a is homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 165°C, a melt flow rate of 8.1g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry, with an impact strength of 25KJ / m under 23°C test conditions. 2 , ethylene content is 8%wt, melt flow rate is 3.2g / 10min, melting point is 155°C; graphene is edge-modified graphene produced by Sinopec Beijing Research Institute of Chemical Industry.
[0141] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 70 parts by weight, the mass fraction Wb of component b is 30 parts by weight, and graphene is 2 parts by weight. 0.05 parts by weight of a β-crystal nucleating agent with the grade VP101B is added. Then the mixture is added to a high-speed stirrer and mixed evenly, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 200-230°C, and the screw is melt-mixed, extruded, granulated and dried to obtain antistatic polypropylene composition pellets. The melt mass flow rate MFRA is detected to be 7.0 / 10min, and the melting point of the antistatic polypropylene composition A is 161°C.
[0142] (2) Preparation of antistatic polypropylene composition B:
[0143] Component x is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 134°C, an ethylene-propylene-butene terpolymer, and a melt flow rate of 5.2 g / 10 min; component y is a polyolefin elastomer produced by Sinopec Beijing Research Institute of Chemical Industry, an ethylene-propylene copolymer, with an ethylene content of 15% wt, a melting point of 105°C, and a melt flow rate of 9 g / 10 min at 230°C and a load of 2.16 kg; graphene is edge-modified graphene produced by Sinopec Beijing Research Institute of Chemical Industry.
[0144] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 80 parts by weight, the mass fraction Wy of component y is 20 parts by weight, and the graphene is 2 parts by weight. The other steps are the same as step (1), and finally the antistatic polypropylene composition B pellets are obtained. The melt mass flow rate MFRB is detected to be 9.5 g / 10 min. The melting point of the antistatic polypropylene composition B is 130°C.
[0145] (3) Preparation of three-layer co-extruded antistatic polypropylene sheet:
[0146] The preparation process is the same as step (3) of Example 1.
[0147] (4) Preparation of antistatic polypropylene fabric:
[0148] The preparation process is the same as step (4) of Example 1.
[0149] (5) Preparation of antistatic polypropylene composite materials:
[0150] The preparation process is the same as step (5) of Example 1.
[0151] The thickness of the prepared antistatic polypropylene composite material is close to that of Example 1.
[0152] Example 3
[0153] This example is used to illustrate the preparation of the antistatic polypropylene composition, the three-layer co-extruded antistatic polypropylene sheet, the antistatic polypropylene fabric, and the antistatic polypropylene composite material provided by the present invention.
[0154] (1) Preparation of antistatic polypropylene composition A:
[0155] Same as Example 1, wherein the mass fraction Wa of component a is 90 parts by weight, the mass fraction Wb of component b is 10 parts by weight, and the content of carbon nanotubes is 3 parts by weight. 0.05 parts by weight of a β-crystal nucleating agent with a grade of VP101B is added. Antistatic polypropylene composition A pellets are obtained, and the melt mass flow rate MFRA is detected to be 6.6 / 10min, and the melting point of the antistatic polypropylene composition A is 158°C.
[0156] (2) Preparation of antistatic polypropylene composition B:
[0157] The same as Example 1, wherein the mass fraction Wx of component x is 90 parts by weight, the mass fraction Wy of component y is 10 parts by weight, and the carbon nanotubes are 3 parts by weight, and finally an antistatic polypropylene composition B pellet is obtained. The melt mass flow rate MFRB is detected to be 8.3 g / 10 min, and the melting point of the antistatic polypropylene composition B is 139°C.
[0158] (3) Preparation of three-layer co-extruded antistatic polypropylene sheet:
[0159] The preparation process is the same as step (3) of Example 1.
[0160] (4) Preparation of antistatic polypropylene fabric:
[0161] The preparation process is the same as step (4) of Example 1.
[0162] (5) Preparation of antistatic polypropylene composite materials:
[0163] The preparation process is the same as step (5) of Example 1.
[0164] The thickness of the prepared antistatic polypropylene composite material is close to that of Example 1.
[0165] Example 4
[0166] This example is used to illustrate the preparation of the antistatic polypropylene composition, the three-layer co-extruded antistatic polypropylene sheet, the antistatic polypropylene fabric, and the antistatic polypropylene composite material provided by the present invention.
[0167] (1) Preparation of antistatic polypropylene composition A:
[0168] The preparation process is the same as step (1) of Example 1.
[0169] (2) Preparation of antistatic polypropylene composition B:
[0170] The preparation process is the same as step (2) of Example 1.
[0171] (3) Preparation of three-layer co-extruded antistatic polypropylene sheet:
[0172] The main steps are the same as those of Example 1. The thickness of the polypropylene sheet is 82 μm, wherein the thickness of the film layer Ai accounts for 90% of the total thickness of the sheet.
[0173] (4) Preparation of antistatic polypropylene fabric:
[0174] The preparation process is the same as step (4) of Example 1.
[0175] (5) Preparation of antistatic polypropylene composite materials:
[0176] The preparation process is the same as step (5) of Example 1.
[0177] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0178] Example 5
[0179] This example is used to illustrate the preparation of the antistatic polypropylene composition, the three-layer co-extruded antistatic polypropylene sheet, the antistatic polypropylene fabric, and the antistatic polypropylene composite material provided by the present invention.
[0180] (1) Preparation of antistatic polypropylene composition A:
[0181] The preparation process is the same as step (1) of Example 1.
[0182] (2) Preparation of antistatic polypropylene composition B:
[0183] The preparation process is the same as step (2) of Example 1.
[0184] (3) Preparation of three-layer co-extruded antistatic polypropylene sheet:
[0185] The main steps are the same as those of Example 1. The thickness of the polypropylene sheet is 80 μm, wherein the thickness of the film layer A accounts for 70% of the total thickness of the sheet.
[0186] (4) Preparation of antistatic polypropylene fabric:
[0187] The preparation process is the same as step (4) of Example 1.
[0188] (5) Preparation of antistatic polypropylene composite materials:
[0189] The preparation process is the same as step (5) of Example 1.
[0190] The thickness of the prepared antistatic polypropylene composite material is close to that of Example 1.
[0191] Example 6
[0192] This example is used to illustrate the preparation of the antistatic polypropylene composition, the three-layer co-extruded antistatic polypropylene sheet, the antistatic polypropylene fabric, and the antistatic polypropylene composite material provided by the present invention.
[0193] (1) Preparation of antistatic polypropylene composition A:
[0194] The preparation process is the same as step (1) of Example 1.
[0195] (2) Preparation of antistatic polypropylene composition B:
[0196] The preparation process is the same as step (2) of Example 1.
[0197] (3) Preparation of three-layer co-extruded antistatic polypropylene sheet:
[0198] The preparation process is the same as step (3) of Example 1.
[0199] (4) Preparation of antistatic polypropylene fabric:
[0200] The main steps are the same as step (4) of Example 1. The oriented flat tape is woven using a commercial weaving machine according to the designed fabric structure to obtain a satin antistatic polypropylene fabric.
[0201] (5) Preparation of antistatic polypropylene composite materials:
[0202] The preparation process is the same as step (5) of Example 1.
[0203] The thickness of the prepared antistatic polypropylene composite material is close to that of Example 1.
[0204] Example 7
[0205] This example is used to illustrate the preparation of the antistatic polypropylene composition, the three-layer co-extruded antistatic polypropylene sheet, the antistatic polypropylene fabric, and the antistatic polypropylene composite material provided by the present invention.
[0206] (1) Preparation of antistatic polypropylene composition A:
[0207] The preparation process is the same as step (1) of Example 1.
[0208] (2) Preparation of antistatic polypropylene composition B:
[0209] The preparation process is the same as step (2) of Example 1.
[0210] (3) Preparation of three-layer co-extruded antistatic polypropylene sheet:
[0211] The main preparation process is the same as step (3) of Example 1, wherein the sheet stretching ratio is 10 times.
[0212] (4) Preparation of antistatic polypropylene fabric:
[0213] The preparation process is the same as step (4) of Example 1.
[0214] (5) Preparation of antistatic polypropylene composite materials:
[0215] The preparation process is the same as step (5) of Example 1.
[0216] The thickness of the prepared antistatic polypropylene composite material is close to that of Example 1.
[0217] Example 8
[0218] This example is used to illustrate the preparation of the antistatic polypropylene composition, the three-layer co-extruded antistatic polypropylene sheet, the antistatic polypropylene fabric, and the antistatic polypropylene composite material provided by the present invention.
[0219] (1) Preparation of antistatic polypropylene composition A:
[0220] The preparation process is the same as step (1) of Example 1.
[0221] (2) Preparation of antistatic polypropylene composition B:
[0222] The preparation process is the same as step (2) of Example 1.
[0223] (3) Preparation of three-layer co-extruded antistatic polypropylene sheet:
[0224] The main preparation process is the same as step (3) of Example 1. The stretching process is a multi-stage stretching process, in which the temperature in the first stage solid phase stretching process is 138°C, the stretching rate is 2m / min, and the stretching ratio is 7 times. The stretched sheet is subjected to a second stage free stretching, the stretching temperature is 140°C, the stretching rate is 0.5m / min, and the stretching ratio is 2 times.
[0225] The obtained polypropylene sheet (composite film) was stretched to a ratio of 14 times.
[0226] (4) Preparation of antistatic polypropylene fabric:
[0227] The preparation process is the same as step (4) of Example 1.
[0228] (5) Preparation of antistatic polypropylene composite materials:
[0229] The preparation process is the same as step (5) of Example 1.
[0230] The thickness of the prepared antistatic polypropylene composite material is 1.59 mm.
[0231] Example 9
[0232] This example is used to illustrate the preparation of the antistatic polypropylene composition, the three-layer co-extruded antistatic polypropylene sheet, the antistatic polypropylene fabric, and the antistatic polypropylene composite material provided by the present invention.
[0233] (1) Preparation of antistatic polypropylene composition A:
[0234] The preparation process is the same as step (1) of Example 1.
[0235] (2) Preparation of antistatic polypropylene composition B:
[0236] The preparation process is the same as step (2) of Example 1.
[0237] (3) Preparation of three-layer co-extruded antistatic polypropylene sheet:
[0238] The preparation process is the same as step (3) of Example 1.
[0239] (4) Preparation of antistatic polypropylene fabric:
[0240] The preparation process is the same as step (4) of Example 1.
[0241] (5) Preparation of antistatic polypropylene composite materials:
[0242] The main preparation process is the same as step (5) of Example 1. The polypropylene fabric is placed at 45° between the warp directions.
[0243] The thickness of the prepared antistatic polypropylene composite material is close to that of Example 1.
[0244] Example 10
[0245] This example is used to illustrate the preparation of the antistatic polypropylene composition, the three-layer co-extruded antistatic polypropylene sheet, the antistatic polypropylene fabric, and the antistatic polypropylene composite material provided by the present invention.
[0246] (1) Preparation of antistatic polypropylene composition A:
[0247] The preparation process is the same as step (1) of Example 1.
[0248] (2) Preparation of antistatic polypropylene composition B:
[0249] The preparation process is the same as step (2) of Example 1.
[0250] (3) Preparation of three-layer co-extruded antistatic polypropylene sheet:
[0251] The preparation process is the same as step (3) of Example 1.
[0252] (4) Preparation of antistatic polypropylene fabric:
[0253] The preparation process is the same as step (4) of Example 1.
[0254] (5) Preparation of antistatic polypropylene composite materials:
[0255] The main preparation process is the same as step (5) of Example 1. The polypropylene fabric is placed at 0° between the warp directions.
[0256] The thickness of the prepared antistatic polypropylene composite material is close to that of Example 1.
[0257] Embodiment 11
[0258] This example is used to illustrate the preparation of the antistatic polypropylene composition, the three-layer co-extruded antistatic polypropylene sheet, the antistatic polypropylene fabric, and the antistatic polypropylene composite material provided by the present invention.
[0259] (1) Preparation of antistatic polypropylene composition A:
[0260] The preparation process is the same as step (1) of Example 1.
[0261] (2) Preparation of antistatic polypropylene composition B:
[0262] The preparation process is the same as step (2) of Example 1.
[0263] (3) Preparation of three-layer co-extruded antistatic polypropylene sheet:
[0264] The preparation process is the same as step (3) of Example 1.
[0265] (4) Preparation of antistatic polypropylene fabric:
[0266] The preparation process is the same as step (4) of Example 1.
[0267] (5) Preparation of antistatic polypropylene composite materials:
[0268] The main steps are the same as those in Example 1. The laminated antistatic polypropylene sheet includes two layers of antistatic polypropylene fabric. The hot pressing conditions are: temperature 140°C, hot pressing pressure 2MPa, preheating time 120s, hot pressing time 10s, and cooling time 300s. The thickness of the prepared antistatic polypropylene composite material is 130μm.
[0269] Example 12
[0270] This example is used to illustrate the preparation of the antistatic polypropylene composition, the three-layer co-extruded antistatic polypropylene sheet, the antistatic polypropylene fabric, and the antistatic polypropylene composite material provided by the present invention.
[0271] (1) Preparation of antistatic polypropylene composition A:
[0272] The preparation process is the same as step (1) of Example 1.
[0273] (2) Preparation of antistatic polypropylene composition B:
[0274] The preparation process is the same as step (2) of Example 1.
[0275] (3) Preparation of three-layer co-extruded antistatic polypropylene sheet:
[0276] The preparation process is the same as step (3) of Example 1.
[0277] (4) Preparation of antistatic polypropylene fabric:
[0278] The preparation process is the same as step (4) of Example 1.
[0279] (5) Preparation of antistatic polypropylene composite materials:
[0280] The main steps are the same as those in Example 1. The laminated polypropylene sheet includes 100 layers of antistatic polypropylene fabric. The hot pressing conditions used are: 159°C, hot pressing pressure of 10 MPa, preheating time of 300 seconds, hot pressing time of 300 seconds, and cooling time of 700 seconds. The thickness of the prepared polypropylene composite material is 7.27 mm.
[0281] Embodiment 13
[0282] This example is used to illustrate the preparation of the antistatic polypropylene composition, the three-layer co-extruded antistatic polypropylene sheet, the antistatic polypropylene fabric, and the antistatic polypropylene composite material provided by the present invention.
[0283] (1) Preparation of antistatic polypropylene composition A:
[0284] The preparation process is the same as step (1) of Example 1.
[0285] (2) Preparation of antistatic polypropylene composition B:
[0286] The preparation process is the same as step (2) of Example 1.
[0287] (3) Preparation of three-layer co-extruded antistatic polypropylene sheet:
[0288] The preparation process is the same as step (3) of Example 1.
[0289] (4) Preparation of antistatic polypropylene fabric:
[0290] The preparation process is the same as step (4) of Example 1.
[0291] (5) Preparation of antistatic polypropylene composite materials:
[0292] The main steps are the same as those in Example 1. The temperature is 155° C., the hot pressing pressure is 8 MPa, the preheating time is 300 s, the hot pressing time is 300 s, and the cooling time is 700 s. The thickness of the prepared antistatic polypropylene composite material is 1.58 mm.
[0293] Embodiment 14
[0294] This example is used to illustrate the preparation of the antistatic polypropylene composition, the three-layer co-extruded antistatic polypropylene sheet, the antistatic polypropylene fabric, and the antistatic polypropylene composite material provided by the present invention.
[0295] (1) Preparation of antistatic polypropylene composition A:
[0296] The preparation process is the same as step (1) of Example 1.
[0297] (2) Preparation of antistatic polypropylene composition B:
[0298] The preparation process is the same as step (2) of Example 1.
[0299] (3) Preparation of three-layer co-extruded antistatic polypropylene sheet:
[0300] The preparation process is the same as step (3) of Example 1.
[0301] (4) Preparation of antistatic polypropylene composite materials:
[0302] The polypropylene fabric was not prepared, but the three-layer co-extruded antistatic polypropylene sheet prepared in step (3) was used to replace the antistatic polypropylene fabric obtained in step (4) of Example 1, and the layers were stacked and hot-pressed in sequence according to step (5) of Example 1. The thickness of the prepared antistatic polypropylene composite material was 1.51 mm.
[0303] Embodiment 15
[0304] This example is used to illustrate the preparation of the antistatic polypropylene composition, the three-layer co-extruded antistatic polypropylene sheet, the antistatic polypropylene fabric and the antistatic polypropylene composite material provided by the present invention.
[0305] (1) Antistatic Polypropylene Composition A i Preparation:
[0306] Component a is homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 160°C, a melt flow rate of 3.2g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry, with an ethylene content of 11wt%, a melting point of 155°C, and an Izod impact strength of 23KJ / m 2 (23°C), melt flow rate of 2.0g / 10min; conductive filler: edge-modified graphene made by Sinopec Beijing Research Institute of Chemical Industry. The above-prepared components were weighed and mixed according to the proportion, wherein the mass fraction Wa of component a was 80 parts by weight, the mass fraction Wb of component b was 20 parts by weight, and graphene was 2 parts by weight.
[0307] 0.05 parts by weight of a β-crystal nucleating agent of grade VP101B was added. The mixture was then added to a high-speed stirrer for uniform mixing, and then the mixed material was added to the feeder of a twin-screw extruder manufactured by W&P. The material entered the twin screw through the feeder. During the processing, the temperature of the screw was maintained between 200-230°C. The screw was melt-mixed, extruded, granulated and dried to obtain polypropylene composite pellets A. i , the polypropylene composition pellets A were tested i The melting point is 157°C.
[0308] (2) Antistatic Polypropylene Composition B i Preparation:
[0309] Component x 1 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melt flow rate of 8.1g / 10min and a melting point of 130℃; component x 2 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melt flow rate of 7.2g / 10min and a melting point of 135℃; component x 3 It is a random copolymer polypropylene made by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melt flow rate of 6.6g / 10min and a melting point of 140°C; component y is a polyolefin elastomer with brand number 6102, purchased from Exxon, which is an ethylene-propylene copolymer; the conductive filler is edge-modified graphene made by Sinopec Beijing Research Institute of Chemical Industry.
[0310] The components prepared above are weighed and mixed according to the ratio, wherein component x i The mass fraction Wx i The weight fraction Wy of component y is 85 parts by weight, the weight fraction Wy of component y is 15 parts by weight, the weight fraction of graphene is 2 parts by weight, and the other steps are the same as step (1), and finally an antistatic polypropylene composition B is obtained. i Granules (i.e. x i +y=B i , i = 1, 2, 3), after testing, B 1 The melting point of B is 127℃. 2 The melting point of B is 132°C. 3 The melting point is 138°C.
[0311] (3) Preparation of three-layer co-extruded antistatic polypropylene sheet:
[0312] The antistatic polypropylene composition A prepared in the above steps (1) and (2) i And antistatic polypropylene composition B iThe pellets are dried and then the antistatic polypropylene composition A is i Add the antistatic polypropylene composition B into the core layer extruder of the multi-layer extrusion calendering. i Add the pellets to the upper and lower surface extruders of the multi-layer extrusion casting machine. After the pellets are co-extruded and compounded through the extruder die, they pass through the calendering roller and the traction roller in sequence, and then undergo solid phase stretching, trimming and winding to obtain sheet B. 1 AB 1 , B 2 AB 2 , B 3 AB 3 The temperature of the extrusion casting was 230°C, and the temperature of the calendering roller was 58°C. The temperature during the solid phase stretching process was 140°C, the stretching rate was 2m / min, and the stretching ratio was 7 times.
[0313] The antistatic composite film (polypropylene sheet) made by stretching and rolling is composed of an upper surface layer (outer film B i ), core layer (film A) and lower surface layer (outer film B i The thickness of the antistatic composite film is 80 μm, wherein the thickness of the film layer A accounts for 80% of the total thickness of the sheet.
[0314] (4) Preparation of antistatic polypropylene fabric:
[0315] The three-layer co-extruded antistatic polypropylene sheet obtained in the above step (3) is cut by a high-speed slitting machine with multiple blades to obtain an oriented polypropylene flat ribbon with a width of 3 mm; the oriented flat ribbon is woven by a commercial weaving machine according to the designed fabric structure to obtain a plain weave antistatic polypropylene fabric B 1 AB 1 , B 2 AB 2 , B 3 AB 3 .
[0316] (5) Preparation of antistatic polypropylene composite materials:
[0317] The antistatic polypropylene fabrics prepared in step (4) are stacked in order, from bottom to top: B 3 A 3 B 3 , B 2 A 2 B 2 , B 1 A 1 B 1 , B 2 A 2 B 2 , B 3 A 3 B3 The total number of layers is 5, and the laminated polypropylene fabric is hot-pressed and fused, and then cooled and shaped to form an antistatic polypropylene composite material. The polypropylene fabric is placed at 90 degrees between the warp and the warp. The hot pressing conditions are: temperature 145°C, hot pressing pressure 5MPa, preheating time 90s, hot pressing time 90s, and cooling time 300s. The thickness of the prepared polypropylene composite material is 391μm.
[0318] Example 16
[0319] This example is used to illustrate the preparation of the antistatic polypropylene composition, the three-layer co-extruded antistatic polypropylene sheet, the antistatic polypropylene fabric, and the antistatic polypropylene composite material provided by the present invention.
[0320] (1) Antistatic Polypropylene Composition A i Preparation:
[0321] The preparation process is the same as step (1) of Example 3.
[0322] (2) Antistatic Polypropylene Composition B i Preparation:
[0323] The main preparation process is the same as step (2) of Example 3. The difference is that component B i and x i The materials are as follows:
[0324] Component x 1 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 110°C; component x 2 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 115°C; component x 3 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 120°C; component x 4 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 125°C; component x 5 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 130°C; component x 6 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 135°C; component x 7 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C; component x 8It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 145°C; component x 9 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 150°C; 1 -x 9 The melt flow rate is 1-20g / 10min.
[0325] Finally, the antistatic polypropylene composition B is obtained. i Granules (i.e. x i +y=B i , i = 1, 2, 3, 4, 5, 6, 7, 8, 9), after testing, B 1 The melting point of B is 110℃. 2 The melting point of B is 113℃. 3 The melting point of B is 117℃. 4 The melting point of B is 123℃. 5 The melting point of B is 127℃. 6 The melting point of B is 133°C. 7 The melting point of B is 137℃. 8 The melting point of B is 142°C. 9 The melting point is 148°C.
[0326] (3) Preparation of three-layer co-extruded antistatic polypropylene sheet:
[0327] The preparation process is the same as step (3) of Example 3.
[0328] (4) Preparation of antistatic polypropylene fabric:
[0329] The preparation process is the same as step (4) of Example 3.
[0330] (5) Preparation of antistatic polypropylene composite materials:
[0331] The antistatic polypropylene fabrics prepared in step (4) are stacked in order, from bottom to top: B 9 A 9 B 9… B 3 A 3 B 3 , B 2 A 2 B 2 , B 1 A 1 B 1 , B 2 A 2 B 2 , B 3 A 3 B3 , …B 9 A 9 B 9 The total number of stacked layers is 17, and the laminated polypropylene fabric is hot-pressed and fused, and then cooled and shaped to form an antistatic polypropylene composite material. The polypropylene fabric is placed at 90 degrees between the warp and the warp. The hot pressing conditions used are: temperature 150°C, hot pressing pressure 5MPa, preheating time 300s, hot pressing time 180s, and cooling time 600s. The thickness of the prepared polypropylene composite material is 1.25mm.
[0332] Comparative Example 1
[0333] A three-layer co-extruded antistatic polypropylene sheet was prepared according to the method of Example 1, except that only the antistatic polypropylene composition A was used for extrusion casting into a single-layer film with a thickness of 81 μm. An antistatic polypropylene fabric and an antistatic polypropylene composite material were prepared according to the method of Example 1.
[0334] The thickness of the prepared antistatic polypropylene composite material is close to that of Example 1.
[0335] Comparative Example 2
[0336] A three-layer co-extruded antistatic polypropylene sheet was prepared according to the method of Example 1, except that only the antistatic polypropylene composition B was used for extrusion casting into a single-layer film with a thickness of 79 μm. An antistatic polypropylene fabric and an antistatic polypropylene composite material were prepared according to the method of Example 1.
[0337] The thickness of the prepared antistatic polypropylene composite material is close to that of Example 1.
[0338] Comparative Example 3
[0339] A three-layer co-extruded antistatic polypropylene sheet was prepared according to the method of Example 1, except that the antistatic polypropylene composition A contained only component b. Antistatic polypropylene fabrics, antistatic polypropylene composite materials were prepared according to the method of Example 1.
[0340] The thickness of the prepared antistatic polypropylene composite material is close to that of Example 1.
[0341] Comparative Example 4
[0342] A three-layer co-extruded antistatic polypropylene sheet was prepared according to the method of Example 1, except that the antistatic polypropylene composition B contained only component y. An antistatic polypropylene fabric and an antistatic polypropylene composite material were prepared according to the method of Example 1.
[0343] The thickness of the prepared antistatic polypropylene composite material is close to that of Example 1.
[0344] Comparative Example 5
[0345] A three-layer co-extruded antistatic polypropylene sheet was prepared according to the method of Example 1, and the thickness of the film layer A accounted for 95% of the total thickness of the sheet. An antistatic polypropylene fabric and a polypropylene antistatic composite material were prepared according to the method of Example 1.
[0346] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0347] Comparative Example 6
[0348] A three-layer co-extruded antistatic polypropylene sheet was prepared according to the method of Example 1, and the thickness of the antistatic film layer A accounted for 50% of the total thickness of the sheet. An antistatic polypropylene fabric and an antistatic polypropylene composite material were prepared according to the method of Example 1.
[0349] The thickness of the prepared antistatic polypropylene composite material is close to that of Example 1.
[0350] Comparative Example 7
[0351] The coextruded antistatic polypropylene sheet was prepared according to the method of Example 15, except that component Bi was selected in the following manner: component x 1 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C; component x 2 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 135°C; component x 3 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 130°C; component x 1 -x 3 The melt flow rate is 2-10g / 10min.
[0352] Finally, the antistatic polypropylene composition B is obtained. i Granules (i.e. x i +y=B i , i = 1, 2, 3), after testing, B 1 The melting point of B is 138℃. 2 The melting point of B is 132°C. 3 The melting point is 127° C. According to the method of Example 15, antistatic polypropylene fabric and antistatic polypropylene composite material were prepared.
[0353] The thickness of the prepared polypropylene composite material is close to that of Example 15.
[0354] Comparative Example 8
[0355] A three-layer co-extruded antistatic polypropylene sheet was prepared according to the method of Example 1. An antistatic polypropylene fabric was prepared according to the method of Example 1. The main steps for preparing the antistatic polypropylene composite material were the same as those of Example 1. The only difference was that the hot pressing temperature was 110° C., the hot pressing pressure was 12 MPa, the preheating time was 300 s, the hot pressing time was 300 s, and the cooling time was 700 s. The thickness of the prepared polypropylene composite material was 1.50 mm.
[0356] Comparative Example 9
[0357] A three-layer co-extruded antistatic polypropylene sheet was prepared according to the method of Example 1. An antistatic polypropylene fabric was prepared according to the method of Example 1. The main steps for preparing the antistatic polypropylene composite material were the same as those of Example 1. The only difference was that the hot pressing temperature was 175°C, the hot pressing pressure was 2MPa, the preheating time was 300s, the hot pressing time was 300s, and the cooling time was 700s. The thickness of the prepared antistatic polypropylene composite material was 1.57mm.
[0358] Comparative Example 10
[0359] A three-layer co-extruded polypropylene sheet was prepared according to the method of Example 1, except that no conductive filler was added. A polypropylene fabric and a polypropylene composite material were prepared according to the method of Example 1.
[0360] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0361] Experimental example
[0362] The polypropylene composite materials obtained in the above examples and comparative examples were tested according to the following method. The test results are shown in Table 1.
[0363] (1) Tensile strength: Prepare samples and measure them according to the method specified in GB / T1040.1-2018;
[0364] (2) Interlayer peel strength: Sample preparation and measurement shall be carried out according to the method specified in QB / T2358-98.
[0365] (3) Drop weight impact strength: measured according to the method specified in GB / T14153-1993.
[0366] (4) Volume resistivity: measured using a Keithley 6517B Electrometer.
[0367] Among them, when the polypropylene composite materials obtained in the corresponding embodiments and comparative examples are close to that in Example 1, the thicknesses are all around 1.6 mm, and are all within the range of 1.6 mm±1 mm.
[0368] Table 1
[0369]
[0370] From the results of the examples in Table 1, it can be concluded that the antistatic polypropylene composite material prepared according to the present invention has good tensile properties, impact resistance and electrical properties, and has good interlayer peel strength at a relatively low hot pressing temperature. The antistatic polypropylene composite sheet of the present invention has a longitudinal (MD) tensile strength of ≥160MPa, an interlayer peel strength of ≥1.10N / mm, and a volume resistivity of less than 10 7 Ω·m; The antistatic polypropylene composite material is composed of 24 layers of antistatic polypropylene fabrics, and the thickness is about 1.6mm, and the surface density is 1520g / m 2 The drop hammer impact strength is ≥226 J. The antistatic polypropylene composite material with a melting point gradient structure of the present invention has a longitudinal (MD) tensile strength of ≥160 MPa, an interlayer peel strength of ≥1.3 N / mm, and a volume resistivity of less than 10 7 Ω·m; when the composite material is only composed of 5 layers of polypropylene fabrics hot pressed together and the thickness is only about 391μm, the drop hammer impact strength is ≥42J.
[0371] It can be seen from the preferred embodiments 1-3 that the antistatic polypropylene composite material prepared by the present invention has a longitudinal (MD) tensile strength of ≥170 MPa, an interlayer peel strength of ≥1.2 N / mm, and a volume resistivity of less than 10 7 Ω·m; The antistatic polypropylene composite material is composed of 24 layers of antistatic polypropylene fabrics, and the thickness is about 1.6mm, and the surface density is 1520g / m 2 When it is about 200mm, the drop weight impact strength is ≥240J.
[0372] It can be seen from the preferred embodiments 15-16 that the antistatic polypropylene composite material with a melting point gradient structure prepared by the present invention has a longitudinal (MD) tensile strength of ≥180 MPa, an interlayer peel strength of ≥1.5 N / mm, and a volume resistivity of less than 10 7 Ω·m; when the composite material is only composed of 5 layers of antistatic polypropylene fabrics hot pressed together and is only about 391μm, the drop hammer impact strength is ≥45J.
[0373] It can be seen from Comparative Examples 1-9 that only using a single-layer sheet structure or using an interlayer ratio outside the scope of the embodiment will lead to a decrease in the performance of the laminated antistatic polypropylene sheet or fabric, and using process conditions outside the scope of the embodiment will greatly reduce the tensile strength, impact properties or interlayer peeling strength of the obtained antistatic polypropylene composite material.
[0374] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
[0375] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A polypropylene sheet, comprising a layer A and layers B and B' located on both sides of the layer A, with a structure of BAB'; Wherein layer A contains a polypropylene composition A and a conductive filler, layer B and layer B' are the same or different, each containing a conductive filler and each correspondingly containing a polypropylene composition B and a polypropylene composition B', and the melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B'; The polypropylene composition A comprises homopolypropylene a and impact copolymer polypropylene b; the polypropylene composition B and the polypropylene composition B' each comprise random copolymer polypropylene x and thermal bonding enhancer y.
2. The polypropylene sheet according to claim 1, characterized in that: Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-99wt% of homopolypropylene a and 1-50wt% of impact copolymer polypropylene b; preferably, the polypropylene composition A comprises 70-90wt% of homopolypropylene a and 10-30wt% of impact copolymer polypropylene b; and / or, Relative to 100 parts by weight of the polypropylene composition A, the content of the conductive filler in layer A is 0.1-10 parts by weight, preferably 1-3 parts by weight; and / or, Based on the total weight of the polypropylene composition B and the polypropylene composition B', the polypropylene composition B and the polypropylene composition B' each comprise 70-99 wt% of random copolymerized polypropylene x and 1-30 wt% of thermal bonding enhancer y; preferably, the polypropylene composition B and the polypropylene composition B' each comprise 80-90 wt% of random copolymerized polypropylene x and 10-20 wt% of thermal bonding enhancer y; and / or, The content of the conductive filler in the layer B and the layer B' is 0.1-10 parts by weight, preferably 1-3 parts by weight, respectively, based on 100 parts by weight of the polypropylene composition B and the polypropylene composition B'.
3. The polypropylene sheet according to claim 1, characterized in that: Based on the total thickness of the polypropylene sheet, the thickness of layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%.
4. The polypropylene sheet according to claim 1, characterized in that: The homopolymer polypropylene a has: The melting point is 150-170°C, preferably 160-170°C; and / or, The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or, The isotacticity (mm) is not less than 96%.
5. The polypropylene sheet according to claim 1, characterized in that: The melting point of the impact-resistant copolymer polypropylene b is 150-170° C.: and / or, The monomer of the impact copolymer polypropylene b and propylene copolymer is ethylene or butene, preferably butene; and / or, The impact copolymer polypropylene b has a melt flow rate of 0.5-50 g / 10 min at 230° C. and a load of 2.16 kg, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or, The cantilever beam impact strength of the impact-resistant copolymer polypropylene b is not less than 20KJ / m 2 .
6. The polypropylene sheet according to claim 1, characterized in that: The random copolymer polypropylene x has: The melting point is 110-150°C, preferably 120-140°C; and / or, The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 3-18 g / 10 min; and / or, It is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene binary copolymer.
7. The polypropylene sheet according to claim 1, characterized in that: The thermal bonding enhancer y has: The melting point or viscosity flow temperature is 70-110°C; and / or, The melt flow rate at 190°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 1-18 g / 10 min; and / or, One or more selected from polyolefin elastomer, EPDM rubber, SEBS, SBS, EVA, petroleum resin; preferably, polyolefin elastomer and / or petroleum resin; preferably, The polyolefin elastomer is a copolymer elastomer of ethylene and propylene and / or alpha olefin, wherein the alpha olefin is preferably a C4-C12 alpha olefin, more preferably 1-butene and / or 1-octene; and / or, The petroleum resin is a C5 and / or C9 hydrogenated petroleum resin with a softening point of 100-150° C. and is preferably a cyclopentadiene type resin.
8. The polypropylene sheet according to any one of claims 1 to 7, characterized in that: The layer A also contains a β-crystalline nucleating agent; preferably, The β-crystal nucleating agent is at least one selected from the group consisting of condensed aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates; and / or, Relative to 100 parts by weight of the polypropylene composition A, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight.
9. The polypropylene sheet according to any one of claims 1 to 7, characterized in that: The conductive filler is selected from at least one of carbon black conductive fillers, graphite conductive fillers, carbon nanotube conductive fillers, carbon fiber conductive fillers, conductive metal particles, conductive metal fibers, fillers coated with conductive metals, and metal oxides; preferably, The carbon black conductive filler is at least one of acetylene black, superconducting carbon black and special conductive carbon black; and / or, the graphite conductive filler is at least one of natural graphite, expandable graphite, expanded graphite and graphene; and / or, the carbon nanotube conductive filler is at least one of the following carbon nanotubes that are not surface-modified or surface-modified: single-walled carbon nanotubes and / or multi-walled carbon nanotubes; and / or, the conductive metals in the conductive metal particles and conductive metal fibers are each independently at least one of silver, aluminum, copper, iron, nickel and stainless steel; and / or, the filler coated with conductive metal is selected from at least one of the following materials plated with lead, nickel and silver: glass balls, glass fibers and mica sheets; and / or, the metal oxide is at least one of titanium oxide, zinc oxide, tin oxide, indium oxide and cadmium oxide.
10. The polypropylene sheet according to any one of claims 1 to 7, characterized in that: The melting point of the homopolymer polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymer polypropylene x in the polypropylene composition B and the polypropylene composition B', and the temperature difference of the corresponding melting points is preferably greater than or equal to 10 degrees; and / or, The BAB' sheet structure of the polypropylene sheet is obtained by coextruding a layer A raw material comprising a polypropylene composition A and a conductive filler, a layer B raw material comprising a polypropylene composition B and a conductive filler, and a layer B' raw material comprising a polypropylene composition B' and a conductive filler.
11. The method for preparing the polypropylene sheet according to any one of claims 1 to 10, comprising co-extruding, casting or calendering, and stretching a layer A raw material comprising a polypropylene composition A and a conductive filler, a layer B raw material comprising a polypropylene composition B and a conductive filler, and a layer B' raw material comprising a polypropylene composition B' and a conductive filler in a BAB' structure to obtain the polypropylene sheet.
12. The method for preparing a polypropylene sheet according to claim 11, characterized in that: The preparation of the raw material of layer A comprises melt blending the components including the homopolypropylene a, the impact copolymer polypropylene b and the conductive filler; and / or, The preparation of the raw materials of the layer B and the layer B' comprises melt blending the components including the random copolymer polypropylene x, the thermal bonding enhancer y and the conductive filler; and / or, The co-extrusion and casting temperatures are independently selected from 200-240° C.; and / or, The calendering temperature is 50-70°C; and / or, The stretching conditions include: the stretching temperature is 90-165° C., preferably 90-140° C., and more preferably 90-119° C.; and the stretching ratio is 1-20 times.
13. A polypropylene fabric, a three-dimensional polypropylene fabric obtained by weaving the polypropylene sheet according to any one of claims 1 to 10; Preferably, the polypropylene fabric is obtained by slitting and weaving the polypropylene sheet; and / or the polypropylene fabric has a three-dimensional structure of plain, twill and / or satin.
14. A polypropylene composite material, wherein the polypropylene composite material is prepared by thermally pressing multiple layers of the polypropylene sheet according to any one of claims 1 to 10 and / or the polypropylene fabric according to claim 13; preferably, The polypropylene composite material is prepared by thermally pressing multiple layers of the polypropylene sheets or the polypropylene fabric; and / or, The multi-layer polypropylene sheets are stacked from top to bottom in the direction of 0-90° along their respective machine directions; and / or, The multi-layer polypropylene fabric is stacked from top to bottom with the warp direction being 0-90° to the warp direction; and / or, The number of layers of the multi-layer polypropylene sheet and / or the multi-layer polypropylene fabric is greater than or equal to 2 layers, more preferably 2-200 layers, and most preferably 4-100 layers.
15. The polypropylene composite material according to claim 14, characterized in that: The polypropylene composite material comprises a plurality of polypropylene sheet unit groups stacked in sequence; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, and each polypropylene sheet unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B i A i B' i The structure of the polypropylene composite material is, from bottom to top, the nth group... the ith group... the second group, the first group, the second group... the ith group... the nth group, and the total number of stacked groups of polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n; Among them, the core layer A in the polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition B i , polypropylene composition B' i , The polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than the average melting point of all outer layers in the i-1-th group; preferably, Polypropylene composition A i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points of each is greater than or equal to 5°C, preferably greater than or equal to 10°C, more preferably greater than or equal to 20°C; and / or, The difference between the average melting point of all outer layers in the i-th group and the average melting point of all outer layers in the i-1th group is the same or different, and is 1-40°C, preferably 1-10°C, more preferably 1-5°C; and / or, 2≤n≤100, preferably, 2≤n≤50; and / or, Each group of polypropylene ply units, independently of one another, comprises 1 to 10, preferably 1 to 5, identical or different polypropylene ply units.
16. The method for preparing the polypropylene composite material according to claim 14 or 15, comprising laminating and hot-pressing the polypropylene sheet and / or the polypropylene fabric, and then cooling and shaping to prepare the polypropylene composite material; preferably, The temperature of the hot pressing fusion is 115-170°C, preferably 115-159°C, and more preferably 140-159°C; and / or, The pressure of the hot pressing fusion is 2-10 MPa; and / or, The preheating time of the hot pressing fusion is 5-600s, and the hot pressing time is 1-600s, preferably 10-500s; and / or, The cooling and shaping pressure is 2-8 MPa, and the cooling and shaping time is 30-700 s; and / or, The number of layers of the polypropylene sheet and / or the polypropylene fabric laminate is greater than or equal to 2 layers, preferably 2-200 layers; more preferably 4-100 layers; and / or, Adjacent layers of the polypropylene fabric laminate are placed at an angle of 0-90° between the warp direction; and / or, Adjacent layers of the polypropylene sheet stack are placed at 0-90 degrees along their respective machine directions.
17. Use of the polypropylene sheet according to any one of claims 1 to 10, the polypropylene fabric according to claim 13, the polypropylene composite material according to claim 14 or 15, and the polypropylene composite material prepared by the preparation method according to claim 16 in the fields of sports protection, automobile manufacturing, military materials and consumer products.
Citation Information
Patent Citations
Antistatic polypropylene composite film as well as preparation method and application thereof
CN115991030A
Polypropylene composite film as well as preparation method and application thereof
CN115991031A
Low-haze high-impact heat-sealing polypropylene composite film as well as preparation method and application thereof
CN115991039A
Heat-conducting high-strength polypropylene composite sheet, fabric of heat-conducting high-strength polypropylene composite sheet, polypropylene composite and preparation method and application of polypropylene composite
CN118849574A
Conductive high-strength polypropylene sheet and fabric thereof, polypropylene composite material and preparation method and application thereof
CN118849575A
Cited By
Conductive high-strength polypropylene sheet and fabric thereof, polypropylene composite material and preparation method and application thereof
CN118849575A
Electrically conductive high-strength polypropylene sheet and fabric thereof, polypropylene composite material and its manufacturing method and application