Preparation method and application of hollow porous cuprous oxide and copper micro-nanosphere catalyst
By preparing hollow porous copper oxide @ copper micro-nanosphere catalyst, the problems of high cost of electroplating wastewater treatment, high energy consumption and poor stability of photocatalytic materials are solved, and the resource regeneration of electroplating wastewater and the improvement of photocatalytic efficiency are achieved.
Patent Information
- Application Number
- CN202411168318.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-03
AI Technical Summary
The existing electroplating wastewater treatment technology has problems such as high treatment costs, possible secondary pollution, high energy consumption and low quality of the copper products obtained, and the existing photocatalytic materials have low catalytic efficiency and poor stability.
The preparation method of hollow porous copper oxide @ copper micro-nanosphere catalyst is adopted. By dissolving styrene and polyvinylpyrrolidone and mixing with electroplating copper waste liquid for reduction reaction, polystyrene microspheres supported by copper and copper oxide are formed. The polystyrene template was removed by centrifugation to obtain hollow porous copper oxide @ copper micro-nanosphere catalyst, used for electroplating wastewater treatment and photocatalytic carbon dioxide.
It effectively reduces the cost of electroplating wastewater treatment, avoids secondary pollution, improves photocatalytic efficiency and material stability, improves the quality of copper products, and realizes the resource regeneration of electroplating wastewater.
Smart Images

Figure CN119056449A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electroplating wastewater treatment, and more specifically to a preparation method of a hollow porous cuprous oxide@copper micro-nanosphere catalyst and its application. Background Art
[0002] With the continuous improvement of environmental awareness and the development of science and technology, electroplating wastewater treatment has become an important bottleneck in the development of the industry. Therefore, advanced technology is needed to inject new vitality into the development of the electroplating industry. Nanomaterials are widely used in various fields due to their unique physical and chemical properties. Among them, nano-scale polyethylene balls are a new type of nanomaterial with good stability and biocompatibility, and are widely used in drug delivery, bioimaging and other fields. At the same time, electroplating wastewater treatment is an important topic in the field of environmental protection. How to effectively treat low-concentration copper ions and realize resource recycling is a hot topic in current research.
[0003] Existing electroplating wastewater treatment technologies mainly include chemical precipitation, ion exchange, adsorption, etc. These methods can effectively remove copper ions in wastewater and achieve standard discharge of wastewater. However, these methods often require the consumption of a large amount of chemical reagents, are costly, and may cause secondary pollution. In addition, there are some methods that convert copper ions into copper elements by electrolysis or chemical reduction to achieve copper recovery, but usually require high energy consumption, and the quality of the resulting copper products is not high.
[0004] In summary, electroplating wastewater treatment technology has the following main problems: first, high treatment cost, second, possible secondary pollution, third, high energy consumption, and fourth, the quality of the copper products obtained is not high. In addition, although the existing photocatalytic materials can effectively catalyze the conversion of carbon dioxide into methane or carbon monoxide, their catalytic efficiency needs to be improved, and their stability is poor and they are easily deactivated.
[0005] Therefore, how to use technology to make high-quality use of resources to prepare photocatalytic materials and realize the resource regeneration of electroplating wastewater is an important challenge facing current technology. Summary of the invention
[0006] The purpose of the present invention is to provide a preparation method and application of a hollow porous cuprous oxide@copper micro-nanosphere catalyst in order to solve the problem that electroplating wastewater in a centralized control area contains alkaline copper heavy metal ions and is difficult to effectively recycle.
[0007] To achieve the above object, the technical solution of the present invention is as follows:
[0008] A method for preparing a hollow porous cuprous oxide@copper micro-nanosphere catalyst comprises the following steps:
[0009] (1) dissolving styrene and polyvinyl pyrrolidone in a solvent, adding an initiator and a surfactant to polymerize, and obtaining a polystyrene microsphere suspension;
[0010] (2) adjusting the pH of the copper electroplating waste liquid to 9-10, and mixing it with the polystyrene microsphere suspension and a strong reducing agent to carry out a reduction reaction, so that copper and cuprous oxide are loaded on the surface of the polystyrene microspheres, thereby obtaining polystyrene microspheres loaded with copper and cuprous oxide;
[0011] (3) centrifuging the polystyrene microspheres loaded with copper and cuprous oxide, and using an organic solvent to dissolve the polystyrene microsphere template in the obtained centrifugal product to obtain the hollow porous cuprous oxide@copper micro-nanosphere catalyst.
[0012] The invention also discloses a hollow porous cuprous oxide@copper micro-nanosphere catalyst prepared by the above-mentioned preparation method.
[0013] The present invention also discloses a hollow porous cuprous oxide@copper micro-nanosphere catalyst prepared by the above preparation method, or the use of the hollow porous cuprous oxide@copper micro-nanosphere catalyst in photocatalytic carbon dioxide reduction.
[0014] Implementing the embodiments of the present invention will have the following beneficial effects:
[0015] The present invention combines micro-nano polystyrene balls with electroplating copper waste liquid, reduces and adsorbs copper ions on the surface of the polystyrene balls twice to obtain a hollow porous cuprous oxide / copper shell core structure, which can effectively reduce the cost of electroplating wastewater treatment and avoid secondary pollution. At the same time, the present invention has a simple preparation process, low cost, reduced energy consumption, stable process, high production efficiency, and easy control.
[0016] The hollow porous cuprous oxide@copper micro-nanospheres prepared by the present invention are used as photocatalytic materials for photocatalytically converting carbon dioxide into methane or carbon monoxide, which can not only improve the photocatalytic efficiency, but also improve the stability of the photocatalytic material, thereby solving the problems of low catalytic efficiency, poor stability, and easy deactivation of existing photocatalytic materials.
[0017] The present invention prepares micro-nano photocatalytic materials based on electroplating copper waste liquid, can achieve high-quality conversion of waste, thereby realizing resource regeneration of electroplating wastewater, and can improve the quality of copper products, solving the problems of electroplating wastewater treatment cost, high energy consumption, secondary pollution, and low quality of the obtained copper products in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The present invention is a flow chart of the preparation process of the hollow porous cuprous oxide@copper micro-nanosphere catalyst. DETAILED DESCRIPTION
[0019] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited in any way.
[0020] The present invention discloses a method for preparing a hollow porous cuprous oxide@copper micro-nanosphere catalyst, comprising the following steps:
[0021] (1) Styrene and polyvinyl pyrrolidone are dissolved in a solvent, and an initiator and a surfactant are added to polymerize to obtain a polystyrene microsphere suspension.
[0022] (2) The copper electroplating waste liquid is adjusted to a pH of 9 to 10, and mixed with polystyrene microspheres and a strong reducing agent for a reduction reaction, so that copper and cuprous oxide are loaded on the surface of the polystyrene microspheres, thereby obtaining polystyrene microspheres loaded with copper and cuprous oxide.
[0023] (3) The polystyrene microspheres loaded with copper and cuprous oxide are centrifuged, and the polystyrene microsphere template is removed from the obtained centrifugal product by dissolving it with an organic solvent to obtain a hollow porous cuprous oxide@copper micro-nanosphere catalyst.
[0024] In a specific embodiment, in step (1), the initiator includes one or more of potassium persulfate, ammonium persulfate, sodium persulfate, potassium thiosulfate, sodium thiosulfate, and azobisisobutyronitrile; the surfactant includes one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, and sodium fatty alcohol alkyl sulfonate; and the solvent includes one or more of water, N,N-dimethylformamide, N,N-dimethylacetamide, acetone, xylene, dichloromethane, and chloroform.
[0025] In a specific embodiment, step (2) specifically includes the following steps:
[0026] (2.1) The pH of the electroplating copper waste liquid is adjusted to 9-10 by adding ammonia water to obtain an alkaline electroplating copper waste liquid.
[0027] (2.2) In a nitrogen protective atmosphere, polystyrene microspheres and alkaline copper electroplating waste liquid are mixed, and a first strong reducing agent is added to carry out a reduction reaction at 70° C. to 80° C. for 0.5 h to 1 h, so that elemental copper is adsorbed on the surface of the polystyrene microspheres to obtain polystyrene microspheres loaded with elemental copper.
[0028] (2.3) Stop nitrogen protection, mix the polystyrene microspheres loaded with copper and the second strong reducing agent at 70°C to 80°C for a secondary reduction reaction for 0.5h to 1h, so that cuprous oxide is loaded on the surface of the polystyrene microspheres loaded with copper, thereby obtaining polystyrene microspheres loaded with copper and cuprous oxide.
[0029] In a specific embodiment, in step (2), the mass ratio of polystyrene microspheres, alkaline copper electroplating waste liquid, the first strong reducing agent and the second strong reducing agent is (1-5): (1-5): (0.5-2.5): (0.5-2.5).
[0030] In a specific embodiment, in step (2), the concentration of copper ions in the electroplating copper waste liquid is 10 mg / L to 50 mg / L.
[0031] In a specific embodiment, in step (2), the first strong reducing agent and the second strong reducing agent respectively include one or more of sodium borohydride, hydrazine hydrate, and ascorbic acid.
[0032] In a specific embodiment, in step (1), the mass ratio of styrene, polyvinyl pyrrolidone, initiator and surfactant is (50-100): (5-10): (0.1-0.5): (1-2); the polymerization temperature is 70°C-90°C; and the polymerization time is 12h-24h.
[0033] In a specific embodiment, in step (3), the organic solvent includes one or more of N,N-dimethylformamide, N,N-dimethylacetamide, acetone, xylene, dichloromethane, and chloroform.
[0034] The present invention also discloses a hollow porous cuprous oxide@copper micro-nanosphere catalyst prepared by the preparation method of any embodiment of the present invention.
[0035] In one specific embodiment, the specific surface area of the hollow porous cuprous oxide@copper micro-nanosphere catalyst is 10 m 2 / g~20m 2 / g.
[0036] In a specific embodiment, the particle size of the hollow porous cuprous oxide@copper micro-nanosphere catalyst is 0.5 μm to 3 μm.
[0037] In a specific embodiment, the porosity of the hollow porous cuprous oxide@copper micro-nanosphere catalyst is 40% to 70%.
[0038] In a specific embodiment, the pore size of the hollow porous cuprous oxide@copper micro-nanosphere catalyst is 50 nm to 300 nm.
[0039] The present invention also discloses an application of a hollow porous cuprous oxide@copper micro-nanosphere catalyst prepared by the preparation method of any embodiment of the present invention in photocatalytic carbon dioxide reduction.
[0040] The following are specific embodiments
[0041] Example 1
[0042] The preparation method of the hollow porous cuprous oxide@copper micro-nanosphere catalyst of this embodiment comprises the following steps:
[0043] Step 1: Dissolve 1 g of styrene in 100 mL of 0.5 wt% PVP solution, add 0.3 g of surfactant (sodium dodecyl sulfate), control the temperature at 80°C, stir for 0.5 h, then quickly add 5 mmol / L potassium persulfate as an initiator, react for 12 h, and cool to room temperature to obtain an emulsion solution A which is a monodisperse colloidal polystyrene sphere.
[0044] Step 2: Take 100mL of 50mg / L electroplating copper waste liquid and adjust the pH to 10 with ammonia water, mix the micro-nano polystyrene balls and alkaline electroplating copper waste water in a ratio of 1:1, introduce nitrogen for 10 minutes, keep the temperature at 80°C, add 50mL of 1mol / L sodium borohydride and continue stirring for 0.5h, so that a copper inner layer is adsorbed on the surface of the polystyrene balls, stop passing nitrogen protection, and then add 50mL of 0.5mol / L ascorbic acid (AA) for secondary reduction reaction and deposition for 0.5h to obtain an outer layer of cuprous oxide.
[0045] Step 3: After centrifuging the above solution to remove the solvent, add it into 50 mL of N,N-dimethylformamide solution and react for 0.5 h to remove polystyrene, forming a hollow porous core-shell Cu2O / Cu structure, and obtaining a hollow porous cuprous oxide@copper micro-nanosphere catalyst.
[0046] Example 2
[0047] The preparation method of the hollow porous cuprous oxide@copper micro-nanosphere catalyst of this embodiment comprises the following steps:
[0048] Step 1: Dissolve 1 g of styrene in 100 mL of 1 wt% PVP solution, add 0.2 g of surfactant (sodium dodecyl sulfate), control the temperature at 75°C, stir for 1 h, then quickly add 5 mmol / L potassium persulfate as an initiator, react for 18 h, and cool to room temperature to obtain an emulsion solution A which is a monodisperse colloidal polystyrene sphere.
[0049] Step 2: Take 100mL of 50mg / L electroplating copper waste liquid and adjust the pH to 9 with ammonia water, mix the micro-nano polystyrene balls and alkaline electroplating copper waste water in a ratio of 1:1, introduce nitrogen for 10 minutes, keep the temperature at 80°C, add 50mL of 1mol / L sodium borohydride and continue stirring for 0.5h, so that a copper inner layer is adsorbed on the surface of the polystyrene balls, stop passing nitrogen protection, and then add 50mL of 0.5mol / L ascorbic acid (AA) for secondary reduction reaction and deposition for 0.5h to obtain an outer layer of cuprous oxide.
[0050] Step 3: After centrifuging the above solution to remove the solvent, add 50 mL of N, N-dimethylacetamide solution to react for 0.5 h to remove polystyrene, form a hollow porous core-shell Cu2O / Cu structure, and obtain a hollow porous cuprous oxide@copper micro-nanosphere catalyst.
[0051] Example 3
[0052] The preparation method of the hollow porous cuprous oxide@copper micro-nanosphere catalyst of this embodiment comprises the following steps:
[0053] Step 1: Dissolve 5 g of styrene in 100 mL of 5 wt% PVP solution, add 0.5 g of surfactant (sodium fatty alcohol alkyl sulfonate), control the temperature at 70°C, stir for 0.5 h, then quickly add 10 mmol / L ammonium persulfate as an initiator, react for 24 h, and cool to room temperature to obtain an emulsion solution A which is a monodisperse colloidal polystyrene sphere.
[0054] Step 2: Take 100mL of 20mg / L electroplating copper waste liquid and adjust the pH to 10 with ammonia water, mix the micro-nano polystyrene balls and alkaline electroplating copper waste water in a ratio of 1:1, introduce nitrogen for 10 minutes, keep the temperature at 70°C, add 50mL of 1mol / L sodium borohydride and continue stirring for 1h, so that a copper inner layer is adsorbed on the surface of the polystyrene balls, stop nitrogen protection, and then add 50mL of 0.5mol / L ascorbic acid (AA) for secondary reduction reaction and deposition for 0.5h to obtain an outer layer of cuprous oxide.
[0055] Step 3: After centrifuging the above solution to remove the solvent, add it into 100 mL of acetone solution and react for 0.5 h to remove polystyrene, forming a hollow porous core-shell Cu2O / Cu structure, and obtaining a hollow porous cuprous oxide@copper micro-nanosphere catalyst.
[0056] Test Case
[0057] 1. The structure of the hollow porous cuprous oxide@copper micro-nanosphere catalyst prepared in Examples 1-3 was tested, and the results are shown in Table 1.
[0058] Table 1 Average particle size and pore size distribution of different samples
[0059]
[0060] 2. The catalysts obtained in Examples 1-3 and the existing catalysts were used for photocatalytic carbon dioxide reduction reaction. The specific operation was to expose the hollow porous cuprous oxide / copper micro-nanospheres to light with an intensity of 1000 W / m 2 The illumination time is 2 hours. The test results are shown in Table 2.
[0061] Table 2 Different samples C2+ Comparison of conversion rates
[0062]
[0063] According to the results in Table 1, in the process of photocatalytic reduction of CO2, compared with the existing catalysts, Examples 1-3 show higher photocatalytic efficiency in photocatalytic reduction of CO2. It can be seen that the photocatalytic performance of the catalyst proposed in the present invention is significantly improved, thereby proving that the composite material obtained in the present invention has good catalytic activity for photocatalytic reduction of carbon dioxide.
[0064] In summary, the present invention combines micro-nano polystyrene balls with electroplating copper waste liquid, and reduces and adsorbs copper ions twice on the surface of polystyrene balls to obtain a hollow porous cuprous oxide / copper shell core structure, which can effectively reduce the cost of electroplating wastewater treatment and avoid secondary pollution. At the same time, the preparation process of the present invention is simple, low in cost, reduces energy consumption, has a stable process, high production efficiency, and is easy to control. The hollow porous cuprous oxide-copper micro-nano balls prepared by the present invention are used as photocatalytic materials for photocatalytic conversion of carbon dioxide into methane or carbon monoxide, which can not only improve the photocatalytic efficiency, but also improve the stability of the photocatalytic materials, solving the problems of low catalytic efficiency, poor stability, and easy inactivation of existing photocatalytic materials. The present invention prepares micro-nano photocatalytic materials based on electroplating copper waste liquid, can achieve high-quality conversion of waste, thereby realizing resource regeneration of electroplating wastewater, and can improve the quality of copper products, solving the problems of electroplating wastewater treatment cost, high energy consumption, secondary pollution, and low quality of the obtained copper products in the prior art.
[0065] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a hollow porous cuprous oxide@copper micro-nanosphere catalyst, characterized in that: The following steps are involved: (1) dissolving styrene and polyvinyl pyrrolidone in a solvent, adding an initiator and a surfactant to polymerize, and obtaining a polystyrene microsphere suspension; (2) adjusting the pH of the copper electroplating waste liquid to 9-10, and mixing it with the polystyrene microsphere suspension and a strong reducing agent to carry out a reduction reaction, so that copper and cuprous oxide are loaded on the surface of the polystyrene microspheres, thereby obtaining polystyrene microspheres loaded with copper and cuprous oxide; (3) centrifuging the polystyrene microspheres loaded with copper and cuprous oxide, and using an organic solvent to dissolve the polystyrene microsphere template in the obtained centrifugal product to obtain the hollow porous cuprous oxide@copper micro-nanosphere catalyst.
2. The method for preparing the hollow porous cuprous oxide@copper micro-nanosphere catalyst according to claim 1, characterized in that: The specific surface area of the hollow porous cuprous oxide@copper micro-nanosphere catalyst is 10m 2 / g~20m 2 / g; The particle size of the hollow porous cuprous oxide@copper micro-nanosphere catalyst is 0.5 μm to 3 μm; The porosity of the hollow porous cuprous oxide@copper micro-nanosphere catalyst is 40% to 70%; The pore size of the hollow porous cuprous oxide@copper micro-nanosphere catalyst is 50nm to 300nm.
3. The method for preparing the hollow porous cuprous oxide@copper micro-nanosphere catalyst according to claim 1, characterized in that: Step (2) specifically includes the following steps: The electroplating copper waste liquid is adjusted to a pH of 9 to 10 by adding ammonia water to obtain an alkaline electroplating copper waste liquid; In a nitrogen protective atmosphere, the polystyrene microsphere suspension and the alkaline copper electroplating waste liquid are mixed, and a first strong reducing agent is added to carry out a reduction reaction at 70° C. to 80° C. for 0.5 h to 1 h, so that the surface of the polystyrene microspheres adsorbs elemental copper to obtain polystyrene microspheres loaded with elemental copper; Stop nitrogen protection, mix the polystyrene microspheres loaded with copper and the second strong reducing agent at 70° C. to 80° C. for a secondary reduction reaction for 0.5 h to 1 h, so that cuprous oxide is loaded on the surface of the polystyrene microspheres loaded with copper, to obtain the polystyrene microspheres loaded with copper and cuprous oxide.
4. The method for preparing the hollow porous cuprous oxide@copper micro-nanosphere catalyst according to claim 3, characterized in that: In step (2), the mass ratio of the polystyrene microsphere suspension, the copper ions in the alkaline copper electroplating waste liquid, the first strong reducing agent and the second strong reducing agent is (1-5): (1-5): (0.5-2.5): (0.5-2.5).
5. The method for preparing the hollow porous cuprous oxide@copper micro-nanosphere catalyst according to claim 3, characterized in that: In step (2), the concentration of copper ions in the electroplating copper waste liquid is 10 mg / L to 50 mg / L.
6. The method for preparing the hollow porous cuprous oxide@copper micro-nanosphere catalyst according to claim 3, characterized in that: In step (2), the first strong reducing agent and the second strong reducing agent respectively include one or more of sodium borohydride, hydrazine hydrate and ascorbic acid.
7. The method for preparing the hollow porous cuprous oxide@copper micro-nanosphere catalyst according to claim 1, characterized in that: In step (1), the mass ratio of styrene, polyvinyl pyrrolidone, initiator and surfactant is (50-100): (5-10): (0.1-0.5): (1-2); the polymerization temperature is 70° C. to 90° C.; the polymerization time is 12 h to 24 h; In step (1), the initiator includes one or more of potassium persulfate, ammonium persulfate, sodium persulfate, potassium thiosulfate, sodium thiosulfate, and azobisisobutyronitrile; The surfactant includes one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, and sodium fatty alcohol alkyl sulfonate; The solvent includes one or more of water, N,N-dimethylformamide and N,N-dimethylacetamide.
8. The method for preparing the hollow porous cuprous oxide@copper micro-nanosphere catalyst according to claim 1, characterized in that: In step (3), the organic solvent includes one or more of N,N-dimethylformamide, N,N-dimethylacetamide, acetone, xylene, dichloromethane and chloroform.
9. A hollow porous cuprous oxide@copper micro-nanosphere catalyst prepared by the preparation method according to any one of claims 1 to 8.
10. Use of a hollow porous cuprous oxide@copper micro-nanosphere catalyst prepared by the preparation method according to any one of claims 1 to 8, or a hollow porous cuprous oxide@copper micro-nanosphere catalyst according to claim 9 in photocatalytic carbon dioxide reduction.
Citation Information
Cited By
Preparation method and application of cuprous oxide hollow nano-microspheres
CN119980311A
Recyclable porous copper / cuprous oxide filamentous catalytic material and preparation method thereof
CN120443229A
Preparation method and application of fern-leaf-shaped Cu-coated Cu2O nano composite material based on liquid metal induction
CN122559212A