Friction self-powered flexible force sensor based on conductive ionic gel
Through a friction nanogenerator based on conductive ion gel, combining friction activation and electrostatic induction, self-power supply of flexible force sensing sensors is achieved, solving the balance of conductivity and mechanical properties, and improving the output performance and adaptability of the sensor. Suitable for flexible robotics applications.
Patent Information
- Application Number
- CN202411060877.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-05
AI Technical Summary
Existing flexible force sensing sensors are difficult to balance between high mechanical properties and conductivity, and require continuous power supply, limiting their application and development.
Using a friction nanogenerator based on conductive ionic gel, a friction self-powered flexible force sensing sensor with good tensile and electrical conductivity is prepared by combining ionic liquid gel and silicone rubber, and the coupling of frictional activation and electrostatic induction is used. The effect realizes self-powered.
The flexible electrode with high conductivity, tensile and electrochemical stability is achieved, which simplifies the sensor structure, reduces moisture loss, improves output performance, can accurately measure force perception, and is suitable for the application of flexible robots.
Smart Images

Figure CN118984074A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of flexible sensors, and in particular to a friction self-powered flexible force sensing sensor based on conductive ion gel. Background Art
[0002] Force sensors made of flexible and extensible materials can provide safer and more robust human-machine interaction, bridging the gap between machines and humans. High-precision flexible and stretchable force sensors are essential for realizing force feedback for electronic skin and wearable devices. At present, flexible pressure sensors mainly include capacitive, resistive, piezoelectric and triboelectric. Capacitive sensors are suitable for measuring pressure changes in a small range, resistive sensors are simple, durable and low-cost, and piezoelectric sensors are suitable for high-precision pressure measurement; sensors often have large deformations, and even thin-film sensors with simple structures and small volumes cannot withstand large deformations during application, and data accuracy cannot be guaranteed under bending; in addition, existing sensors require continuous power supply. Triboelectric sensors have simple structures and a wide range of material choices, which can better adapt to the needs of flexible structures. At the same time, triboelectric sensors can realize self-powered sensors. These characteristics make triboelectric sensors an ideal choice for flexible sensors.
[0003] The flexible friction layer based on friction-based flexible sensors can be made of flexible materials such as polydimethylsiloxane (PDMS), polyurethane (PU) and silicone rubber. However, the electrodes of TENG (Triboelectric nanogenerator) are usually made of metal materials that lack stretchability, such as silver, gold or copper, which greatly limits the application and development of stretchable TENG. Electrodes with high mechanical properties and conductivity are the core of flexible TENG, and liquid metal, graphene, carbon nanotubes, conductive fibers and hydrogels are considered to be suitable materials. However, liquid metal is not safe enough for use in the field of fresh food; the high cost and irreversible damage of graphene and carbon nanotubes limit their development. But there are still few examples of using hydrogels, especially ionic liquid gels, as TENG electrodes.
[0004] Good mechanical properties and high conductivity are prerequisites for ion gels to be used as flexible electrodes. The patent "CN115466355B A multifunctional conductive ion gel, preparation method and application thereof" introduces a method for preparing ion gels by ionizing radiation technology, and its ion conductivity reaches 4.9ms / cm; when the maximum strain is 546%, the tensile strength level is low, about 50Kpa; when the tensile strength is increased to 225Kpa, the tensile strain is reduced to less than 275%. The patent "CN115028769A A super-stretchable conductive ion gel and its preparation method and application" introduces a method for preparing a super-stretchable conductive ion gel. Although the prepared ion gel has certain stretchability and tensile strength, its conductivity is only 2.02ms / cm. It can be seen that designing ion gels with excellent comprehensive performance as flexible electrodes to achieve a balance between high conductivity and good mechanical strength is still a huge challenge. Summary of the invention
[0005] In view of the above-mentioned prior art, the purpose of the present invention is to provide a friction self-powered flexible force sensing sensor based on conductive ion gel. The flexible force sensing self-powered sensor has good stretchability and sensitivity, overcomes the conflict between conductivity and mechanical properties, has a mapping relationship between pressure value and sensor output voltage, and can realize force sensing through self-power supply.
[0006] To achieve the above object, the present invention adopts the following technical solution:
[0007] In a first aspect of the present invention, a friction nanogenerator is provided, the friction nanogenerator comprising an ionic liquid gel, silicone rubber attached to opposite sides of the ionic liquid gel, and a wire connecting the ionic liquid gel and the silicone rubber, wherein the silicone rubber is Ecoflex silicone rubber; the ionic liquid gel is made of the following raw materials: an ionic liquid, a monomer, a photoinitiator, and a crosslinking agent;
[0008] The ionic liquid is 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, the monomer is selected from at least one of N,N-dimethylacrylamide or acrylamide; the photoinitiator is initiator 1173, and the crosslinker is methylenebisacrylamide;
[0009] The mass ratio of the ionic liquid, the monomer, the photoinitiator and the cross-linking agent is (1-10):1:(0.0001-0.05):(0.0001-0.05).
[0010] The second aspect of the present invention provides a method for preparing the triboelectric nanogenerator, comprising the following steps:
[0011] (1) mixing an ionic liquid, a monomer, a photoinitiator and a cross-linking agent, heating and stirring to obtain a precursor solution, and subjecting the precursor solution to ultraviolet light reaction to obtain an ionic liquid gel;
[0012] (2) Prepare silicone rubber, connect wires to the silicone rubber, and sandwich the ionic liquid gel between two pieces of silicone rubber to obtain a friction nanogenerator.
[0013] Furthermore, the mass ratio of the ionic liquid to the monomer is (5-8):1, and the sum of the mass of the photoinitiator and the cross-linking agent accounts for (0.1-5)% of the mass of the monomer.
[0014] Furthermore, in step (1), in the monomers, the mass ratio of N,N-dimethylacrylamide to acrylamide is (1-10):1.
[0015] Furthermore, in step (1), the heating and stirring temperature is 90-130° C., the stirring speed is 400-1500 rpm, and the stirring time is 1-10 min.
[0016] Furthermore, in step (1), the wavelength of ultraviolet light used is 365 nm, and the irradiation time is 5-30 min.
[0017] Furthermore, in step (2), the ionic liquid gel and the two pieces of silicone rubber are clamped by van der Waals force.
[0018] Furthermore, in step (2), after the ionic liquid gel is sandwiched between two pieces of silicone rubber, Ecoflex-00-30 silicone rubber is used to connect the junction of the ionic liquid gel and the Ecoflex silicone rubber, and heated and cured at a temperature of 90-110° C. for 0.5-5 min.
[0019] A third aspect of the present invention provides a friction self-powered flexible force sensing sensor based on conductive ion gel, wherein the friction self-powered flexible force sensing sensor includes the friction nanogenerator.
[0020] The fourth aspect of the present invention provides the application of the friction self-powered flexible force sensing sensor based on conductive ion gel in the manufacture of flexible manipulators.
[0021] Beneficial effects of the present invention:
[0022] (1) The flexible conductive ion gel provided by the present invention is prepared by a one-pot method, which has a simple preparation process and low production cost. It has good conductivity, stretchability and electrochemical stability and is a flexible electrode with excellent performance.
[0023] (2) The self-powered flexible force sensing sensor provided by the present invention adopts a sandwich structure, simplifies the internal structure of the sensor, and effectively reduces its water loss by completely wrapping the hydrogel film, preventing the external environment from affecting the gel inside the sensor, and has good environmental adaptability. The sensor has excellent tensile performance, can be modularly connected in series, improve output performance, and realize energy self-supply of the sensor through the coupling effect of electrostatic induction and friction electrification.
[0024] (3) The self-powered flexible force sensing sensor provided by the present invention has good stability, durability and hydrophobicity, wherein the silicone rubber used as the friction layer and the encapsulation layer is beneficial to protecting the flexible electrode and enhancing the output performance of the sensor, and the conductive ion gel plays a conductive role. The self-powered flexible force sensing sensor provided by the present invention has good output performance, and has a mapping relationship between the pressure value and the output voltage of the sensor, and can accurately measure the force received by the flexible hand contact surface. The prepared flexible sensor can be stretched, twisted and bent. The self-powered flexible force sensing sensor can be flexibly attached to the surface of the manipulator without damaging the fruit, and can realize real-time and dynamic monitoring of the clamping force, which is helpful to realize the mechanization and intelligent harvesting of fruits and vegetables. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Flow chart for the preparation of conductive ion gel;
[0026] Figure 2 This is the structural diagram of the flexible force sensing self-powered sensor;
[0027] Figure 3 This is a working principle diagram of a sensor based on a single-electrode friction nanogenerator;
[0028] Figure 4 This is a physical picture of the flexible force sensing self-powered sensor of the present invention;
[0029] Figure 5 are the tensile stress curves of Examples 1-4 of the present invention;
[0030] Figure 6 It is a line graph of resistivity and conductivity of Examples 1-4 of the present invention;
[0031] Figure 7 This is a comparison diagram of the output voltages of the triboelectric nanogenerators prepared in Examples 1-4 of the present invention;
[0032] Figure 8 This is a fitting diagram of output voltages at different pressures according to Example 3 of the present invention;
[0033] Fig. 9 This is an anti-fatigue test diagram of Example 3 of the present invention. DETAILED DESCRIPTION
[0034] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0035] In order to enable those skilled in the art to more clearly understand the technical solution of the present application, the technical solution of the present application will be described in detail below in conjunction with specific embodiments.
[0036] The experimental materials used in the examples of the present invention but not specifically described are all conventional experimental materials in the art and can be purchased through commercial channels.
[0037] It is often difficult to satisfy both the mechanical properties and the conductive properties of ionic liquid gels at the same time. In the formulation of ionic gels, the ratio of ionic liquid to monomer often faces a contradiction between conductivity and stretchability. When a large amount of ionic liquid is added to improve the conductive properties, an excessively high ionic liquid content will cause the mechanical strength and tensile properties of the gel to decrease significantly, and the gel will become too soft and easy to break, making it difficult to meet the mechanical requirements in practical applications; and if the proportion of monomers is increased to enhance the mechanical properties and tensile properties, the insufficient ionic liquid content in the gel will affect the formation of ion conduction channels and reduce the conductive properties of the material. Therefore, it is of great significance to obtain an ionic liquid gel that has efficient conductive properties while ensuring excellent mechanical properties, which led to the present invention.
[0038] Example 1
[0039] The preparation method of ion gel TENG can be found in Figure 1 , Figure 2 , specifically including the following steps:
[0040] (1) 2.40 g of ionic liquid BMIMTF2N (1-Butyl-3-methylimidazolium bis(trifluoromethylsulf onyl)imide) was added to a glass container, and 0.384 g of monomer DMAA (N,N-Dimethylacrylamide) and 0.096 g of monomer AM (Acryla mide), photoinitiator 1173 and crosslinker MBAA (N,N'-methylenediacrylamide) were added in sequence to obtain a precursor solution. The mass of photoinitiator 1173 and crosslinker MBAA was 1 wt% of the total monomer mass. Both were stirred in a constant temperature magnetic stirrer at 110°C and 800 rpm for 5 min until completely dissolved and then added. The mass ratio of ionic liquid to total monomers (monomer DMAA and monomer AM) was 5:1.
[0041] (2) The uniform and transparent precursor solution was immediately transferred to a mold and cooled to room temperature, and then initiated under 365 nm ultraviolet light for 15 min to finally obtain an ionic liquid gel.
[0042] (3) Silicone rubber solution A and B (Ecoflex-00-30) were mixed in a mass ratio of 1:1 and poured into a polytetrafluoroethylene mold with a hollow structure. The bubbles were removed by vacuum in an electric constant temperature blast drying oven, and after curing at 65°C for 2 hours, the silicone rubber (20 mm × 4 mm) was demolded from the polytetrafluoroethylene mold. The above process was repeated to obtain two pieces of Ecoflex silicone rubber of the same size.
[0043] (4) The previously prepared ion gel was cut into pieces with a size of 15 mm × 20 mm × 2 mm and placed in the groove of the Ecoflex layer. A copper wire was connected to the surface of the ion gel. Another piece of the same silicone rubber was taken. The two silicone rubbers sandwiched the gel in the middle, encapsulated the hydrogel, and squeezed out the air to achieve close adhesion between the materials through van der Waals forces. In order to ensure the airtightness of the device, a small amount of Ecoflex-00-30 silicone rubber was used to bond the joints of the two relative silicone rubbers, and then heated and cured at 100 ° C for 1 min by a hot air gun to obtain an ion gel-based TENG with a thickness range of 4 mm.
[0044] Example 2
[0045] The preparation method of ion gel TENG specifically includes the following steps:
[0046] (1) Take 2.88g of ionic liquid BMIMTF2N and add it to a glass container, then add 0.384g of monomer DMAA and 0.096g of monomer AM, photoinitiator 1173 and crosslinker MBAA in sequence to obtain a precursor solution. The mass of photoinitiator 1173 and crosslinker MBAA is 1wt% of the total monomer mass. Both are stirred in a constant temperature magnetic stirrer at 110°C and 800 rpm for 5 min until completely dissolved and then added. The mass ratio of ionic liquid to total monomers (monomer DMAA and monomer AM) is 6:1.
[0047] (2) The uniform and transparent precursor solution was immediately transferred to a mold and cooled to room temperature, and then initiated under 365 nm ultraviolet light for 15 min to finally obtain an ionic liquid gel.
[0048] (3) Silicone rubber solution A and B (Ecoflex-00-30) were mixed in a mass ratio of 1:1 and poured into a polytetrafluoroethylene mold with a hollow structure. The bubbles were removed by vacuum in an electric constant temperature blast drying oven and cured at 65°C for 2 hours. The silicone rubber (2 mm × 4 mm) was demolded from the polytetrafluoroethylene mold and the above process was repeated to obtain two pieces of Ecoflex silicone rubber of the same size.
[0049] (4) The previously prepared ion gel was cut into pieces with a size of 15 mm × 20 mm × 2 mm and placed in the groove of the Ecoflex layer. A copper wire was connected to the surface of the ion gel. Another piece of the same silicone rubber was taken. The two silicone rubbers sandwiched the gel in the middle, encapsulated the hydrogel, and squeezed out the air to achieve close adhesion between the materials through van der Waals forces. In order to ensure the airtightness of the device, a small amount of Ecoflex-00-30 silicone rubber was used to bond the joints of the two relative silicone rubbers, and then heated and cured at 100 ° C for 1 min by a hot air gun to obtain an ion gel-based TENG with a thickness range of 4 mm.
[0050] Example 3
[0051] The preparation method of ion gel TENG specifically includes the following steps:
[0052] (1) 3.36 g of ionic liquid BMIMTF2N was added to a glass container, and 0.384 g of monomer DMAA and 0.096 g of monomer AM, photoinitiator 1173 and crosslinker MBAA were added in sequence to obtain a precursor solution. The mass of photoinitiator 1173 and crosslinker MBAA was 1 wt % of the total monomer mass. Both were stirred in a constant temperature magnetic stirrer at 110°C and 800 rpm for 5 min until completely dissolved and then added. The mass ratio of ionic liquid to total monomers (monomer DMAA and monomer AM) was 7:1.
[0053] (2) The uniform and transparent precursor solution was immediately transferred to a mold and cooled to room temperature, and then initiated under 365 nm ultraviolet light for 15 min to finally obtain an ionic liquid gel.
[0054] (3) Silicone rubber solution A and B (Ecoflex-00-30) were mixed in a mass ratio of 1:1 and poured into a polytetrafluoroethylene mold with a hollow structure. The bubbles were removed by vacuum in an electric constant temperature blast drying oven and cured at 65°C for 2 hours. The silicone rubber (2 mm × 4 mm) was demolded from the polytetrafluoroethylene mold and the above process was repeated to obtain two pieces of Ecoflex silicone rubber of the same size.
[0055] (4) The previously prepared ion gel was cut into pieces with a size of 15 mm × 20 mm × 2 mm and placed in the groove of the Ecoflex layer. A copper wire was connected to the surface of the ion gel. Another piece of the same silicone rubber was taken. The two silicone rubbers sandwiched the gel in the middle, encapsulated the hydrogel, and squeezed out the air to achieve close adhesion between the materials through van der Waals forces. In order to ensure the airtightness of the device, a small amount of Ecoflex-00-30 silicone rubber was used to bond the joints of the two relative silicone rubbers, and then heated and cured at 100 ° C for 1 min by a hot air gun to obtain an ion gel-based TENG with a thickness range of 4 mm.
[0056] Example 4
[0057] The preparation method of ion gel TENG specifically includes the following steps:
[0058] (1) 3.84 g of ionic liquid BMIMTF2N was added to a glass container, and 0.384 g of monomer DMAA and 0.096 g of monomer AM, photoinitiator 1173 and crosslinker MBAA were added in sequence to obtain a precursor solution. The mass of photoinitiator 1173 and crosslinker MBAA was 1 wt % of the total monomer mass. Both were stirred in a constant temperature magnetic stirrer at 110°C and 800 rpm for 5 min until completely dissolved and then added. The mass ratio of ionic liquid to total monomers (monomer DMAA and monomer AM) was 8:1.
[0059] (2) The uniform and transparent precursor solution was immediately transferred to a mold and cooled to room temperature, and then initiated under 365 nm ultraviolet light for 15 min to finally obtain an ionic liquid gel.
[0060] (3) Silicone rubber solution A and B (Ecoflex-00-30) were mixed in a mass ratio of 1:1 and poured into a polytetrafluoroethylene mold with a hollow structure. The bubbles were removed by vacuum in an electric constant temperature blast drying oven and cured at 65°C for 2 hours. The silicone rubber (2 mm × 4 mm) was demolded from the polytetrafluoroethylene mold and the above process was repeated to obtain two pieces of Ecoflex silicone rubber of the same size.
[0061] (4) The previously prepared ion gel was cut into pieces with a size of 15 mm × 20 mm × 2 mm and placed in the groove of the Ecoflex layer. A copper wire was connected to the surface of the ion gel. Another piece of the same silicone rubber was taken. The two silicone rubbers sandwiched the gel in the middle, encapsulated the hydrogel, and squeezed out the air to achieve close adhesion between the materials through van der Waals forces. In order to ensure the airtightness of the device, a small amount of Ecoflex-00-30 silicone rubber was used to bond the joints of the two relative silicone rubbers, and then heated and cured at 100 ° C for 1 min by a hot air gun to obtain an ion gel-based TENG with a thickness range of 4 mm.
[0062] The TENG of the present invention is based on the coupling effect of triboelectric charging and electrostatic induction. The working principle of the TENG prepared in Examples 1-4 is as follows Figure 3 As shown: When another material with different electronegativity comes into contact with the silicone rubber film, the silicone rubber has a stronger tendency to lose electrons. Due to the principle of friction charging, the charge is transferred from the surface of the red square object to the silicone rubber film, causing the surface of the red square object to be positively charged, while the surface of the silicone rubber film generates an equal amount of negative charge to achieve electrostatic balance ( Figure 3 ai). When the red square object is separated from the silicone rubber film, the electrostatic balance is broken, and the electrostatic induction causes the corresponding positive charge to be generated on the ion gel electrode, while driving the transient charge to transfer from the external circuit to the ground, generating an electrical signal ( Figure 3 aii). When the red square object is far enough away from the silicone rubber, an electrostatic equilibrium is formed and no electrical signal is generated ( Figure 3 a-iii). When the red square object approaches the silicone rubber again, the whole process will be reversed, and the positive charge induced in the ion gel electrode will be neutralized by the electrons from the ground, generating an opposite electrical signal ( Figure 3 a-iv). When the red square surface and the silicone rubber repeatedly make contact and separate movements, an alternating current is generated.
[0063] In this process, the conductive ions in the ion gel electrode play an important role in improving the output of TENG. The conductive ions further promote the charge transfer by forming another triboelectric layer at the interface between the ion gel electrode and silicone rubber, which makes the ion gel electrode have good conductivity.
[0064] Test Example 1: Gel tensile test
[0065] The gel samples prepared in Examples 1-4 were subjected to a tensile test using a texture analyzer. The size of the gel samples used for the tensile test was 20 mm×2 mm×3 mm (length×width×thickness), and the tensile rate was 50 mm / min. -1 .
[0066] The results are as follows Figure 5 As shown, when the ionic liquid gel is constructed with a higher ionic liquid content (Example 4, the mass ratio of ionic liquid to total monomer is 8:1), its formability and operability are low, and the tensile fracture stress and strain are both the lowest. When the ionic liquid gels of Examples 1 to 3 (the mass ratio of ionic liquid to total monomer is 5:1, 6:1 and 7:1) are used, the gel forming rate and operability are high. From the tensile stress-strain curve of the gel sample, as the mass ratio increases from 5:1 to 7:1, the tensile fracture strain of the ionic gel increases from 614% to 711%, and the fracture stress decreases from 196Kpa to 101Kpa. In Example 4, due to the excessively high ionic liquid concentration, the network structure of the gel becomes loose, reducing the mechanical strength and durability of the material. At the same time, the high concentration of ionic liquid increases the viscosity of the gel, making processing and handling more difficult. Operational difficulties may occur during the preparation, coating and molding process, affecting the production efficiency and the quality of TENG as a sensor.
[0067] Test Example 2: Gel conductivity test
[0068] The resistance of the samples prepared in Examples 1-4 was measured by an electrochemical workstation, and the test temperature was 26 degrees Celsius. The method used was the AC impedance method. The sample sizes of Examples 1-4 were all 5mm high and 10mm in diameter cylinders. The samples were clamped by two pieces of ITO conductive glass (20mm×40mm) and then AC impedance tests were performed using the four-probe method to obtain resistivity and conductivity data. Resistivity and conductivity are both parameters that describe the conductivity of a material. The lower the resistivity and the higher the conductivity, the better the conductivity of the material. Conductivity is represented by σ:
[0069] σ=L / R·A
[0070] Where, L is the height of the sample, in meters (m);
[0071] R is the resistance of the sample, in ohms (Ω);
[0072] A is the cross-sectional area of the sample, in square meters (m 2 ).
[0073] The test results are as follows Figure 6 As shown, the resistivity of the ion gel gradually decreases with the increase of the ionic liquid concentration, and the conductivity gradually increases with the increase of the ionic liquid concentration.
[0074] Test example 3: TENG output performance test
[0075] In order to evaluate the output performance differences of the TENG (20 mm × 40 mm) of Examples 1-4, a constant force test system was built as follows:
[0076] Copper foil (20×40mm 2 ) is used as the triboelectric layer for standard testing. The conductive copper wire of TENG as a sensor is connected to an electrometer (Keithley 6517B). The glass slide attached with copper foil generates force with the sensor to generate output voltage. The real-time data is collected and recorded through LabVIEW interface programming. The output voltage response of the sensor under the same periodic pressure (1kPa, 0.25Hz) is recorded.
[0077] The experimental results are as follows Figure 7 As shown, the sensor response is consistent with the conductivity change, and Example 4 presents the highest output voltage. The high conductivity of the ion gel helps to quickly conduct the charge, and can effectively reduce the internal resistance loss, so that the charge can move faster between the electrodes, thereby increasing the output voltage.
[0078] Test Example 4
[0079] The mechanical properties and output performance of Examples 1-4 were analyzed in combination with the data of Experimental Examples 1-3. Considering the balance between elongation and conductivity as well as the output performance of TENG, Example 3 was selected as the final example.
[0080] In order to evaluate the output performance of the TENG (20 mm × 40 mm) manufactured in Example 3, a constant force test system was built as follows:
[0081] Copper foil (20×40mm 2 ) is used as the triboelectric layer for standard testing. The conductive copper wire of TENG as a sensor is connected to an electrometer (Keithley 6517B). The glass slide attached with copper foil generates a force with the sensor to generate an output voltage. The real-time data is collected and recorded through LabVIEW interface programming.
[0082] Different contact pressures produce different output voltages. The output voltage increases with the increase of contact pressure and returns to the baseline after the pressure is released. Sensitivity is an important indicator of the sensor. It refers to the ratio of the output change to the input change of the sensor under stable working conditions, expressed by k:
[0083] k=Δy / Δx
[0084] Where Δy is the increment of output; Δx is the increment of input.
[0085] The output voltage response and sensitivity of the sensor under periodic pressure (0-40 kPa, 0.25 Hz) were recorded.
[0086] The results are as follows Figure 8As shown in the figure, the sensitivity of the sensor is about 49.83V / kPa in the range of 0–1.16kPa, and it drops rapidly to 4.02V / kPa in the range of 1.16–15.75kPa. As the pressure increases further, the output voltage reaches saturation at 15.75–33.13kPa, and the sensitivity drops to 0.31V / kPa. When the force exceeds 33.13kPa, the output voltage shows a downward trend. This is due to the large dielectric constant of the silicone rubber film and the air gap between the two layers. Under the pressure of 0 to 15.75kPa, the output voltage change during the contact-separation process is greatly enhanced. When the contact area reaches the maximum, the sensitivity begins to decrease. As the pressure continues to increase, due to the small Young's modulus of the film, the friction layer and the electrode layer will deform, and the thickness of these films will decrease. The elastic deformation of the film causes the output voltage to increase slowly. When the elastic deformation reaches saturation, continuing to apply pressure will cause the friction layer and the electrode layer to be damaged. At this time, the pressure value exceeds the maximum range of the sensor, and the output voltage shows a downward trend.
[0087] The sensor output voltage shows good linearity (R 2 =0.97), and has extremely high sensitivity and response time. As the force increases in 1.16–15.75 kPa, the sensor sensitivity decreases, reaching saturation at 15.75–33.13 kPa, and the sensitivity drops to 0.31 V / kPa. The output voltage in these two stages shows better linearity (R 2 =0.99).
[0088] In order to evaluate the electrical output performance of TENG under constant pressure and different tapping frequencies, a constant force test system was used to test the output characteristics of different frequencies. First, the constant pressure was set to 1Kpa. As the operating frequency increased from 0.25Hz to 2Hz, Voc showed a stable output. The short-circuit current (Isc) at different tapping frequencies gradually increased with the increase of frequency. This is because the high-frequency reciprocating motion shortens the contact time with the sensor, resulting in an increase in the output current. However, the number of friction charges at constant pressure is unchanged, so the output voltage remains constant.
[0089] The results are as follows Fig. 9 As shown in the figure, Voc remains basically constant during 4000 consecutive contact-separation movements, and the sensor exhibits good fatigue resistance and stable electrical output performance. At the same time, the 0-33.13kPa pressure detection range and good linearity can accurately reflect the linear relationship between the applied force and the output voltage, and has high reliability.
[0090] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A friction nanogenerator, characterized in that: The friction nanogenerator comprises an ionic liquid gel, silicone rubber attached to opposite sides of the ionic liquid gel, and a wire connecting the ionic liquid gel and the silicone rubber, wherein the silicone rubber is Ecoflex silicone rubber; the ionic liquid gel is made of the following raw materials: an ionic liquid, a monomer, a photoinitiator, and a crosslinking agent; The ionic liquid is 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, the monomer is selected from at least one of N,N-dimethylacrylamide or acrylamide; the photoinitiator is initiator 1173, and the crosslinker is methylenebisacrylamide; The mass ratio of the ionic liquid, the monomer, the photoinitiator and the cross-linking agent is (1-10):1:(0.0001-0.05):(0.0001-0.05).
2. The method for preparing the triboelectric nanogenerator according to claim 1, characterized in that: The following steps are involved: (1) mixing an ionic liquid, a monomer, a photoinitiator and a cross-linking agent, heating and stirring to obtain a precursor solution, and subjecting the precursor solution to ultraviolet light reaction to obtain an ionic liquid gel; (2) Prepare silicone rubber, connect wires to the silicone rubber, and sandwich the ionic liquid gel between two pieces of silicone rubber to obtain a friction nanogenerator.
3. The method for preparing the friction nanogenerator according to claim 2, characterized in that: The mass ratio of the ionic liquid to the monomer is (5-8):1, and the sum of the mass of the photoinitiator and the crosslinking agent accounts for (0.1-5)% of the mass of the monomer.
4. The method for preparing the triboelectric nanogenerator according to claim 2, characterized in that: In step (1), in the monomers, the mass ratio of N,N-dimethylacrylamide to acrylamide is (1-10):
1.
5. The method for preparing the triboelectric nanogenerator according to claim 2, characterized in that: In step (1), the heating and stirring temperature is 90-130° C., the stirring speed is 400-1500 rpm, and the stirring time is 1-10 min.
6. The method for preparing the triboelectric nanogenerator according to claim 2, characterized in that: In step (1), the wavelength of ultraviolet light used is 365nm, and the irradiation time is 5-30min.
7. The method for preparing the triboelectric nanogenerator according to claim 2, characterized in that: In step (2), the ionic liquid gel and two pieces of silicone rubber are clamped together by van der Waals force.
8. The method for preparing the triboelectric nanogenerator according to claim 2, characterized in that: In step (2), after the ionic liquid gel is sandwiched between two pieces of silicone rubber, Ecoflex-00-30 silicone rubber is used to connect the junction of the ionic liquid gel and the Ecoflex silicone rubber, and heated and cured at a temperature of 90-110° C. for 0.5-5 minutes.
9. A friction self-powered flexible force sensing sensor based on conductive ion gel, characterized in that: The friction self-powered flexible force sensing sensor includes the friction nanogenerator described in claim 1.
10. Application of the friction self-powered flexible force sensing sensor based on conductive ion gel as described in claim 9 in the manufacture of flexible manipulators.
Citation Information
Patent Citations
Piezoelectric-triboelectric composite sensor based on flexible porous PVDF-BTO film and preparation method of piezoelectric-triboelectric composite sensor
CN114221572A
Preparation method and application of polyvinyl alcohol / liquid metal hydrogel single-electrode flexible friction nano-generator
CN116566237A
A-PAA / KOH / KB hydrogel friction nano-generator and preparation method and application thereof
CN118199436A
Polymer gel for triboelectric nanogenerator comprising ionic liquid, and triboelectric nanogenerator comprising same
WO2024123062A1
KR20240118035A
Cited By
Self-power-generation sensing sensor, mechanical claw and mechanical claw clamping force sensing method
CN119880204A
Triboelectric hemispherical composite film pressure sensing device and control method thereof
CN121298097A